Secondary battery and negative current collector

By using a combination of oxygen-containing resin film and transition metal layer in the negative electrode current collector of lithium secondary batteries, the problem of PET film embrittlement is solved, and the durability of the resin film and the cycle characteristics of the battery are improved.

CN123076936APending Publication Date: 2026-11-10PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580024291.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-28
Filing Date
2025-03-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the prior art, polyethylene terephthalate (PET) films coated with metal materials are prone to embrittlement due to contact with transition metals, especially when lithium metal is deposited and dissolved in lithium secondary batteries, which exacerbates this phenomenon, resulting in the embrittlement problem of resin films not being effectively solved.

Method used

A resin membrane containing oxygen-containing resin is used, with at least the surface resin layer containing oxygen-containing resin, and a transition metal layer is stacked on it to form a negative current collector. The transition metal ions are stabilized by the oxygen-containing resin, the breakage of polymer bonds is inhibited, and the durability of the resin membrane is improved.

Benefits of technology

It significantly inhibits the embrittlement of the resin film, improves the mechanical strength of the negative electrode current collector and the cycle characteristics of the battery, and extends the battery's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076936A_ABST
    Figure CN123076936A_ABST
Patent Text Reader

Abstract

A secondary battery comprises: a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte having lithium-ion conductivity. The negative electrode comprises a negative current collector, the negative current collector comprises a resin film and a transition metal layer stacked with the resin film, the resin film comprising a substrate resin layer and a surface resin layer, the surface resin layer comprising an oxygen-containing resin.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference of related applications

[0002] This disclosure claims priority to Japanese Patent Application No. 2024-054195, filed with the Japan Patent Office on March 28, 2024, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] This disclosure relates to secondary batteries and negative electrode current collectors. Background Technology

[0004] The anode electrode structure proposed in Patent Document 1 includes a current collector comprising copper. The anode electrode structure also includes a lithium metal film formed on the current collector. The anode electrode structure further includes a solid electrolyte interface (SEI) film stack formed on the lithium metal film. In one embodiment, at least one of the current collectors 110 and 160 includes a polyethylene terephthalate film coated with a metallic material.

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Publication No. 2021-502671 Summary of the Invention

[0008] The problem the invention aims to solve

[0009] Patent Document 1 describes a polyethylene terephthalate (PET) film coated with a metallic material that is prone to degradation. It is known that when a transition metal comes into contact with a polymer, metal ions transfer to the polymer, causing bond breakage through free radical reactions, thus leading to polymer embrittlement. For example, in the case of copper contact with a PET film, copper ions migrate to the PET film, causing PET embrittlement (copper damage). Therefore, if a transition metal layer is laminated on the surface of a resin film, embrittlement of the resin film gradually develops. While resin film embrittlement mostly develops slowly, it is desirable to suppress such embrittlement as much as possible.

[0010] On the other hand, when a negative electrode current collector with a transition metal layer stacked on the surface of the resin film is used in a lithium metal secondary battery (hereinafter referred to as "lithium secondary battery"), the embrittlement of the resin film is significantly promoted. In the negative electrode of the lithium secondary battery, lithium metal is deposited during charging and dissolves in the non-aqueous electrolyte during discharging. This means that when the transition metal in contact with the resin film comes into contact with lithium metal, the embrittlement of the resin film is significantly promoted. No reports of such a phenomenon have been found in previous literature.

[0011] Solution for solving the problem

[0012] One aspect of this disclosure relates to a secondary battery comprising: a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte having lithium-ion conductivity, wherein the negative electrode comprises a negative current collector, the negative current collector comprises a resin film and a transition metal layer laminated with the resin film, the resin film comprising a substrate resin layer and a surface resin layer, at least the surface resin layer comprising an oxygen-containing resin.

[0013] Another aspect of this disclosure relates to a negative current collector comprising: a resin film and a transition metal layer stacked thereon, wherein the resin film comprises a substrate resin layer and a surface resin layer, and at least the surface resin layer comprises an oxygen-containing resin.

[0014] Another aspect of this disclosure relates to a negative electrode for a secondary battery, comprising: the aforementioned negative electrode current collector; and a lithium metal layer laminated on the surface of the aforementioned transition metal layer.

[0015] The effects of the invention

[0016] According to this disclosure, in a secondary battery, the embrittlement of the negative electrode current collector containing a resin film is significantly suppressed.

[0017] The novel features of the invention are set forth in the claims, but the invention relates to both its structure and content, and will be better understood, together with other objects and features of the invention, by reference to the following detailed description of the accompanying drawings. Attached Figure Description

[0018] Figure 1 This is a schematic longitudinal cross-sectional view of a lithium secondary battery according to one embodiment of the present disclosure.

[0019] Figure 2 yes Figure 1 Enlarged cross-sectional view of region II in the diagram.

[0020] Figure 3 yes Figure 1 Enlarged cross-sectional view of region III in the image. Detailed Implementation

[0021] The following examples illustrate embodiments of this disclosure, but this disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc., are sometimes cited, but other numerical values, materials, etc., can be applied as long as the effects of this disclosure are achieved. It should be noted that known components of secondary batteries can also be applied to components other than the characteristic parts in this disclosure. In this specification, when referring to a "range of numerical value A to numerical value B," this range includes both numerical value A and numerical value B.

[0022] Embodiments of this disclosure relate to secondary batteries. A secondary battery includes a positive electrode, a negative electrode, a separator disposed between the positive and negative electrodes, and a non-aqueous electrolyte with lithium-ion conductivity. Examples of secondary batteries include lithium-ion secondary batteries that use a material reversibly absorbing and releasing lithium ions as the negative electrode active material, lithium secondary batteries in which lithium metal is deposited at the negative electrode during charging and dissolves during discharging, and all-solid-state batteries, among other non-aqueous electrolyte secondary batteries.

[0023] In lithium-ion batteries, over 70% of the rated capacity is achieved through the deposition and dissolution of lithium metal. The migration of electrons in the negative electrode during charging and discharging primarily depends on the deposition and dissolution of lithium metal therein. Specifically, 70–100% (e.g., 80–100%, 90–100%) of the electron migration (or current, in other views) in the negative electrode during charging and discharging depends on the deposition and dissolution of lithium metal. That is, the negative electrode of a lithium-ion battery differs from a negative electrode where the migration of electrons during charging and discharging primarily depends on the absorption and release of lithium ions by the active material (graphite, etc.).

[0024] In a battery where lithium metal is deposited at the negative electrode during charging, the open-circuit voltage (OCV) of the negative electrode at a fully charged state is, for example, below 70 mV relative to the lithium metal (the dissolution and deposition potential of lithium). A fully charged state refers to the state of charge (SOC) reached, for example, 0.98 × C or higher, when the battery's rated capacity is set to C. The open-circuit voltage (OCV) of the negative electrode at a fully charged state can be determined by disassembling the fully charged battery under an argon atmosphere, removing the negative electrode, assembling a battery cell using lithium metal as the counter electrode, and then measuring the result. The non-aqueous electrolyte of the battery cell can have the same composition as the non-aqueous electrolyte in the disassembled battery. Alternatively, as a non-aqueous electrolyte for the battery cell, a non-aqueous electrolyte containing LiPF6 dissolved at a concentration of 1 mol / L and LiBF2(C2O4) dissolved at a concentration of 0.1 mol / L can be used, which is a mixed solvent of 1,2-dimethoxyethane and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether in a volume ratio of 1:2.

[0025] The following sections will explain each component of a secondary battery in turn.

[0026] [negative electrode]

[0027] The negative electrode has a negative current collector. The negative current collector has a resin film and a transition metal layer laminated with the resin film. The resin film includes a substrate resin layer and a surface resin layer. The transition metal layer is also a layer in contact with the resin film or the surface resin layer.

[0028] Resin films are lightweight, which facilitates increased energy density in secondary batteries. They are also less prone to breakage during roller conveying and are easy to handle. Like copper foil and other common negative electrode current collectors, resin films do not become brittle even at low negative electrode potentials. Resin films are excellent current collector materials due to their high resistance to stress during electrode expansion and contraction and their resistance to breakage. In lithium-ion secondary batteries, lithium metal is deposited at the negative electrode during charging, leading to significant expansion of the negative electrode. "Negative electrode expansion" refers to the increase in the total volume of the negative electrode and the deposited lithium metal. This expansion is further amplified when lithium metal is deposited in a dendritic form. Consequently, stress is easily generated at the negative electrode.

[0029] The main surface of the resin membrane can be smooth or roughened, and can also undergo plasma treatment, corona treatment, etc. When the main surface of the resin membrane is smooth, the maximum vertical roughness Rz is less than 2.0 μm. When the main surface of the resin membrane is roughened, the maximum vertical roughness Rz is, for example, 2.0 μm or more, 2.5 μm or more, or 8 μm or more. The maximum vertical roughness Rz is measured according to JIS B 0601:2013. The main surface of the resin membrane refers to the surface other than the end faces of the resin membrane, specifically the two surfaces with the largest area. In this specification, "surface" usually refers to the "main surface".

[0030] From the viewpoint of improving the energy density of secondary batteries, the resin membrane thickness is preferably as thin as possible, provided that mechanical strength is ensured. An example of a preferred range for resin membrane thickness is 1.5 μm or more and 30 μm or less. The resin membrane thickness can be determined by measuring the thickness at any 10 points on a cross-section of the resin membrane using a scanning electron microscope (SEM) and calculating their average value.

[0031] In the resin film, at least the surface resin layer comprises an oxygen-containing resin. The oxygen-containing resin contains oxygen atoms (O). At least 90% by mass of the surface resin layer may be composed of the oxygen-containing resin. The oxygen-containing resin may be a polymer having oxygen atoms in its main chain or side chains. The mass content of oxygen atoms (O) in the oxygen-containing resin (hereinafter also referred to as "O content") may be at least 3% by mass.

[0032] The oxygen-containing resin may further contain nitrogen atoms (N). The mass content of nitrogen atoms (N) in the oxygen-containing resin (hereinafter also referred to as "N content") may be 3% by mass or more. The ratio of O content to N content (O content / N content) is preferably greater than 1.

[0033] When using the surface resin layer as a reference, the mass content of oxygen atoms in the surface resin layer can be 2.5% by mass or more. The mass content of nitrogen atoms in the surface resin layer can be 2.5% by mass or more.

[0034] In resin films, the surface resin layer may contain, for example, oxygen-hydrogen bonds (OH bonds), oxygen-carbon bonds (CO bonds, C=O bonds, etc.), ester bonds (OC=O bonds), ether bonds (COC bonds), amide bonds (NH-C=O bonds), N=C=O bonds, etc. The presence or absence of these bonds can be determined by infrared absorption analysis. For example, the characteristic infrared absorption peaks of OH bonds, CO bonds, C=O bonds, and N=C=O bonds are at 3396, 1278, 1726, and 2260 cm⁻¹, respectively. -1 Observed nearby.

[0035] Samples of the surface resin layer or resin film can also be prepared by dissolving the transition metal layer in a diluted aqueous solution of distilled water and 65% nitric acid (volume ratio 1:1) after the active material has been removed from the negative electrode current collector or wet-processed. In this case, the outermost surface resin layer can be analyzed using infrared absorption analysis. An example of the analytical conditions is shown below.

[0036] FT-IR (ATR method)

[0037] Measurement apparatus: Varian 670FTIR (manufactured by Varian)

[0038] Measurement mode: Attenuated total internal reflection

[0039] Light source: special ceramic

[0040] Detector: DLaTGS (deuterated L-alanine-doped triglycine sulfate)

[0041] Resolution: 4cm -1

[0042] Total number of times: 256

[0043] IRE: Ge

[0044] Angle of incidence: 60 degrees

[0045] Attachment: Attachment for Single-Reflection ATR (Seagull)

[0046] Alternatively, chemical shifts can be used to analyze individual bonds using X-ray electron spectroscopy (XPS).

[0047] The oxygen-containing resin can be a polymer containing at least one functional group selected from the group consisting of epoxy, (meth)acryloyl, peroxy, hydroxyl, ester, ether, and (meth)acrylate groups. Such polymers can be polymers modified with urethane, urea, melamine, amide, aromatic polyamide, imide, etc.

[0048] The polymers of the aforementioned compounds may contain, for example, oxygen-hydrogen bonds (OH bonds), oxygen-carbon bonds (CO bonds, C=O bonds, etc.), ester bonds (OC=O bonds), ether bonds (COC bonds), and amide bonds (NH-C=O bonds). Among these, the β-hydroxy ether structure derived from epoxy groups (COCC-OH) is excellent as a current collector material due to its high oxygen content, high flexibility, high resistance to stress during electrode expansion and contraction, and resistance to breakage.

[0049] The polymers of the above compounds can be acrylic resins. Acrylic resins are polymers of acrylic monomers. Acrylic monomers can include acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, isobutyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, n-butyl methacrylate, and other (meth)acrylates. Copolymers of acrylic acid with acrylonitrile, butadiene, vinyl acetate, etc., can also be used.

[0050] The polymers of the above compounds can be polyester acrylate resins, polyether acrylate resins, polyurethane acrylate resins, polyester polyol resins, polyether polyol resins, polyurethane polyol resins, polyester polyurethane resins, polyether polyurethane resins, etc.

[0051] Oxygen-containing resins can be polymers of compounds with unsaturated hydrocarbon structures. Compounds with unsaturated hydrocarbon structures can be polyesters with unsaturated bonds. That is, oxygen-containing resins can be unsaturated polyester resins. Unsaturated polyester resins can be polymers of polyesters obtained through the condensation reaction of unsaturated organic acids (e.g., maleic anhydride, phthalic anhydride, etc.) with polyols (e.g., ethylene glycol, propylene glycol, etc., polyether polyols, polyester polyols, polycarbonate polyols, polyurethane polyols, acrylic polyols, etc.) and vinyl monomers (e.g., styrene, acrylic monomers). The vinyl monomers function as diluents and crosslinking agents. Unsaturated polyester resins may also contain polymerization inhibitors (e.g., hydroquinone), catalysts (benzoyl peroxide, ethyl methyl ketone peroxide, cyclohexanone peroxide, lauroyl peroxide, azobisisobutyronitrile), and accelerators (dimethylaniline, cobalt naphthenate, etc.).

[0052] Oxygen-containing resins can be cured products of curable resin compositions. These curable resin compositions possess a three-dimensional network structure or a cross-linked structure. Therefore, when transition metals come into contact with polymers, metal ions are less likely to migrate to the surface resin layer, effectively inhibiting resin film embrittlement caused by free radical reactions. The curable resin compositions can be thermosetting or photocurable.

[0053] The curable resin composition may include a main agent and a curing agent. As a main agent, epoxy resin is preferred in that it produces a β-hydroxy ether structure with a high oxygen content (COCC-OH) and a high crosslinking density of the cured product.

[0054] There are no particular limitations on the type of epoxy resin. Bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD ​​type epoxy resin, bisphenol S type, bisphenol fluorene type epoxy resin, biscresol fluorene type epoxy resin, naphthalene type epoxy resin, biphenyl type epoxy resin, tetramethylbiphenyl type epoxy resin, p-aminophenol type epoxy resin, aniline type epoxy resin, toluidine type epoxy resin, glycidylamine type epoxy resin, alicyclic epoxy resin, dicyclopentadiene type epoxy resin, trimethylolmethyl alkane type epoxy resin, polyether type epoxy resin, silicone-modified epoxy resin, and phenolic varnish type epoxy resin are all acceptable. These can be used alone or in combination of two or more types. Among these, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AD ​​type epoxy resin, naphthalene type epoxy resin, and phenolic varnish type epoxy resin are preferred. These can be used alone or in combination of two or more types.

[0055] As a curing agent, for example, at least one selected from the group consisting of phenolic resin, amine compound, acid anhydride, peroxide, styrene, isocyanate, formaldehyde, etc. can be used.

[0056] There are no particular limitations on the phenolic resin used, but phenolic varnish resin is preferred. Phenolic varnish resin is a resin formed by the condensation polymerization of phenolic compounds or naphthol compounds with formaldehyde. Specifically, phenolic varnish resin, cresol varnish resin, aralkyl phenolic varnish resin, biphenyl phenolic varnish resin, terpene phenolic varnish resin, α-naphthol varnish resin, β-naphthol varnish resin, etc., can be used. They can be used alone or in combination of two or more.

[0057] As amine compounds, there are no particular limitations. Examples include primary, secondary, or tertiary aliphatic polyamines (e.g., polyethylene polyamine, diethylenetriamine, m-xylenediamine, polyoxypropylenediamine), alicyclic polyamines (e.g., isophoronediamine, 1,3-diaminomethylcyclohexane), aromatic amines (e.g., diaminodiphenylmethane, diaminodiphenyl sulfone, 2,4-diethyltoluenediamine, 2,6-diethyltoluenediamine), N-aminoethylpiperazine, triethyltetramine, diethylaminopropylamine, m-phenylenediamine, dicyandiamide, BF3 monoethylamine, polyamide amines, imidazole compounds, etc. They can be used alone or in combination of two or more.

[0058] Examples of acid anhydrides include phthalic anhydride, hexahydrophthalic anhydride, methyl nadic anhydride, dodecenyl phthalic anhydride, pyromellitic anhydride, maleic anhydride mixtures, and chlorobridged anhydride (Hite anhydride). They can be used alone or in combination of two or more.

[0059] Examples of isocyanates include hexamethylene diisocyanate (HMDI), xylene diisocyanate (XDI), methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), and isophorone diisocyanate (IPDI). They can be used alone or in combination of two or more.

[0060] When the main agent is polymerized through cationic polymerization, anionic polymerization, free radical polymerization, etc., photopolymerization initiators, photocationic polymerization initiators, etc. can be used as curing agents.

[0061] As photopolymerization initiators, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-one, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-(4-(2-hydroxyethoxy)-phenyl)-2-hydroxy-2-methyl-1-propane-1-one, oligomeric (2-hydroxy-2-methylvinyl)phenyl)propane, and 2,4,6-trimethylbenzoyl-diphenyl Photoradical polymerization initiators such as phosphine oxide, 2,4,6-trimethylbenzoyl-phenylethoxy-phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; and photocationic polymerization initiators such as triarylsulfonium hexafluorophosphate, triarylsulfonium hexafluoroantimonate, triarylsulfonium iodonium salt, and (4-methylphenyl)(4-(2-methylpropyl)phenyl)-hexafluorophosphate (1-)tolylcumyliodonium tetra(pentafluorophenyl)borate.

[0062] As a result of generating an oxygen-containing resin from the materials described above, the oxygen-containing resin may comprise at least one structure selected from the group consisting of structures derived from epoxy resins, phenolic resins, amine compounds, acid anhydrides, peroxides, polyols, and styrene. The oxygen-containing resin preferably has, for example, a three-dimensional network structure derived from epoxy resins.

[0063] The resin film may contain fillers. At least one of the substrate resin layer and the base resin layer may contain fillers. The resin film is intended to improve adhesion to the transition metal layer and the metal layer containing lithium metal (hereinafter also referred to as the "lithium metal layer"). By including fillers in the resin film, the adhesion between the negative electrode current collector and the lithium metal layer is significantly improved when the lithium metal layer is attached to the negative electrode current collector. In addition, it is understood that the negative electrode current collector holding the lithium metal layer becomes a negative electrode with uniform overall resistance, and the cycle characteristics of the secondary battery are improved. For example, by adding fillers such as silica or alumina to the surface resin layer, an uneven surface is formed in the surface resin layer, increasing the surface area, and an improvement in adhesion based on the anchoring effect can be expected. There are no particular limitations as long as the filler can roughen the surface of the surface resin layer or the substrate resin layer and does not undergo side reactions with the non-aqueous electrolyte in the battery, thereby reducing the battery characteristics. The filler can be particles of resin, metal oxide, ceramic, metal, etc.

[0064] The main surface of the negative electrode current collector can be smooth, but it is preferable to roughen it as in the case where fillers are included in the resin film. The maximum height roughness Rz of the main surface of the negative electrode current collector can be 2.0 μm or more, 2.5 μm or more, or more than 2.5 μm, or 8 μm or more. The maximum height roughness Rz of the main surface of the negative electrode current collector is the same as that of the main surface of the resin film, and is measured according to JIS B 0601:2013. The main surface of the negative electrode current collector refers to the surface other than the end face of the negative electrode current collector, specifically the two surfaces with the largest area. In addition, the arithmetic mean roughness Ra is preferably 0.15 μm or more.

[0065] The average particle size of the filler is, for example, 0.5 μm or more and 20 μm or less, or 1 μm or more and 10 μm or less. The average particle size of the filler is determined by averaging the diameter of an equivalent circle with an area equal to the area enclosed by the outlines of any 30 observed particles on a cross-section of the surface resin layer formed by scanning electron microscopy (SEM). However, excessive unevenness can affect the charge-discharge reaction; therefore, the maximum particle size of the filler is preferably 30 μm or less. The particle size distribution of the filler can be wide.

[0066] The surface resin layer can be formed by coating an oxygen-containing resin onto the surface of the substrate resin layer, for example. In this case, the oxygen-containing resin can be a thermoplastic resin soluble in a solvent, a thermosetting resin (resin composition), or a light-curing or UV-curing resin (resin composition). The oxygen-containing resin can be diluted with a solvent and then coated onto the surface of the substrate resin layer.

[0067] The thickness of the surface resin layer is, for example, less than 5 μm, and a preferred thickness range is 0.05 μm to 1.5 μm. The thickness of the surface resin layer can be determined by measuring the thickness of any 10 points of the surface resin layer in a cross-section of the negative electrode, negative electrode current collector, or resin film using a scanning electron microscope (SEM) and calculating their average value.

[0068] When fillers are added to the surface resin layer, the particle size of the fillers usually exceeds the thickness of the surface resin layer. In this case, the thickness of the surface resin layer is measured in areas where no large, protruding filler particles are present.

[0069] Most resin films are non-conductive. The transition metal layer imparts good conductivity to the negative electrode current collector. The transition metal layer simply needs to contain a transition metal and possess electronic conductivity. Preferably, the transition metal layer contains a transition metal in a metallic state that has electronic conductivity based on free electrons.

[0070] In the use of negative electrode current collectors in lithium-ion secondary batteries and lithium secondary batteries, from the viewpoint of easily ensuring corrosion resistance and conductivity, the transition metal layer preferably includes copper, nickel, chromium, titanium, iron, silver, gold, tin, etc. The transition metal layer preferably includes at least one of copper, copper alloys, stainless steel, nickel, nickel alloys, etc., and is particularly preferably including copper or copper alloys with excellent conductivity. The transition metal layer sometimes discolors due to corrosion; therefore, chromium oxide coating (chromate coating) or rust prevention treatment using benzotriazole, etc., can be performed as needed.

[0071] Transition metals can cause resin film embrittlement. This embrittlement is particularly pronounced when the transition metal layer contains copper. As a previously unreported insight, it has also been established that lithium metal significantly accelerates resin film embrittlement caused by transition metals (e.g., copper damage). For example, when a lithium metal layer is bonded to a negative electrode current collector with copper deposited on a polyethylene terephthalate (PET) film, the appearance of the negative electrode current collector deteriorates to a level that can be clearly observed visually, becoming uneven and irregular. In other words, in lithium secondary batteries where lithium metal is deposited at the negative electrode, significant resin film degradation due to the transition metal layer occurs. In contrast, by including at least the surface resin layer of the resin film in an oxygen-containing resin, resin film embrittlement is significantly suppressed.

[0072] It should be noted that a nickel-chromium alloy layer is used as a metal layer to shield the transfer of copper ions to the resin film. However, in lithium-ion batteries, the shielding effect based on the nickel-chromium alloy layer is completely lost. This is presumably because, when easily ionized lithium metal comes into contact with transition metals such as copper, the ionization of the transition metal is accelerated, and the breaking of polymer bonds is accelerated by the transition metal ions. On the other hand, a surface resin layer containing oxygen-containing resin can significantly suppress polymer breakage.

[0073] The breaking of carbon-carbon bonds has the greatest impact on the embrittlement of resin films. When the resin film contains oxygen-containing resin, at least one carbon-oxygen bond exists within the oxygen-containing resin. It is believed that the carbon-oxygen bond is not easily affected by transition metals or their ions. It is possible that the transition metal is stabilized by oxygen atoms, inhibiting the breaking of carbon-carbon bonds.

[0074] The transition metal layer can be formed by deposition on the surface of the surface resin layer using liquid-phase or vapor-phase methods. Examples of liquid-phase methods include electrodeposition methods such as electroplating and electroless plating. Examples of vapor-phase methods include evaporation, sputtering, and atomic layer deposition (ALD). Alternatively, a substrate can be formed by sputtering, and a thicker transition metal layer can be formed on it using a wet electroplating method. In other words, multiple methods can be combined. The transition metal layer can also be formed by lamination. However, there are no particular limitations on the method for forming the transition metal layer.

[0075] The thickness of the transition metal layer is, for example, 5 μm or less, or even 3 μm or less. A preferred range for the thickness of the transition metal layer is 0.05 μm to 1.5 μm, or even 0.1 μm to 1.5 μm. The thickness of the transition metal layer can be determined by measuring the thickness at any 10 points in the cross-section of the negative electrode or negative electrode current collector using a scanning electron microscope (SEM) and calculating their average value. The transition metal layer can consist of multiple layers containing different metals.

[0076] The substrate resin layer is the main component of the negative electrode current collector, and is typically thicker than the surface resin layer and thicker than the transition metal layer. At least 51% by mass of the substrate resin layer is composed of resin or organic matter. To improve adhesion to the transition metal layer and the lithium metal layer (lithium metal layer), the substrate resin layer may contain inorganic materials such as inorganic particles. The substrate resin layer can be a stretched film, a non-porous film, or a film with a regularly arranged plurality of pores. The substrate resin layer can be insulating, conductive, or non-conductive. There are no particular limitations on the morphology and physical properties of the substrate resin layer.

[0077] The substrate resin layer is formed by molding general-purpose plastics or general-purpose engineering plastics into sheets, for example. Examples of raw materials include: polyester resin, polyolefin resin, polyphenylene sulfide resin, acrylic resin, polycarbonate resin, polyetheretherketone resin, polysulfone resin, polyphenylene sulfone resin, polyethersulfone resin, polyamide resin, polyimide resin, polyetherimide resin, polybenzimidazole resin, liquid crystal polymer resin, polyacetal resin, polyvinyl chloride resin, polyarylate resin, silicone resin, nylon resin, polyvinylidene chloride resin, ethylene-vinyl alcohol copolymer, polyvinyl alcohol resin, polystyrene resin, epoxy resin, polyurethane resin, phenolic resin, melamine resin, urea-formaldehyde resin, unsaturated polyester resin, etc. The resins included in the substrate resin layer can be a single type or a combination of two or more types.

[0078] The resin contained in the substrate resin layer is preferably a resin with aromatic rings, a resin without fluorine atoms, or an olefin resin. When the resin has aromatic rings (e.g., benzene rings) within its molecules, the affinity between the substrate resin layer and the lithium metal layer increases, and the adhesion between the two is improved.

[0079] As a polyester resin, aromatic polyesters are preferred, especially unstretched polyethylene terephthalate, biaxially stretched polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. As an acrylic resin, polymethyl methacrylate is an example. As a polyimide resin, aromatic polyimide is preferred. As a polyamide resin, aromatic polyamide (aramid resin) is preferred. As a polyolefin resin, unstretched polypropylene, biaxially stretched polypropylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, metallocene polyethylene, ethylene-vinyl acetate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, and ionomers are preferred.

[0080] The extrusion method for the substrate resin layer can be either T-die extrusion or blow extrusion, and can be unstretched, uniaxially stretched, successively biaxially stretched, or simultaneously biaxially stretched. The combination of monomers, serving as the bonding mechanism of the resin, can be a homopolymer, a copolymer, or a terpolymer. The arrangement of the monomers is not limited; it can be a random copolymer or a block copolymer. Two or more substrate resin layers can also be combined. For example, two or more substrate resin layers can be laminated. The crystalline resin can be in a crystalline state, for example, an amorphous state produced by rapid cooling, or a mixture of both. Furthermore, a polymer alloy containing two or more of the aforementioned resins can also be used.

[0081] To ensure adhesion to other layers such as vapor-deposited films, the surface of the substrate resin layer can be subjected to corona treatment or plasma treatment. Alternatively, unevenness can be created in the substrate resin layer to improve adhesion to the surface resin layer. In this case, fillers such as ceramics, resins, or metals can be added to the substrate resin layer to form unevenness on its surface.

[0082] The tensile strength of the substrate resin layer can be, for example, 100 MPa or more, 200 MPa or more, 250 MPa or more, or 300 MPa or more. There is no particular upper limit to the tensile strength of the substrate resin layer; from the viewpoint of ensuring sufficient flexibility to relax stress, it can be, for example, 500 MPa or less.

[0083] The tensile strength of the substrate resin layer is determined by the maximum load when a test piece of the substrate resin layer is stretched at a constant speed in a direction perpendicular to its cross-section using the following formula. That is, the tensile strength is the nominal stress obtained by dividing the maximum load by the initial cross-sectional area. The tensile strength is determined according to the method of JIS C 2151. The test piece is made by punching the substrate resin layer into a specified shape. The shape of the test piece is set to test piece type 2 of JIS C 2151. The thickness of the test piece is set to the thickness of the substrate resin layer.

[0084] ρ=P max / A0

[0085] ρ: Tensile strength (MPa)

[0086] P max Maximum load (N)

[0087] A0: Initial cross-sectional area (mm²) 2 )

[0088] The elongation at break of the substrate resin layer can be, for example, 20% or more, 80% or more, 100% or more, or 200% or more. There is no particular upper limit to the elongation at break of the substrate resin layer; from the viewpoint of ensuring sufficient mechanical strength, it can be, for example, 400% or less.

[0089] The elongation at break of the substrate resin layer is calculated by the following formula, using the length at break and the initial length when a test piece of the substrate resin layer is stretched at a constant speed in a direction perpendicular to its cross-section. The elongation at break is determined according to the method of JIS K7127. The shape of the test piece is set to test piece type 2 of JIS K 7127. The thickness of the test piece is set to the thickness of the substrate resin layer.

[0090] Elongation at break δ (%) = 100 × (Length at break L - Initial length Lo) / Initial length Lo

[0091] δ: Elongation at break (%)

[0092] L: Length at break

[0093] Lo: Initial length

[0094] The thickness of the substrate resin layer can be, for example, less than 20 μm, or between 4 μm and 12 μm. The thickness of the substrate resin layer can be determined by measuring the thickness of any 10 points in the cross-section of the substrate resin layer using a scanning electron microscope (SEM) on the negative electrode, negative electrode current collector, or resin film, and then calculating their average value.

[0095] The negative electrode may further have a lithium metal layer (lithium metal layer) stacked on the surface of the transition metal layer. In this case, the metal layer is in contact with the transition metal layer. The metal layer typically promotes embrittlement of the resin film caused by the transition metal. On the other hand, when the resin film has a surface resin layer containing an oxygen-containing resin, such embrittlement is significantly suppressed. In other words, the negative electrode current collector of this disclosure is particularly suitable for lithium secondary batteries in which lithium metal is deposited at the negative electrode during charging and dissolves during discharging.

[0096] However, when the negative electrode active material is a non-lithium metal, such as carbon materials like graphite or silicon-containing materials, the negative electrode current collector disclosed herein is sometimes preferred for long-term reliability.

[0097] The lithium metal layer can function as a current collector. During charging, lithium ions in the non-aqueous electrolyte accept electrons on the lithium metal layer to become lithium metal, which is then deposited on the surface of the lithium metal layer. The lithium metal deposited on the surface of the lithium metal layer dissolves as lithium ions in the non-aqueous electrolyte due to discharge.

[0098] The lithium metal layer can be formed from at least one of lithium metal and a lithium alloy. The lithium alloy preferably contains magnesium. The magnesium content in the lithium alloy is, for example, 0.1% by mass or more, preferably 0.5% by mass or more, or 1% by mass or more, or possibly 3% by mass or more, or 5% by mass or more. When the magnesium content in the lithium alloy is within this range, the dendritic precipitation of lithium metal can be suppressed. Furthermore, a SEI coating with excellent physical properties can be easily formed on the surface of the lithium metal layer. The magnesium content in the lithium alloy is, for example, 30% by mass or less, or possibly 15% by mass or less, or 10% by mass or less. When the magnesium content in the lithium alloy is within this range, magnesium readily dissolves in lithium, easily forming a stable lithium alloy.

[0099] Lithium alloys may contain a third element in addition to lithium (the first element) and magnesium (the second element). Examples of third elements include aluminum, indium, calcium, lead, hydrogen, sodium, bismuth, gold, silver, copper, and zinc. Lithium alloys may contain one or more third elements. The content of the third element in a lithium alloy may be, for example, less than 10% by mass, less than 1% by mass, or less than 0.1% by mass.

[0100] A lithium metal layer can be formed by lamination, where a lithium metal foil is adhered to the surface of a transition metal layer. Alternatively, the lithium metal layer can be formed by deposition on the surface of the transition metal layer using either a liquid-phase or vapor-phase method. Examples of liquid-phase methods include electrodeposition. Examples of vapor-phase methods include evaporation and sputtering. However, there are no particular limitations on the method for forming the lithium metal layer.

[0101] The thickness of the lithium metal layer can be, for example, 1 μm or more, or 5 μm or more, under a discharge state with a depth of discharge (DOD) of 90% or more. On the other hand, from the viewpoint of improving the energy density of the secondary battery, the thickness of the lithium metal layer under a discharge state with a depth of discharge of 90% or more can be 30 μm or less, or 25 μm or less. An example of a preferred range for the thickness of the lithium metal layer is 5 μm to 20 μm. It should be noted that a discharge state with a depth of discharge (DOD) of 90% or more is synonymous with a state of charge (SOC) of 0.1 × C or less when the battery's rated capacity is set to C. The thickness of the lithium metal layer can be determined by measuring the thickness of any 10 points of the lithium metal layer in the cross-section of the negative electrode using a scanning electron microscope (SEM) and calculating their average value.

[0102] The surface resin layer and the transition metal layer can be formed on only one side of the substrate resin layer or on both sides. Similarly, the lithium metal layer can be formed on only one side of the substrate resin layer or on both sides.

[0103] When a surface resin layer and a transition metal layer are respectively stacked on both sides of a substrate resin layer, the total thickness of the substrate resin layer, the surface resin layer, and the transition metal layer can be, for example, 10 μm to 80 μm. Such a negative electrode current collector is suitable for forming a wound-type electrode assembly where a positive electrode and a negative electrode are wound together with a separator. In wound-type electrode assemblies, stress is easily generated during charging and discharging, especially in commonly used copper foil negative electrode current collectors, which become embrittled and prone to breakage. Furthermore, sometimes a large tensile tension is applied to the negative electrode on the outer periphery of the wound-type electrode assembly. On the other hand, when using the negative electrode current collector of this disclosure, since the negative electrode current collector contains a resin film, even when a large tensile tension is applied to the negative electrode on the outer periphery of the wound-type electrode assembly, breakage of the negative electrode can be significantly suppressed.

[0104] The surface resin layer is preferably disposed on the entire surface of each main surface of the substrate resin layer. However, if it is less than 10% of the area of ​​the main surface of the substrate resin layer, there may be portions not covered by the surface resin layer. The main surface of the substrate resin layer refers to the two surfaces with the largest area, excluding the end faces of the substrate resin layer.

[0105] The transition metal layer is preferably disposed on the entire surface of each main surface of the surface resin layer. However, if it is less than 30% of the area of ​​the main surface of the surface resin layer, there may be portions not covered by the transition metal layer. It should be noted that if a portion of the main surface of the substrate resin layer is not covered by the surface resin layer, it is preferable that this portion of the surface does not come into contact with the transition metal layer.

[0106] When forming a lithium metal layer, the lithium metal layer is preferably disposed on the entire surface of each main surface of the transition metal layer. If it is less than 30% of the area of ​​the main surface of the transition metal layer, there may be a portion that is not covered by the lithium metal layer.

[0107] A preferred embodiment of the negative current collector includes: a substrate resin layer, surface resin layers formed on both sides of the substrate resin layer, and a transition metal layer formed on the surfaces of the two surface resin layers (i.e., both sides of the resin film).

[0108] In one preferred embodiment, the negative electrode comprises: a substrate resin layer, surface resin layers formed on both sides of the substrate resin layer, a transition metal layer formed on the surfaces of the surface resin layers (i.e., both sides of the resin film), and a lithium metal layer formed on the surfaces of the transition metal layers (i.e., both sides of the negative electrode current collector). The substrate resin layer, surface resin layers, and transition metal layers constitute the negative electrode current collector. The lithium metal layer functions as both the negative electrode current collector and the negative electrode active material layer.

[0109] A preferred embodiment of the negative electrode is suitable for lithium secondary batteries in which lithium metal is deposited at the negative electrode during charging and dissolves in the non-aqueous electrolyte during discharging. The lithium contained in the lithium metal layer may or may not dissolve in the non-aqueous electrolyte during discharge. That is, the lithium deposited at the negative electrode during charging and dissolved from the negative electrode during discharging can originate from the positive electrode, or from both the positive electrode and the lithium metal layer.

[0110] [positive electrode]

[0111] The positive electrode, for example, comprises a positive current collector and a positive electrode composite material layer loaded on the positive current collector. The positive electrode composite material layer is formed by coating a positive electrode slurry, which disperses the positive electrode composite material in a dispersion medium, onto the surface of the positive current collector and allowing it to dry. Alternatively, the dried coating can be calendered as needed. The positive electrode composite material contains a positive electrode active material as an essential component and may contain binders, conductive agents, etc., as arbitrary components. The positive electrode composite material layer may be formed on only one side of the positive current collector or on both sides.

[0112] The positive electrode active material is a material that exhibits capacity by absorbing and releasing lithium ions. Examples of positive electrode active materials include lithium-containing transition metal oxides, transition metal fluorides, polyanions, fluorinated polyanions, and transition metal sulfides. Among these, lithium-containing transition metal oxides are preferred due to their low manufacturing cost and high average discharge voltage.

[0113] Transition metal elements included in lithium-containing transition metal oxides include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, and W. Lithium-containing transition metal oxides can contain one or more transition metal elements. The transition metal elements can be Co, Ni, and / or Mn. Lithium-containing transition metal oxides may contain more than one typical element as needed. Typical elements include Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, and Bi. Al is a typical example.

[0114] Conductive materials can be, for example, carbon materials. Examples of carbon materials include carbon black, acetylene black, Ketjen black, carbon nanotubes, and graphite.

[0115] Examples of adhesive materials include fluoropolymers, polyacrylonitrile, polyimide resins, acrylic resins, polyolefin resins, and rubber-like polymers. Examples of fluoropolymers include polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF).

[0116] The positive current collector uses foil, film, etc. Carbon material can be coated onto the surface of the positive current collector. Examples of materials used for the positive current collector include metallic materials containing Al, Ti, and Fe. The metallic material can be Al, Al alloys, Ti, Ti alloys, Fe alloys, etc. Fe alloys can also be stainless steel (SUS). Materials with metallic materials applied to the surface of a resin film via physical vapor deposition (PVD) or similar methods can also be used. There are no particular limitations on the thickness of the positive current collector; for example, it can be 5 μm or more and 30 μm or less.

[0117] [Separator]

[0118] Typically, a separator is desired between the positive and negative electrodes. The separator should have high ion permeability, moderate mechanical strength, and insulation. Microporous membranes, woven fabrics, and nonwoven fabrics can be used as separators. Preferred materials for the separator include polypropylene, polyethylene and other polyolefins, polymethylpentene, polyethylene terephthalate, polybutylene terephthalate, aromatic polyamides, and cellulose.

[0119] To improve the heat resistance of the separator, a heat-resistant coating containing ceramic particles can be applied to the surface of the separator (on one or both sides).

[0120] The separator can be one piece or multiple pieces sandwiched between the positive and negative electrodes. When multiple separators are sandwiched between the positive and negative electrodes, multiple pieces of one type of microporous film, woven fabric, or nonwoven fabric can be overlapped, or at least two types of microporous film, woven fabric, or nonwoven fabric can be overlapped. The thickness of the separator when only one piece is sandwiched is not particularly limited, but is preferably 5 to 80 μm. The thickness of the separator when multiple pieces are sandwiched is also not particularly limited, but is preferably 5 to 80 μm.

[0121] [Non-aqueous electrolytes]

[0122] Non-aqueous electrolytes with lithium-ion conductivity can be solid electrolytes or liquid electrolytes (electrolytes). Non-aqueous electrolytes can also be gel electrolytes (polymer electrolytes) containing a matrix polymer that absorbs non-aqueous solvents and gels.

[0123] Polymer electrolytes may contain, for example, lithium salts and a matrix polymer, or non-aqueous solvents, lithium salts and a matrix polymer. Examples of matrix polymers used include fluoropolymers, acrylic resins, and polyether resins.

[0124] As a solid electrolyte, for example, an inorganic solid electrolyte is used. As an inorganic solid electrolyte, for example, materials known in all-solid-state lithium-ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halide-based solid electrolytes, etc.) are used.

[0125] The electrolyte may contain, for example, a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. By dissolving the lithium salt in the non-aqueous solvent, lithium ions and anions are generated.

[0126] As an anion, well-known anions used in non-aqueous electrolytes can be used. Specifically, BF4 can be listed as an example. - ClO4 - PF6 - CF3SO3 - CF3CO2 - Anions of imides, anions of oxalate complexes, etc. Examples of imide anions include N(SO₂F)₂. - N(SO2CF3)2 - The anions of oxalate complexes may contain boron and / or phosphorus. Examples of anions in oxalate complexes include dioxoborate anion and BF2(C2O4). - PF4(C2O4) - PF2(C2O4)2 - Non-aqueous electrolytes can contain one type of lithium salt or two or more types of lithium salts.

[0127] In lithium-ion secondary batteries, from the viewpoint of suppressing the dendritic precipitation of lithium metal, it is preferable that the non-aqueous electrolyte contains at least an oxalate complex anion. Through the interaction between the oxalate complex anion and lithium, lithium metal readily and uniformly precipitates in fine particles. Therefore, localized precipitation of lithium metal is easily suppressed. The non-aqueous electrolyte may contain an oxalate complex anion and other anions. Other anions may include PF6. - Anions of imides, etc.

[0128] Examples of non-aqueous solvents include ester compounds, ether compounds, nitrile compounds, and amide compounds. These compounds include halogen-substituted derivatives. Examples of halogen-substituted derivatives include fluorides. Non-aqueous electrolytes may contain only one of these non-aqueous solvents or two or more.

[0129] The non-aqueous solvent of lithium secondary batteries may contain ether compounds as the main component. It should be noted that "main component" refers to the ether compound content in the non-aqueous solvent being 50% by mass or more, and can be 80% by mass or more. Furthermore, the ether compound content in the non-aqueous solvent can be 95% by mass or less, and can also be 100% by mass or less. The range of ether compound content in the non-aqueous solvent can be any combination of the aforementioned upper and lower limits.

[0130] It is believed that ether compounds have excellent stability (especially resistance to reduction) and can suppress the formation of decomposition products on the surface of the negative electrode, thus suppressing the expansion of the negative electrode.

[0131] Examples of ether compounds include cyclic ethers and chain ethers. Examples of cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, and 2-methyltetrahydrofuran. Examples of chain ethers include 1,2-dimethoxyethane, diethyl ether, ethyl vinyl ether, methyl phenyl ether, benzyl ethyl ether, diphenyl ether, dibenzyl ether, 1,2-diethoxyethane, diethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether. Among these, 1,2-dimethoxyethane and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether are preferred. They can be used alone or in combination of two or more.

[0132] Examples of ester compounds include carbonates and carboxylic esters. Examples of cyclic carbonates include ethylene carbonate and propylene carbonate. Examples of chain carbonates include dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate. Examples of cyclic carboxylic esters include γ-butyrolactone and γ-valerolactone. Examples of chain carboxylic esters include ethyl acetate, methyl propionate, and methyl fluoropropionate. These compounds can be used alone or in combination of two or more.

[0133] The concentration of lithium salt in the non-aqueous electrolyte is, for example, 0.5 mol / L or higher and 3.5 mol / L or lower. The concentration of anion in the non-aqueous electrolyte can also be set to 0.5 mol / L or higher and 3.5 mol / L or lower. Alternatively, the concentration of anion of oxalate complex in the non-aqueous electrolyte can be set to 0.05 mol / L or higher and 1 mol / L or lower.

[0134] Non-aqueous electrolytes may contain additives. These additives can form a coating on the negative electrode. By forming a coating derived from the additive on the negative electrode, dendrite formation can be further suppressed. Examples of additives include vinylene carbonate, fluoroethylene carbonate (FEC), and ethylene ethylene carbonate (VEC).

[0135] [Lithium-ion rechargeable battery]

[0136] The following description uses a cylindrical battery with a wound electrode assembly as an example to illustrate the structure of the lithium secondary battery of this disclosure, with reference to the accompanying drawings. However, this disclosure is not limited to the following structure.

[0137] Figure 1 This is a longitudinal cross-sectional view schematically illustrating an example of a lithium secondary battery according to an embodiment of the present disclosure. Figure 2 It is Figure 1 An enlarged view of the portion enclosed by region II (containing part of the positive electrode). Figure 3 It is Figure 1 An enlarged view of the portion enclosed by region III (containing a portion of the negative electrode). It should be noted that all figures are schematic representations, and the ratios of dimensions (e.g., thickness) of the constituent components differ from the actual figures.

[0138] The lithium secondary battery 10 includes a cylindrical battery casing, a wound electrode assembly 14 housed within the battery casing, and a non-aqueous electrolyte (not shown). The electrode assembly 14 is constructed by winding a strip-shaped positive electrode 11 and a strip-shaped negative electrode 12 such that a spacer 13 is sandwiched between the positive electrode 11 and the negative electrode 12.

[0139] The negative electrode 12 in the example diagram is in a discharge state with a depth of discharge (DOD) of 100%, and is composed of a negative electrode current collector 40 and a lithium metal layer 41. The negative electrode current collector 40 is composed of a substrate resin layer 42, surface resin layers 43 formed on two surfaces of the substrate resin layer 42, and a transition metal layer 44 formed on the surfaces of the two surface resin layers 43. Not limited to the example diagram, the negative electrode 12 may also be in a discharge state with a depth of discharge (DOD) of 100% and be composed only of a negative electrode current collector.

[0140] The negative electrode 12 is electrically connected to the housing body 15, which also serves as the negative terminal, via the negative electrode lead 20. One end of the negative electrode lead 20 is connected to the end of the negative electrode 12 along its long side, and the other end is welded to the inner bottom surface of the housing body 15.

[0141] The positive electrode 11 includes a positive current collector 30 and a positive composite material layer 31, and is electrically connected to a cover 26, which also serves as a positive terminal, via a positive lead 19. One end of the positive lead 19 is connected, for example, near the center along the long side of the positive electrode 11. The positive lead 19 extending from the positive electrode 11 extends through a through-hole (not shown) formed in the insulating plate 17 to a perforated metal plate 22. The other end of the positive lead 19 is welded to the surface of the perforated metal plate 22 on the side of the electrode assembly 14.

[0142] The battery casing consists of a bottomed cylindrical metal container body 15 and a sealing body 16 that seals the opening of the body 15. A gasket 27 is disposed between the body 15 and the sealing body 16 to ensure the airtightness of the battery casing. Inside the body 15, insulating plates 17 and 18 are respectively disposed at both ends of the electrode assembly 14 in the winding axis direction.

[0143] The housing body 15, for example, has a stepped portion 21 formed by partially pressing the side wall of the housing body 15 from the outside. The stepped portion 21 may also be formed in a ring shape along the circumference of the side wall of the housing body 15. In this case, the sealing body 16 is supported by the surface on the opening side of the stepped portion 21.

[0144] The sealing body 16 comprises a perforated metal plate 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cover 26. These components are stacked in this order within the sealing body 16. The sealing body 16 is installed at the opening of the housing body 15 with the cover 26 located outside the housing body 15 and the perforated metal plate 22 located inside the housing body 15. The aforementioned components constituting the sealing body 16 are, for example, circular or annular in shape. The lower valve body 23 and the upper valve body 25 are interconnected at their respective central portions, and the insulating member 24 is sandwiched between their respective peripheral portions. The perforated metal plate 22 and the lower valve body 23 are interconnected at their respective peripheral portions. The upper valve body 25 and the cover 26 are interconnected at their respective peripheral portions. That is, all components except the insulating member 24 are electrically connected to each other.

[0145] A vent (not shown) is formed in the lower valve body 23. Therefore, when the internal pressure of the battery casing rises due to abnormal heating, the upper valve body 25 expands towards the cover 26 and exits from the lower valve body 23. This disconnects the electrical connection between the lower valve body 23 and the upper valve body 25. If the internal pressure rises further, the upper valve body 25 breaks, and gas is released from the opening (not shown) formed in the cover 26.

[0146] In the illustrated example, a cylindrical lithium secondary battery is described, but the application of this embodiment is not limited to this case. Depending on its intended use, the shape of the secondary battery can be appropriately selected from various shapes besides cylindrical, such as coin-shaped, square, sheet-shaped, and flat. Furthermore, while a wound electrode assembly is shown in the illustrated example, the shape of the electrode assembly is not particularly limited; it can also be a stacked electrode assembly formed by layering the positive and negative electrodes with a separator. Additionally, known configurations can be used for the secondary battery's structure, excluding the electrode assembly and the non-aqueous electrolyte, without particular limitations.

[0147] (Postscript)

[0148] The following technology is disclosed through the above description.

[0149] (Technology 1)

[0150] A secondary battery, comprising:

[0151] positive electrode,

[0152] negative electrode,

[0153] The separator disposed between the positive electrode and the negative electrode, and

[0154] Non-aqueous electrolytes with lithium-ion conductivity

[0155] The aforementioned negative electrode has a negative current collector.

[0156] The aforementioned negative electrode current collector comprises a resin film and a transition metal layer stacked with the resin film.

[0157] The aforementioned resin film comprises a substrate resin layer and the aforementioned surface resin layer.

[0158] At least the aforementioned surface resin layer contains an oxygen-containing resin.

[0159] (Technology 2)

[0160] According to the secondary battery of technology 1, lithium metal is deposited in the negative electrode during charging and dissolves in the non-aqueous electrolyte during discharging.

[0161] (Technology 3)

[0162] According to the secondary battery of technology 1 or 2, the oxygen-containing resin comprises a polymer of a compound containing at least one functional group selected from the group consisting of epoxy group, (meth)acryloyl group, peroxy group, hydroxyl group, ester bond, ether bond and (meth)acrylate group.

[0163] (Technology 4)

[0164] The secondary battery according to any one of techniques 1 to 3, wherein the oxygen-containing resin comprises a polymer of a compound having an unsaturated hydrocarbon structure.

[0165] (Technology 5)

[0166] The secondary battery according to any one of techniques 1 to 4, wherein the oxygen-containing resin comprises at least one type of bond selected from the group consisting of OH bond, CO bond, C=O bond, OC=O bond, COC bond, N=C=O bond and NH-C=O bond.

[0167] (Technology 6)

[0168] According to any one of the techniques 1 to 5, the non-aqueous electrolyte secondary battery, wherein the oxygen-containing resin is a cured product of a curable resin composition.

[0169] (Technology 7)

[0170] According to the non-aqueous electrolyte secondary battery of technology 6, the above-mentioned curable resin composition comprises a main agent and a curing agent.

[0171] The curing agent described above comprises at least one selected from the group consisting of phenolic resins, amine compounds, acid anhydrides, peroxides, and styrene.

[0172] (Technology 8)

[0173] According to any one of the technologies 1 to 7, the secondary battery wherein the oxygen-containing resin comprises at least one selected from the group consisting of structures derived from epoxy resins, structures derived from phenolic resins, structures derived from amine compounds, structures derived from acid anhydrides, structures derived from peroxides, structures derived from polyols, and structures derived from styrene.

[0174] (Technology 9)

[0175] The secondary battery according to any one of art 1 to 8, wherein the surface resin layer comprises a filler.

[0176] (Technology 10)

[0177] According to the secondary battery of technology 9, the average particle size of the filler is 0.5 μm or more and 20 μm or less.

[0178] (Technology 11)

[0179] The secondary battery according to any one of Artificial Principles 1 to 10, wherein the thickness of the aforementioned transition metal layer is 3 μm or less.

[0180] (Technology 12)

[0181] The secondary battery according to any one of art 1 to 11, wherein a metal layer containing lithium metal is stacked on the surface of the aforementioned transition metal layer.

[0182] (Technology 13)

[0183] The secondary battery according to any one of Artificial Intelligence 1 to 12, wherein the thickness of the resin film is 20 μm or less.

[0184] (Technology 14)

[0185] The secondary battery according to any one of techniques 1 to 13, wherein the substrate resin layer comprises at least one selected from the group consisting of polyester and polyolefin.

[0186] (Technology 15)

[0187] A negative electrode current collector comprising: a resin film and a transition metal layer laminated therewith.

[0188] The aforementioned resin film comprises a substrate resin layer and the aforementioned surface resin layer.

[0189] At least the aforementioned surface resin layer contains an oxygen-containing resin.

[0190] (Technology 16)

[0191] According to the negative electrode current collector of technology 15, the oxygen-containing resin comprises a polymer of a compound containing at least one functional group selected from the group consisting of epoxy group, (meth)acryloyl group, peroxy group, hydroxyl group, ester bond, ether bond and (meth)acrylate group.

[0192] (Technology 17)

[0193] According to the negative electrode current collector of technology 15 or 16, the oxygen-containing resin is a cured product of a curable resin composition.

[0194] (Technology 18)

[0195] According to the negative electrode current collector of technology 17, the above-mentioned curable resin composition comprises a main agent and a curing agent.

[0196] The curing agent described above comprises at least one selected from the group consisting of phenolic resins, amine compounds, acid anhydrides, peroxides, and styrene.

[0197] (Technology 19)

[0198] According to any one of art 15 to 18, the negative electrode current collector, wherein the oxygen-containing resin comprises at least one selected from the group consisting of structures derived from epoxy resins, structures derived from phenolic resins, structures derived from amine compounds, structures derived from acid anhydrides, structures derived from peroxides, structures derived from polyols, and structures derived from styrene.

[0199] (Technology 20)

[0200] The negative electrode current collector according to any one of art 15 to 19, wherein the surface resin layer comprises a filler.

[0201] (Technology 21)

[0202] According to the negative electrode current collector of technology 20, the average particle size of the filler is 0.5 μm or more and 20 μm or less.

[0203] (Technology 22)

[0204] According to the negative electrode current collector of technology 21, the arithmetic mean roughness Ra on the main surface of the negative electrode current collector is 0.15 μm or more, and the maximum height roughness Rz is 2 μm or more.

[0205] (Technology 23)

[0206] A negative electrode for a secondary battery, comprising:

[0207] The negative current collector as described in any one of techniques 15 to 22; and

[0208] A lithium metal layer is stacked on the surface of the aforementioned transition metal layer.

[0209] <Example>

[0210] The lithium secondary battery of this disclosure will now be described in detail based on embodiments and comparative examples. This disclosure is not limited to the following embodiments.

[0211] Example 1

[0212] (1) Production of the positive electrode

[0213] A lithium-containing transition metal oxide (NCA; positive electrode active material) containing Li, Ni, Co, and Al, acetylene black (AB; conductive material), and polyvinylidene fluoride (PVdF; binder) were mixed at a mass ratio of NCA:AB:PVdF = 95:2.5:2.5. N-methyl-2-pyrrolidone (NMP) was then added in appropriate amounts and stirred to prepare a positive electrode composite slurry. Next, the obtained positive electrode composite slurry was coated onto both sides of an Al foil (15 μm thick) that functions as the positive electrode current collector, dried, and then calendered using rollers. Finally, the resulting laminate of the positive electrode current collector and positive electrode composite layer was cut to the specified electrode size, and a positive electrode composite layer (65 μm thick, 245 g / m²) was fabricated on both sides of the positive electrode current collector. 2 The positive electrode of ).

[0214] (2) Fabrication of the negative electrode

[0215] (2-1) Negative electrode current collector

[0216] A thermosetting acrylic resin (polyester acrylate resin) is coated on both sides of a 12μm thick polypropylene (PP) substrate resin layer as an oxygen-containing resin. The layer is then cured at a specified temperature to form a 1μm thick surface resin layer. Next, a 1μm thick copper vapor-deposited film is formed on the surface of the surface resin layer as a transition metal layer, resulting in a negative electrode current collector. The polyester acrylate resin is a polyester-type polyurethane-acrylate-acrylamide copolymer.

[0217] (2-2) Negative electrode

[0218] A negative electrode active material containing silicon-containing materials (composite particles in which nano-silicon particles are dispersed at a mass content of 55% by mass in the lithium silicate phase) and graphite particles, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) were mixed at a mass ratio of negative electrode active material:CMC-Na:SBR = 97.5:1:1.5. Water was then added in appropriate amounts and stirred to prepare a negative electrode composite slurry. Next, the obtained negative electrode composite slurry was coated on both sides of the negative electrode current collector and dried. The coating of the negative electrode composite material was then calendered using rollers. Finally, the resulting laminate of the negative electrode current collector and the negative electrode composite layer was cut to the specified electrode size, forming a negative electrode composite layer (75 μm thick, 226 g / m²) on both sides of the negative electrode current collector. 2 The negative electrode of ).

[0219] (3) Preparation of non-aqueous electrolytes

[0220] A liquid non-aqueous electrolyte was prepared by dissolving LiPF6 in a non-aqueous solvent at a concentration of 1 mol / L and LiBF2(C2O4) at a concentration of 0.1 mol / L. The non-aqueous solvent used was a mixture of 1,2-dimethoxyethane and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether in a volume ratio of 1:2.

[0221] (4) Battery manufacturing

[0222] An Al-made tab is attached to the positive electrode. A Ni-made tab is attached to the lithium metal layer of the negative electrode. A wound electrode assembly is fabricated by winding the positive and negative electrodes in an inert gas atmosphere, with a separator between them. The separator is a microporous polyethylene film (25 μm thick). The electrode assembly is housed in a pouch-shaped casing formed from a laminate with an Al layer. A non-aqueous electrolyte is injected into the casing containing the electrode assembly. The casing is then sealed to fabricate a lithium secondary battery. In Table 1, battery E1 is the battery of Example 1.

[0223] Example 2

[0224] In an inactive gas atmosphere, lithium metal foil (25 μm thick) was pressed onto both sides of a negative electrode current collector prepared in the same manner as in Example 1 to fabricate a negative electrode without a negative electrode composite layer. Using this negative electrode, a lithium secondary battery E2 was fabricated in the same manner as in Example 1.

[0225] Example 3

[0226] The polypropylene (PP) substrate resin layer of the negative electrode current collector was replaced with a polyethylene terephthalate (PET) substrate resin layer (12 μm thick). Silica with an average particle size of 7 μm was mixed into the acrylic resin of the surface resin layer as a filler. Otherwise, the negative electrode was fabricated in the same manner as in Example 2. 20 parts by mass of silica were mixed with every 100 parts by mass of the acrylic resin. Using this negative electrode, a lithium secondary battery E3 was fabricated in the same manner as in Example 1.

[0227] Example 4

[0228] The silica was replaced with aluminum oxide with an average particle size of 7 μm, and the negative electrode was fabricated in the same manner as in Example 3. Using this negative electrode, a lithium secondary battery E4 was fabricated in the same manner as in Example 1.

[0229] Example 5

[0230] Instead of the surface resin layer, a PET substrate resin layer containing silicon dioxide at a content of 10% by mass was used to fabricate the negative electrode, as in Example 3. Using this negative electrode, a lithium secondary battery E5 was fabricated in the same manner as in Example 1.

[0231] Example 6

[0232] For every 100 parts by weight of acrylic resin in the surface resin layer, 40 parts by weight of silica are mixed. Otherwise, the negative electrode is fabricated in the same manner as in Example 3. Using this negative electrode, a lithium secondary battery E6 is fabricated in the same manner as in Example 1.

[0233] Example 7

[0234] The acrylic resin in the surface resin layer was replaced with a thermosetting polyether polyurethane resin, and cured by heating at a specified temperature. Otherwise, the negative electrode was fabricated in the same manner as in Example 6. Using this negative electrode, a lithium secondary battery E7 was fabricated in the same manner as in Example 6.

[0235] Example 8

[0236] The acrylic resin in the surface resin layer was replaced with a light-curing polyurethane acrylate resin, which was then cured by UV irradiation. Otherwise, the negative electrode was fabricated in the same manner as in Example 6. Using this negative electrode, a lithium secondary battery E8 was fabricated in the same manner as in Example 6.

[0237] Example 9

[0238] The acrylic resin in the surface resin layer was replaced with a thermosetting polyurethane-modified bisphenol F epoxy resin composition, and cured by heating at a specified temperature. Otherwise, the negative electrode was fabricated in the same manner as in Example 6. Using this negative electrode, a lithium secondary battery E9 was fabricated in the same manner as in Example 6.

[0239] Example 10

[0240] The acrylic resin in the surface resin layer was replaced with a thermosetting aromatic polyester polyurethane resin, and cured by heating at a specified temperature. Otherwise, the negative electrode was fabricated in the same manner as in Example 6. Using this negative electrode, a lithium secondary battery E10 was fabricated in the same manner as in Example 6.

[0241] Comparative Example 1

[0242] A copper vapor-deposited film (1 μm thick) is directly formed on both sides of a polypropylene (PP) substrate resin layer (12 μm thick) as a transition metal layer, without forming a surface resin layer, to obtain the negative electrode current collector. A negative electrode active material containing only graphite particles is used, and a negative electrode composite slurry is prepared in the same manner as in Example 1. This slurry is used to fabricate negative electrode composite layers (75 μm thick, 226 g / m³) on both sides of the negative electrode current collector. 2 The negative electrode of ).

[0243] Using this negative electrode, a lithium secondary battery R1 was fabricated in the same manner as in Example 1.

[0244] Comparative Example 2

[0245] The substrate resin layer of the negative electrode current collector, made of polypropylene (PP), was replaced with a substrate resin layer made of polyethylene terephthalate (PET) (12 μm thick). Otherwise, the negative electrode was fabricated in the same manner as in Comparative Example 1. Using this negative electrode, a lithium secondary battery R2 was fabricated in the same manner as in Example 1.

[0246] Comparative Example 3

[0247] A copper vapor-deposited film (1 μm thick) is directly formed as a transition metal layer on both sides of a polypropylene (PP) substrate resin layer (1 μm thick) without forming a surface resin layer, thus obtaining a negative electrode current collector. A lithium metal foil (25 μm thick) is then pressed onto both sides of this negative electrode current collector in an inactive gas atmosphere to create a negative electrode without a negative electrode composite layer. Using this negative electrode, a lithium secondary battery R3 is fabricated in the same manner as in Example 1.

[0248] Comparative Example 4

[0249] The substrate resin layer of the negative electrode current collector, made of polypropylene (PP), was replaced with a substrate resin layer of polyethylene terephthalate (PET) (12 μm thick). Otherwise, the negative electrode was fabricated in the same manner as in Comparative Example 3. Using this negative electrode, a lithium secondary battery R4 was fabricated in the same manner as in Example 1.

[0250] Comparative Example 5

[0251] Before forming copper vapor-deposited films on both sides of the substrate resin layer, a nickel-chromium alloy (NiCr) layer with a thickness of 0.02 μm is formed on both sides of the substrate resin layer. Then, a copper vapor-deposited film is formed. Otherwise, the negative electrode is fabricated in the same manner as in Comparative Example 4. Using this negative electrode, a lithium secondary battery R5 is fabricated in the same manner as in Example 1.

[0252] The composition of each negative electrode is summarized in Table 1. It should be noted that the initial design capacity of each battery is roughly the same.

[0253] [Table 1]

[0254]

[0255] The obtained non-aqueous electrolyte secondary battery was used to conduct the following charge-discharge cycle test at 25°C.

[0256] [Charge-discharge cycle test]

[0257] (Charge)

[0258] First, perform constant current charging in steps 1 through 3 below.

[0259] Step 1: At 0.1C (0.55mA / cm)2 The current is constant and charged to the first charging rate (15%) using a constant current.

[0260] Step 2: At 0.4C (2.2mA / cm) 2 The current is constant and charged to 50% at a second charging rate of 2.

[0261] Step 3: At 0.6C (3.3mA / cm) 2 The current is constant and charged to 100% at the third charging rate (3x3).

[0262] The end of steps 1 and 2 is controlled by charging time. The charging time (in hours) is set as the time calculated by (1 / I) × (X / 100) when the amount of charge corresponding to the charging rate X (%) is charged at a current value I (C). The end of step 3 is controlled by voltage. Specifically, in step 3, constant current charging is performed until a voltage of 4.1V, presumably representing 100% charging, is reached.

[0263] Subsequently, after the aforementioned constant current charging, a constant voltage charging at 4.1V is performed until the current reaches 0.02C (0.11mA / cm). 2 ).

[0264] (Discharge)

[0265] After a 10-minute pause, at 0.6°C (3.3 mA / cm²) 2 The current is used to discharge at a constant current until the voltage reaches 3V.

[0266] [evaluate]

[0267] The above charge-discharge cycle is considered as one cycle, and 100 cycles are performed. The ratio of the discharge capacity in the 100th cycle to the discharge capacity in the 1st cycle is calculated as the capacity retention rate. Table 1 shows the relative values ​​when the capacity retention rate of Example 1 is set to 100.

[0268] As shown in Table 1, when the surface resin layer is formed by an oxygen-containing resin, the capacity retention rate increases dramatically. This is believed to be because the oxygen-containing resin suppresses the embrittlement of the negative electrode current collector containing the resin film, thus extending the period until cracks form in the negative electrode current collector.

[0269] Industrial availability

[0270] The negative current collector and secondary battery disclosed herein can be used in electronic devices such as mobile phones, smartphones, and tablet computers, including hybrid and plug-in hybrid electric vehicles, and household batteries combined with solar cells.

[0271] The present invention has been described with reference to preferred embodiments, but such disclosure should not be interpreted as limiting. Various modifications and alterations will be apparent to those skilled in the art from the foregoing disclosure. Therefore, the appended claims should be construed as encompassing all modifications and alterations without departing from the true spirit and scope of the invention.

[0272] Explanation of reference numerals in the attached figures

[0273] 10 Lithium secondary batteries

[0274] 11 Positive electrode

[0275] 12 Negative electrode

[0276] 13. Separators

[0277] 14 Electrode Groups

[0278] 15. Main body of the shell

[0279] 16 Sealing body

[0280] 17, 18 Insulation Boards

[0281] 19 Positive lead

[0282] 20 Negative lead

[0283] 21 Steps

[0284] 22 Perforated metal plate

[0285] 23 Lower valve body

[0286] 24 Insulating components

[0287] 25 Upper valve body

[0288] 26. Lid

[0289] 27 Gasket

[0290] 30 Positive current collector

[0291] 31 Positive electrode composite material layer

[0292] 40 Resin Film

[0293] 41 Lithium metal layer

[0294] 42 Substrate resin layer

[0295] 43 Surface resin layer

[0296] 44 Transition metal layer

Claims

1. A secondary battery, comprising: positive electrode, negative electrode, The separator disposed between the positive electrode and the negative electrode, and Non-aqueous electrolytes with lithium-ion conductivity The negative electrode has a negative current collector. The negative electrode current collector has a resin film and a transition metal layer stacked with the resin film. The resin film comprises a substrate resin layer and a surface resin layer. At least the surface resin layer comprises an oxygen-containing resin.

2. The secondary battery according to claim 1, wherein, In the negative electrode, lithium metal is deposited during charging and dissolves in the non-aqueous electrolyte during discharging.

3. The secondary battery according to claim 1, wherein, The oxygen-containing resin comprises a polymer of a compound containing at least one functional group selected from the group consisting of epoxy, (meth)acryloyl, peroxy, hydroxyl, ester, ether and (meth)acrylate groups.

4. The secondary battery according to claim 1, wherein, The oxygen-containing resin comprises a polymer of a compound having an unsaturated hydrocarbon structure.

5. The secondary battery according to claim 1, wherein, The oxygen-containing resin contains at least one type of bond selected from the group consisting of OH bond, CO bond, C=O bond, OC=O bond, COC bond, N=C=O bond and NH-C=O bond.

6. The non-aqueous electrolyte secondary battery according to claim 1, wherein, The oxygen-containing resin is a cured product of a curable resin composition.

7. The non-aqueous electrolyte secondary battery according to claim 6, wherein, The curable resin composition comprises a main agent and a curing agent. The curing agent comprises at least one selected from the group consisting of phenolic resins, amine compounds, acid anhydrides, peroxides, isocyanates, and styrene.

8. The secondary battery according to claim 1, wherein, The oxygen-containing resin comprises at least one structure selected from the group consisting of structures derived from epoxy resins, phenolic resins, amine compounds, acid anhydrides, peroxides, polyols, and styrene.

9. The secondary battery according to claim 1, wherein, The surface resin layer contains filler.

10. The secondary battery according to claim 9, wherein, The average particle size of the filler is greater than 0.5 μm and less than 20 μm.

11. The secondary battery according to claim 1, wherein, The thickness of the transition metal layer is less than 3 μm.

12. The secondary battery according to claim 1, wherein, A metal layer containing lithium metal is stacked on the surface of the transition metal layer.

13. The secondary battery according to claim 1, wherein, The thickness of the resin film is less than 20 μm.

14. The secondary battery according to claim 1, wherein, The substrate resin layer comprises at least one selected from the group consisting of polyester and polyolefin.

15. A negative current collector comprising: a resin film and a transition metal layer laminated therewith the resin film, The resin film comprises a substrate resin layer and a surface resin layer. At least the surface resin layer comprises an oxygen-containing resin.

16. The negative current collector according to claim 15, wherein, The oxygen-containing resin comprises a polymer of a compound containing at least one functional group selected from the group consisting of epoxy, (meth)acryloyl, peroxy, hydroxyl, ester, ether and (meth)acrylate groups.

17. The negative current collector according to claim 15, wherein, The oxygen-containing resin is a cured product of a curable resin composition.

18. The negative current collector according to claim 17, wherein, The curable resin composition comprises a main agent and a curing agent. The curing agent comprises at least one selected from the group consisting of phenolic resins, amine compounds, acid anhydrides, peroxides, and styrene.

19. The negative current collector according to claim 15, wherein, The oxygen-containing resin comprises at least one structure selected from the group consisting of structures derived from epoxy resins, phenolic resins, amine compounds, acid anhydrides, peroxides, polyols, and styrene.

20. The negative current collector according to claim 15, wherein, The surface resin layer contains filler.

21. The negative current collector according to claim 20, wherein, The average particle size of the filler is greater than 0.5 μm and less than 20 μm.

22. The negative current collector according to claim 21, wherein, On the main surface of the negative current collector, the arithmetic mean roughness Ra is 0.15 μm or more, and the maximum height roughness Rz is 2 μm or more.

23. A negative electrode for a secondary battery, comprising: The negative current collector as described in claim 15; and A lithium metal layer stacked on the surface of the transition metal layer.

Citation Information

Patent Citations

  • Ex-situ solid electrolyte interface modification with chalcogenides for lithium metal anodes

    JP2021502671A

  • In-mold composite surface film

    JP2024054195A