Fluorine-containing copolymer composition, method for producing the same, and fluoroelastomer article

By crushing the crosslinking agent into small particles and mixing it with fluorinated copolymers, a fluororubber with excellent heat resistance is formed, which solves the problem of insufficient heat resistance of fluororubber in the prior art and is suitable for sealing and cushioning materials in multiple industrial fields.

CN123076641APending Publication Date: 2026-11-10AGC INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202580028284.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-22
Filing Date
2025-04-16
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the prior art, the crosslinking agent in fluorinated copolymer compositions has a large particle size, which leads to insufficient heat resistance of fluororubber, especially poor performance at high temperatures.

Method used

A fluorinated copolymer composition is formed by pulverizing a crosslinking agent into solid particles with a median particle size of less than 40 μm on a volume basis and then mixing it with a fluorinated copolymer at a mixing energy of more than 10 J/g. The crosslinking agent is a polyamine compound, preferably a bisaminophenol compound.

Benefits of technology

It improves the heat resistance of fluororubber, especially with low compression set at high temperatures and excellent heat resistance, making it suitable for sealing and cushioning materials in semiconductor manufacturing, vehicles, aircraft, general machinery, construction, chemical plants and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a fluorinated copolymer composition capable of producing fluororubber articles with excellent heat resistance, a method for manufacturing the same, and fluororubber articles. The fluorinated copolymer composition of this invention comprises a fluorinated copolymer and a crosslinking agent, wherein the crosslinking agent is a polyamine compound, the fluorinated copolymer has units based on nitrile-containing monomers and units based on tetrafluoroethylene, and the crosslinking agent is a solid particle with a median particle size of less than 40 μm on a volume basis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to fluorinated copolymer compositions and methods for manufacturing the same, as well as fluororubber articles formed by crosslinking the aforementioned fluorinated copolymer compositions. Background Technology

[0002] Fluororubber products obtained by crosslinking fluorinated copolymers are widely used in semiconductor manufacturing, vehicles, aircraft, general machinery, construction, chemical plants and other fields as sealing materials and cushioning materials such as O-rings, seals, oil seals and gaskets due to their excellent heat resistance, chemical resistance, oil resistance and weather resistance.

[0003] As a method of crosslinking fluorinated copolymers, for example, from the viewpoint of improving the heat resistance of fluororubber articles, it is known to introduce units based on monomers having nitrile groups (cyano groups) into fluorinated copolymers, using nitrile groups as crosslinking sites, and to form a crosslinking structure containing an oxazole ring using a diaminophenol-based crosslinking agent (see Patent Documents 1-3).

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Publication No. 2-59177

[0007] Patent Document 2: International Publication No. 2007 / 013997

[0008] Patent Document 3: International Publication No. 2021 / 210503 Summary of the Invention

[0009] The problem the invention aims to solve

[0010] The aforementioned crosslinking agent is typically in solid form and exists as aggregated particles in the uncrosslinked state of a fluorinated copolymer composition containing the fluorinated copolymer and the crosslinking agent. Therefore, sometimes the fluorinated copolymer composition contains relatively coarse particles of the crosslinking agent (e.g., a median particle size of 50 μm or more on a volume basis).

[0011] However, the particle size of the crosslinking agent is not mentioned in existing art documents, represented by Patent Documents 1 to 3.

[0012] Therefore, the inventors investigated the effect of crosslinking agent particle size on the properties of crosslinked fluorinated copolymers, i.e., fluororubber, and found the conditions under which fluororubber with excellent heat resistance at high temperatures of around 300°C can be obtained.

[0013] The present invention was made under such circumstances, and its object is to provide a fluorinated copolymer composition capable of producing fluororubber articles with excellent heat resistance, a method for manufacturing the same, and fluororubber articles.

[0014] Solution for solving the problem

[0015] This invention is based on the discovery that the heat resistance of fluororubber articles can be improved by making the solid crosslinking agent particles of a specific size.

[0016] The present invention provides the following means.

[0017] [1] A fluorinated copolymer composition comprising a fluorinated copolymer and a crosslinking agent, said fluorinated copolymer having units based on nitrile-containing monomers and units based on tetrafluoroethylene, said crosslinking agent being a polyamine compound.

[0018] The crosslinking agent is a solid particle with a median particle size of less than 40 μm on a volume basis.

[0019] [2] The fluorinated copolymer composition according to [1], wherein the fluorinated copolymer further comprises a unit based on a perfluoroalkyl vinyl ether.

[0020] [3] The fluorinated copolymer composition according to claim [1] or [2], wherein the fluorinated copolymer is a perfluorinated polymer.

[0021] [4] The fluorinated copolymer composition according to any one of claims [1] to [3], wherein the content of the crosslinking agent is 0.1 to 10.0 parts by weight relative to 100 parts by weight of the fluorinated copolymer.

[0022] [5] The fluorinated copolymer composition according to any one of [1] to [4], wherein the crosslinking agent is a bisaminophenol compound.

[0023] [6] A method for manufacturing a fluorinated copolymer composition, wherein the fluorinated copolymer composition comprises a fluorinated copolymer and a solid crosslinking agent, the fluorinated copolymer having units based on a nitrile-containing monomer and units based on tetrafluoroethylene, and the crosslinking agent being a polyamine compound.

[0024] The manufacturing method includes the following steps: pulverizing the crosslinking agent by mixing the fluorinated copolymer and the crosslinking agent at a mixing energy of 10 J / g or higher.

[0025] [7] The method for manufacturing the fluorinated copolymer composition according to [6], wherein the crosslinking agent is pulverized into solid particles with a median particle size of less than 40 μm on a volume basis.

[0026] [8] A method for manufacturing a fluorinated copolymer composition according to any one of [1] to [5], wherein,

[0027] The fluorinated copolymer composition is obtained by mixing the fluorinated copolymer and the crosslinking agent at a mixing energy of 10 J / g or higher, thereby pulverizing the crosslinking agent.

[0028] [9] A fluororubber article, which is formed by crosslinking a fluorinated copolymer composition of any one of [1] to [5].

[0029] The effects of the invention

[0030] According to the present invention, a fluorinated copolymer composition capable of producing fluororubber articles with excellent heat resistance, a method for manufacturing the same, and fluororubber articles can be provided. Detailed Implementation

[0031] The following shows the definitions and meanings of the terms used in this specification.

[0032] The expression "X~Y" (where X and Y are numerical values) refers to a numerical range with X as the lower limit and Y as the upper limit. Within this numerical range (e.g., a range of content, etc.), the lower and upper limits recorded in stages can be combined independently. The lower and upper limits of the numerical range can be replaced with the numerical values ​​described in the examples.

[0033] A "unit" refers to the chemical structure of a single monomer molecule that makes up the polymer, and also includes some chemically transformed structures. The molar ratio of monomer-based units in fluorinated copolymers is determined by... 19 The value was calculated using F-nuclear magnetic resonance (NMR) spectroscopy.

[0034] "Rubber" refers to rubber that exhibits the properties defined by JIS K 6200:2008, as opposed to "resin".

[0035] Melting point is the temperature at which the melting peak reaches its maximum value, as determined by differential scanning calorimetry (DSC).

[0036] [Fluorine-containing copolymer composition]

[0037] The fluorinated copolymer composition of the embodiments of the present invention (hereinafter referred to as this embodiment) comprises a fluorinated copolymer and a crosslinking agent, wherein the crosslinking agent is a polyamine compound, the fluorinated copolymer has units based on a nitrile-containing monomer and units based on tetrafluoroethylene (TFE), and the crosslinking agent is a solid particle with a median particle size (hereinafter also referred to as D50) of 40 μm or less on a volume basis.

[0038] According to the fluorinated copolymer composition of this embodiment, fluororubber articles with excellent heat resistance, especially low compression set at high temperatures (e.g., 300°C), can be obtained.

[0039] (Fluorine-containing copolymer)

[0040] The fluorinated copolymer of this embodiment is a copolymer having units based on nitrile-containing monomers and TFE-based units. The fluorinated copolymer itself does not possess rubber elasticity, but acquires it through crosslinking.

[0041] From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, the content of fluorinated copolymer in the fluorinated copolymer composition is preferably 60.0 to 99.9% by mass, more preferably 70.0 to 99.9% by mass, and even more preferably 80.0 to 99.9% by mass.

[0042] From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, the unit of the monomer based on the nitrile group preferably has fluorine atoms, and more preferably is the monomer shown in the following formula (1).

[0043] CR 11 R 12 =CR 13 R 14 CN (1)

[0044] In equation (1), R 11 ~R 13 Each can be independently a hydrogen atom, a fluorine atom, or a methyl group. R 14 It is a perfluorocarbon group with 1 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon atoms.

[0045] From the perspective of good polymerization reactivity, R 11 ~R 13 Preferably, the atoms are fluorine atoms or hydrogen atoms, and more preferably, they are all fluorine atoms or hydrogen atoms. From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorine-containing copolymers, it is particularly preferred that they are all fluorine atoms.

[0046] R 14 It can be any of linear, branched, and cyclic forms, but from the viewpoint of good polymerization reactivity, linear or branched forms are preferred. 14 The number of carbon atoms is preferably 2 to 8, more preferably 3 to 7, even more preferably 3 to 6, and even more preferably 3 to 5.

[0047] From the perspective of the good rubber elasticity of fluororubber obtained by crosslinking fluorinated copolymers, R 14 Preferably, it has an ether-like oxygen atom. R 14 The number of ether oxygen atoms in the ether is preferably 1 to 3, more preferably 1 or 2.

[0048] Specific examples of nitrile-containing monomers include CF2=CFOCF2CF(CF3)OCF2CF2CN (abbreviated as 8CNVE), CF2=CFO(CF2)5CN (abbreviated as MV5CN), CF2=CFOCF2CF2CF2OCF(CF3)CN, and CF2=CFO(CF2)3CN. A single nitrile-containing monomer can be used, or two or more can be used in combination. From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, 8CNVE and MV5CN are preferred, with 8CNVE being more preferred.

[0049] From the viewpoint of the good rubber elasticity and heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, fluorinated copolymers preferably have units based on perfluoroalkyl vinyl ethers (PAVE) in addition to units based on nitrile monomers and TFE-based units.

[0050] From the viewpoint of good polymerization reactivity and good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, PAVE is preferably the monomer shown in the following formula (2).

[0051] CF2 = CF - OR f2 (2)

[0052] In equation (2), R f2 It is a perfluoroalkyl group with 1 to 10 carbon atoms. Perfluoroalkyl groups can be linear or branched. From the viewpoint of good polymerization reactivity, R... f2 The number of carbon atoms is preferably 1 to 8, more preferably 1 to 6, further preferably 1 to 5, and even more preferably 1 to 3.

[0053] Specific examples of PAVE include perfluoromethyl vinyl ether (PMVE), perfluoroethyl vinyl ether (PEVE), and perfluoropropyl vinyl ether (PPVE). PAVE can be used alone or in combination with two or more. From the viewpoint of good polymerization reactivity and ease of acquisition, PMVE and PPVE are preferred, with PMVE being more preferred.

[0054] From the viewpoint of the good rubber elasticity and heat resistance of crosslinked fluororubber, in addition to units based on monomers containing nitrile groups and units based on TFE, fluoropolymers can also have units based on other monomers, in addition to units based on monomers containing nitrile groups and units based on TFE.

[0055] Other monomers include, for example, vinylidene fluoride (VdF), hexafluoropropylene, trifluorochloroethylene, monomers having two or more polymerizable unsaturated bonds (DV), monomers shown in formula (6) below, ethylene, propylene, etc. In addition, monomers having halogen atoms other than those mentioned above (e.g., bromotrifluoroethylene, iodotrifluoroethylene) can also be cited as monomers.

[0056] Examples of polymerizable unsaturated bonds in a fluoropolymer (DV) include carbon-carbon double bonds (C=C) and carbon-carbon triple bonds (C≡C). From the viewpoint of good polymerization reactivity, the number of polymerizable unsaturated bonds in the DV is preferably 2 to 6, more preferably 2 or 3, and particularly preferably 2. From the viewpoint of good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, the DV preferably has fluorine atoms.

[0057] From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, DV is preferably the monomer shown in the following formula (3).

[0058] (CR 31 R 32 =CR 33 ) a3 R 34 (3)

[0059] In equation (3), R 31 ~R 33 Each atom can be independently a hydrogen atom, a fluorine atom, a methyl group, or a trifluoromethyl group. a3 is an integer from 2 to 6. R 34 It is a perfluorocarbon group with 1 to 10 carbon atoms in the α3 valence, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon atoms.

[0060] Multiple R 31 ~R 33 They can be the same or different, but being the same is preferred. From the viewpoint of good polymerization reactivity, R 31 ~R 33 Preferably, the atoms are fluorine atoms or hydrogen atoms, and more preferably, they are all fluorine atoms or hydrogen atoms. From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorine-containing copolymers, it is particularly preferred that they are all fluorine atoms.

[0061] a3 is preferably 2 or 3, and particularly preferably 2.

[0062] R 34 It can be any of linear, branched, and cyclic forms. From the viewpoint of good polymerization reactivity, linear or branched forms are preferred, and linear forms are more preferred. 34 The number of carbon atoms is preferably 2 to 10, more preferably 3 to 8, even more preferably 3 to 6, and even more preferably 3 to 5.

[0063] From the perspective of the good rubber elasticity of fluororubber obtained by crosslinking fluorinated copolymers, R 34 Preferably, it has an ether-like oxygen atom. R 34 The number of ether oxygen atoms in the form is preferably 1 to 3, more preferably 1 or 2. 34 The ether oxygen atom in R is preferably associated with R. 34 The terminal carbon atoms are bonded.

[0064] For DV, among the monomers shown in formula (3), the monomers shown in formula (4) or (5) below are more preferred.

[0065] (CF2=CF)2R 41 (4)

[0066] (CH2=CH)2R 51 (5)

[0067] In equation (4) or (5), R 41 and R 51 It is a perfluorocarbon group with 2 to 10 carbon atoms in a divalent state, or a group having an ether-like oxygen atom at the end of the perfluorocarbon group or between carbon atoms.

[0068] As specific examples of DV, examples can be given for the monomers shown in equation (4): CF2=CFO(CF2)2OCF=CF2, CF2=CFO(CF2)3OCF=CF2, CF2=CFO(CF2)4OCF=CF2, CF2=CFO(CF2)6OCF=CF2, CF2=CFO(CF2)8OCF=CF2, CF2=CFO(CF2)2OCF(CF3)CF2OCF=CF2, CF2=CFO(CF2)2O[CF(CF3)CF2O]2CF=CF2, CF2=CFO CF2O(CF2CF2O)2CF=CF2, CF2=CFO(CF2O)3O[CF(CF3)CF2O]2CF=CF2, CF2=CFOCF2CF(CF3)O(CF2)2OCF(CF3)CF2OCF=CF2, CF2=CFO(CF2)2O(CF2O)2(CF2)2OCF=CF2, or CH2=CH(CF2)2CH=CH2, CH2=CH(CF2)4CH=CH2, CH2=CH(CF2)6CH=CH2 in the monomers shown in formula (5). DV can use one or more of these monomers. Among them, CF2=CFO(CF2)3OCF=CF2, CF2=CFO(CF2)4OCF=CF2, and CH2=CH(CF2)6CH=CH2 are preferred.

[0069] Equation (6) is shown below.

[0070] CF2 = CF - OR f6 (6)

[0071] In equation (6), R f6 It is a perfluoroalkyl group having 1 to 8 carbon atoms and containing 1 to 5 ether-containing oxygen atoms. R f6 The number of carbon atoms is preferably 1 to 6, more preferably 1 to 5.

[0072] Specific examples of the monomers shown in formula (6) include perfluorinated (3,6-dioxa-1-heptene), perfluorinated (3,6-dioxa-1-octene), and perfluorinated (5-methyl-3,6-dioxa-1-nonene).

[0073] From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, the content of units based on nitrile monomers in all units of the fluorinated copolymer is preferably 0.05 to 5 mol%, more preferably 0.1 to 3 mol%, and even more preferably 0.2 to 1.5 mol%.

[0074] From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, the content of TFE units in all units of the fluorinated copolymer is preferably 60-80 mol%, more preferably 63-75 mol%, and even more preferably 66-72 mol%.

[0075] When the fluorinated copolymer contains PAVE units, from the viewpoint of the good rubber elasticity and heat resistance of the fluororubber obtained by crosslinking the fluorinated copolymer, the content of PAVE units in all units is preferably 19 to 39 mol%, more preferably 24 to 36 mol%, and even more preferably 27 to 33 mol%. The same content is preferred when PAVE is PMVE, PEVE, or PPVE, or when it is a mixture of two or more of them.

[0076] In the case where the fluorinated copolymer contains units based on other monomers in addition to units based on nitrile monomers, TFE-based units and PAVE-based units, from the viewpoint of the good heat resistance of the fluororubber obtained by crosslinking the fluorinated copolymer, the content of units based on other monomers in all units is preferably 0.01 to 10 mol%, more preferably 0.05 to 10 mol%, and even more preferably 0.1 to 5 mol%.

[0077] From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, fluorinated copolymers are preferably perfluorinated polymers.

[0078] The glass transition temperature of the fluorinated copolymer is preferably -20~20℃, more preferably -10~10℃, and even more preferably -5~5℃.

[0079] The glass transition temperature of fluorinated copolymers varies depending on the type of monomers constituting the copolymer, the unit composition based on those monomers, and the molecular weight. For example, the higher the proportion of TFE-based units, the higher the glass transition temperature of the fluorinated copolymer tends to be.

[0080] The glass transition temperature can be determined using a differential scanning calorimeter (DSC). Specifically, it can be determined using the method described in the examples.

[0081] (Method for manufacturing fluorinated copolymers)

[0082] There are no particular limitations on the manufacturing method of fluorinated copolymers; well-known methods can be used. For example, in the presence of a free radical polymerization initiator, the monomers constituting the units of the fluorinated copolymer can be copolymerized by emulsion polymerization, solution polymerization, suspension polymerization, etc.

[0083] Free radical polymerization initiators can be substances known in the manufacture of fluorinated copolymers, and can be appropriately selected according to the polymerization method.

[0084] In emulsion polymerization in aqueous media such as water, water-soluble free radical polymerization initiators are preferred. Examples include persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate, disuccinate peroxide, azobisisobutyramidine dihydrochloride, tert-butyl hydroperoxide, and dicarbonate peroxides. Among these, persulfates are preferred, and ammonium persulfate is more preferred. Alternatively, redox polymerization initiators composed of persulfates or hydroperoxide combined with reducing agents such as sodium bisulfite and sodium thiosulfate can be used, and / or small amounts of metals or metal compounds such as iron, ferrous salts, and silver sulfate can be further incorporated into the redox polymerization initiator.

[0085] As free radical polymerization initiators in solution polymerization using solvents such as 1H-perfluorohexane, organic peroxides such as bis(pentafluoropropionyl) peroxide, tert-butyl peroxypentanoate, and diisopropyl peroxydicarbonate can be used.

[0086] The addition of the free radical polymerization initiator can be done all at once or in stages. The amount of free radical polymerization initiator used relative to 100 parts by mass of all monomers involved in the polymerization reaction is preferably 0.0001 to 3 parts by mass, more preferably 0.001 to 2 parts by mass, and even more preferably 0.01 to 1 part by mass.

[0087] A pH buffer can be added to the reaction system. Examples of pH buffers include disodium hydrogen phosphate, sodium dihydrogen phosphate, sodium bicarbonate, sodium carbonate, and their hydrates.

[0088] Examples of emulsifiers used in emulsion polymerization include hydrocarbon-based emulsifiers such as sodium dodecyl sulfate and sodium dodecylbenzene sulfonate; ammonium perfluorooctanoate, sodium perfluorooctanoate, ammonium perfluorohexanoate, CF3(CF2)2O(CF(CF3)CF2O)2CF(CF3)COONH4, CF3(CF2)2OCF(CF3)CF2OCF(CF3)COONH4, CF3(CF2)2O(CF2)2OCF2COONH4, and CF3(CF2)2O(CF2)2COONH4. CF2O)2CF2COONH4, CF3(CF2)3OCF2CF2OCF2COONH4, CF3(CF2)3O(CF2CF2O)2CF2COONH4, CF3(CF2)2O(CF2) 2OCF2COONa, CF3(CF2)2O(CF2CF2O)2CF2COONa, CF3(CF2)3OCF2CF2OCF2COONa, CF3(CF2)3O(CF2CF2O)2CF 2COONa, C2F5O(CF2)2OCF2COONH4 (EEA-NH4 for short), C2F5O(CF2CF2O)2CF2COONH4, C2F5O(CF2)2OCF2COONa, C2 F5O(CF2CF2O)2CF2COONa, CF3O(CF2)3OCF2COONH4, CF3O(CF2)3OCF(CF3)COONH4, CF3O(CF2)3OCF2COONa, Fluorinated emulsifiers include CF3O(CF2)3OCF(CF3)COONa, CF3O(CF2O)3CF2COONH4, CF3O(CF2O)3CF2COONa, CF3OCF(CF3)CF2OCF(CF3)COONH4, CF3OCF(CF3)CF2OCF(CF3)COONa, CF3O(CF2CF2O)2CF2COONH4, and CF3O(CF2CF2O)2CF2COONa. One emulsifier can be used alone, or two or more can be used in combination. Preferred emulsifiers include ammonium perfluorooctanoate, CF3(CF2)3O(CF2)2OCF2COONH4, CF3(CF2)2O(CF2)2OCF2COONH4, EEA-NH4, and CF3O(CF2)3OCF2COONH4.

[0089] The emulsifier can be added all at once or in stages. The amount of emulsifier used relative to 100 parts by weight of the aqueous medium is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 15 parts by weight, and even more preferably 0.1 to 10 parts by weight.

[0090] The raw material mixture may be substantially free of water-soluble emulsifiers. "Substantially free of emulsifiers" means that the emulsifier content in the raw material mixture is 0.03 ppm by mass or less, preferably 0.02 ppm by mass or less, and more preferably 0 ppm by mass.

[0091] The pressure and temperature conditions of the polymerization reaction are appropriately set according to the monomer composition and the decomposition temperature of the free radical polymerization initiator. Typically, the pressure is preferably 0.1~20 MPaG, more preferably 0.3~10 MPaG, and even more preferably 0.3~5 MPaG. The temperature is preferably 0~100℃, more preferably 10~90℃, and even more preferably 20~85℃.

[0092] In emulsion polymerization, fluorinated copolymers are obtained in the form of latex, which can be purified by appropriate coagulation.

[0093] In the case of solution polymerization, purification can be achieved by washing with an aqueous medium such as methanol.

[0094] There are no particular limitations on the aggregation method of fluorinated copolymers. Examples include freeze aggregation, acid aggregation, alkali aggregation, mechanical aggregation, and aggregation using coagulants.

[0095] In the case of freeze-coagulation, the coagulation temperature is preferably -20 to 0°C. The coagulation time is preferably 1 hour or more, more preferably 2 hours or more.

[0096] In the case of acid coagulation, examples of added acids include hydrochloric acid, nitric acid, sulfuric acid, oxalic acid, and hydrofluoric acid, with nitric acid being preferred. The concentration of the added acid is preferably 0.1 to 50% by mass, more preferably 1 to 30% by mass, and even more preferably 1 to 10% by mass.

[0097] In the case of alkali coagulation, examples of alkali added include sodium hydroxide, potassium hydroxide, and ammonium carbonate, with sodium hydroxide being preferred. The concentration of the alkali added is preferably 0.1 to 50% by mass, more preferably 1 to 30% by mass, and even more preferably 1 to 10% by mass.

[0098] When using a coagulant for coagulation, known coagulants can be used, such as aluminum salts, calcium salts, and magnesium salts. Specifically, aluminum sulfate, alum represented by the general formula M'Al(SO4)2·12H2O [where M' is a monovalent cation other than lithium], calcium nitrate, and magnesium sulfate are examples, with alum being preferred, and potassium alum, where M' is potassium, being more preferred.

[0099] (Cross-linking agent)

[0100] The crosslinking agent in the fluorinated copolymer composition of this embodiment is a polyamine compound, which is a solid particle with a D50 of less than 40 μm.

[0101] By using such a crosslinking agent to crosslink fluorinated copolymers, fluororubber articles with excellent heat resistance can be obtained.

[0102] It should be noted that solid particles refer to particles that are solid in the uncrosslinked state of the fluorinated copolymer composition. From the viewpoint of easily controlling the crosslinking reaction, the melting point of the crosslinking agent is preferably 80~400℃, more preferably 100~350℃, and even more preferably 120~300℃.

[0103] Polyamine compounds are compounds having two or more amino groups per molecule, and these amino groups can form a crosslinking structure with the nitrile groups of fluorinated copolymers. From the viewpoint of obtaining fluororubber articles with excellent heat resistance, crosslinking agents are preferably crosslinking agents capable of forming crosslinking structures containing oxazole rings or imidazole rings. From the viewpoint of heat resistance and crosslinking density, crosslinking agents capable of forming crosslinking structures containing oxazole rings are more preferred. As a crosslinking agent capable of forming crosslinking structures containing oxazole rings, bisaminophenol compounds are preferred, for example.

[0104] From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, polyamine compounds preferably contain fluorine atoms.

[0105] Specific examples of crosslinking agents include 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (abbreviated as BOAP, also known as bisaminophenol AF; melting point 243°C), 2,2-bis(3-amino-4-anilinephenyl)hexafluoropropane (abbreviated as NPh-AF; melting point 177~178°C), 3,3'-diaminobenzidine (melting point 179°C), the compound obtained in Synthesis Example 1 of International Publication No. 2022 / 230706 (melting point 179°C), the compound obtained in Synthesis Example 2 (melting point 134°C), and the compound obtained in Synthesis Example 3 (melting point 249°C), 4,4'-methylenediphenylamine (melting point 92°C), m-phenylenediamine (melting point 64~66°C), adipic acid dihydrazide (melting point 182°C), and (CF2)6[C(NH2)=NC(=NH)(CF2)5CF3]2, etc. From the viewpoint of the good heat resistance of fluororubber obtained by crosslinking fluorinated copolymers, BOAP and NPh-AF are preferred, and BOAP is more preferred.

[0106] The crosslinking agent exists in the fluorinated copolymer composition as solid particles with a D50 of less than 40 μm.

[0107] Here, the D50 of the crosslinking agent in this embodiment refers to the D50 of the volume-based particle size distribution when 200 aggregated particles identified by optical microscopy are extracted from a sheet sample of the fluorinated copolymer composition in a specified uncrosslinked state and assumed to be spheres with the longest diameter of the aggregated particles as the diameter. Specifically, it can be determined by the method described in the examples.

[0108] By ensuring that the D50 of the crosslinking agent in the fluorinated copolymer composition is below 40 μm, the specific surface area of ​​the solid particles of the crosslinking agent is large, and the crosslinking reaction of the fluorinated copolymer can easily proceed at a uniform and moderate rate. As a result, it is predicted that fluororubber articles with improved crosslinking density and excellent heat resistance can be obtained.

[0109] From the viewpoint of ensuring that the crosslinking reaction of the fluorinated copolymer used to obtain fluororubber articles with excellent heat resistance is carried out appropriately, the D50 of the crosslinking agent is preferably 2.0 to 35 μm, more preferably 5.0 to 30 μm, and even more preferably 6.0 to 28 μm.

[0110] From the viewpoint of achieving sufficient crosslinking density and good heat resistance in fluororubber obtained by crosslinking fluorinated copolymers, the content of crosslinking agent in the fluorinated copolymer composition is preferably 0.1 to 10 parts by weight, more preferably 0.3 to 5 parts by weight, and even more preferably 0.5 to 3 parts by weight relative to 100 parts by weight of the fluorinated copolymer.

[0111] (Other ingredients)

[0112] Without impairing the effects of the present invention, the fluorinated copolymer composition may contain other components besides the fluorinated copolymer and the crosslinking agent. Examples of other components include fillers and reinforcing materials (e.g., carbon black, barium sulfate, calcium metasilicate, calcium carbonate, titanium dioxide, silica, clay, talc, etc.), scorch retarders (e.g., compounds containing phenolic hydroxyl groups such as bisphenol A, quinones such as hydroquinone, α-methylstyrene dimers such as 2,4-di(3-isopropylphenyl)-4-methyl-1-pentene, etc.), crown ethers (e.g., 18-crown-6), release agents (e.g., sodium stearate), pigments, etc. Other components may be used individually or in combination of two or more.

[0113] When the fluorinated copolymer composition contains other components, the total content of the other components relative to 100 parts by weight of the fluorinated copolymer is preferably more than 0 parts by weight and less than 30 parts by weight, more preferably less than 25 parts by weight, and even more preferably less than 20 parts by weight.

[0114] [Method for manufacturing fluorinated copolymer compositions]

[0115] The method for manufacturing the fluorinated copolymer composition of this embodiment is a method for manufacturing a fluorinated copolymer composition comprising a fluorinated copolymer and a solid crosslinking agent, wherein the fluorinated copolymer has units based on a nitrile-containing monomer and units based on TFE, and the crosslinking agent is a polyamine compound. The manufacturing method includes the following steps: pulverizing the crosslinking agent by mixing the fluorinated copolymer and the crosslinking agent at a mixing energy of 10 J / g or more.

[0116] By going through this mixing process, a fluorinated copolymer composition in which the solid crosslinking agent is fully pulverized and dispersed can be obtained, resulting in fluororubber products with excellent heat resistance.

[0117] The fluorinated copolymer and crosslinking agent in the manufacturing method of this embodiment are preferably the same as those in the fluorinated copolymer composition described above. Furthermore, other components that may be included in the fluorinated copolymer composition are also the same as those described above.

[0118] The method for manufacturing the fluorinated copolymer composition of this embodiment can be achieved by mixing the fluorinated copolymer of this embodiment and the crosslinking agent of this embodiment at a mixing energy of 10 J / g or more, thereby pulverizing the crosslinking agent and obtaining the fluorinated copolymer composition of this embodiment.

[0119] Solid crosslinking agents can be pre-crushed, but from the viewpoint of uniform mixing with fluorinated copolymers and the manufacturing efficiency of fluorinated copolymer compositions, it is preferable to crush them during the mixing process with fluorinated copolymers.

[0120] The crosslinking agent is pulverized into solid particles with a D50 preferably below 40 μm, more preferably 2.0 to 35 μm, further preferably 5.0 to 30 μm, and even more preferably 6.0 to 30 μm.

[0121] From the viewpoint of ease of operation, the D50 of the crosslinking agent in solid form before being crushed by mixing with the fluorinated copolymer is preferably 1000 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0122] From the viewpoint that the crosslinking agent is pulverized and uniformly dispersed in the fluorinated copolymer composition during the process of compounding with the fluorinated copolymer as described above, the compounding energy when compounding the fluorinated copolymer with the crosslinking agent is set to 10 J / g or more, preferably 100 to 15000 J / g, more preferably 500 to 10000 J / g, even more preferably 1000 to 7500 J / g, and particularly preferably 1500 to 6500 J / g.

[0123] The mixing process can be performed once or more than twice. The mixing energy is the sum of the mixing energy of each process.

[0124] As a means of mixing fluorinated copolymers with crosslinking agents, known rubber mixing equipment can be used, such as rollers, kneaders, Banbury mixers, single-screw or twin-screw extrusion mixers, etc. Extrusion mixers can be used individually or multiple extrusion mixers of the same or different types can be connected in series. From the viewpoint of providing sufficient mixing energy, twin-screw extrusion mixers are preferred. Examples of twin-screw extrusion mixers include non-meshing co-rotating, meshing co-rotating, non-meshing counter-rotating, and meshing counter-rotating types.

[0125] Specific examples of extrusion mixing machines include "HAAKE Minilab II" (manufactured by Thermo Fisher Scientific), "Labo Plastomill" (manufactured by Toyo Seiki Co., Ltd.), and "Plastics Labo Station" (manufactured by Brabender).

[0126] To obtain a fluorinated copolymer containing a solid crosslinking agent, the mixing temperature (chamber temperature) is set below the melting point of the crosslinking agent. The melting point of the crosslinking agent is as described above. The mixing temperature is preferably above the glass transition temperature of the fluorinated copolymer.

[0127] The mixing temperature is preferably 20~100℃, more preferably 30~85℃.

[0128] From the viewpoint of thorough mixing and pulverization of the crosslinking agent, the mixing time (residence time in the mixing apparatus) is preferably 1 to 120 minutes, more preferably 20 to 60 minutes. When the residence time in the mixing apparatus is 1 to 120 minutes, the screw speed is preferably 50 to 2000 rpm, more preferably 500 to 1500 rpm.

[0129] [Fluororubber products]

[0130] The fluororubber article of this embodiment is formed by crosslinking the fluorinated copolymer composition of this embodiment described above.

[0131] The fluororubber article of this embodiment exhibits particularly low high-temperature compression set and excellent heat resistance. Specifically, the high-temperature compression set under the conditions of 300°C, a compression ratio of 16.7%, and a holding time of 70 hours is preferably 48% or less, more preferably 45% or less, and even more preferably 40% or less. More specifically, the high-temperature compression set is measured using the method described in the examples.

[0132] Examples of crosslinking methods for fluorinated copolymer compositions include heating and radiation irradiation, with heating being the preferred method. Examples of heating methods include hot pressing, steam, and hot air. Examples of radiation used in radiation irradiation include electron beams and ultraviolet light. The crosslinking method is selected appropriately based on the form and intended use of the fluororubber article.

[0133] In heat-based crosslinking, for example, heating at 80–300°C for 0.1–24 hours. Alternatively, after initial crosslinking by temporary heating, a secondary crosslinking process can be performed by further heating at a different temperature. From the viewpoint of ensuring a moderate crosslinking reaction, it is preferable, for example, to perform a primary crosslinking at 80–200°C for 0.1–6 hours, followed by a secondary crosslinking at 200–300°C for 1–24 hours. By performing secondary crosslinking, the high-temperature compression set and other rubber properties of fluororubber articles can be stabilized or improved.

[0134] Temperature control can also involve raising or lowering the temperature in stages.

[0135] During a single crosslinking process, the fluorinated copolymer composition can be appropriately shaped.

[0136] Examples of molding methods include compression molding, injection molding, extrusion molding, calendering, and molding by dissolving in a solvent and impregnating or coating onto a substrate.

[0137] The fluororubber articles of this embodiment are suitable, for example, as sealing materials and cushioning materials such as O-rings, V-rings, seals, oil seals, gaskets, diaphragms, and sealing sheets. Furthermore, they can be suitably applied to various applications including heat-resistant and chemical-resistant sealing materials, heat-resistant and oil-resistant sealing materials, wire sheathing materials, sealing materials for semiconductor devices, corrosion-resistant rubber coatings, urea-based grease-resistant sealing materials, rubber coatings, adhesive rubber, hoses, pipes, calendered sheets (rollers), sponges, rubber rollers, components for oil excavation, heat sinks, solution crosslinking agents, rubber sponges, bearing seals, liners, automotive insulating sheets, insulating sheets for electronic devices, rubber belts for watches, endoscope seals, corrugated hoses, water heater seals / valves, fender materials, fiber / non-woven fabrics (protective clothing, etc.), base sealing materials, rubber gloves, stators for single-shaft eccentric screw pumps, components for urea SCR systems, vibration damping agents, shock absorbers, sealants, additives in other materials, toys, and more.

[0138] Example

[0139] The present invention will now be described in detail based on embodiments, but the present invention is not limited to the following embodiments, and various modifications can be made without departing from the spirit of the present invention.

[0140] [Compounds used]

[0141] The following is a description of the abbreviations of the various compounds used.

[0142] • EEA-NH4: Perfluoro(2-ethoxy-ethoxy)ammonium acetate (C2F5O(CF2)2OCF2COONH4), emulsifier

[0143] ·8CNVE: Perfluoro(8-cyano-5-methyl-3,6-dioxa-1-octene)(CF2=CFCF2CF(CF3)OCF2CF2CN)

[0144] TFE: Tetrafluoroethylene

[0145] PMVE: Perfluoromethyl vinyl ether

[0146] • APS: Ammonium persulfate

[0147] • BOAP: 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, manufactured by Tokyo Chemical Industry Co., Ltd.; crosslinking agent, D50: 50μm

[0148] Synthesis of Fluorinated Copolymers

[0149] After degassing in a 20L stainless steel pressure reactor equipped with anchor blades, 7.2L of ultrapure water, 880g of a 30% (w / w) aqueous solution of EEA-NH4, 7.3g of 8CNVE, and 15.9g of a 5% (w / w) aqueous solution of disodium hydrogen phosphate dodecahydrate were added. After purging the reactor with nitrogen, 137g of TFE and 635g of PMVE were added under pressure while stirring with anchor blades (375 rpm), raising the reactor temperature to 80°C. The reactor pressure was 0.90 MPaG. 28mL of a 3% (w / w) aqueous solution of APS was added to the reactor to begin polymerization (the molar ratio of monomers before polymerization was TFE / PMVE / 8CNVE = 26.3 / 73.3 / 0.4).

[0150] During polymerization, TFE is injected when the reactor pressure reaches 0.89 MPaG, and the pressure is increased to 0.90 MPaG. This operation is repeated, with 3.7 g of 8CNVE, 74 g of PMVE, and 3.7 g of 8CNVE added sequentially whenever the total amount of TFE injected reaches 119.3 g.

[0151] Additionally, when the polymerization rate decreases, add an appropriate amount of 3% (by mass) aqueous solution of APS (total additional addition amount 35 mL).

[0152] When the total TFE injection reached 1073.7g, the additional injection of each monomer was completed, and 119.3g of TFE was injected, ending the additional monomer injection (total additional monomers: TFE 1193g, PMVE 666g, 8CNVE 66.6g). The reactor temperature was then lowered to 10℃ to stop the polymerization reaction, yielding a latex containing the fluorinated copolymer (polymerization time 6.25 hours; additional monomer molar ratio TFE / PMVE / 8CNVE = 74.0:25.0:1.0).

[0153] The obtained latex was added to a 5% (w / w) aqueous solution of potassium aluminum sulfate to cause the fluorinated copolymer to agglomerate. The fluorinated copolymer was separated by filtration, washed with ultrapure water, and then vacuum dried at 50°C to obtain a white fluorinated copolymer (based on the molar ratio of TFE unit / PMVE unit / 8CNVE unit = 69.1:30.3:0.6, glass transition temperature -3°C).

[0154] It should be noted that the glass transition temperature was determined by DSC as follows.

[0155] A 10 mg sample of the fluorinated copolymer was cooled from room temperature (25 °C) to -30 °C at a cooling rate of -10 °C / min, and then heated to 350 °C at a heating rate of 10 °C / min. Based on a curve plotted with heat flux [mW] on the vertical axis and temperature [ °C] on the horizontal axis, the temperature at which the minimum heat flux deviates from the baseline during heating was identified was taken as the glass transition temperature of the fluorinated copolymer.

[0156] [Example 1]

[0157] 100 parts by weight of the fluorinated copolymer and 1.0 parts by weight of BOAP (total 20.2 g) obtained above were fed into a twin-screw extruder ("HAAKE Minilab II", Thermo Fisher Scientific KK) and mixed under the conditions of chamber temperature 40°C, screw speed 100 rpm and residence time 48 minutes to prepare the fluorinated copolymer composition.

[0158] The obtained fluorinated copolymer composition was put into a mold. While degassing the mold with a diaphragm pump, it was heated and compressed at 180°C for 20 minutes with a hydraulic press ("SA-301 50T type", made by TESTER SANGYO CO., LTD., with a plunger diameter of 180 mm; the same applies below) to produce an O-ring (P-12) (a primary crosslink).

[0159] The O-ring was placed in an inert oven (“DN411I”, manufactured by Yamato Scientific Co., Ltd.) and heated at 90°C for 2 hours under a nitrogen atmosphere. Then, the temperature was increased to 200°C over a period of 2 hours and held for 4 hours. Subsequently, the temperature was increased to 305°C over a period of 2 hours and held for 12 hours, thereby producing a fluororubber O-ring test piece (secondary crosslinking).

[0160] [Examples 2~4]

[0161] Fluorinated copolymer compositions were prepared under the mixing conditions shown in Table 1, except that those in Example 1, to produce O-ring test pieces of fluororubber.

[0162] [Measurement and Evaluation]

[0163] The torque and mixing energy during the mixing operation were measured in each case, as well as the D50 of the crosslinking agent in the fluorinated copolymer composition and the high-temperature compression set of the O-ring test piece.

[0164] The determination methods are described below. The determination results are shown in Table 1. In Table 1, Examples 1-3 are exemplary cases, and Example 4 is a comparative case.

[0165] (Mixed Energy)

[0166] The work per unit mass (W[J / g]) of the fluorinated copolymer composition calculated by the following formula (I) is used as the mixing energy, based on the mixing conditions (mass of the fluorinated copolymer composition (m[g]), screw speed (r[rpm]), residence time (t[min])) and torque value (T[N·m]) during mixing of the fluorinated copolymer in a twin-screw extruder.

[0167] W = 2π × r × T × t / m (I)

[0168] It should be noted that the torque value T is set as the torque output value when the fluorinated copolymer composition has been filled into the chamber of the biaxial extrusion mixer. The residence time t is the time measured by a timer from the moment when the filling of the fluorinated copolymer and crosslinking agent into the chamber is completed until the end of the mixing operation.

[0169] (Median particle size (D50) of the crosslinking agent based on volume)

[0170] 0.5 g of the fluorinated copolymer composition was heated and compressed for 5 minutes at 60°C and 0.4 MPa using a hydraulic press. The resulting uncrosslinked sheet sample (0.125 mm thick) was observed perpendicularly to the sheet plane under coaxial epi-illumination using an optical microscope (“VHX-8000”, “VHX-E100” lens, KEYENCE Co., Ltd.; magnification 500x).

[0171] The agglomerated particles identified in the observed images were considered cross-linking agents, and 200 agglomerated particles were extracted. If fewer than 200 agglomerated particles could be identified, uncross-linked sheet samples were further prepared, and a total of 200 agglomerated particles were extracted. The agglomerated particles were assumed to be spheres with the longest diameter in the observed images, and the D50 was calculated.

[0172] It should be noted that, for the preparation of fluorinated copolymer compositions, the D50 is calculated in the same way as above from the observation image directly unfolded on the stage of an optical microscope before use of BOAP.

[0173] (High-temperature compression set)

[0174] For the O-ring test piece (nominal number P12; according to JIS B 2401-1:2012), the high-temperature compression set was determined using the method with reference to JIS K 6262:2013.

[0175] The O-ring test piece (thickness h0 (wire diameter) 2.4mm) was compressed using a compression device (spacer thickness h). s The sample was compressed to 2.0 mm and held at 300°C with a compression ratio of 16.7% for 70 hours. After being removed from the compression device, the sample was left to stand at room temperature (23°C) for 30 minutes, and the thickness (h1 [mm]) of the test piece was measured. The high-temperature compression set CS [%] was calculated using the arithmetic mean of the measurements from two points on the test piece by the following formula (II).

[0176] CS=(h0-h1) / (h0-h s )×100

[0177] =(2.4-h1)×250 (II)

[0178] The smaller the permanent deformation under high-temperature compression, the better the heat resistance.

[0179] [Table 1]

[0180]

[0181] As shown in Table 1, it was confirmed that when the D50 of the crosslinking agent in the fluorinated copolymer composition is 40 μm or less, the high-temperature compression set of the obtained fluororubber articles is reduced (Examples 1-3). Furthermore, it was confirmed that by mixing the fluorinated copolymer composition at a mixing energy of 10 J / g or more, the D50 of the crosslinking agent in the fluorinated copolymer composition can be reduced to 40 μm or less.

Claims

1. A fluorinated copolymer composition comprising a fluorinated copolymer and a crosslinking agent, said fluorinated copolymer having units based on a nitrile-containing monomers and units based on tetrafluoroethylene, said crosslinking agent being a polyamine compound. The crosslinking agent is a solid particle with a median particle size of less than 40 μm on a volume basis.

2. The fluorinated copolymer composition according to claim 1, wherein, The fluorinated copolymer also has units based on perfluoroalkyl vinyl ethers.

3. The fluorinated copolymer composition according to claim 1, wherein, The fluorinated copolymer is a perfluorinated polymer.

4. The fluorinated copolymer composition according to claim 1, wherein, The content of the crosslinking agent is 0.1 to 10.0 parts by weight relative to 100 parts by weight of the fluorinated copolymer.

5. The fluorinated copolymer composition according to claim 1, wherein, The crosslinking agent is a bisaminophenol compound.

6. A method for manufacturing a fluorinated copolymer composition, wherein, The fluorinated copolymer composition comprises a fluorinated copolymer and a solid crosslinking agent, the fluorinated copolymer having units based on nitrile-containing monomers and units based on tetrafluoroethylene, and the crosslinking agent being a polyamine compound. The manufacturing method includes the following steps: pulverizing the crosslinking agent by mixing the fluorinated copolymer and the crosslinking agent at a mixing energy of 10 J / g or higher.

7. The method for manufacturing the fluorinated copolymer composition according to claim 6, wherein, The crosslinking agent is pulverized into solid particles with a median particle size of less than 40 μm on a volume basis.

8. A method for manufacturing a fluorinated copolymer composition according to any one of claims 1 to 5, wherein, The fluorinated copolymer composition is obtained by mixing the fluorinated copolymer and the crosslinking agent at a mixing energy of 10 J / g or higher, thereby pulverizing the crosslinking agent.

9. A fluororubber article, which is formed by crosslinking the fluorinated copolymer composition according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Vulcanizable perfluoro elastomer

    JP1990059177B2

  • Inhibition of the RAF / MEK / p-ERK pathway for treating cancer

    WO2007013997A2

  • Fluorocopolymer composition and crosslinked rubber article

    WO2021210503A1

  • Bisdiaminophenyl compound, crosslinking agent, composition, and molded article

    WO2022230706A1