Method for manufacturing a press-formed part
By adjusting the opening angle of the outer longitudinal wall and using cam pressing technology during the stamping process, the problem of cracking at the corner of the roughly L-shaped stamped part was solved, achieving a higher quality forming effect.
Patent Information
- Application Number
- CN202480090647.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-08
- Filing Date
- 2024-11-28
- Publication Date
- 2026-11-10
AI Technical Summary
In roughly L-shaped stamped parts, cracking and wrinkling are prone to occur, especially at curved and corner parts, and existing technologies are not effective in preventing cracking at corner parts.
By setting the opening angle of the outer longitudinal wall to gradually increase from the far end to the near end during the stamping process, and using a cam to press the outer longitudinal wall from the outside during the formal forming process, the outer longitudinal wall of the target part is formed, reducing stress concentration at the corner.
It effectively suppressed cracking at corners, improving the forming quality and reliability of stamped parts.
Smart Images

Figure CN123076451A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing stamped parts. Background Technology
[0002] In recent years, stamped parts made from high-strength sheet metal have been used in automotive components to improve crash safety and reduce vehicle weight. However, issues arising from the use of high-strength sheet metal in stamping include cracking due to reduced sheet ductility and wrinkling due to increased yield strength. Particularly in stamped parts with concave bends, cracking occurs not only at the flange of the bend but also at the top plate or punch shoulder of the bend.
[0003] Cracking at the flange of the bent portion is caused by the stress that stretches the flange in the circumferential direction during stamping. Furthermore, wrinkles formed in the top plate or the punch shoulder are caused by the reaction force of this stress. As a method to prevent such cracking or wrinkling, for example, it has been proposed to increase the bending radius of the punch shoulder provided in the bent portion from the center of the bent portion toward both ends (see Patent Document 1). In addition, for example, for a generally L-shaped stamped part having two straight portions with intersecting extending directions and a bent portion provided between these straight portions, it has been conceived to provide a rib in the top plate of either of the two straight portions (see Patent Document 2).
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-166997
[0007] Patent Document 2: International Publication No. 2012 / 070623 Summary of the Invention
[0008] The problem that the invention aims to solve
[0009] Hereinafter, the longitudinal wall portion on the side where the curved portion is located in a roughly L-shaped stamped part will sometimes be referred to as the inner longitudinal wall portion, and the longitudinal wall portion on the back side of the curved portion will sometimes be referred to as the outer longitudinal wall portion. In addition, the portion on the opposite side of the curved portion in a stamped part will sometimes be referred to as the corner portion.
[0010] However, in roughly L-shaped stamped parts, there are cases where one of the two straight sections lacks an outer longitudinal wall, or where the outer longitudinal walls of the two straight sections are discontinuous and independently located near the corner. In such stamped parts, cracking or wrinkling occurs not only at the curved sections but also at the corners. The corner cracking is caused by the portion corresponding to the top plate of the straight section being pulled inwards towards the inner longitudinal wall during stamping, and the manufacturing methods disclosed in Patent Document 1 or Patent Document 2 are insufficient to prevent corner cracking. Therefore, a new countermeasure is needed to prevent corner cracking.
[0011] The present invention was made in view of the above-mentioned problems, and its object is to provide, for example, a new forming technique that can suppress cracking at the corner when manufacturing a generally L-shaped stamped part having two straight sections with intersecting extension directions and a curved section between these straight sections.
[0012] Methods for solving problems
[0013] According to one aspect, a method for manufacturing a stamped part is a method for manufacturing a stamped part having the following portions: the stamped part comprises: a top plate portion, which is L-shaped when viewed from above by having two straight portions having different extending directions and a curved portion disposed between the two straight portions; an inner longitudinal wall portion, which is continuous with the top plate portion at one of its two ends in the width direction, at the end where the curved portion is disposed; and an outer longitudinal wall portion, which is disposed at at least one of the two straight portions, and is continuous with the top plate portion at the other end of its two ends in the width direction, on the opposite side of the end where the curved portion is disposed; the method of manufacturing a stamped part comprises: a top plate portion having two straight portions having two straight portions having two straight portions having two straight portions and a curved portion being continuous with the top plate portion at the other end of its two ends in the width direction, on the opposite side of the end where the curved portion is disposed; the method of manufacturing a stamped part comprises: a top plate portion having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions and a curved portion being continuous with the top plate portion; the method of manufacturing a stamped part comprises: a top plate portion having two straight portions having two straight portions having two straight portions having two straight portions and a curved portion being disposed between the two ends of ... having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions having two straight portions The manufacturing method includes: a first forming step of stamping a blank into an intermediate forming part; and a second forming step of forming the intermediate forming part into a target forming part. In the intermediate forming part, among two straight sections, the end of the straight section with an outer longitudinal wall portion extending in the extension direction that is closer to the other straight section is designated as the proximal end, and the end opposite to the proximal end is designated as the distal end. When the angle between the outer longitudinal wall portion of the target forming part and the outer longitudinal wall portion of the intermediate forming part is defined as the opening angle, in the first forming step, stamping is performed with the opening angle of the proximal end being greater than the opening angle of the distal end, and the opening angle of the proximal end being a positive value. Here, the width direction of the top plate portion refers to the direction orthogonal to the extension direction of the straight section.
[0014] Furthermore, the shape of the middle section of the outer longitudinal wall is preferably such that the opening angle gradually increases as it approaches the proximal end. In this case, the opening angle at the proximal end is preferably 2 to 20°.
[0015] In addition, the second forming process preferably uses a cam member to press the middle shape of the outer longitudinal wall portion from the outside to form the middle shape of the outer longitudinal wall portion into the outer longitudinal wall portion of the target formed part.
[0016] The effects of the invention
[0017] According to this disclosure, it is possible to suppress the occurrence of cracks at corner locations. Attached Figure Description
[0018] Figure 1 This is a schematic perspective view showing an example of a stamped part as described in this embodiment.
[0019] Figure 2 This is a schematic flowchart illustrating an example of the manufacturing process of a stamped part.
[0020] Figure 3 This is a schematic perspective view showing an example of a preform.
[0021] Figure 4 (a) is an end view showing the structure of the preform at the far end P1. Figure 4 (b) is an end view of the structure of the preform at the proximal end P2 in the extension direction D3.
[0022] Figure 5 This is an end view showing an example of a mold used in the preforming process.
[0023] Figure 6 This is an end view showing an example of a mold used in the formal forming process.
[0024] Figure 7 (a) is an end view showing an example of the force acting on the proximal end P2 during the preforming process. Figure 7 (b) is an end view showing an example of the force acting on the distal end P1 during the preforming process. Detailed Implementation
[0025] The stamped part shown in this embodiment will be described below with reference to the accompanying drawings. Figure 1 As shown, the stamped part 10 is a generally L-shaped component having two straight portions 11 and 12 extending in different directions and whose ends intersect. The stamped part 10 is formed by... Figure 2 The part is manufactured using the preforming process S100 and the formal forming process S200 shown. Here, the stamped part 10 corresponds to the target formed part described in the claims. Furthermore, the preforming process corresponds to the first forming process described in the claims, and the formal forming process corresponds to the second forming process described in the claims.
[0026] The stamped part 10 has a concave curved portion 13 between the straight portions 11 and 12. Hereinafter, the portion located on the opposite side of the curved portion 13 in the intersection of the straight portions 11 and 12 will sometimes be referred to as... Figure 1 The part indicated by reference numeral 14 in the attached drawing is called the corner part. In addition, in the stamped part 10, the direction orthogonal to the extension direction of the straight parts 11 and 12 is defined as the width direction of the top plate part 21. Furthermore, in the width direction of the top plate part 21, the side where the curved part 13 is provided is defined as the inner side, and the side where the corner part 14 is provided is defined as the outer side.
[0027] An inner longitudinal wall portion 23, which extends from the top plate portion 21 via the upper bend portion 22, and an inner flange portion 25, which extends from the inner longitudinal wall portion 23 via the lower bend portion 24, are provided on the inner side of the stamped part 10. In the following text, the upper bend portion 22, the inner longitudinal wall portion 23, the lower bend portion 24, and the inner flange portion 25 are sometimes collectively referred to as inner component element E1.
[0028] An outer longitudinal wall portion 28, which extends from the top plate portion 21 via the upper bend portion 27, and an outer flange portion 30, which extends from the outer longitudinal wall portion 28 via the lower bend portion 29, are provided on the outer side of the straight portion 11 of the stamped part 10. Hereinafter, the upper bend portion 27, the outer longitudinal wall portion 28, the lower bend portion 29, and the outer flange portion 30 are sometimes collectively referred to as the outer component element E2.
[0029] Furthermore, an extension portion 33, connected to the top plate portion 21 and extending outward, is provided on the outer side of the straight portion 12 of the stamped part 10. The extension portion 33 is located on a plane substantially the same as the top plate portion 21. The extension portion 33 is provided independently and discontinuously with the outer longitudinal wall portion 28 connected to the straight portion 11. A rib 34 is provided on the extension portion 33 along the extending direction D2 of the straight portion 12. The rib 34 is provided to prevent material from being pulled towards the curved portion 13 during the stamping process described later.
[0030] In this embodiment, a stamped part 10 is illustrated, comprising an inner component E1 having an inner flange portion 25, an outer component E2 having an outer flange portion 30, and an extension portion 33. However, the inner flange portion 25, the outer flange portion 30, and the extension portion 33 are not essential components of the stamped part 10. Therefore, any one of these components may be omitted.
[0031] In the stamped part 10 of this embodiment, an extension portion 33 connected to the top plate portion 21 is provided in the straight section 12. However, it is also possible for a stamped part to have a straight section 12 having an outer longitudinal wall portion that is discontinuous with and independent of the outer longitudinal wall portion 28.
[0032] like Figure 2 As shown, the aforementioned stamped part 10 is manufactured, for example, by a manufacturing process consisting of a pre-forming process S100 and a formal forming process S200. Details will be explained later. The pre-forming process S100 is a process of stamping a metal sheet (hereinafter referred to as blank B) processed into a predetermined shape to manufacture the pre-formed part 40. The formal forming process S200 is a process of stamping or cam-bending the pre-formed part 40 to manufacture it. Figure 1 The process of stamping the part 10 shown. Here, the preform 40 corresponds to the intermediate formed part described in the claims.
[0033] First, use Figure 3 The structure of the preform 40 is described. For example... Figure 3 As shown, an intermediate shape of the inner component E1 and the outer component E2 of the stamped part 10 is formed on the preform 40. Hereinafter, the intermediate shape of the outer component E2 of the stamped part 10 is sometimes referred to as the outer component E2'.
[0034] The outer component E2' of the preform 40 is configured to include an outer longitudinal wall portion 43 that is continuous with the top plate portion 41 via the upper bending portion 42 and an outer flange portion 45 that is continuous from the outer longitudinal wall portion 43 via the lower bending portion 44.
[0035] Hereinafter, the extension direction of the straight portion 11' of the preform 40 will be referred to as D3. Of the two ends of the straight portion 11' in the extension direction D3, the end that does not intersect with the straight portion 12 will be referred to as the distal end P1. In addition, of the two ends of the straight portion 11' in the extension direction D3, the end opposite to the distal end P1, that is, the end on the side where the straight portion 11' intersects with the straight portion 12, will be referred to as the proximal end P2.
[0036] exist Figure 3 In the example of the preform 40 shown, the outer longitudinal wall 43 of the straight portion 11' at the distal end P1 is formed at the same angle as the outer longitudinal wall 28 of the straight portion 11 (see reference). Figure 4 (a)). On the other hand, the outer longitudinal wall 43 of the straight portion 11' at the proximal end P2 is in a state where it is opened outward from the outer longitudinal wall 28 of the straight portion 11 at a predetermined angle θ (see reference). Figure 4 (b)).
[0037] Hereinafter, the angle θ between the outer longitudinal wall portion 43 of the preform 40 and the outer longitudinal wall portion 28 of the stamped part 10 will be referred to as the opening angle θ. The opening angle θ is defined as follows: Figure 4The counterclockwise direction is the positive direction. Furthermore, the opening angle at the distal end P1 is called θ1, and the opening angle at the proximal end P2 is called θ2. In the preform 40, the opening angles θ1 at the distal end P1 and θ2 at the proximal end P2 are set as follows.
[0038] The opening angle θ1 at the distal end P1 is set to, for example, θ1 = 0°. However, the opening angle θ1 at the distal end P1 is preferably set appropriately, taking into account springback in stamping, forming load in preforming or formal forming processes, etc. Therefore, the opening angle θ1 can be a positive value or a negative value.
[0039] Furthermore, the opening angle θ2 at the proximal end P2 is preferably set to θ2 > θ1 relative to the opening angle θ1 at the distal end P1. However, when the opening angle θ2 at the proximal end P2 is set to, for example, θ2 < 2°, the effect of suppressing cracking during stamping may be too small. Additionally, if the opening angle θ2 at the proximal end P2 is too large, the deformation in the formal forming process increases, requiring attention to the dimensional or shape accuracy of the stamped part. When the opening angle θ2 is set to θ2 = 20°, the effect of suppressing cracking during stamping can be sufficiently obtained. Therefore, the opening angle θ2 at the proximal end P2 is preferably set to, for example, an opening angle θ2 = 2 to 20°, and more preferably, an opening angle θ2 = 5° to 15°.
[0040] Furthermore, in this embodiment, the opening angle θ of the outer longitudinal wall portion 43 in the preform 40 gradually increases from the distal end P1 toward the proximal end P2, and the opening angle θ2 is the largest at the proximal end P2. However, as long as the opening angle θ2 at the proximal end P2 is a positive value (for example, θ2 = 2° to 20°), the opening angle θ does not need to be the maximum value at the proximal end P2. For example, the opening angle θ can also be the maximum value between the distal end P1 and the proximal end P2.
[0041] Furthermore, the outer flange portion 45 is continuous with the outer longitudinal wall portion 43 via the lower bend portion 44. The outer flange portion 45 and the lower bend portion 44 form a certain angle. At the distal end P1, the outer flange portion 45 is, for example, parallel to the horizontal plane. At the proximal end P2, the outer flange portion 45 is, for example, inclined at an angle θ2 relative to the horizontal plane.
[0042] Next, the mold used in the preforming process S100 will be explained. For example... Figure 5 (a) and Figure 5 As shown in (b), the mold 50 used in the preforming process S100 is, for example, composed of a lower mold 51 and an upper mold 52. The lower mold 51 has, for example, a punch 53.
[0043] like Figure 5 (a) and Figure 5 As shown in (b), in the extension direction D3 ( Figure 5 At the far end P1 (in the direction perpendicular to the paper), the angle θ3 of the inclined surface 53c of the punch 53 relative to the upper surface 53a is set to the same angle as the inclination angle of the outer longitudinal wall portion 28 of the stamped part 10 relative to the top plate portion 21.
[0044] At the proximal end P2 in the extending direction D3, the angle θ4 of the inclined surface 53c of the punch 53 relative to the upper surface 53a is opened outward by the opening angle θ2 relative to the inclination angle of the outer longitudinal wall portion 28 of the stamped part 10. That is, the inclined surface 53c of the punch 53 is inclined in a shape in which the opening angle θ gradually increases from the distal end P1 toward the proximal end P2.
[0045] The bottom surface 53e of the punch 53 maintains a certain angle relative to the inclined surface 53c. That is, as the opening angle θ of the inclined surface 53c increases, the inclination angle of the bottom surface 53e relative to the horizontal plane also increases. In addition, the inclination angle of the bottom surface 53e relative to the horizontal plane is the same as the opening angle θ.
[0046] The upper die 52 includes a die cavity 54 and a pressure pad 55. The die cavity 54 has an inclined surface 54c that is continuous via a die shoulder 54b connected to the lower surface 54a. For example, at the distal end P1 in the extension direction D3, the inclination angle θ5 of the inclined surface 54c of the die cavity 54 relative to the lower surface 54a is set to the same angle θ3 of the inclined surface 53c of the punch 53 relative to the upper surface 53a. Furthermore, the inclined surface 54c at the proximal end P2 in the extension direction D3 has an inclination angle θ6 relative to the inclined surface 54c at the distal end P1 in the extension direction D3. This angle θ6 is the same as the opening angle θ2. That is, the inclined surface 54c has a shape that gradually increases in the opening angle θ from the distal end P1 towards the proximal end P2.
[0047] The lower surface 54a of the die 54 maintains a certain angle relative to the inclined surface 54c. As described above, the inclined surface 54c is inclined such that the opening angle θ gradually increases from the distal end P1 towards the proximal end P2. Therefore, the lower surface 54a is inclined from the distal end P1 towards the proximal end P2.
[0048] The pressure pad 55 is forced toward the lower die 51 by a force application means (not shown in the figure). When the upper die 52 moves toward the lower die 51, the pressure pad 55 abuts against the blank B before the die cavity 54 of the upper die 52 contacts the blank B, and clamps the blank B between the upper die 52 and the lower die 51.
[0049] Next, the molds used in the formal forming process will be explained. For example... Figure 6As shown, the mold 60 used in the formal forming process is composed of, for example, a lower mold 61 and an upper mold 62. The lower mold 61 has, for example, a punch 63 and a cam slider 64 arranged at a distance from the punch 63. In addition, an insertion space 65 is provided between the punch 63 and the cam slider 64 for the insertion of a cam 68, which will be described later.
[0050] The punch 63 has an upper surface 63a, a punch shoulder 63b connected to the upper surface 63a, an inclined surface 63c that is continuous with the upper surface 63a via the punch shoulder 63b, a curved surface 63d that is continuous with the lower end of the inclined surface 63c, and a bottom surface 63e connected to the curved surface 63d.
[0051] Although the illustration is omitted, the tilt angle θ7 of the inclined surface 63c of the punch 63 relative to the upper surface 63a is the same as the tilt angle of the outer longitudinal wall portion 28 of the stamped part 10 relative to the top plate portion 21.
[0052] The cam slider 64 has a guide surface 64a that slopes downward toward the punch 63. The guide surface 64a of the cam slider 64 slides in contact with the cam 68, causing the cam 68 to move toward the punch 63.
[0053] When the lower mold 61 moves relative to the upper mold 62, the pressure pad 67 abuts against the preform 40 positioned on the punch 63 of the lower mold 61 and clamps the preform 40 between the pressure pad 67 and the punch 63.
[0054] When the lower die 61 moves relative to the upper die 62, the cam 68 moves along the guide surface 64a of the cam slider 64 and clamps the outer component E2' of the preform 40 between it and the punch 63, forming the outer component E2 in the stamped part 10.
[0055] The cam 68 has an inclined surface 68a, a curved portion 68b, and a lower surface 68c. Although the figure is omitted, the inclination angle θ8 of the inclined surface 68a of the cam 68 relative to the lower surface 68c is the same as the inclination angle θ7 of the inclined surface 63c of the punch 63 relative to the upper surface 63a.
[0056] Finally, the manufacturing method of the stamped part 10 will be described. In the preforming process S100, for example, using Figure 5 The die 50 shown stamps the blank B. This produces a preform 40 (see reference 10) having the inner component E1 and the outer component E2' of the stamped part 10. Figure 3 ).
[0057] As described above, the opening angle θ of the inclined surface 53c of the punch 53 and the inclined surface 54c of the die 54 of the mold 50 increases from the distal end P1 towards the proximal end P2 in the extending direction D3. As a result, as... Figure 7 As shown in (a), in the outer longitudinal wall portion 43, the height H2 at the proximal end P2 is lower than the height H1 at the distal end P1. That is, when forming the outer longitudinal wall portion 43, the distance the material is stretched from the upper bend portion 42 toward the lower bend portion 44 is shortened. In other words, the force F1 stretching the corner portion 14' located on the upper bend portion 42 is reduced, suppressing cracking of the corner portion 14'.
[0058] Furthermore, during the forming of the inner longitudinal wall portion 23, the distal P1-side portion 41a of the top plate portion 41 is pulled into the inner longitudinal wall portion 23. As a result, at the distal P1-side portion 41a, a flow towards... Figure 3 Material movement occurs in the direction of M1. As this material moves, at location 41b on the proximal P2 side, a movement occurs towards... Figure 3 Material movement in the M2 direction. Orientation Figure 3 As material movement in the M1 direction increases, the direction towards Figure 3 The material movement in the M2 direction also increased. This is the cause of the crack at the corner 14'. Figure 7 As shown in (b), if the opening angle θ1 at the distal end P1 is reduced and the force F2 that stretches the material from the upper bend 42 toward the lower bend 44 is increased, then the force can be made to act on the obstacle that is moving toward the lower bend 44. Figure 7 (b) The direction of material movement in direction M1. As a result, towards Figure 3 The material movement in the M2 direction is reduced, thus suppressing cracking at the corner 14'.
[0059] After the preforming process S100, the formal forming process S200 is performed. In the formal forming process S200, the preformed part 40 manufactured in the preforming process S100 is either stamped or bent into a cam. For example, the cam bending process uses... Figure 6 The mold 60 shown is used for forming. Cam bending forming is a process that bends the upper bent portion 2, which is formed in the preforming process S100, by an opening angle θ. In the formal forming process S200, the force that stretches the upper bent portion 42 toward the lower bent portion 44 is less than the force in the preforming process S100. As a result, cracking at the corner portion 14 can be suppressed. In addition, although cam bending forming is used in the formal forming process, the same effect can be obtained even if stamping is used.
[0060] When manufacturing the aforementioned stamped part 10, it is preferable to use a metal sheet with a thickness of 0.6 to 4.0 mm and a tensile strength of 270 to 1800 MPa as the blank material B. The reasons are as follows: metal sheets with a tensile strength lower than 270 MPa and a thickness of less than 0.6 mm are rarely used in general automotive or home appliance parts; metal sheets with a tensile strength exceeding 1800 MPa usually have poor ductility and are prone to cracking; in the stamping of metal sheets with a thickness exceeding 4.0 mm, the stamping load is prone to increase, and the die is prone to damage.
[0061] Finally, the thickness reduction rate was measured during the pre-forming and final forming processes when manufacturing stamped parts using 1180MPa grade steel sheet. An example of the thickness reduction rate measurement results is shown in Table 1 below. Furthermore, in measuring the thickness reduction rate, steel with a thickness of 1.2 mm, a yield stress of 820 MPa, a tensile strength of 1230 MPa, and an elongation of 10% was used as blank B.
[0062] Table 1
[0063]
[0064] First, Comparative Example 1 describes a case where the opening angle θ of the distal end P1 and the proximal end P2 in the preforming process is set to θ = 0°, and stamping is performed in the formal forming process. Comparative Example 2 describes a case where the opening angle θ of the distal end P1 and the proximal end P2 in the preforming process is set to θ = 15°, and stamping is performed in the formal forming process. Furthermore, Comparative Example 3 describes a case where the opening angle θ of the distal end P1 and the proximal end P2 in the preforming process is set to θ = 0°, and cam bending is performed in the formal forming process.
[0065] Furthermore, cases where the proximal opening angle θ in the preforming process is set to θ = 2, 5, 15, or 20° and stamping is performed in the formal forming process are designated as Invention Examples 1 to 4. Further cases where the proximal opening angle θ in the preforming process is set to θ = 2, 5, 10, 15, or 20° and cam bending is performed in the formal forming process are designated as Invention Examples 5 to 9.
[0066] In this case, in Comparative Example 1, the thickness reduction rate was 11.2% at the bending portion 13 and 10.7% at the corner portion. Furthermore, in Comparative Example 2, the thickness reduction rate at the corner portion during the pre-forming process was 11.6%, and the thickness reduction rate at the corner portion during the formal forming process was 12.2%. Further, in Comparative Example 3, the thickness reduction rate at the corner portion during the formal forming process was 11.2%. However, when the thickness reduction rate reaches 10% or more, cracking is prone to occur. That is, in each of Comparative Examples 1 to 3, the result of easy cracking was obtained.
[0067] On the other hand, in Examples 1 to 9 of the Invention, even after performing each step in the pre-forming process and the formal forming process, the thickness reduction rate was less than 10%. Therefore, it can be seen that in Examples 1 to 9 of the Invention, the occurrence of cracking can be suppressed compared with Comparative Examples 1 to 3.
[0068] In this embodiment, the inner components of the preform are formed into the same shape as the inner components of the stamped part by performing a preforming process. However, stamping can also be performed multiple times in the preforming process to form the inner components of the preform 40 into the same shape as the inner components E1 of the stamped part 10.
[0069] Furthermore, although the radius of the upper bending portion 22 of the respective bending portion 13 in the preform 40 and the stamped part 10 is not specifically described, the radius may be the same at the center of the bending direction Cd of the bending portion 13 and at both ends of the bending direction Cd, or it may increase from the center of the bending direction Cd of the bending portion 13 toward both ends.
[0070] For example, when the radius of the upper bend 22 is increased from the center of the bending direction Cd of the bend 13 toward both ends, during stamping, the material moves from both ends of the upper bend 22 along the ridge line toward the center of the bend 13, and at the inner flange 25, the material is pulled toward the midpoint (central part) of the bend 13.
[0071] Furthermore, as described above, since the bent portion 13 is formed from material moving from both ends of the upper bent portion 22, the material located at the center of the upper bent portion 22 adjacent to the top plate portion 21 in the bent portion 13 no longer needs to be moved from the upper bent portion 22 during the forming of the bent portion 13. Therefore, when the radius of the upper bent portion 22 increases from the center of the bending direction Cd of the bent portion 13 toward both ends, it has the effect of suppressing cracking that occurs in the inner flange portion 25 of the bent portion 13 and wrinkling that occurs in the top plate portion 21 and the upper bent portion 22 of the bent portion 13.
[0072] <Summary of Results>
[0073] The manufacturing method of the present invention for a stamped part comprises a method for manufacturing a stamped part 10 having the following portions: a top plate portion 21, which is L-shaped when viewed from above by having two straight portions 11 and 12 with different extending directions and a curved portion 13 disposed between the two straight portions 11 and 12; an inner longitudinal wall portion 23, which is continuous with the top plate portion 21 at one of its two ends in the width direction, where the curved portion 13 is disposed; and an outer longitudinal wall portion 28, which is disposed at at least one of the two straight portions 11 and 12, and is continuous with the top plate portion 21 at the other end of its two ends in the width direction, opposite to the end where the curved portion 13 is disposed. The manufacturing method includes: a preforming step of stamping a blank B to form a preform 40; and forming the preform 40 into a target formed part. In the formal forming process of the stamped part, in the two straight sections 11' and 12 of the preform 40, the end of the straight section 11' with the outer longitudinal wall 43 that is closer to the other straight section in the extension direction is designated as the proximal end P2, and the end opposite to the proximal end P2 is designated as the distal end P1. The angle between the outer longitudinal wall 28 of the stamped part 10, which is the target formed part, and the outer longitudinal wall 43 of the preform 40 is designated as the opening angle. The characteristic feature is that the preforming process forms the outer longitudinal wall 43, which is the intermediate shape of the outer longitudinal wall 28, on the preform 40. The outer longitudinal wall 43 is inclined outward relative to the outer longitudinal wall 28 of the stamped part 10, which is the target formed part, and its opening angle θ relative to the outer longitudinal wall 28 of the stamped part 10, which is the target formed part, increases from the distal end P1 toward the proximal end P2.
[0074] In the preforming process S100, the stress concentration at the corner 14' is suppressed and the cracking at the corner 14' is prevented because the force F1 and material movement M2 at the stretching corner 14' are reduced.
[0075] In addition, the formal forming process uses a cam 68 to press the outer longitudinal wall portion 43 of the preform 40 from the outside, forming the outer longitudinal wall portion 43 of the preform 40 into the outer longitudinal wall portion 28 of the stamped part 10, which is the target formed part.
[0076] The formal forming process S200 is to bend the upper bent portion 42 formed in the preforming process S100 by opening it at an angle θ. Therefore, it does not promote stress concentration at the corner portion 14, and thus also suppresses the occurrence of cracking at the corner portion 14 in the formal forming process.
[0077] Explanation of reference numerals in the attached figures
[0078] 10 Stamped parts
[0079] 11, 11', 12 Straight sections
[0080] 13. Bending section
[0081] 21 Top Plate
[0082] 23 Inner longitudinal wall portion
[0083] 28. Outer longitudinal wall portion
[0084] 40 Preforms
[0085] 43. Outer longitudinal wall portion
[0086] 68 Cam
[0087] P1 Remote
[0088] P2 proximal
[0089] θ opening angle
[0090] θ1 is the opening angle on the distal side.
[0091] θ2 is the opening angle on the proximal side.
[0092] B billet
Claims
1. A method for manufacturing a stamped part, wherein the stamped part comprises: The top plate portion is L-shaped when viewed from above by having two straight sections with different extending directions and a curved section disposed between the two straight sections; The inner longitudinal wall portion is continuous with the top plate portion at one of its two ends in the width direction, where the curved portion is provided; and The outer longitudinal wall portion is provided at at least one of the two straight portions, and is continuous with the top plate portion at one of its two ends in the width direction of the top plate portion, on the opposite side of the end where the curved portion is provided. The manufacturing method comprises: The first forming process stamps the blank into an intermediate formed part; and The second forming process shapes the intermediate forming part into the target forming part; In the two straight sections of the intermediate forming member, the end of the straight section with the outer longitudinal wall portion that is closer to the other straight section in the extension direction is designated as the proximal end, and the end opposite to the proximal end is designated as the distal end. When the angle between the outer longitudinal wall portion of the target molded part and the outer longitudinal wall portion of the intermediate molded part is set as the opening angle... In the first forming process, stamping is performed with the opening angle at the proximal end being greater than the opening angle at the distal end, and the opening angle at the proximal end being a positive value.
2. The method for manufacturing a stamped part according to claim 1, characterized in that, The middle shape of the outer longitudinal wall portion is such that the opening angle gradually increases as it moves from the distal end to the proximal end.
3. The method for manufacturing a stamped part according to claim 1 or claim 2, characterized in that, The opening angle at the proximal end is 2–20°.
4. The method for manufacturing a stamped part according to claim 1 or claim 2, characterized in that, The second forming process uses a cam member to press the middle shape of the outer longitudinal wall portion from the outside, forming the middle shape of the outer longitudinal wall portion into the outer longitudinal wall portion of the target formed part.
Citation Information
Patent Citations
Press molding method
JP2021166997A
Method for manufacturing l-shaped product
WO2012070623A1