Method for producing fibrous webs containing fluorinated copolymers

By using environmentally friendly solvents such as γ-valerol to mix with PVDF copolymers, PVDF copolymer fibers with high β-phase content are produced by electrospinning, solving the problems of health hazards and insufficient performance, and realizing the production of environmentally friendly and efficient filter materials.

CN123076434APending Publication Date: 2026-11-10ARKEMA FRANCE SA +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580027152.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-29
Filing Date
2025-04-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing electrospinning methods use solvents such as DMF, NMP, and DMAC that are harmful to health and make it difficult to obtain a high proportion of β-phase PVDF fibers to improve ferroelectric properties, thus failing to meet the needs of green environmental protection and filtration devices.

Method used

PVDF copolymer fibers are produced by electrospinning using γ-valerol and other low-boiling-point solvents such as acetone and dimethyl carbonate, resulting in a fiber web with a high β-phase content.

Benefits of technology

PVDF copolymer fibers with high crystallinity and high β-phase content were obtained, which improved the ferroelectric properties of the fiber network. Furthermore, environmentally friendly bio-based solvents were used, making the fibers suitable for filtration devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076434A_ABST
    Figure CN123076434A_ABST
Patent Text Reader

Abstract

This invention relates to a method for producing fibrous webs by electrospinning a solution of a fluorinated polymer, the fibrous web comprising fibers based on a copolymer of repeating units derived from vinylidene fluoride (VDF). The invention also relates to fibrous webs obtainable using the described method. Finally, the invention relates to various applications of the fibrous webs as filtration devices for filtering air and / or liquids.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for producing fibrous webs by electrospinning a solution of a fluoropolymer, the fibrous web comprising fibers based on a copolymer of repeating units derived from vinylidene fluoride (VDF). The invention also relates to fibrous webs obtainable by this method. Finally, the invention relates to various applications of the fibrous webs intended for use as filtration devices for filtering air and / or liquids. Background Technology

[0002] Electrospinning is an electrohydrodynamic method that allows the production of polymer nanofibers from one or more polymer solutions by applying a high electrostatic field. The resulting submicron diameter fibers accumulate to form a fibrous web.

[0003] Submicron-diameter poly(vinylidene fluoride-copoly-hexafluoropropylene) (P(VDF-HFP)) fibers are used in various fields, such as filtration, due to their chemical resistance and good heat resistance. Currently, the main solvents used in the electrospinning of P(VDF-HFP) are N,N-dimethylacetamide (DMAC), dimethylformamide (DMF), and N-methylpyrrolidone (NMP), which are hazardous solvents and classified as Substances of Very High Concern (SVHC) by the European Chemicals Agency (ECHA). DMF, NMP, and DMAC are labeled "H360D - May harm an unborn fetus." Therefore, they are considered CMR solvents (carcinogenic, mutagenic, or reproductively toxic).

[0004] P(VDF-HFP) is a semi-crystalline thermoplastic copolymer that exhibits a complex structure depending on the chain conformation, attributed to five crystalline phases: α, β, γ, δ, and e. The β phase is the most polar phase and exhibits piezoelectric, thermoelectric, and ferroelectric properties. Gade wait people The publication "Effect of electrospinning conditions on β-phase and surface charge potential of PVDF fibers", Polymer, 2021, vol. 228, p. 123902, describes that the presence of the β-phase in PVDF homopolymer fibers is particularly advantageous for aerosol filtration applications because it allows the generation of charges attached to the material and thus improves the efficiency of electrostatic filtration (higher electrostatic efficiency compared to fibers of nonferroelectric dielectric materials).

[0005] Andrew et al.The publication "Effect of electrospinning on the ferroelectric phase content of polyvinylidene difluoride fibers", Langmuir, 2008, vol. 24, no. 3, pp. 670-672, describes the electrospinning of PVDF homopolymer solutions in DMF. By varying certain parameters of the method, specifically the concentration of PVDF homopolymer in the solution and the voltage applied during electrospinning, the authors successfully obtained a network of PVDF homopolymer fibers with a crystallinity of 49% to 58%, and a β-phase percentage of up to 75% in the crystalline phase. Therefore, the obtained fibers have a β-phase content of 37% to 47% by weight, relative to the weight of the fibers.

[0006] To improve the durability of electrospinning technology, a suitable strategy is to use solvents with low toxicity and bio-based properties (i.e., alternative green solvents).

[0007] In document WO 2021 / 255389, the applicant describes a method for producing nonwoven webs of PVDF homopolymer or copolymer fibers by electrospinning a solution or homopolymer dispersion, wherein the solution or homopolymer dispersion comprises at least 15% by weight of dimethyl sulfoxide and at least one second liquid having a pressure of 7 MPa. 1 / 2 Up to 15 MPa 1 / 2 It has the Hansen solubility parameter δp and a boiling point strictly above 100°C. DMSO is a green solvent with a melting point of 18°C, which limits its use in methods that operate at room temperature (e.g., electrospinning) due to the risk of polymer solution gelation.

[0008] It is still necessary to provide an electrospinning method using a liquid carrier, which is not considered carcinogenic, mutagenic, or reproductively toxic based on its composition.

[0009] An electrospinning method is also required, which provides a means of obtaining a fibrous web with a high proportion of β phase (relative to the weight of the fiber) in order to improve the ferroelectric properties of the web.

[0010] A method for obtaining fibrous meshes intended for use as filtration devices also needs to be proposed.

[0011] Another object of the present invention (at least according to some embodiments) is to provide an electrospinning method that provides a means of obtaining a fibrous web having a larger proportion of β phase (relative to the weight of the fiber) in order to improve the ferroelectric properties of the web. Summary of the Invention

[0012] The present invention relates to a method for producing a nonwoven web of PVDF copolymer fibers by electrospinning a solution comprising the fluorinated copolymer dissolved in a solvent mixture, characterized in that the mixture comprises a first solvent (which is γ-valerol (GVL)) and a second solvent (which is a solvent mixture or a pure solvent having a boiling point below 100°C).

[0013] Typically, the second solvent is selected from acetone, dimethyl carbonate (DMC), methyl ethyl ketone (MEK), 2-methyltetrahydrofuran (2MTHF), or mixtures thereof.

[0014] Advantageously, none of the compositions of the solutions used to dissolve PVDF copolymers are considered carcinogenic, mutagenic, or reproductively toxic (CMR).

[0015] According to one embodiment, the solution has a Brinell viscosity of 50 to 3000 cP, preferably 75 to 1500 cP, and more preferably 80 to 500 cP at 20°C, as measured according to standard ASTM D1238-13. According to one embodiment, the PVDF copolymer accounts for 6% to 25% by weight, preferably 10% to 21% by weight, relative to the total weight of the solution.

[0016] PVDF copolymers are copolymers having repeating units derived from VDF and at least one repeating unit derived from monomers other than VDF, wherein the other monomers are selected from the following list: vinyl fluoride (VF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), vinyl chlorofluoroethylene (CFE), dichlorofluoroethylene, trichlorofluoroethylene (CTFE), dichlorodifluoroethylene, trichlorofluoroethylene, hexafluoropropylene (HFP), trifluoropropylene, tetrafluoropropylene, trichlorofluoropropylene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropylene, perfluoroethers, especially perfluoroalkyl vinyl ethers, ethylene, acrylic monomers, methacrylic monomers, and mixtures thereof.

[0017] According to one embodiment, the fluorinated copolymer is a P(VDF-HFP) copolymer.

[0018] The present invention also relates to a fibrous web that can be obtained by electrospinning, wherein the P(VDF-HFP) web is characterized by a crystallinity of 29% to 34% (a degree determined by DSC from the melting enthalpy of P(VDF-HFP) at 104.5 J / g) and a percentage of the β phase in the crystalline phase between 41% and 69% (a content determined by infrared spectroscopy).

[0019] The present invention also relates to the use of the PVDF copolymer fiber mesh intended for use as a filtration device.

[0020] This invention overcomes the shortcomings of existing technologies. The use of γ-valerol for electrospinning PVDF copolymers is a more sustainable and improved approach for producing fluoropolymer fiber webs. γ-valerol is a sustainable solvent derived from biomass and is not classified as a reproductively toxic CMR solvent. Attached Figure Description

[0021] [ Figure 1 The diagram schematically illustrates a reactor used to prepare an electrospinning solution intended for use in the method according to the invention.

[0022] [ Figure 2 [Image showing a scanning electron microscope (SEM) image obtained by electrospinning a fiber web according to the invention, the fiber web being obtained from a mixture of γ-valerolactone and acetone solvent (see embodiments according to the invention).] Detailed Implementation

[0023] Endpoints are included in the entire scope listed in this patent application unless otherwise stated.

[0024] The fluorinated copolymer used in the method according to the invention is based on repeating units derived from vinylidene fluoride (VDF). The proportion of repeating units derived from VDF is at least 50 mol%, relative to the total number of moles of repeating units in the fluorinated polymer.

[0025] According to some embodiments, the fluorinated copolymer comprises at least 60 mol%, or at least 70 mol%, or at least 75 mol%, or at least 80 mol%, or at least 85 mol%, or at least 90 mol%, or at least 95 mol% of units derived from VDF. The term "polymer" refers to a polymer obtained by copolymerization of at least two chemically different monomers (referred to as comonomers).

[0026] The copolymer has repeating units derived from VDF and repeating units derived from at least one monomer other than VDF, wherein the comonomer is selected from the following list: vinyl fluoride (VF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), vinyl chlorofluoroethylene (CFE), dichlorofluoroethylene, trifluorochloroethylene (CTFE), dichlorodifluoroethylene, trichlorofluoroethylene, hexafluoropropylene (HFP), trifluoropropylene, tetrafluoropropylene, chlorotrifluoropropylene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropylene, perfluoroethers (especially perfluoroalkyl vinyl ethers), ethylene, acrylic monomers, methacrylic monomers, and mixtures thereof.

[0027] It should be clearly understood that all geometric isomers of the fluorinated compounds mentioned above are included in the above terminology, such as: 1,1-chlorofluoroethylene (1,1-CFE), 1,2-chlorofluoroethylene (1,2-CFE), 1,2-dichloro-1,2-difluoroethylene, 1,1-dichloro-1,1-difluoroethylene and 1,1,2-trichloro-2-fluoroethylene, 3,3,3-trifluoropropylene, 2-chloro-3,3, 3-Trifluoropropene (1233xf), 1-chloro-3,3,3-trifluoropropene (1233zd), 1,3,3,3-tetrafluoropropene, 2,3,3,3-tetrafluoropropene (or 1234yf), 3-chloro-2,3,3-trifluoropropene (or 1233yf), 3-chloro-3,3,3-trifluoropropene, 1,1,3,3,3-pentafluoropropene or 1,2,3,3,3-pentafluoropropene.

[0028] Among perfluoroalkyl vinyl ethers, those of the general formula can be mentioned: R f -O-CF-CF2, R f It is an alkyl group, preferably a C1 to C4 alkyl group, and for example, methyl vinyl ether (MVE) or isopropyl vinyl ether (PVE).

[0029] According to certain variants, the fluorinated copolymer is a mixture of one or more copolymers selected from: P(VDF-TrFE), P(VDF-HFP), P(VDF-TFE), P(VDF-TrFE-CFE), P(VDF-TrFE-CTFE), P(VDF-TFE-CFE), and P(VDF-TFE-CTFE).

[0030] According to one embodiment, the fluoropolymer is a P(VDF-HFP) copolymer. P(VDF-HFP) advantageously has a molar proportion of 5% to 35% repeating units derived from HFP.

[0031] Fluoropolymer solution

[0032] The fluoropolymer solution comprises the polymer dissolved in a solvent mixture, the mixture comprising a first solvent (which is γ-valerol (GVL)) and a second solvent (which is a solvent mixture or a pure solvent having a boiling point below 100°C).

[0033] Advantageously, the second solvent is selected from acetone, dimethyl carbonate (DMC), methyl ethyl ketone (MEK), 2-methyltetrahydrofuran (2MTHF), or mixtures thereof.

[0034] The solvent mixture can dissolve the polymer to form a true solution (i.e., a single-phase or homogeneous solution at the molecular level); in this way, it is easier to obtain nonwoven webs of PVDF copolymer fibers with a high proportion of β phase.

[0035] The mass content of the first solvent is between 10% and 70%, preferably between 30% and 50%, relative to the weight of the solution. The mass content of the PVDF copolymer is between 6% and 25%, preferably between 10% and 21%, relative to the weight of the solution.

[0036] The preparation of electrospinning solutions involves dissolving PVDF copolymers in a solvent mixture.

[0037] According to one implementation method, such as Figure 1 As shown, first and second solvents (or solvent mixtures) are introduced into an 8 L jacketed vertical reactor equipped with a three-bladed propeller agitator and a condenser. The PVDF copolymer, in powder form, is slowly introduced into the solvent under mechanical stirring. Dissolution is carried out under thermal conditions and with stirring at temperatures between 30 and 70°C.

[0038] The hydrodynamic conditions depend on the type of agitator used. Agitators that promote axial flow are particularly preferred. The agitation time is typically from 30 minutes to 24 hours. The agitation time is preferably less than or equal to 12 hours, more preferably less than or equal to 6 hours, and most preferably less than or equal to 4 hours.

[0039] According to one embodiment, the PVDF copolymer in powder form is dissolved in a solvent mixture over a time range of 1 to 5 hours at a temperature between 30 and 70°C.

[0040] When all particles have dissolved and the solution is clear, the electrospinning solution can be used for electrospinning.

[0041] According to certain embodiments, the solutions (each a homogeneous dispersion) have a Brinell viscosity of 50 to 3000 cP, preferably 75 to 1500 cP, and more preferably 80 to 500 cP at a measurement temperature of 20°C to 25°C, preferably 20°C. To measure the Brinell viscosity, a Brinell viscometer such as the DV II+ PRO can be used.

[0042] Electrospinning method

[0043] The present invention relates to a method for producing a nonwoven web of PVDF copolymer fibers by electrospinning the solution described above to form the web.

[0044] The term "fiber" is understood to refer to filamentous elements that can usually be described by their diameter and length.

[0045] "Nonwoven fiber webs" are understood to refer specifically to collections of fibers obtained by assembling fibers without weaving or knitting. An additional definition has been proposed by EDANA (…). European Disposable Goods and Nonwovens Association According to standard EN ISO 9092, it means a sheet made of single fibers that are directly or randomly oriented and bonded by friction, cohesion or adhesion.

[0046] According to one embodiment, the electrospinning method is implemented using an electrospinning apparatus, which may be a needle, thread or cable, cylinder, disc or rotating disc, cone, spiral or pyramidal system, or another system capable of producing fibers under the influence of an electric field. The apparatus includes an electrospinning solution tank and a system for supplying the solution to the electrospinning apparatus at a controlled flow rate. The electrospinning apparatus is connected to a positive high-voltage generator. A metal collecting electrode is placed opposite the electrospinning apparatus and connected to a negative high-voltage generator or ground. The voltage difference during electrospinning generates an electric field. Multiple solution filaments are generated at the electrospinning apparatus under the influence of the field and guided to the collecting electrode. Whip movement between the electrospinning apparatus and the collecting electrode causes solvent evaporation. Solid PVDF copolymer fibers are deposited on a substrate placed above the collecting electrode.

[0047] Several parameters of the method can be adjusted to obtain a mesh with advantageous properties, particularly good filtration efficiency and / or resulting in low pressure drop. Specifically, parameters are adjusted to obtain fibers of a desired size with a substantially uniform appearance and minimized polymer bead presence. The electrospinning parameters are, in particular: - Voltage on the electrospinning device: between 1 kV and 80 kV - Voltage on the collecting electrode: between 0 kV and -40 kV - Distance between the electrospinning device and the collecting electrode: between 1 cm and 50 cm - Flow rate of polymer solution: between 0.1 g / min and 20 g / min - Belt speed: between 0.01 m / min and 15 m / min - Relative humidity of the air in the electrospinning room: between 0% and 50% - Indoor air temperature: between 10°C and 40°C.

[0048] The fibrous web enters the drying oven at the exit of the electrospinning chamber. The oven temperature is between 25°C and 70°C. The fibrous web is then cooled to ambient temperature (25°C). This drying step can (where appropriate) evaporate residual solvent and optionally increase crystallinity, and thus improve the ferroelectric properties of the fluoropolymer.

[0049] The electrospun fiber web has a crystallinity of 29% to 34% (as determined by differential scanning calorimetry (DSC) from the melting enthalpy of P(VDF-HFP) at 104.5 J / g).

[0050] The percentage of the β phase in the crystalline phase is between 41% and 69% (as determined by Fourier transform infrared spectroscopy or FTIR spectroscopy). The fibers have different weight contents of the β phase, and the maximum content relative to the weight of the fiber, calculated by multiplying the degree of crystallinity by the percentage of the β phase in the crystalline phase, is 21% for the fiber web produced from a mixture of acetone and P(VDF-HFP) in γ-valerolactone. More specifically, this percentage of the β phase in the crystalline phase is greater than the percentage obtained for the fiber web produced from a mixture of acetone and P(VDF-HFP) in dimethyl sulfoxide.

[0051] According to certain embodiments, the β-phase weight content (relative to fiber weight) of PVDF copolymer fibers electrospun from γ-valerol is higher than that of PVDF copolymer fibers electrospun from other more sustainable solvents and conventional CMR as assessed. These notable properties are also advantageous in piezoelectric applications.

[0052] Depending on the operating conditions of the electrospinning method, and especially the distance between electrodes, voltage, and solution flow rate, the diameter of electrospun PVDF copolymer fibers can be less than 200 nm.

[0053] Applications of PVDF copolymer fiber networks

[0054] The term "filtration device" refers to a fibrous mesh used for filtering air and / or liquids. Fiber meshes used for air filtration include filter membranes used for respiratory protection, filter membranes in protective equipment and / or protective clothing, and any fibrous meshes used for aerosol filtration.

[0055] Depending on the selected electrospinning conditions, according to the permeation tests described in standards EN143 and EN149 (classification of FFP2 face masks), the electrospun fiber webs according to the present invention exhibit a filtration efficiency greater than 94% and a pressure drop less than 240 Pa for particles with an average diameter of 0.2 to 0.6 µm. More specifically, the filtration efficiency measured on fiber webs electrospun from a mixture of acetone and γ-valerolactone containing P(VDF-HFP) is greater than that obtained on fiber webs electrospun from a mixture of acetone and dimethyl sulfoxide containing P(VDF-HFP).

[0056] These noteworthy properties are advantageous in air and liquid filtration applications.

[0057] The mesh is composed of PVDF copolymer fibers and has a basis weight that varies depending on the application.

[0058] In air filtration applications, the basis weight of the PVDF copolymer mesh varies from 0.01 to 30 g / m², preferably from 0.02 to 15 g / m². The mesh has a thickness of 0.1 to 60 micrometers.

[0059] In liquid filtration applications, the basis weight of the PVDF copolymer mesh varies from 0.01 to 100 g / m², preferably from 0.02 to 50 g / m². The mesh has a thickness from 0.1 to 200 micrometers.

[0060] In aerosol filtration applications, the fibers are deposited on a substrate to ensure the mechanical properties of the assembly. This substrate is a nonwoven or fibrous fabric with a very low pressure drop (<10 Pa, measured at an airflow rate of 95 L / min over 100 cm²). It typically consists of a nonwoven or woven fabric of thermoplastic fibers obtained through spinning techniques such as spunbond or meltblown. It is preferably composed of polypropylene (PP) or polyethylene terephthalate (PET) fibers. Other polymers, such as polyacrylonitrile (PAN) or PVDF, can be used.

[0061] Respiratory protective masks can be composed of an assembly of electrospun PVDF copolymer fiber mesh and spunbond and / or meltblown PP nonwoven mesh.

[0062] Example

[0063] exist Figure 1 An electrospinning solution containing 14 wt% P (VDF-HFP, with 10% HFP), 43 wt% acetone, and 43 wt% γ-valerolactone was prepared in the reactor described herein. First, γ-valerolactone and acetone were introduced into the reactor. Powdered P (VDF-HFP) was slowly introduced into the solvent mixture under cold conditions and with mechanical stirring at 300 rpm. Dissolution was carried out for 2 to 3 hours under a constant temperature bath at 50°C with stirring. Electrospinning was performed on the electrospinning solution when all particles were dissolved and the solution was clear.

[0064] The prepared fluoropolymer solution was electrospun using the following electrospinning parameters: - Flow rate of polymer solution = 3 g / min -Spinning speed of the electrospinning device = 11,000 rpm -Electrode distance = 18 cm - Relative humidity = 15% -Air temperature = 30°C.

[0065] The obtained fibrous network was characterized by scanning microscopy, such as... Figure 2 As shown. The measured average fiber diameter is 136 + / - 75 nm.

[0066] According to standards EN143 and EN149, the obtained fibrous mesh was tested on a filtration tester (Lorenz FMP03) certified for paraffin oil aerosol permeation measurement. The measured aerosol filtration efficiency was 94.3%, with a pressure drop of 192 Pa measured at 100 cm² at 95 L / min. An aerosol filtration efficiency greater than 94% and a pressure drop <240 Pa measured at 100 cm² at 95 L / min are required for FFP2 class respiratory protective filters according to standards EN143 and EN149.

[0067] The fibrous web is electrospun on a second electrospinning apparatus using a mixture of different solvents. The degree of crystallinity is determined by the enthalpy of melting ΔH. mea (It is measured by integrating the melting peak on the DSC thermogram) and compared with the literature value ΔH for 100% crystalline PVDF. lit (104.5 J / g) was used for comparison. The following formula is used to calculate the relative crystallinity X. c : [Chemical Formula 1]

[0068] The percentage of the β phase in the crystalline phase of the PVDF copolymer was determined by interpreting the spectrum obtained by Fourier transform infrared spectroscopy (FTIR).

[0069] The results obtained (crystallization) X C The degree of β phase, the percentage of β phase in the crystalline phase of P(VDF-HFP), and the weight content of β phase in the powder and fiber network are shown in Table 1.

[0070] [Table 1]

[0071] The fibers have different β-phase weight contents, with the maximum content obtained being 21% relative to the weight of the fibers for a fibrous web produced from a mixture of acetone and γ-valerolactone P(VDF-HFP).

[0072] The obtained fibrous webs were tested on a filtration tester (Lorenz FMP03) certified for paraffin oil aerosol permeation measurement, according to standards EN143 and EN149. Aerosol filtration efficiency and pressure drop for various fibrous webs were measured at 95 L / min over 100 cm² and are shown in Table 2.

[0073] [Table 2]

[0074] Fiber webs electrospun from different solvent mixtures have different filtration efficiencies and pressure drops. The fiber webs with the best filtration efficiency (accompanied by low pressure drop) are electrospun from a mixture of P(VDF-HFP) in acetone and γ-valerolactone and a mixture of P(VDF-HFP) in dimethylacetamide (classified as CMR).

Claims

1. A method for producing a nonwoven web of PVDF copolymer fibers by electrospinning a solution, wherein the solution comprises a fluoropolymer dissolved in a solvent mixture, characterized in that... The mixture comprises a first solvent and a second solvent, the first solvent being γ-valerolactone, and the second solvent being a solvent mixture or a pure solvent having a boiling point below 100 °C, the second solvent being selected from acetone, dimethyl carbonate, methyl ethyl ketone, 2-methyltetrahydrofuran, or mixtures thereof.

2. The production method according to claim 1, wherein the mass content of the first solvent is between 10% and 70%, preferably between 30% and 50%, relative to the weight of the solution.

3. The production method according to any one of claims 1 and 2, wherein the mass content of the PVDF copolymer is between 6% and 25%, preferably between 10% and 21%, relative to the weight of the solution.

4. The production method according to any one of claims 1 to 3, wherein the PVDF copolymer comprises at least 50 mol% vinylidene fluoride (VDF) and at least one comonomer selected from the following list: vinyl fluoride (VF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), vinyl chlorofluoroethylene (CFE), dichlorofluoroethylene, trichlorofluoroethylene (CTFE), dichlorodifluoroethylene, trichlorofluoroethylene, hexafluoropropylene (HFP), trifluoropropylene, tetrafluoropropylene, trichlorofluoropropylene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropylene, perfluoroethers, especially perfluoroalkyl vinyl ethers, ethylene, acrylic monomers, methacrylic monomers, and mixtures thereof.

5. The production method according to any one of claims 1 to 4, wherein the solution has a Brinell viscosity of 50 to 3000 cP, preferably 75 to 1500 cP, and more preferably 80 to 500 cP at 20 °C, as measured according to standard ASTM D1238-13.

6. The production method according to any one of claims 1 to 5, wherein the fluoropolymer is a P(VDF-HFP) copolymer.

7. The production method according to claim 6, wherein the P(VDF-HFP) has a molar ratio of 5% to 35% of repeating units derived from HFP.

8. The production method according to any one of claims 1 to 7, wherein the fluoropolymer in powder form is dissolved in a solvent mixture at a temperature between 30 and 70 °C for 1 to 5 h.

9. The production method according to any one of claims 1 to 8, carried out by means of an apparatus comprising: an electrospinning solution tank; a system for supplying the electrospinning solution to an electrospinning apparatus connected to a positive high voltage generator; a metal collecting electrode placed opposite the electrospinning apparatus and connected to a negative high voltage generator or ground; and a substrate placed above the collecting electrode, on which the PVDF copolymer fibers are deposited.

10. The method according to claim 9, wherein, At the exit of the electrospinning chamber, the PVDF copolymer fibers undergo a drying step in an oven at a temperature between 25 °C and 70 °C.

11. A network obtainable by the method according to any one of claims 1 to 10, wherein the PVDF copolymer fiber network is characterized by a crystallinity of 29% to 34% and a percentage of β phase in the crystalline phase between 41% and 69%.

12. The use of the mesh according to claim 11 for air filtration, wherein the mesh has a thickness ranging from 0.1 to 60 micrometers and a basis weight ranging from 0.01 g / m² to 30 g / m², preferably from 0.02 g / m² to 15 g / m².

13. The use of the mesh according to claim 11 for liquid filtration, wherein the mesh has a thickness ranging from 0.1 to 200 micrometers and a basis weight ranging from 0.01 g / m² to 100 g / m², preferably from 0.02 g / m² to 50 g / m².

Citation Information

Patent Citations

  • Method for producing an assembly of fibres comprising a fluorinated polymer made from vdf

    WO2021255389A1