Abrasive articles having selective coatings and methods of making the same
By setting a selective conformal protective layer on abrasive products, the problem of abrasive pad dressers being susceptible to corrosion in corrosive environments is solved, and the corrosion resistance and stability in chemical mechanical polishing processes are improved.
Patent Information
- Application Number
- CN202580016300.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-04
- Filing Date
- 2025-02-14
- Publication Date
- 2026-11-10
AI Technical Summary
Abrasive pad dressers are susceptible to corrosion in chemical mechanical polishing processes, leading to premature failure and metal leaching, which affects the performance and integrity of the polishing pad.
A selective conformal protective layer is applied to the working surface of the abrasive product, coating the non-abrasive surface and some abrasive elements to form a local coating to improve corrosion resistance and prevent metal leaching.
It enhances the stability of abrasive products in corrosive environments, maintains grinding performance, reduces material consumption, and extends service life.
Smart Images

Figure CN123076470A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to abrasive articles. Specifically, it relates to abrasive articles having a selective protective coating. This invention also relates to a method for preparing abrasive articles. Background Technology
[0002] The fabrication of semiconductor devices and integrated circuits involves repeated deposition and etching of silicon wafers to form multilayer structures. These wafers are polished using chemical mechanical planarization (CMP) polishing methods to remove surface irregularities. This polishing method involves the use of abrasive slurries and polishing pads. During the CMP process, material is removed from the wafer, and this material accumulates on the surface of the polishing pads, causing surface glazing and degrading their performance, shortening their lifespan, and increasing the wafer defect rate. To restore the polishing pads and remove deposits on them, pad conditioners are used during the CMP process. Pad conditioners are designed to regenerate the polishing pads through a grinding mechanism that removes unwanted waste build-up and re-creates a rough texture on the polishing pad surface.
[0003] However, these abrasive pad dressers are susceptible to chemical corrosion in the highly corrosive environments used in CMP processes, leading to premature dresser failure. Pad dressers with metal components (such as stainless steel and nickel-chromium alloys) may experience metal leaching due to the use of acidic slurries during CMP processes. Metal leaching causes defects / voids to form at the surface and subsurface levels of the pad dresser, accelerating corrosion and compromising the integrity of the pad dresser.
[0004] Therefore, abrasive pad dressers must be designed to resist metal leaching and withstand corrosive environments. Thus, there is a great need for abrasive pad dressers with improved stability, corrosion resistance, and reduced metal leaching. Summary of the Invention
[0005] In one embodiment, the present disclosure provides an abrasive article comprising a substrate including: a working surface having a non-abrasive surface on which abrasive elements are dispersed; and a protective layer disposed non-uniformly on the working surface, the protective layer forming a conformal coating on the non-abrasive surface and forming a localized coating on the abrasive elements.
[0006] In another aspect, this disclosure provides a method for preparing an abrasive article. The method includes: a) providing a substrate including a working surface having a non-abrasive surface on which abrasive elements are dispersed; b) laminating the working surface using a sheet to obtain an unmasked region and a masked region, the unmasked region including a first portion of the abrasive element and the non-abrasive surface, the masked region masking a second portion of the abrasive element; c) depositing a protective layer on the unmasked region, wherein the protective layer forms a conformal coating on the non-abrasive surface and the first portion of the abrasive element; and d) peeling the sheet from the masked region to expose the second portion of the abrasive element, and obtaining the abrasive article including the protective layer selectively disposed on the working surface.
[0007] In another aspect, this disclosure provides a method for preparing an abrasive article, the method comprising the steps of: a) providing a substrate including a working surface having a non-abrasive surface on which abrasive elements are dispersed; b) providing a coating over a portion of the abrasive elements to obtain a coated abrasive element having a covered portion and an uncovered portion; c) depositing a protective layer on the working surface, wherein the protective layer forms a conformal coating on the uncovered portion of the abrasive element and the non-abrasive surface; and d) removing the coating from the covered portion of the abrasive element to obtain the abrasive article including the protective layer selectively disposed on the working surface.
[0008] The above overview of this disclosure is not intended to describe every embodiment of this disclosure. Details of one or more embodiments of this disclosure are also set forth in the following description. Other features, objectives, and advantages of this disclosure will become apparent from the description and claims. Attached Figure Description
[0009] This disclosure can be more fully understood in conjunction with the accompanying drawings and the following detailed description of various embodiments thereof, wherein:
[0010] Figure 1A , Figure 1B and Figure 1C A schematic diagram depicts an example abrasive article with a protective layer selectively disposed on a working surface.
[0011] Figure 2A and Figure 2B A schematic diagram depicts an example abrasive article with a protective layer selectively disposed on a working surface.
[0012] Figure 3 A schematic diagram depicts a process for manufacturing an abrasive layer with a protective layer selectively applied to a working surface.
[0013] Figure 4A schematic diagram depicts an abrasive article with covered and uncovered portions.
[0014] Figure 5 This is a graph showing the coating loss over time for fully coated and selectively coated pad trimmer samples.
[0015] These figures are not drawn to scale and are for illustrative purposes only. Detailed Implementation
[0016] Reference will now be made in detail to specific embodiments of the subject matter disclosed herein, examples of which are partially illustrated in the accompanying drawings. While the subject matter disclosed herein will be described in conjunction with the enumerated claims, it should be understood that the exemplary subject matter is not intended to limit the claims to the subject matter disclosed herein.
[0017] Unless the context clearly indicates otherwise, the terms “a,” “an,” or “the / said” are used herein to include one or more. Unless otherwise specified, the term “or” is used to mean a non-exclusive “or.” The expression “at least one of A and B” has the same meaning as “A, B, or A and B.” Furthermore, it should be understood that the wording or terms used herein, unless otherwise defined, are for illustrative purposes only and are not restrictive. Any use of section headings is intended to aid in the understanding of the document and should not be construed as restrictive; information relating to a section heading may appear within or outside that particular section.
[0018] In the methods described herein, various actions can be performed in any order without departing from the principles of the invention, except where a specific sequence of time or operation is explicitly enumerated. Furthermore, the prescribed actions can be performed simultaneously unless the explicit language of the claims implies that they are performed separately. For example, the claimed action X and the claimed action Y can be performed simultaneously in a single operation, and the resulting process will fall within the literal scope of the claimed process.
[0019] Unless otherwise specified, all figures for expressions or measurements of components, properties, etc., used in this specification and embodiments should in all cases be understood to be modified by the term "about". Therefore, unless stated to the contrary, the numerical parameters shown in the foregoing specification and the appended list of embodiments may vary according to the desired properties sought by those skilled in the art using the teachings of this disclosure. At a minimum, and without attempting to limit the application of the doctrine of equivalence to the embodiments protected by the claims, each numerical parameter should be interpreted at least according to the number of significant digits reported and by applying customary rounding.
[0020] In chemical mechanical planarization (CMP) applications, a polishing system may include: a polishing pad (typically a polymer-based material, such as polyurethane); an abrasive article designed as a grinding pad, such as a pad dresser; a substrate to be polished, such as a semiconductor wafer; and a working fluid, such as a polishing slurry containing abrasive particles, designed to polish / grind the substrate to be polished. During wafer polishing with a polishing slurry and polishing pad, the polishing pad may become glazed by slurry particles from the slurry, which reduces the pad's ability to polish the wafer in a consistent manner. Pad dressers, which may contain abrasive layers (such as diamond abrasive layers, ceramic abrasive layers, or diamond-coated ceramic abrasive layers), are typically used to grind the polishing pad to remove glazing and / or expose a fresh polishing pad surface, thereby maintaining consistent polishing performance of the pad over extended polishing periods. However, during use, pad dressers may easily accumulate chips, for example, polishing pad material ground from the polishing pad and / or abrasive particles from the slurry can adhere to the grinding surface of the pad dresser. These ground materials and acids in the polishing slurry expose the dresser to a corrosive environment. Therefore, dressers may be susceptible to corrosion, leading to material release in the slurry or polishing pad, and subsequently onto the wafer. Therefore, abrasive articles (such as pad dressers) should be corrosion-resistant. Accordingly, the present invention provides an abrasive article for use in corrosive environments and a method for manufacturing such an abrasive article.
[0021] This invention provides an abrasive article with a protective coating. The protective coating on the abrasive article forms a selectively conformal coating, thereby leaving a portion of the abrasive particles uncoated while the metal-based substrate of the abrasive article is covered by the coating. This selective coating is achieved by the method described herein. The selectively conformal coating ensures that the dresser maintains its normal abrasive performance, and simultaneously, even in corrosive environments, the un-abrasive surface remains intact and unaffected. Therefore, this invention provides an abrasive article with a protective coating that conforms to the substrate, reduces or inhibits metal leaching, does not add consumable material / volume to the working surface, and provides corrosion resistance.
[0022] Abrasive products
[0023] In one embodiment, this disclosure provides an abrasive article. The abrasive article includes a substrate. The substrate includes a working surface and a protective layer, the protective layer being non-uniformly disposed on the working surface. The working surface has a non-abrasive surface on which abrasive elements are dispersed. The protective layer, selectively disposed on the working surface, forms a conformal protective coating on the non-abrasive surface. The protective layer forms a locally conformal protective coating on the abrasive elements. At least one portion of the abrasive element is coated with the protective layer.
[0024] In some embodiments, the abrasive article includes a working surface, a primer layer, and a protective layer. The working surface has a non-abrasive surface on which abrasive elements are dispersed. The primer layer is applied to the working surface. The protective layer is unevenly disposed on the primer layer. The protective layer, selectively disposed on the primer-coated working surface, forms a conformal protective coating on the non-abrasive surface and a locally conformal protective coating on the abrasive elements. At least one portion of the abrasive element is coated with the primer layer, and the protective layer is disposed on the primer layer.
[0025] In some embodiments, the substrate of the abrasive article is made of a metal or a metal alloy. The substrate is made of a metal selected from chromium, tungsten, cobalt, titanium, zinc, manganese, silicon, iron, nickel, and copper. The substrate is made of a metal alloy comprising two or more metals selected from chromium, tungsten, cobalt, titanium, zinc, manganese, silicon, iron, nickel, and copper. The substrate includes a working surface and a protective layer. The working surface has a non-abrasive surface with an abrasive element. The abrasive element is an engineered feature or an abrasive particle.
[0026] In some implementations, the abrasive element is a precisely shaped engineered feature or an abrasive particle embedded in the non-abrasive surface.
[0027] Figure 1A , Figure 1B and Figure 1C A schematic diagram depicts an example abrasive article having a protective layer selectively disposed on a working surface, wherein the abrasive element is an abrasive particle embedded in a non-abrasive surface. As shown, Figure 1A A top view of an abrasive article (100a) including a substrate (102) is depicted, the substrate comprising: a working surface (104) having a non-abrasive surface (106) on which abrasive particles (108) are dispersed; and a protective layer (110) unevenly disposed on the working surface. Figure 1B A cross-sectional view of an abrasive article (100b) including a substrate (102) is depicted. The substrate (102) includes a working surface (104). The working surface (104) includes a non-abrasive surface (106) in which abrasive particles (108) are embedded. A protective layer (110) is unevenly disposed on the working surface (104). Figure 1C The protective layer (110) of the abrasive article is specifically described, which forms a conformal coating on the non-abrasive surface (106) and a local coating on the abrasive particles (108).
[0028] In some embodiments, the abrasive element is formed of carbide and is about 99% carbide ceramic by weight. In one embodiment, the carbide ceramic is silicon carbide, boron carbide, zirconium carbide, titanium carbide, tungsten carbide, or a combination thereof. In some embodiments, 99% of the carbide ceramic by weight is substantially silicon carbide. Specifically, the carbide ceramic is at least about 90% silicon carbide by weight. The abrasive element is manufactured without the use of carbide forming agents and is substantially free of oxide sintering aids. In one embodiment, the abrasive element includes less than about 1% oxide sintering aids. The abrasive element is also substantially free of silicon and specifically includes less than about 1% elemental silicon.
[0029] Figure 2A and Figure 2B A schematic diagram depicts an example abrasive article with a protective layer selectively disposed on a working surface, wherein the abrasive element is a precisely shaped engineered feature. As shown, Figure 2A A top view of an abrasive article (200a) including a substrate (202) is depicted. The substrate (202) includes a working surface (204) having a non-abrasive surface (206) with engineered features (208) distributed on it. A protective layer (210) is unevenly disposed on the working surface (204). Figure 2B A cross-sectional view of an abrasive article (200b) including a substrate (202) is depicted. The substrate (202) includes a working surface (204) having a non-abrasive surface (206) with engineered features (208) distributed thereon. A protective layer (210) is non-uniformly disposed on the working surface, forming a conformal coating on the non-abrasive surface (206) and a local coating on the engineered features (208).
[0030] In some embodiments, the abrasive element includes precisely shaped engineered features or protrusions within the abrasive element that project toward the workpiece. The abrasive element may have any one or more shapes (polygonal or non-polygonal) and may have the same or varying height. Furthermore, the abrasive element may have the same base size or varying base dimensions. The abrasive elements may be spaced in a regular or irregular array and may be fabricated into a pattern composed of unit cells.
[0031] In one embodiment, the abrasive element includes a peripheral region or a region around the abrasive element in which there are no abrasive features.
[0032] In one embodiment, the engineered feature comprises molded and sintered ceramics spaced in an array on the non-abrasive surface. In one embodiment, the abrasive element is made from a molded green body. In such cases, the abrasive element can be considered as a molded abrasive element. Precision engineered abrasive is ceramic pressed into a mold and sintered. The mold itself can be used to manufacture the precision engineered feature. In some embodiments, when molding the abrasive element, the abrasive element is a subset of the precision engineered features imparted to its structure by the molding process. For example, the shape can be reversed with respect to the mold cavity such that the shape is retained after the abrasive element green body has been removed from the mold. Various ceramic forming processes can be used, including (but not limited to): injection molding, flow casting, compression molding, hot pressing, stamping, transfer molding, gel casting, etc. In one embodiment, the compression molding process is used at room temperature, followed by sintering. Typically, ceramic compression molding near room temperature is referred to as ceramic dry pressing. Generally, the difference between ceramic dry pressing and ceramic injection molding is that it is completed at a lower temperature, uses a much smaller amount of binder, uses molding, and the materials suitable as binders are not limited to thermoplastics.
[0033] In some embodiments, the abrasive elements dispersed on the non-abrasive surface of the working surface of the polished layer are abrasive particles. In some embodiments, the abrasive particles are embedded in the non-abrasive surface of the working surface. The abrasive particles are made of materials including oxides, carbides, nitrides, borides, oxynitrides, boron oxides, diamond, or combinations thereof. In some embodiments, the abrasive particles may include diamond or cubic boron nitride. In a particular embodiment, the abrasive particles may include diamond.
[0034] The abrasive particles are fixed to the substrate using a matrix material. The matrix material comprises a brazing alloy and a sintered corrosion-resistant powder selected from at least one of stainless steel, nickel, nickel-chromium alloy, titanium, zirconium, tungsten carbide, and silicon carbide. The brazing alloy comprises at least one of aluminum, boron, carbon, chromium, tungsten, cobalt, titanium, zinc, iron, manganese, or silicon. When heated to a predetermined temperature, the brazing alloy becomes liquid and flows around the abrasive particles. Furthermore, the brazing alloy reacts with the abrasive particles to form chemical bonds. To form these chemical bonds, the brazing alloy composition contains pre-selected elements known to react with specific abrasive particles to form chemical bonds. For example, if diamond abrasive particles are used, the brazing alloy may contain at least one of the following elements that react with diamond to form chemical bonds: chromium, tungsten, cobalt, titanium, zinc, iron, manganese, or silicon. For example, if cubic boron nitride abrasive particles are used, the brazing alloy may contain at least one of the following elements that can form chemical bonds with the abrasive particles: aluminum, boron, carbon, and silicon; if alumina abrasive particles are used, the brazing alloy may contain at least one of aluminum, boron, carbon, and silicon. However, it should be recognized that, in addition to containing one or more elements that react with the abrasive particles to form chemical bonds, the brazing alloy may also contain a variety of inert elements.
[0035] Some corrosion-resistant powders are blended with brazing alloys to improve bonding properties, increase strength, enhance corrosion resistance, and reduce the cost of the matrix material. Corrosion-resistant powders may comprise metals and metal alloys, including stainless steel, titanium, titanium alloys, zirconium, zirconium alloys, nickel, and nickel alloys. More specifically, nickel alloys may include nickel-chromium alloys, comprising 80% nickel and 20% chromium by weight. Alternatively, corrosion-resistant powders may be formed from ceramic powders containing carbides such as silicon carbide or tungsten carbide.
[0036] Therefore, it should be understood that this abrasive product can have various types of abrasive elements. (See above reference.) Figures 1A to 1C The abrasive particles discussed and as referenced Figures 2A to 2B The examples of the engineered features discussed are provided for illustrative purposes only and not as limitations. Other methods may be used to arrange abrasive elements on abrasive articles, and those skilled in the art will understand that these methods are also included within the scope of this specification.
[0037] In some embodiments, the abrasive article including the substrate includes a protective layer that is non-uniformly disposed on the working surface to selectively coat the non-abrasive surface and portions of the abrasive element. The protective layer comprises materials selected from: poly(ethylene oxide), poly(propylene oxide), silicone-based polymers, methane-based polymers, polytetrafluoroethylene, polytetramethyldisiloxane, conductive polymers, poly(p-xylene) polymers, or polymers derived from photopolymerizable, electron beam-curable, or thermocurable monomers or oligomers. Examples of methane-based polymers can be found in Wang, Jia et al., “Microbial polymers produced from methane: Overview of recent progress and new perspectives,” Chapter 6 (Microbial and Natural Macromolecules. https: / / doi.org / 10.1016 / B978-0-12-820084-1.00006-5) (2021). In some embodiments, the protective layer is preferably selected from poly(p-xylene)N, poly(p-xylene)C, poly(p-xylene)D, poly(p-xylene)F, poly(p-xylene)HT, or derivatives thereof, more preferably from poly(p-xylene)N, poly(p-xylene)C, and poly(p-xylene)D. In some embodiments, the protective layer comprises an inorganic oxide. The inorganic oxide is preferably selected from alumina, titanium dioxide, silicon dioxide, or combinations thereof.
[0038] In some embodiments, the abrasive article includes: a working surface coated with a primer layer; and a protective layer unevenly disposed on the primer layer. In some embodiments, the primer layer comprises a binder material. The binder material is silicone or non-silicone. The binder material is selected from methacryloyloxypropyltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, modified silanes, non-silicones, or combinations thereof. The modified silane includes silane adhesion promoters containing functional groups, including but not limited to acrylates and methacrylates, vinyl and olefins, epoxy groups, amino groups, amines, halogens, hydrides, carboxylic acid esters, phosphonates and sulfonates, hydroxyl groups, sulfur groups, phosphine and phosphate esters, esters, acid anhydrides, azides, aldehydes, or combinations thereof. The non-silicone material may include, but is not limited to, primers based on zinc, phosphates, epoxy resins, polyesters, acrylates, and methacrylates. These non-silicone materials can be used as binders to form a primer layer. This primer layer provides improved adhesion of the protective layer to the abrasive article, thereby providing improved stability to the protective layer. Including a primer layer helps improve the adhesion of the protective layer, so that the abrasive article remains unaffected for a longer period of time in harsh corrosive environments. An exemplary primer layer is described in U.S. Patent No. 6,923,840.
[0039] method
[0040] In one embodiment, this disclosure provides a method for preparing an abrasive article (300), for example as... Figure 3As shown. The method includes step 300A, which includes obtaining a substrate (302) as described herein, wherein the substrate includes a working surface having a non-abrasive surface with abrasive elements (308) dispersed thereon. The method includes step 300B, which includes adhesively laminating the working surface using a sheet (304), the sheet being a porous sheet. The sheet may include a perforated sheet or a non-perforated sheet. In one embodiment, the sheet includes a perforated sheet. The perforated sheet is formed from a polymeric film or a non-polymeric film together with an adhesive. Adhesives used to manufacture the perforated sheet include, but are not limited to: silicone, rubber, and acrylic-based adhesives; or hot melt adhesives such as polyethylene, ethylene-vinyl acetate copolymer, polyolefins, polypropylene, and ethylene-acrylate. The film of the perforated sheet includes one of a polymeric or non-polymeric material selected from paper, polyethylene terephthalate, polyethylene, nylon, polyvinyl chloride, polypropylene, polycarbonate, or any thermosetting film. The perforated sheet is preferably made of a polymer film with an adhesive. The perforated sheet has perforations such that, during adhesive lamination of the working surface, the adhesive ends of the perforated sheet mask the top portion of the abrasive element. When laminating using this perforated sheet, the non-abrasive surface and the first portion of the abrasive element are unmasked, while the second portion or top portion of the abrasive element is masked.
[0041] The method further includes step 300C, which includes depositing a protective layer (306) on the unmasked area. The deposition of the protective layer can be performed by any of known methods, including but not limited to laser deposition, chemical vapor deposition, physical vapor deposition, electroplating, spin coating, dip coating, and multilayer lamination. The protective layer comprises a polymer or an inorganic oxide. The protective layer is coated on the unmasked area using a material selected from: poly(ethylene oxide), poly(propylene oxide), silicone-based polymers, methane-based polymers, polytetrafluoroethylene, polytetramethyldisiloxane, conductive polymers, poly(p-xylene) polymers, or polymers derived from photopolymerizable, electron beam curable, or thermocurable monomers or oligomers. In an alternative embodiment, the protective layer comprises an inorganic oxide selected from alumina, titanium dioxide, silica, or combinations thereof.
[0042] The method also includes step 300D, which includes peeling the perforated sheet from the shielding area to expose the second portion of the abrasive element.
[0043] The method optionally includes applying an adhesive material to form a primer layer before laminating the working surface to the perforated sheet. The adhesive material is selected from methacryloyloxypropyltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, modified silanes, organosilicones, or combinations thereof. The modified silane includes silane adhesion promoters containing functional groups, including but not limited to acrylates and methacrylates, vinyl and olefins, epoxy groups, amino groups, amines, halogens, hydrides, carboxylic acid esters, phosphonates and sulfonates, hydroxyl groups, sulfur groups, phosphine and phosphate esters, esters, acid anhydrides, azides, aldehydes, or combinations thereof. The organosilicones include, but are not limited to, zinc, phosphates, epoxy resins, polyesters, and primers based on acrylates and methacrylates. Organosilicones can be used as adhesives to form the primer layer.
[0044] In one embodiment, a method of preparing an abrasive article includes the following steps: A substrate including a working surface is coated with an adhesive material to form a primer layer on the working surface, the working surface having a non-abrasive surface on which abrasive elements are dispersed. The working surface is laminated together with a perforated sheet to obtain an unmasked region and a masked region, the unmasked region including a first portion of the abrasive element and the non-abrasive surface, the masked region masking a second portion of the abrasive element. A protective layer is deposited on the unmasked region, wherein the protective layer forms a conformal coating on the first portion of the abrasive element and the non-abrasive surface, and subsequently the perforated sheet is peeled off from the masked region to expose the second portion of the abrasive element, thereby obtaining an abrasive article including the protective layer selectively disposed on the working surface.
[0045] In another embodiment, this disclosure provides a method for preparing an abrasive article. The method includes the steps of: a) providing a substrate including a working surface having a non-abrasive surface on which abrasive elements are dispersed; b) providing a coating over a portion of the abrasive elements to obtain a coated abrasive element having a covered portion and an uncovered portion; c) depositing a protective layer on the working surface, wherein the protective layer forms a conformal coating on the uncovered portion of the abrasive element and the non-abrasive surface; and d) removing the coating from the covered portion of the abrasive element to obtain the abrasive article including the protective layer selectively disposed on the working surface.
[0046] In some embodiments, a method of preparing an abrasive article includes: a) providing a substrate including a working surface having a non-abrasive surface on which abrasive elements are dispersed; b) applying a silane primer over the working surface to form a primer layer; c) providing a coating over a portion of the abrasive elements to obtain a coated abrasive element having covered and uncovered portions; d) depositing a protective layer on the working surface; and e) removing the coating from the covered portion of the abrasive element to obtain the abrasive article. The protective layer is selectively disposed on the working surface and forms a conformal coating on the uncovered portion and the non-abrasive surface of the abrasive element.
[0047] In some embodiments, the method includes applying a silane primer over the work surface, wherein the silane primer is selected from methacryloxypropyltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, modified silanes, organosilicones, or combinations thereof. The modified silane includes silane adhesion promoters containing functional groups, including but not limited to acrylates and methacrylates, vinyl and olefins, epoxy groups, amino groups, amines, halogens, hydrides, carboxylic esters, phosphonates and sulfonates, hydroxyl groups, sulfur groups, phosphine and phosphate esters, esters, acid anhydrides, azides, aldehydes, or combinations thereof. The organosilicones include, but are not limited to, zinc, phosphates, epoxy resins, polyesters, and primers based on acrylates and methacrylates. The organosilicones can be used as a bonding material to form a primer layer.
[0048] In one implementation scheme, such as Figure 4 As shown, in alternative method 400, plastic or non-plastic end caps can be directly coated or covered onto the abrasive article (408). This covering step can be performed over a portion of the abrasive element to obtain a coated abrasive element (408) having a covered portion (402) and an uncovered portion (404). The coating comprises one or more layers of siloxane polymers, polyethylene terephthalate, epoxy resins, acrylates, ethylene-vinyl acetate, polypropylene, and polyethylene. In some embodiments, the coating can be transferred from a removable lamination transfer sheet.
[0049] In some embodiments, the method includes depositing a protective layer on a working surface using any of the known methods, including but not limited to laser deposition, chemical vapor deposition, physical vapor deposition, electroplating, spin coating, dip coating, and multilayer lamination. The protective layer comprises a polymer or an inorganic oxide. The protective layer is coated on the working surface using a material selected from: poly(propylene oxide), silicone-based polymers, methane-based polymers, polytetrafluoroethylene, polytetramethyldisiloxane, conductive polymers, poly(p-xylene) polymers, poly(ethylene oxide), or polymers derived from photopolymerizable, electron beam-curable, or thermosetting monomers or oligomers. In another embodiment, the protective layer comprises an inorganic oxide selected from alumina, titanium dioxide, silica, or combinations thereof. The protective layer is coated such that it selectively forms a conformal coating on the uncovered portion and the non-abrasive surface of the abrasive element. After depositing the protective layer, the coating on the covered portion of the abrasive element can be removed. In some embodiments, removing the coating from the cover portion includes polishing the cover portion of the abrasive element using a polishing pad. In some embodiments, removing the coating from the cover portion includes peeling or removing the cover portion using adhesive tape. Thus, an abrasive article is obtained having a selectively conformal coating of the protective layer on the non-abrasive surface and on the side surface of the abrasive element.
[0050] application
[0051] This disclosure discloses an abrasive article having a conformal coating on a non-abrasive surface and a localized coating on an abrasive element, which can be used in conventional chemical mechanical planarization (CMP) processes. Various materials can be polished or planarized in this conventional CMP process, including (but not limited to): copper, copper alloys, aluminum, tantalum, tantalum nitride, tungsten, titanium, titanium nitride, nickel, nickel-iron alloys, nickel silicide, germanium, silicon, silicon nitride, silicon carbide, silicon dioxide, silicon oxides, hafnium dioxide, materials with low dielectric constants, and combinations thereof. The pad dresser can be configured to be mounted on a conventional CMP tool and operated under conventional operating conditions in this CMP process. In one embodiment, the CMP process is operated with a rotational speed ranging from about 20 RPM to about 150 RPM, an applied load ranging from about 1 lb to about 90 lb, and a rate of about 1 scan per minute to about 25 scans per minute, using a conventional scan distribution (such as a sinusoidal or linear scan), scanning back and forth across the entire pad. As will be apparent to those skilled in the art who are familiar with this disclosure, other CMP process speeds and loads may also be applied.
[0052] Example
[0053] The invention is described in more detail in the following embodiments which are intended to be illustrative only, since many modifications and variations within the scope of the invention will be apparent to those skilled in the art.
[0054] Materials used
[0055] To achieve the purpose of this disclosure, the following materials are used to prepare the abrasive article.
[0056]
[0057] Example 1
[0058] Preparation of abrasive products – Method 1
[0059] A perforated sheet is used to bond and laminate a sintered abrasive (SA) dresser (substrate) containing diamond abrasive particles. A 2-mil thick VHB (Very High Bond) adhesive sheet, laminated onto a 5-mil thick PET (polyethylene terephthalate) film, is perforated using a laser to obtain perforations with an average size of 100µm to 150µm. The perforated sheet is then laminated onto the dresser at 500lb to 2000lb using a hydraulic press, creating masked and unmasked areas within the dresser. The top portion of the diamond particles is masked by the perforated sheet. The sides of the diamond particles and the non-abrasive portions of the dresser are unmasked and exposed for subsequent coating. A protective layer is then deposited onto the bonded and laminated dresser. In the Labcoater 2 PDS 2010 system (Specialty Coating Systems, Indianapolis, Indiana), a poly(p-xylene) coating is deposited using a vapor deposition polymerization (VDP) process. After the poly(p-xylene) coating is completed, the perforated sheet is removed by peeling. Therefore, the dresser is selectively coated with poly(p-xylene), resulting in a conformal coating on both the non-abrasive and diamond particle portions.
[0060] In another embodiment, a protective layer is formed by depositing alumina and titanium oxide using a vapor deposition method.
[0061] In another embodiment, a silane primer is applied to the trimmer prior to adhesive lamination. The silane primer helps improve the adhesion of the polymer coating to the trimmer.
[0062] Example 2
[0063] Preparation of abrasive products – Method 2
[0064] Abrasive articles with selectively conformal coatings having a protective layer were prepared using the method described herein. In this method, a dresser containing diamond abrasive particles is selectively masked with polyvinylsiloxane, wherein the siloxane coating is transferred and applied only to the tips of the diamond particles to form a covered portion. A layer of poly(p-xylene) is then vapor-deposited on the dresser, such that the poly(p-xylene) layer covers the uncovered portion of the diamond particles and the non-abrasive surface. The siloxane coating on the diamond particles is subsequently removed by polishing the covered portion using a polishing pad. The polishing pad is able to remove all covered tips of the diamond particles without damaging the poly(p-xylene) coating on the diamond base (uncovered portion). Therefore, the resulting dresser has a protective poly(p-xylene) coating on the uncovered portion of the diamond particles and the non-abrasive surface.
[0065] In another embodiment, a protective layer is formed by depositing alumina and titanium oxide using a vapor deposition method.
[0066] In another embodiment, a silane primer is applied to the dresser prior to the deposition of poly(p-xylene). The silane primer helps improve the adhesion of the poly(p-xylene) coating to the dresser.
[0067] Example 3
[0068] Corrosion resistance of abrasive products
[0069] The selectively coated dresser, as described in Example 1 above, was immersed at 25°C in a glass or plastic container filled with AGC 5003 chemical mechanical planarization slurry for 24 hours. The slurry was then analyzed using inductively coupled plasma atomic emission spectrometry (ICP-AES) and inductively coupled plasma mass spectrometry (ICP-MS) to detect leached metal from the dresser. The same experiment was performed on both uncoated and uniformly coated dressers, and the results are shown in Table 1.
[0070]
[0071] As can be observed from Table 1, depositing a coating on the dresser provides protection against metal leaching compared to an uncoated dresser. It has also been observed that the measured metal leaching results for both dressers with uniform coatings and dressers with non-uniform (or selective) coatings are below the detection limit.
[0072] In addition to metal leaching tests, Figure 5A graph comparing the coating coverage over time with uniformly coated and non-uniformly coated dressers is also provided. Using a benchtop-scale version of standard CMP process technology, uniformly coated and non-uniformly coated dressers were compared to determine coating loss over time when using the same CMP polishing process. As observed under magnification, the coating loss over time is significantly higher with uniformly coated dressers. A potential advantage of non-uniformly coated pad dressing is that the abrasive particles of the non-uniformly coated pad dresser can directly contact the polishing pad without any pre-dressing time to remove the coating.
Claims
1. An abrasive article, the abrasive article comprising a substrate, wherein the substrate comprises: A working surface, wherein the working surface has a non-abrasive surface on which abrasive elements are dispersed; and A protective layer is unevenly disposed on the working surface, the protective layer forming a conformal coating on the non-abrasive surface and forming a local coating on the abrasive element.
2. The abrasive article according to claim 1, wherein the abrasive article comprises a primer layer coated on the working surface, wherein the protective layer is unevenly disposed on the primer layer.
3. The abrasive article according to claim 2, wherein the primer layer comprises a binder material selected from methacryloyloxypropyltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, modified silane, non-organosilicon, or combinations thereof.
4. The abrasive article according to claim 1, wherein the abrasive element comprises one or more of engineered features and abrasive particles.
5. The abrasive article of claim 4, wherein the engineered features comprise molded and sintered ceramics spaced apart in an array on the non-abrasive surface.
6. The abrasive article according to claim 4, wherein the abrasive particles are embedded in the non-abrasive surface.
7. The abrasive article according to claim 1, wherein the abrasive element is formed of a material selected from diamond, carbides, oxides, nitrides or combinations thereof.
8. The abrasive article according to claim 1, wherein the protective layer comprises poly(ethylene oxide), poly(propylene oxide), silicone-based polymers, methane-based polymers, polytetrafluoroethylene, polytetramethyldisiloxane, conductive polymers, poly(p-xylene) polymers, or polymers derived from photopolymerizable, electron beam curable, or thermocurable monomers or oligomers.
9. The abrasive article according to claim 1, wherein the protective layer comprises an inorganic oxide, preferably selected from alumina, titanium dioxide, silicon dioxide, or a combination thereof.
10. The abrasive article of claim 1, wherein the substrate is made of a metal or metal alloy selected from the following materials: chromium, tungsten, cobalt, titanium, zinc, manganese, silicon, iron, nickel, copper, or combinations thereof.
11. A method for preparing abrasive articles, the method comprising: a. Providing a substrate, the substrate including a working surface, the working surface having a non-abrasive surface on which abrasive elements are dispersed; b. The working surface is laminated together with a perforated sheet to obtain an unmasked area and a masked area, the unmasked area including a first portion of the abrasive element and the non-abrasive surface, and the masked area masking a second portion of the abrasive element; c. Deposit a protective layer on the unmasked area, wherein the protective layer forms a conformal coating on the first portion of the abrasive element and the non-abrasive surface; as well as d. Peel the perforated sheet from the shielding area to expose the second portion of the abrasive element, and obtain the abrasive article including the protective layer selectively disposed on the working surface.
12. The method according to claim 11, wherein the method comprises: Before laminating the working surface, an adhesive material is applied over the working surface to form a primer layer.
13. The method of claim 11, wherein the perforated sheet is formed of a polymer film, a non-polymer film, or a combination thereof.
14. The method of claim 11, wherein depositing the protective layer comprises: Polymers or inorganic oxides are deposited by laser deposition, vapor deposition, electroplating, spin coating, dip coating, or multilayer lamination.
15. The method of claim 14, wherein the polymer comprises poly(p-xylene), and the inorganic oxide is selected from titanium dioxide or silicon dioxide.
16. A method for preparing abrasive articles, the method comprising: a. Providing a substrate, the substrate including a working surface, the working surface having a non-abrasive surface on which abrasive elements are dispersed; b. Provide a coating on a portion of the abrasive element to obtain a coated abrasive element having a covered portion and an uncovered portion; c. Deposit a protective layer on the working surface, wherein the protective layer forms a conformal coating on the uncovered portion of the abrasive element and the non-abrasive surface; as well as d. Remove the coating from the covered portion of the abrasive element to obtain the abrasive article comprising the protective layer selectively disposed on the working surface.
17. The method of claim 16, wherein the method comprises: Before applying the coating, a silane primer is applied over the working surface to form a primer layer.
18. The method of claim 17, wherein the coating comprises a siloxane polymer, polyethylene terephthalate, epoxy resin, acrylate, ethylene-vinyl acetate, polypropylene, polyethylene, or a combination thereof.
19. The method of claim 16, wherein removing the coating comprises: The covered portion of the abrasive element is polished using a polishing pad.
20. The method of claim 16, wherein removing the coating comprises: The covering portion of the abrasive element is removed using adhesive tape.
21. The method of claim 16, wherein depositing the protective layer comprises: Polymers or inorganic oxides are deposited by laser deposition, vapor deposition, electroplating, spin coating, dip coating, or multilayer lamination.
Citation Information