Method for preparing high-purity quartz sand by purifying low-grade silica through ultrasonic contact electro-catalysis coupled organic mixed acid
Through the combination of fluorine-free acid combined with leaching catalyst and ultrasonic technology, the problem of purification of medium and high-purity quartz sand in low-grade silica is solved, and efficient and environmentally friendly high-purity quartz sand is achieved, avoiding environmental pollution and high cost problems in traditional processes.
Patent Information
- Application Number
- CN202411197721.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The prior art is difficult to efficiently extract high-purity quartz sand from low-grade silica, and the use of inorganic acids in traditional processes leads to environmental pollution, which is complex and costly.
The leaching catalyst is used to treat silica through high-temperature calcination and quenching, combined with ultrasonic waves and organic acids for leaching, and use catalysts such as polytetrafluoroene to promote the removal of impurities, and achieve purification of high-purity quartz sand.
In a short process flow, high-purity quartz sand is successfully obtained above 99.99%, avoiding the use of inorganic acids, achieving green production and efficient purification, and the catalyst is easy to be recycled and reused.
Smart Images

Figure CN119080011A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing high-purity quartz sand from waste silica, belonging to the technical field of purification and utilization of waste silica. Background Art
[0002] Silica is a general term for vein quartz, quartzite, and quartz sandstone. It is mainly used as a raw material for silicon smelting in the metallurgical industry. Its main component is SiO 2 ; Quartz sand is quartz particles processed after silica crushing. It has stable chemical properties and is widely used in glass, forging, ceramics, smelting and other fields; high-purity quartz sand even plays an increasingly important role in many high-tech products, and its high-end products are widely used in large-scale integrated circuits, photovoltaic fields, precision electronic devices, aerospace and other industries.
[0003] At present, the production of high-purity quartz sand mainly depends on natural high-grade silica, which is generally required to be above 99%. In the process of silica formation, a variety of impurity minerals are associated, many of which directly affect the quality of subsequent products. The traditional process of purifying quartz sand mainly involves washing, crushing, grinding, acid leaching, etc. to obtain high-purity quartz sand. The process is complicated and most methods use inorganic acids such as hydrofluoric acid, sulfuric acid, nitric acid, and hydrochloric acid as leaching agents. The leaching solution is not easy to handle and seriously pollutes the environment. For example, a patented high-purity quartz sand purification process (publication number: CN118183764A) has the following specific steps:
[0004] S1. Quartz sand raw material crushing: The quartz sand raw material is vibrated by an electric vibrator and transported to a jaw crusher. After the primary crushing in the jaw crusher, the quartz sand raw material is transferred to an impact crusher by a belt conveyor, and then the impact crusher is crushed for the second time. After the crushing is completed, the quartz sand raw material is transported to a rotary screen by a belt conveyor. After screening, the coarse material should be transported to the impact crusher again by a belt conveyor. The impact crusher continues to crush, and the fine material is transported to the warehouse by a belt conveyor;
[0005] S2. Microwave heating pickling: use microwave to heat the quartz sand fine material, heat to maintain a stable pickling temperature, prepare a certain concentration of mixed acid, add the mixed acid to the quartz sand fine material and continue stirring;
[0006] S3, ultrasonic scrubbing: prepare the cleaning liquid, add an appropriate amount of cleaning agent to the cleaning liquid, put the quartz sand to be cleaned into the cleaning tank of the ultrasonic cleaning machine for scrubbing. Under the action of ultrasonic waves, the iron impurities adhering to the surface of the particles will fall off and enter the liquid phase, thereby achieving the purpose of iron removal;
[0007] S4, flotation: pour the scrubbed quartz sand into the flotation machine for flotation to remove non-magnetic associated impurity minerals such as feldspar and mica from the silica mineral raw materials;
[0008] S5. Magnetic separation: Quartz sand is subjected to dry magnetic separation to remove iron-containing minerals and their intergrowth particles;
[0009] S6, microwave acid leaching: the quartz sand is heated by microwaves, the mixed acid in the above step S2 is added and continuously stirred, the microwave pickling time is set to 45 minutes, and continuous stirring is performed during the microwave acid leaching process, and shock waves or collision and friction between particles are used to prevent the dissolved soluble impurity compounds from being deposited on the surface of the sand particles, thereby increasing the contact area of the reaction and improving the acid leaching impurity removal;
[0010] S7, microwave calcination explosion, acid leaching, water washing: high temperature calcination is used to make the gas inclusions explode, and then acid washing and water washing are used to remove the inclusions. The thermal explosion method removes impurities in the silicon dioxide powder to achieve the purification effect of high-purity quartz sand.
[0011] As high-grade silica veins are becoming increasingly scarce, it is urgent to obtain high-purity quartz sand by simple treatment using low-grade silica as raw material. However, there are no reports on the technology of obtaining high-purity quartz sand by simple treatment using low-grade silica as raw material. Summary of the invention
[0012] In view of the shortcomings of the prior art, the present invention attempts for the first time to use a fluorine-free acid to combine with a leaching catalyst, and obtains high-purity quartz sand in a shorter process flow.
[0013] The present invention provides a method for preparing high-purity quartz sand, comprising the following steps:
[0014] Step 1
[0015] The silica to be treated is placed in a sintering furnace, heated to 600-1000° C. for roasting, and after roasting, a quenching agent is added for quenching to obtain quenched silica;
[0016] Step 2
[0017] The quenched silica is added to a mixed acid solution, a catalyst is added, and leaching is performed. After leaching, solid-liquid separation is performed to obtain a solid phase, wherein the solid phase consists of a catalyst and the leached silica; the catalyst is selected from at least one of polytetrafluoroethylene, polypropylene, and high-density polyethylene; the size of the catalyst particles is larger than the size of the quenched silica; the solid phase is dried, vibrated and screened to separate the leached dry silica; the leached dry silica is washed with water, and then dried to obtain high-purity quartz sand; the mixed acid solution consists of at least two of oxalic acid, citric acid, acetic acid, and ascorbic acid; and the pH value of the mixed acid solution is less than or equal to 1.5.
[0018] The present invention provides a method for preparing high-purity quartz sand, wherein SiO 2 The content is 90~99wt.%.
[0019] The invention discloses a method for preparing high-purity quartz sand. The particle size of the silica to be processed is less than or equal to 60 meshes, preferably 60-300 meshes.
[0020] The present invention discloses a method for preparing high-purity quartz sand, wherein the calcination time in step 1 is 3 to 5 hours.
[0021] The method for preparing high-purity quartz sand of the present invention, the roasting temperature in step 1 is further preferably 600-900°C, and in actual application, it can be roasted at 600-700°C in combination with a subsequent system (including quenching with low-concentration organic acid water), and can also achieve extremely excellent results.
[0022] In step one, after roasting, pour into a quenching agent for quenching, and obtain quenched quartz sand after suction filtration and drying. During the quenching process, the quartz sand to be treated is crushed again. The quenching agent is water or water containing an organic acid. As a further preferred organic acid concentration of 0.1 to 2wt%. When the quenching agent contains water with an organic acid, it can not only play a crushing role, but also use the temperature after roasting for the first rapid impurity removal. More importantly, the number of cracks in the crushed particles produced will increase. The organic acid is selected from at least one of oxalic acid, citric acid, acetic acid, and ascorbic acid.
[0023] The invention discloses a method for preparing high-purity quartz sand. In step 2, when the mixed acid contains oxalic acid, the concentration of the oxalic acid is 2-10wt%; when the mixed acid contains citric acid, the concentration of the citric acid is 1-5wt%; when the mixed acid contains acetic acid, the concentration of the acetic acid is 2-8wt%; when the mixed acid contains ascorbic acid, the concentration of the ascorbic acid is 1-6wt%.
[0024] The present invention provides a method for preparing high-purity quartz sand, wherein in step 2, the mixed acid is composed of at least three of oxalic acid, citric acid, acetic acid, and ascorbic acid. As a further preferred embodiment, in step 2, the mixed acid is composed of oxalic acid, citric acid, acetic acid, and ascorbic acid.
[0025] As a further preferred embodiment of the present invention, a method for preparing high-purity quartz sand, in step 2, in the mixed acid, the concentration of oxalic acid is 8-10wt%, the concentration of citric acid is 4-5wt%, the concentration of acetic acid is 6-8wt%, and the concentration of ascorbic acid is 4-6wt%;
[0026] The present invention discloses a method for preparing high-purity quartz sand. In step 2, the catalyst is preferably polytetrafluoroethylene, and its dosage is: 0.5-10g, preferably 1-6g, and more preferably 4-6g of polytetrafluoroethylene is added to 1 kg of silica to be treated, and the polytetrafluoroethylene is in granular form with a diameter of 0.5-7mm.
[0027] The invention discloses a method for preparing high-purity quartz sand. In step 2, the leaching temperature is 50° C. to 90° C., and the leaching time is greater than or equal to 1 hour, preferably 1 to 6 hours.
[0028] In step 2, during leaching, the liquid-to-solid ratio of the mixed acid solution to the quenched silica is 5 to 20:1.
[0029] The invention discloses a method for preparing high-purity quartz sand. In step 2, leaching is assisted by ultrasound, and the power of the ultrasound is 100-300W.
[0030] The beneficial effects of the present invention are:
[0031] The present invention calcines quartz particles at high temperature to make the quartz undergo phase change and increase its volume, and uses water or water containing organic acid to quench the quartz particles to produce cracks and allow impurities inside the quartz particles to overflow; then uses organic acid for mixed leaching, so that no inorganic acid is used, no fluorine, no nitrate, no chlorine, and green production is achieved. At the same time, the present invention uses ultrasonic waves to match organic acids, so that the organic acids can better react with internal impurities through cracks; uses polytetrafluoroethylene granules as catalysts, and under ultrasonic conditions, electron transfer occurs between the interface and deionized water, and synergistically acts with the acid solution to promote impurity leaching, so that the impurities are fully removed, and the quartz sand itself does not participate in the reaction, is easy to recycle, and can be reused, so as to obtain high-purity quartz sand with a purity of more than 99.99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Attached Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0034] Embodiment 1:
[0035] A method for preparing high-purity quartz sand from low-grade silica, the specific steps are as follows:
[0036] S1, screening and washing low-grade silica, and drying to obtain silica blocks; SiO 2 The content is about 95wt%;
[0037] S2, silica blocks are crushed, ground, and sieved to 60-120 meshes to obtain quartz particles;
[0038] S3, calcining the quartz particles at 600°C at a heating rate of 10°C / min for 3 hours, then adding them into deionized water for quenching, and filtering and drying to obtain quartz sand;
[0039] S4, adding 10g of quartz sand obtained in S3 into an ultrasonic emitting water bath container filled with a mixed acid solution for ultrasonic leaching, the liquid-to-solid ratio of the acid solution to the quartz sand is 5:1, the weight of the added polytetrafluoroethylene granules is 10mg, the diameter is 7mm, the leaching temperature is 50°C, the leaching power is 100W, the leaching time is 1h, washing with water after leaching, filtering to obtain the leaching liquid and leaching residue, simple screening to separate the catalyst and quartz sand, and then ultrasonically washing the quartz sand until neutral, solid-liquid separation, and drying the quartz sand to obtain high-purity quartz sand; wherein the oxalic acid concentration in the mixed acid solution is 4wt%, and the citric acid concentration is 1wt% (the pH value of the mixed acid solution is 1.5);
[0040] The purity of the purified quartz sand in this embodiment is 99.931%.
[0041] Example 2
[0042] A method for preparing high-purity quartz sand from low-grade silica, the specific steps are as follows:
[0043] S1, screening and washing low-grade silica, and drying to obtain silica blocks; SiO 2 The content is about 95wt%;
[0044] S2, silica blocks are crushed, ground, and sieved to 120-180 mesh to obtain quartz particles;
[0045] S3, calcining the quartz particles at 700°C at a heating rate of 10°C / min for 4 hours, then adding them into deionized water for quenching, and filtering and drying to obtain quartz sand;
[0046] S4, adding 10g of quartz sand obtained in S3 into an ultrasonic emitting water bath container filled with a mixed acid solution for ultrasonic leaching, the liquid-to-solid ratio of the acid solution to the quartz sand is 10:1, the weight of the added polytetrafluoroethylene granules is 20mg, the diameter is 5mm, the leaching temperature is 60°C, the leaching power is 150W, the leaching time is 2h, washing with water after leaching, filtering to obtain the leaching liquid and leaching residue, simple screening to separate the catalyst and quartz sand, and then ultrasonically washing to neutrality, solid-liquid separation, and drying the quartz sand to obtain high-purity quartz sand; wherein the oxalic acid concentration in the acid solution is 4wt%, the citric acid concentration is 3wt%, and the acetic acid concentration is 2wt% (the pH value of the mixed acid solution is 1.3);
[0047] The purity of the purified quartz sand in this embodiment is 99.954%.
[0048] Example 3
[0049] A method for preparing high-purity quartz sand from low-grade silica, the specific steps are as follows:
[0050] S1, the recovered low-grade silica is screened and cleaned, and dried to obtain silica blocks; SiO 2 The content is about 95wt%;
[0051] S2, silica blocks are crushed, ground, and sieved to 180-240 meshes to obtain quartz particles;
[0052] S3, calcining the quartz particles at 800°C at a heating rate of 10°C / min for 3 hours, then adding them into deionized water for quenching, and filtering and drying to obtain quartz sand;
[0053] S4, adding 10g of quartz sand obtained in S3 into an ultrasonic emitting water bath container filled with a mixed acid solution for ultrasonic leaching, the liquid-to-solid ratio of the acid solution to the quartz sand is 15:1, the weight of the added polytetrafluoroethylene granules is 30mg, the diameter is 3mm, the leaching temperature is 70°C, the leaching power is 200W, the leaching time is 3h, washing with water after leaching, filtering to obtain the leachate and leach residue, simple screening to separate the catalyst and quartz sand, and then ultrasonically washing to neutrality, solid-liquid separation, and drying the quartz sand to obtain high-purity quartz sand; wherein the oxalic acid concentration in the acid solution is 6wt%, the citric acid concentration is 3wt%, and the acetic acid concentration is 4wt% (the pH value of the mixed acid solution is 1.2);
[0054] The purity of the purified quartz sand in this embodiment is 99.972%.
[0055] Example 4
[0056] A method for preparing high-purity quartz sand from low-grade silica, the specific steps are as follows:
[0057] S1, screening and washing low-grade silica, and drying to obtain silica blocks; SiO 2 The content is about 95wt%;
[0058] S2, silica blocks are crushed, ground, and sieved to 180-240 meshes to obtain quartz particles;
[0059] S3, calcining the quartz particles at 900°C at a heating rate of 10°C / min for 4 hours, then adding them into deionized water for quenching, and filtering and drying to obtain quartz sand;
[0060] S4, adding 10g of quartz sand obtained in S3 into an ultrasonic emitting water bath container filled with a mixed acid solution for ultrasonic leaching, the liquid-to-solid ratio of the acid solution to the quartz sand is 15:1, the weight of the added polytetrafluoroethylene granules is 40mg, the diameter is 1mm, the leaching temperature is 80°C, the leaching power is 250W, the leaching time is 5h, washing with water after leaching, filtering to obtain the leaching solution and leaching residue, simple screening to separate the catalyst and quartz sand, and then ultrasonically washing to neutrality, solid-liquid separation, and drying the quartz sand to obtain high-purity quartz sand; wherein the oxalic acid concentration in the acid solution is 8wt%, the citric acid concentration is 7wt%, the acetic acid concentration is 6wt%, and the ascorbic acid concentration is 2wt% (the pH value of the mixed acid solution is 1.0);
[0061] The purity of the purified quartz sand in this embodiment is 99.985%.
[0062] Example 5
[0063] A method for preparing high-purity quartz sand from low-grade silica, the specific steps are as follows:
[0064] S1, screening and washing low-grade silica, and drying to obtain silica blocks; SiO 2 The content is about 92wt%;
[0065] S2, silica blocks are crushed, ground, and sieved to 240-300 mesh to obtain quartz particles;
[0066] S3, calcining the quartz particles at 1000°C at a heating rate of 10°C / min for 5 hours, then adding them into deionized water for quenching, and filtering and drying to obtain quartz sand;
[0067] S4, adding 10g of quartz sand obtained in S3 into an ultrasonic emitting water bath container filled with a mixed acid solution for ultrasonic leaching, the liquid-to-solid ratio of the acid solution to the quartz sand is 20:1, the weight of the added polytetrafluoroethylene granules is 50mg, the diameter is 0.5mm, the leaching temperature is 90°C, the leaching power is 300W, the leaching time is 6h, washing with water after leaching, filtering to obtain the leaching solution and leaching residue, simple screening to separate the catalyst and quartz sand, and then ultrasonically washing to neutrality, solid-liquid separation, and drying the quartz sand to obtain high-purity quartz sand; wherein the oxalic acid concentration in the acid solution is 10wt%, the citric acid concentration is 5wt%, the acetic acid concentration is 8wt%, and the ascorbic acid concentration is 6wt% (the pH value of the mixed acid solution is 0.8);
[0068] The purity of the purified quartz sand in this embodiment is 99.993%.
[0069] Example 6
[0070] Other conditions are consistent with those in Example 5, except that the sintering temperature is 900° C. and the purity of the purified quartz sand in this example is 99.9955%.
[0071] Example 7
[0072] Other conditions are consistent with those in Example 5, except that the sintering temperature is 800° C., and the purity of the purified quartz sand in this example is 99.9962%.
[0073] Example 8
[0074] Other conditions are consistent with those in Example 5, except that the sintering temperature is 700° C., and the purity of the purified quartz sand in this example is 99.9978%.
[0075] Example 9
[0076] Other conditions are consistent with those in Example 5, except that the sintering temperature is 600° C. After calcination, water with an oxalic acid concentration of 1 wt % is added for quenching; the purity of the purified quartz sand in this example is 99.9985%.
[0077] Comparative Example 1
[0078] Other conditions are consistent with those in Example 1, except that: no polytetrafluoroethylene granules are added to S4; and the purity of the purified quartz sand in this comparative example is 99.892%.
[0079] Comparative Example 2
[0080] The other conditions are the same as those in Example 1, except that S3 in Example 1 is omitted; specifically, as follows:
[0081] S1, screening and washing low-grade silica, and drying to obtain silica blocks; SiO 2 The content is about 95wt%;
[0082] S2, silica blocks are crushed, ground, and sieved to 60-120 meshes to obtain quartz particles;
[0083] S3, adding 10g of quartz sand obtained in S2 into an ultrasonic emitting water bath container filled with a mixed acid solution for ultrasonic leaching, the liquid-to-solid ratio of the acid solution to the quartz sand is 5:1, the weight of the added polytetrafluoroethylene granules is 10mg, the diameter is 7mm, the leaching temperature is 50°C, the leaching power is 100W, the leaching time is 1h, washing with water after leaching, filtering to obtain the leachate and leach residue, simple screening to separate the catalyst and quartz sand, and then ultrasonically washing the quartz sand until neutral, solid-liquid separation, and drying the quartz sand to obtain high-purity quartz sand; wherein the oxalic acid concentration in the mixed acid solution is 4wt%, and the citric acid concentration is 1wt%;
[0084] The purity of the purified quartz sand in this comparative example is 99.653%.
[0085] Comparative Example 3
[0086] Other conditions are consistent with those in Example 1, except that: the acid solution in S4 is an oxalic acid solution with a concentration of 5 wt %; and the purity of the purified quartz sand in this comparative example is 99.851%.
[0087] The specific embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing high-purity quartz sand, characterized in that: The steps include: Step 1 The silica to be treated is placed in a sintering furnace, heated to 600-1000° C. for roasting, and after roasting, a quenching agent is added for quenching to obtain quenched silica; Step 2 The quenched silica is added to a mixed acid solution, a catalyst is added, and leaching is performed. After leaching, solid-liquid separation is performed to obtain a solid phase, wherein the solid phase consists of a catalyst and the leached silica; the catalyst is selected from at least one of polytetrafluoroethylene, polypropylene, and high-density polyethylene; the size of the catalyst particles is larger than the size of the quenched silica; the solid phase is dried, vibrated and screened to separate the leached dry silica; the leached dry silica is washed with water, and then dried to obtain high-purity quartz sand; the mixed acid solution consists of at least two of oxalic acid, citric acid, acetic acid, and ascorbic acid; and the pH value of the mixed acid solution is less than or equal to 1.
5.
2. The method for preparing high-purity quartz sand according to claim 1, characterized in that: The content of SiO2 in the silica to be treated is 90-99wt.%.
3. The method for preparing high-purity quartz sand according to claim 1, characterized in that: The particle size of the silica to be treated is less than or equal to 60 mesh, preferably 60-300 mesh.
4. The method for preparing high-purity quartz sand according to claim 1, characterized in that: The calcination time in step 1 is 3 to 5 hours.
5. The method for preparing high-purity quartz sand according to claim 1, characterized in that: The calcination temperature in step 1 is 600-900°C.
6. The method for preparing high-purity quartz sand according to claim 1, characterized in that: In step 1, after the roasting is completed, the quenching agent is poured into the quenching agent for quenching, and the quenched quartz sand is obtained after filtration and drying. The quenching agent is water or water containing an organic acid. As a further preferred organic acid, the concentration is 0.1-2wt%; the organic acid is selected from at least one of oxalic acid, citric acid, acetic acid, and ascorbic acid.
7. The method for preparing high-purity quartz sand according to claim 1, characterized in that: In step 2, when the mixed acid contains oxalic acid, the concentration of oxalic acid is 2 to 10 wt %; when the mixed acid contains citric acid, the concentration of citric acid is 1 to 5 wt %; when the mixed acid contains acetic acid, the concentration of acetic acid is 2 to 8 wt %; when the mixed acid contains ascorbic acid, the concentration of ascorbic acid is 1 to 6 wt %.
8. The method for preparing high-purity quartz sand according to claim 1, characterized in that: In step 2, the mixed acid is composed of at least three of oxalic acid, citric acid, acetic acid, and ascorbic acid. As a further preferred embodiment, in step 2, the mixed acid is composed of oxalic acid, citric acid, acetic acid, and ascorbic acid.
9. The method for preparing high-purity quartz sand according to claim 1, characterized in that: In step 2, the catalyst is preferably polytetrafluoroethylene, and its dosage is: 0.5-10g, preferably 1-6g, and more preferably 4-6g polytetrafluoroethylene is added to 1 kg of silica to be treated. The polytetrafluoroethylene is in granular form with a diameter of 0.5-7mm.
10. The method for preparing high-purity quartz sand according to claim 1, characterized in that: In step 2, the leaching temperature is 50°C to 90°C, and the leaching time is greater than or equal to 1 hour, preferably 1 to 6 hours; In step 2, during leaching, the liquid-to-solid ratio of the mixed acid solution to the quenched silica is 5 to 20:
1. In step 2, leaching is assisted by ultrasound, and the power of the ultrasound is 100 to 300W.
Citation Information
Patent Citations
Purification method of high-purity quartz sand with SiO2 purity more than or equal to 99.99%
CN110127708A
Preparation of modified dielectric rubber material and application of modified dielectric rubber material in field of water treatment
CN117244590A
Method of purifying quartz sand
US4804422A
Cited By
Preparation method of high-purity silicon dioxide