Lithium secondary battery and manufacturing method

By forming a pattern of alternating recesses and non-recesses on the lithium secondary battery electrode and coating the recesses with film-forming additives, the problems of transition metal dissolution and increased resistance during high-temperature storage are solved, achieving excellent fast charging performance and long lifespan characteristics.

CN123076947APending Publication Date: 2026-11-10LG ENERGY SOLUTION LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580027140.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-10-08
Filing Date
2025-10-01
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing lithium secondary batteries suffer from transition metal dissolution and increased resistance during high-temperature storage, which affects lifespan characteristics and fast-charging performance.

Method used

A method for forming a uniform film on the electrode surface is adopted. By coating the electrode current collector with a pattern of alternating recesses and non-recesses, and coating the interior of the recesses with a second electrode paste containing film-forming additives, the film-forming additives are ensured to be uniformly distributed, thus forming a stable SEI layer.

Benefits of technology

It effectively suppresses the dissolution of transition metals during high-temperature storage, improves the lifespan characteristics and fast-charging performance of the electrodes, and enhances the output characteristics and long-term cycle characteristics of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076947A_ABST
    Figure CN123076947A_ABST
Patent Text Reader

Abstract

The lithium secondary battery manufacturing method according to the present application includes a coating process of first and second electrode slurries, in which in the coating process, the first electrode slurry is coated to have a shape in which two or more recesses recessed toward a current collector are arranged at predetermined intervals, the second electrode slurry is coated to have a shape in which an inside of the recesses is filled, and the second electrode slurry contains a film-forming additive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority to Korean Patent Application No. 10-2024-0136629, filed on October 8, 2024, the disclosure of which is incorporated herein by reference.

[0002] This invention relates to a lithium secondary battery and its manufacturing method. Background Technology

[0003] Recently, with the technological development and increasing demands of mobile devices, the demand for batteries as an energy source has increased rapidly. As HEV, PHEV, and EV vehicles attract attention as vehicles of the future, research has been conducted in various ways to find batteries that can meet diverse needs.

[0004] In particular, we are actively researching lithium-ion batteries with high energy density, excellent lifespan, and good cycle performance.

[0005] Figure 1 This is a cross-sectional view of an electrode according to existing technology. When such conventional electrodes are manufactured using a high-load method, problems arise due to increased resistance and reduced output because the lithium-ion diffusion path becomes longer and the diffusion of lithium ions within the electrode slows down.

[0006] Recently, in order to achieve high energy density and excellent fast charging performance in lithium secondary batteries, such as... Figure 2 As shown, a technique has been attempted to form a pattern in which recesses and non-recesses are alternately arranged on the electrodes.

[0007] However, the problem with batteries assembled using such high-load patterned electrodes is that decomposition reactions of the electrodes, such as the dissolution of transition metals, occur during high-temperature storage, resulting in increased resistance and a corresponding decrease in lifespan characteristics. Summary of the Invention

[0008] Technical issues

[0009] One technical problem solved by the inventive concept is to suppress the dissolution of transition metals during high-temperature storage and improve the lifetime characteristics of the electrode, thereby achieving high energy density and excellent fast-charging performance.

[0010] Another technical problem solved by the inventive concept is to simultaneously improve initial resistance and long-term lifetime characteristics by forming a uniform film on the electrode surface during the activation process.

[0011] Technical solution

[0012] According to the present invention, a method for manufacturing a lithium secondary battery is provided. The method for manufacturing a lithium secondary battery according to an exemplary embodiment includes: Prepare the electrodes; Using electrodes to assemble lithium secondary batteries; and Activate the assembled lithium secondary battery. The preparation of electrodes includes: Prepare a first electrode slurry containing the first electrode active material; Prepare a second electrode slurry containing the second electrode active material and film-forming additives; The coating process of applying the first electrode paste and the second electrode paste to the electrode current collector; and Drying process, In the coating process, The first electrode paste is coated into a shape having two or more recesses facing the current collector recess arranged at predetermined intervals, and The second electrode paste is coated into a shape that fills the interior of the recess.

[0013] In an exemplary embodiment, the film-forming additive may be any one or a mixture of two or more of the following substances: cyclic carbonate compounds containing unsaturated bonds; cyclic or chain carbonate compounds containing halogen atoms; lithium salts having oxalate complexes as anions; imide lithium salts; fluorophosphate lithium salts; six-membered aromatic heterocyclic compounds containing two or more nitrogen atoms in their molecules; and sulfonyl lactone compounds.

[0014] In an exemplary embodiment, the film-forming additive may be any one or a mixture of two or more of the following substances: lithium difluorophosphate (LiF2O2P) or lithium monofluorophosphate (Li2PO3F), 1,3-propane sulfonyl lactone (PS), 1,4-butane sulfonyl lactone, and 1,3-propene sulfonyl lactone.

[0015] In an exemplary embodiment, the solids content of the second electrode slurry is lower than that of the first electrode slurry.

[0016] In an exemplary embodiment, the first electrode slurry may have a composition in which film-forming additives are excluded from the second electrode slurry.

[0017] In an exemplary embodiment, during the coating process, first and second electrode slurries are each coated by a nozzle printer, and the nozzle printer includes: two or more first nozzles configured to discharge the first electrode slurry; and two or more second nozzles configured to discharge the second electrode slurry, wherein the first nozzles and the second nozzles may be alternately arranged along a first direction.

[0018] In an exemplary embodiment, during the coating process, the loading of the second electrode slurry is less than 20% by weight, based on the total loading of the first and second electrode slurries.

[0019] In an exemplary embodiment, the activation process includes a formation process of charging the assembled lithium secondary battery until it reaches a predetermined state of charge, and during the formation process, a film layer is formed at the bottom of the recess.

[0020] In an exemplary embodiment, any one or more of the width (W), depth (H), and spacing of the recesses can be controlled by adjusting the ratio of the loading amount of the first electrode paste to the loading amount of the second electrode paste, or by adjusting the ratio of the solid content of the first electrode paste to the solid content of the second electrode paste.

[0021] According to the present invention, a lithium secondary battery is provided. The lithium secondary battery comprises: a positive electrode; a negative electrode; a separator; and an electrolyte. The positive and / or negative electrodes include: Electrode current collector; An electrode active material layer is disposed on an electrode current collector and has: a recessed portion facing the current collector; and non-recessed portions other than the recessed portion, the electrode active material layer having a structure in which the recessed and non-recessed portions are alternately arranged; and A film layer is formed along the surface of the electrode active material layer. The membrane layer also exists at the bottom of the recess.

[0022] In an exemplary embodiment, the cross-section of the electrode active material layer may have a shape in which the width of the surface side of the electrode active material layer is longer than the width of the current collector side.

[0023] In an exemplary embodiment, the loading of the electrode active material layer can be 4 mAh / cm². 2 above.

[0024] Beneficial effects

[0025] The electrode according to the invention has improved resistance characteristics and can achieve excellent fast charging performance due to the formation of a pattern in which two or more recesses and two or more non-recesses are arranged alternately.

[0026] According to the present invention, as a result of the uniform formation of the film layer on the patterned electrode surface, the battery output characteristics and long-term cycle characteristics are excellent.

[0027] According to the present invention, in order to compensate for the energy density loss caused by the formation of the recess, even if the width of the recess is narrow and the depth of the recess is long, since the film layer on the electrode surface is still present at the bottom of the recess, the effect of inhibiting the decomposition reaction of the electrolyte and the dissolution of transition metals is excellent even during high-temperature storage. Attached Figure Description

[0028] Figure 1This is a cross-sectional view of an electrode based on the prior art.

[0029] Figure 2 This diagram illustrates the problems in manufacturing lithium secondary batteries using patterned electrodes in the prior art.

[0030] Figure 3 This is a flowchart illustrating a method for manufacturing a lithium secondary battery according to an exemplary embodiment.

[0031] Figure 4 This is a flowchart illustrating the process of preparing an electrode according to an exemplary embodiment.

[0032] Figure 5 A diagram illustrating a coating process according to an exemplary embodiment.

[0033] Figure 6 This is a step-by-step cross-sectional view of an electrode according to an exemplary embodiment of the present invention.

[0034] Figure 7 This is a cross-sectional view of an electrode according to an exemplary embodiment. Detailed Implementation

[0035] The present invention will be described in more detail below to aid in understanding it.

[0036] The terms or words used in this specification and claims should not be construed as limited to their conventional or dictionary meanings, but should be interpreted as meanings and concepts consistent with the technical concept of the invention, based on the principle that the inventor is able to appropriately define the concepts of the terms in order to best describe his invention.

[0037] The technical terms used in this specification are for describing exemplary embodiments only and are not intended to limit the invention. Unless the context clearly specifies otherwise, singular expressions include plural expressions.

[0038] In this specification, terms such as “comprising,” “including,” or “having” are intended to indicate the presence of features, figures, steps, constituent elements, or combinations thereof in the implementation, and it should be understood that the possibility of the presence or addition of more than one other feature, figure, step, constituent element, or combination thereof is not excluded in advance.

[0039] In this specification, the term "combination thereof" in the Markush-type representation refers to a mixture or combination of one or more of the constituent elements described in the Markush-type representation, and means including one or more of the constituent elements.

[0040] In this specification, the description of "A and / or B" means "A or B or both".

[0041] In this specification, unless otherwise expressly stated, "%" refers to weight.

[0042] In this specification, the cross-section of the electrode active material layer is defined as the cut surface after cutting in the thickness direction (Z direction) of the electrode.

[0043] In this specification, the bottom of the recess refers to the portion of the recess closest to the current collector side, based on the thickness direction (Z direction).

[0044] Lithium secondary battery manufacturing method

[0045] Typically, when assembling lithium secondary batteries using patterned electrodes with alternating concave and non-concave arrangements, problems arise such as transition metal dissolution during high-temperature storage, increased resistance, and reduced long-term lifespan characteristics.

[0046] The inventors of this invention discovered that these problems in the prior art are caused by the following reasons: the film-forming additive contained in the electrolyte cannot penetrate into the interior of the recess, or the film-forming additive penetrates differently depending on the depth of the recess, resulting in the formation of a film with uneven thickness or local non-formation during the formation process or charge-discharge process, thus leading to the present invention.

[0047] Figure 2 This diagram illustrates the problems in manufacturing lithium secondary batteries using patterned electrodes in the prior art.

[0048] refer to Figure 2 When assembling a lithium secondary battery using a patterned electrode PE with alternating recessed (CC) and non-recessed (NC) portions, the electrolyte is immersed in the electrode. At this time, the film-forming additive in the electrolyte easily reaches the surface of the non-recessed (NC) or recessed (CC) portions of the patterned electrode PE, but does not reach the interior of the recesses, more specifically, not the bottom (CCB) of the recess, which is the deep interior region of the recess. In particular, this phenomenon inevitably becomes more severe as the width (W) of the recess becomes narrower and the depth (H) of the recess becomes deeper. During the formation process, the film thickness varies depending on the degree of diffusion of the film-forming additive, and a film cannot form at the bottom of the recess. The inventors of this invention obtained this invention after repeated research to ensure uniform film formation even inside the recesses.

[0049] Figure 3 This is a flowchart illustrating a method for manufacturing a lithium secondary battery according to an exemplary embodiment. Figure 4 This is a flowchart illustrating the process of preparing an electrode according to an exemplary embodiment. Figure 5 A diagram illustrating a coating process according to an exemplary embodiment.

[0050] refer to Figure 3 and 4 The lithium secondary battery manufacturing method according to an embodiment of the present invention may include: a step of preparing electrodes (P100); a step of assembling lithium secondary batteries (P200); and a step of activating lithium secondary batteries (P300). The step of preparing electrodes (P100) may be a step of manufacturing patterned electrodes in which recesses and non-recesses are alternately arranged.

[0051] In an exemplary embodiment, the electrode preparation process (P100) may include: a process of preparing a first electrode paste (P110); a process of preparing a second electrode paste (P120); a coating process (P130); and a drying process (P140).

[0052] refer to Figure 5 In the coating process (P130), the first electrode paste 21 is coated into a shape having two or more recesses CC facing the current collector recesses arranged at predetermined intervals, and the second electrode paste 22 can be coated into a shape that fills the interior of the recesses CC. Specifically, the second electrode paste 22 can be coated along the surface of the recesses CC. The coating area of ​​the second electrode paste 22 is mainly the interior of the recesses CC, but after filling the interior of the recesses CC, the remaining portion of the second electrode paste can also be coated on the non-recessed NC surfaces adjacent to the recesses CC.

[0053] The second electrode paste 22 filling the interior of the recess CC contains a film-forming additive. Therefore, the film-forming additive also coats the bottom CCB of the recess.

[0054] On the other hand, the film-forming additive has the function of stably forming a film layer on the surface of the electrode during the formation process. The lithium secondary battery assembled using patterned electrodes according to the present invention has a coated film-forming additive even at the bottom CCB of the recess, thus forming a film layer at the bottom CCB of the recess during the formation process. As a result, according to the present invention, since the film layer is uniformly formed on the surface of the patterned electrode, the risk of metal leaching is reduced compared to conventional secondary batteries containing patterned electrodes.

[0055] When the electrolyte comes into contact with the electrode and a redox decomposition reaction of the electrolyte components occurs at the interface, the decomposition products are deposited or adsorbed at these interfaces to form a film. Some of these are re-desorbed or dissolved, but some are permanently deposited and function as a protective layer on the electrode surface. This film has high lithium-ion conductivity and behaves similarly to a solid electrolyte; therefore, it is also called an SEI (solid electrolyte interphase) layer. It is known that such SEI layers can be formed on both the negative and positive electrodes, and the SEI layer formed on the positive electrode is also called a CEI (positive electrolyte interphase) layer. In this invention, the SEI layer or CEI layer formed during the charge-discharge process of the battery is the film layer of this invention.

[0056] In an exemplary embodiment, the step (P100) of preparing an electrode may be a step of manufacturing a patterned electrode in which recessed portions and non-recessed portions are alternately arranged.

[0057] The step (P110) of preparing a first electrode slurry may be a step of manufacturing an electrode slurry containing a first electrode active material. In one embodiment, the step of preparing the first electrode slurry may include adding and mixing the first electrode active material, a binder, and a conductive material into a solvent, and dispersing them.

[0058] The step (P120) of preparing a second electrode slurry may be a step of manufacturing an electrode slurry containing a second electrode active material and a film-forming additive. In one embodiment, the step of preparing the second electrode slurry may include adding and mixing the second electrode active material, a binder, and a conductive material into a solvent, and dispersing them.

[0059] The solvent is not particularly limited, and specific examples thereof may include dimethyl sulfoxide (DMSO), alcohols, N-methylpyrrolidone (NMP), water, acetone, and the like.

[0060] The first electrode active material and the second electrode active material have the same polarity. That is, if the electrode is a positive electrode, the first and second electrode active materials are each a positive electrode active material, and if the electrode is a negative electrode, the first and second electrode active materials are each a negative electrode active material.

[0061] The positive electrode active material is not particularly limited, and compounds known in the art as compounds capable of reversibly intercalating and deintercalating lithium can be used without limitation. As non-limiting examples, the positive electrode active material may include: a lithium transition metal composite oxide containing at least one transition metal selected from the group consisting of nickel, cobalt, manganese, and aluminum, as well as lithium, preferably a lithium transition metal composite oxide containing transition metals including nickel, cobalt, and manganese, as well as lithium.

[0062] More specifically, the lithium transition metal composite oxide includes: lithium manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.), lithium cobalt-based oxides (e.g., LiCoO2, etc.), lithium nickel-based oxides (e.g., LiNiO2, etc.), lithium nickel manganese-based oxides (e.g., LiNi 1-Y Mn Y O2 (where 0<Y<1), LiMn 2-z Ni z O4 (where 0<Z<2), etc.), lithium nickel cobalt-based oxides (e.g., LiNi 1- Y1 Co Y1 O2 (where 0<Y1<1), etc.), lithium manganese cobalt-based oxides (e.g., LiCo 1-Y2Mn Y2 O2 (where 0<Y2<1), LiMn 2- z1 Co z1 O4 (where 0<z1<2), etc.), lithium-nickel-manganese-cobalt-based oxides (for example, Li(Ni p Co q Mn r1 )O2 (where 0<p<1, 0<q<1, 0<r1<1, p+q+r1=1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0<p1<2, 0<q1<2, 0<r2<2, p1+q1+r2=2), etc.) or lithium-nickel-cobalt transition metal (M) oxides (for example, Li(Ni p2 Co q2 Mn r3 M S2 )O2 (where M is selected from Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r3 and s2 are atomic fractions of independent elements, where 0<p2<1, 0<q2<1, 0<r3<1, 0<s2<1, p2+q2+r3+s2=1), etc.), and any one or two or more of these compounds may be included. Herein, in view of being capable of improving the capacity characteristics and stability of the battery, the lithium transition metal composite oxide is: LiCoO2, LiMnO2, LiNiO2, lithium-nickel-manganese-cobalt oxides (for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.) or lithium-nickel-cobalt-aluminum oxides (for example, Li(Ni 0.8 Co 0.15 Al 0.15 )O2, etc.), and in view of the significant improvement effect by controlling the types and content ratios of the constituent elements forming the lithium transition metal composite oxide, the lithium transition metal composite oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn0.15 Co 0.15 O2 or Li(Ni) 0.8 Mn 0.1 Co 0.1 O2, and can be any one or a mixture of two or more of these.

[0063] There are no particular restrictions on the negative electrode active material, and compounds capable of reversibly inserting and deintercalating lithium can be used. Specific examples include: carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fibers, amorphous carbon, and highly crystalline carbon; (semi-metallic) materials capable of forming alloys with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; or composites containing (semi-metallic) materials and carbonaceous materials. Furthermore, low-crystallinity carbon includes soft carbon and hard carbon, and highly crystalline carbon includes high-temperature calcined carbon such as natural graphite, condensed graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, mesophase carbon microspheres, mesophase pitch, and coke derived from petroleum or coal tar pitch. One type or a mixture of two or more of these can be used, and thin films of metallic lithium can also be used as the negative electrode active material.

[0064] The first electrode active material contained in the first electrode slurry and the second electrode active material contained in the second electrode slurry can be the same type of compound or can be different types of compounds.

[0065] Based on the weight of solids in the first electrode slurry, the content of the first electrode active material can be in the range of 80% to 99% by weight, preferably 85% to 98% by weight, and more preferably 90% to 97% by weight.

[0066] Based on the weight of solids in the second electrode slurry, the content of the active material of the second electrode can be in the range of 80% to 99% by weight, preferably 85% to 98% by weight, and more preferably 90% to 97% by weight.

[0067] Unlike the first electrode paste, the second electrode paste contains film-forming additives. That is, the first electrode paste does not contain film-forming additives. In this invention, since the film-forming additives are introduced into the electrode paste to ensure that the film-forming additives are coated inside the recesses of the patterned electrode, it is sufficient to include film-forming additives only in the second electrode paste.

[0068] Film-forming additives may be selected from any one or a mixture of two or more of the following substances: cyclic carbonate compounds containing unsaturated bonds; cyclic or chain carbonate compounds containing halogen atoms; lithium salts with oxalate complexes as anions; imide lithium salts; fluorophosphate lithium salts; six-membered aromatic heterocyclic compounds containing two or more nitrogen atoms in their molecules; and sulfonyl lactone compounds.

[0069] Cyclic carbonate compounds containing unsaturated bonds specifically include: vinylene carbonate compounds such as vinylene carbonate, methyl vinylene carbonate, ethyl vinylene carbonate, propyl vinylene carbonate, dimethyl vinylene carbonate, or vinylene carbonate; or vinylene carbonate compounds such as vinylene carbonate.

[0070] Specifically, cyclic or chain carbonate compounds containing halogen atoms include: cyclic carbonate compounds containing one or more halogen atoms, such as fluoroethylene carbonate or difluoroethylene carbonate; and chain carbonate compounds containing one or more halogen atoms, such as fluoromethyl methyl carbonate or bis(fluoromethyl) carbonate.

[0071] Specific examples of lithium salts having oxalate complexes as anions include: lithium difluoro(oxalate)borate (LiODFB), lithium tetrafluoro(oxalate)phosphate (LiTFOP), lithium tri(oxalate)phosphate (LTOP), or lithium bis(oxalate)borate (LiBOB).

[0072] Specific examples of imide lithium salts include lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), or lithium bis(perfluoroethanesulfonyl)imide (LiBETI).

[0073] Specific examples of lithium fluorophosphates include lithium difluorophosphate (LiF2O2P) and lithium monofluorophosphate (lithium fluorophosphate, Li2PO3F).

[0074] Specific examples of sulfonyl compounds include 1,3-propanesulfonyl lactone (PS), 1,4-butanesulfonyl lactone, or 1,3-propenesulfonyl lactone.

[0075] Six-membered aromatic heterocyclic compounds containing two or more nitrogen atoms in their molecules can be specifically exemplified by pyrimidines and 1,3,5-triazines.

[0076] The film-forming additive is preferably selected from any one or a mixture of two or more of the following substances: lithium difluorophosphate (LiF2O2P), lithium monofluorophosphate (lithium fluorophosphate, Li2PO3F), 1,3-propane sulfonyl lactone (PS), 1,4-butane sulfonyl lactone, and 1,3-propene sulfonyl lactone.

[0077] Based on the total weight of the second electrode slurry, the content of the film-forming additive can be less than 3% by weight, preferably from 0.1% to 2.5% by weight, and more preferably from 0.4% to 2.2% by weight. When the content of the film-forming additive is within the above range, the film derived from the film-forming additive can be uniformly and thinly formed on the electrode after the electrochemical reaction, and the amount of gas generated by charging can also be minimized.

[0078] Adhesives can be selectively added to the electrode paste to bond the electrode active material to the conductive material and provide adhesion between the current collector and the electrode paste. There are no particular limitations on the type of adhesive, as long as it exhibits adhesive properties. For example, the adhesive may include one or more substances selected from: polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose (HPC), regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber.

[0079] To ensure sufficient adhesion between components such as electrode active materials, the binder content can be from 1% to 20% by weight, preferably from 1.2% to 10% by weight, based on the solids of the electrode slurry.

[0080] There are no particular restrictions on conductive materials, as long as they are conductive and do not cause chemical changes in the battery. Examples include: graphite such as natural or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal cracking black; conductive fibers such as carbon fibers or metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0081] Based on the solids of the electrode paste, the content of conductive material can typically be from 1% to 20% by weight, preferably from 1.2% to 10% by weight.

[0082] In an exemplary embodiment, the first electrode slurry may have a composition in which film-forming additives are excluded from the second electrode slurry.

[0083] In an exemplary embodiment, the solids content of the second electrode paste can be lower than that of the first electrode paste. Because the solids content of the second electrode paste is lower than that of the first electrode paste, the pattern of the recess can be maintained while removing the solvent from the second electrode paste during the drying process.

[0084] In an exemplary embodiment, based on the weight of the second electrode paste, the solid content of the second electrode paste can be 50% by weight or less, specifically 45% by weight or less, more specifically 40% by weight or less, and more specifically within the range of 10-40% by weight. From the perspective of compensating for energy density loss, it is preferable that the width W of the recess is narrow and the depth H of the recess is long. When the solid content of the second electrode paste is within the above range, the width of the recess can be adjusted to the desired narrowness and the depth of the recess can be adjusted to the desired length.

[0085] In an exemplary embodiment, the solid content of the first electrode paste can be greater than that of the second electrode paste, and is in the range of 30-75% by weight, specifically 40-70% by weight, and more specifically 50-65% by weight, based on the weight of the first electrode paste.

[0086] The coating process (P130) is the process of applying the first electrode paste and the second electrode paste to the electrode current collector.

[0087] In order to manufacture patterned electrodes in which recesses and non-recesses are arranged alternately, in the coating process (P130), the first and second electrode pastes can be coated by a nozzle printer respectively.

[0088] refer to Figure 5 In an exemplary embodiment, the nozzle printer 30 includes two or more first nozzles 31 configured to discharge a first electrode paste 21; and two or more second nozzles 32 configured to discharge a second electrode paste 22, and the first nozzles 31 and the second nozzles 32 may be arranged alternately along a first direction (Y direction). Therefore, the first electrode paste 21 and the second electrode paste 22 can be coated in an alternately arranged manner.

[0089] Since the first and second electrode pastes 21 and 22 each have fluidity, by appropriately adjusting the ratio of the load of the first electrode paste discharged from the first nozzle to the load of the second electrode paste discharged from the second nozzle, in the coating process P130, the first electrode paste 21 can be coated into a shape having recesses CC that are recessed toward the current collector 110 arranged at predetermined intervals, and the second electrode paste 22 can be coated into a shape having a shape that fills the interior of the recesses CC (see...). Figure 5 ).

[0090] In an exemplary embodiment, during the coating process (P130), the load of the first electrode paste 21 applied to the electrode current collector 110 can be greater than the load of the second electrode paste 22. In this case, the plane of the electrode current collector 110 is completely or substantially covered by the first electrode paste 21, and the second electrode paste 22 can be coated on the first electrode paste 21 at predetermined intervals I. Here, the plane of the current collector is a plane formed by a combination of the Y direction and the X direction.

[0091] In an exemplary embodiment, any one or more of the width W of the recess CC, the depth H of the recess CC, and the interval I of the recess can be controlled by adjusting the ratio of the loading amount of the first electrode paste to the loading amount of the second electrode paste, or by adjusting the ratio of the solid content of the first electrode paste to the solid content of the second electrode paste.

[0092] In an exemplary embodiment, during the coating process (P130), based on the total loading of the first and second electrode pastes, the loading of the second electrode paste can be 20% by weight or less, specifically 15% by weight or less, specifically 10% by weight or less, specifically in the range of 1-15% by weight, specifically 2-10% by weight. Since the second electrode paste is coated to form a pattern of recesses, from the perspective of compensating for the energy density loss caused by the pattern of recesses, it is preferable that the loading of the second electrode paste meets the above range.

[0093] Figure 6 This is a step-by-step cross-sectional view of an electrode according to an exemplary embodiment of the present invention.

[0094] refer to Figure 6 , Figure 6 (A) shows the electrode after the coating process (P130). Figure 6 (B) shows the electrode after the drying process (P140). Reference Figure 6 (A) After the coating process (P130), the first electrode paste 21 has a shape in which the recesses CC that are recessed toward the current collector 110 are arranged at predetermined intervals along the Y direction, and the second electrode paste 22 is coated to have a shape that fills the interior of the recesses CC.

[0095] refer to Figure 6 (B) In the drying process P140, the solvent in each of the first and second electrode slurries is removed, thereby forming: a first electrode active material layer 121 derived from the first electrode slurry 21; and a second electrode active material layer 122 derived from the second electrode slurry 22. The second electrode slurry 22, which has a relatively higher solvent content compared to the first electrode slurry 21, undergoes the drying process (P140) and all solvent is removed, significantly reducing the volume of the second electrode slurry, thus becoming the second electrode active material layer 122. Therefore, the electrode after the drying process (P140) includes the first electrode active material layer 121 formed on the current collector; and the second electrode active material layer 122 formed on the first electrode active material layer, wherein the second electrode active material layer exists in thin film form along the surface of the recess CC. Since the second electrode active material layer 122 contains film-forming additives, the film-forming additives are uniformly distributed along the entire surface of the recess CC.

[0096] The drying process P140 can employ various methods disclosed in the field of electrodes for secondary batteries up to the time of submission of this invention, and their detailed description will be omitted.

[0097] The process P200 of assembling a lithium secondary battery can be a process of assembling a lithium secondary battery using the aforementioned electrodes. For example, the electrodes can be patterned electrodes; specifically, the electrodes can be patterned electrodes including: Figure 6(B) shows a first electrode active material layer 121 having a recess CC and a non-recessed NC; and a second electrode active material layer 122 having a predetermined thickness and formed along the surface of the recess CC.

[0098] In an exemplary embodiment, the composition of the first electrode active material layer 121 may be a composition in which film-forming additives are excluded from the composition of the second electrode active material layer 122, and in this case, the first and second electrode active material layers may not be distinguishable in the electrode. In this specification, the first and second electrode active material layers are distinguished for ease of explanation, but it should be clarified that this is not intended to differentiate the first and second electrode active material layers in the electrode.

[0099] In an exemplary embodiment, the process of assembling a lithium secondary battery may include: storing an electrode assembly containing electrodes in a battery case and injecting an electrolyte into the battery case.

[0100] There are no particular restrictions on the electrode assembly. Examples include: jelly-roll type, in which the separator is located between the positive and negative electrodes and is wound; stacked type, in which multiple cell units with separators between the positive and negative electrodes are stacked; stacked folded type, in which the cell units are wound with long separators; and so on.

[0101] There are no particular restrictions on the battery casing. Depending on the material, it can be a can made of materials such as metal or plastic, or a bag made of flexible polymer materials. Depending on the shape, it can be a prism, a cylinder, a bag, etc.

[0102] The assembly process of a secondary battery can employ various methods disclosed in the field of secondary batteries up to the time of submission of this invention, and detailed descriptions thereof will be omitted.

[0103] The activation process for lithium secondary batteries (P300, hereinafter referred to as the "activation process") is the process of activating the assembled lithium secondary batteries to make them suitable for use. The activation process (P300) is performed to determine if the secondary batteries have defects and to ensure the stability of their performance and lifespan.

[0104] In an exemplary embodiment, the activation process (P300) may include a formation process that charges the assembled lithium secondary battery until it reaches a predetermined state of charge. The formation process is the process of performing the first charge on the lithium secondary battery, during which the electrolyte is reduced / oxidized and decomposed, and the decomposition products are deposited on the electrode surface and function as a passivation film that provides electronic insulation and conducts lithium ions.

[0105] Figure 6(C) shows the electrode state after the formation process. Referring to this figure, in a patterned electrode in which a step pattern of recesses CC and non-recesses NC is formed, a film layer 130 is thinly formed along the pattern shape of the electrode. In particular, according to the present invention, since the film layer 130 is also formed at the bottom of the recesses, a patterned electrode that suppresses the dissolution of transition metals at high temperatures and suppresses the decomposition reaction of the electrolyte can be provided because the film layer is uniformly distributed across the entire electrode surface.

[0106] As described above, the secondary battery manufacturing method according to the present invention has a pattern in which recesses facing the current collector side and non-recesses are arranged alternately, thus enabling excellent fast-charging performance in high-energy-density batteries. Furthermore, the film layer is uniformly formed along the surface of the patterned electrode, thereby suppressing the dissolution of transition metals at high temperatures and suppressing electrolyte decomposition reactions, thereby providing a secondary battery with excellent long-term lifespan characteristics.

[0107] Lithium secondary batteries

[0108] According to one embodiment of the present invention, a lithium secondary battery is provided. The lithium secondary battery according to the present invention comprises: a positive electrode; a negative electrode; a separator; and an electrolyte, wherein the positive electrode and / or the negative electrode may be patterned electrodes.

[0109] Figure 7 This is a cross-sectional view of a patterned electrode according to an exemplary embodiment. (Reference) Figure 7 Electrode 100 includes: Electrode current collector 110; An electrode active material layer 120 is disposed on an electrode current collector and has a recess CC recessed toward the current collector; and a non-recessed portion NC, wherein the electrode active material layer 120 has a structure in which the recessed portion and the non-recessed portion are alternately arranged; and A film layer 130 is formed along the surface of the electrode active material layer, wherein the film layer 130 is also present at the bottom CCB of the recess.

[0110] refer to Figure 7 It can be an electrode in which multiple recessed portions (CC) and multiple non-recessed portions (NC) are arranged alternately, thereby forming a pattern through the step difference between the recessed portions (CC) and the non-recessed portions (NC). Compared with an unpatterned electrode having a flat electrode surface, this type of patterned electrode 100 can improve the problem of increased resistance due to high electrode density / high load and has excellent output performance. In addition, since the space is formed by the step difference between the recessed portions (CC) and the non-recessed portions (NC), it is particularly effective in mitigating side reactions caused by changes in electrode volume.

[0111] In such patterned electrodes, from the perspective of compensating for energy density loss, it is preferable that the width W of the recess CC in the first direction (Y direction) is narrow and the depth in the thickness direction (Z direction) is long.

[0112] The electrode current collector 110 is a highly conductive metal to which the electrode slurry can easily adhere, and any metal that is non-reactive within the voltage range of the secondary battery can be used. The current collector can be a metal foil with a thickness of 3-500 μm, and various forms such as films, sheets, foils, meshes, porous bodies, foams, and nonwoven fabrics are feasible. In some embodiments, the adhesion between the current collector and the electrode active material can be increased by forming fine irregularities on the surface of the metal foil.

[0113] Non-limiting examples of positive electrode current collectors include: aluminum, stainless steel, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. Non-limiting examples of negative electrode current collectors include: copper, stainless steel, nickel, titanium, calcined carbon, or copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.

[0114] The electrode active material layer comprises electrode active material and binder, and may optionally also comprise conductive material or other fillers. Since the electrode active material, binder, and conductive material have already been described in detail above, further explanation will be omitted.

[0115] In exemplary embodiments, the cross-section of the electrode active material layer may have a shape in which the width on the surface side of the electrode active material layer is longer than the width on the current collector side. According to these embodiments, as a result of increasing the surface area per unit volume on the surface side, there is an effect of further improving the output characteristics.

[0116] In an exemplary embodiment, the loading of the electrode active material layer can be 4 mAh / cm². 2 More specifically, at 4 mAh / cm 2 Up to 8 mAh / cm 2 Within this range, high energy density batteries can be achieved by keeping the load within the aforementioned range.

[0117] The separator can be any porous substrate commonly used as a separator in lithium secondary batteries, such as polyolefin porous membranes or nonwoven fabrics, but there are no particular limitations. In particular, it is preferred to have low resistance to the movement of electrolyte ions and excellent electrolyte absorption capacity.

[0118] Examples of polyolefin porous membranes include membranes formed from polyolefin polymers such as polyethylene, high-density polyethylene, linear low-density polyethylene, low-density polyethylene, ultra-high molecular weight polyethylene, polypropylene, polybutene, polypentene, each of the above substances individually or polymers in which these are mixed.

[0119] As for nonwoven fabrics, in addition to polyolefin nonwoven fabrics, nonwoven fabrics formed from polymers such as polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, and polyethylene naphthalate, individually or in combination, can also be mentioned. The structure of the nonwoven fabric can be spunbond nonwoven fabric composed of long fibers or meltblown nonwoven fabric.

[0120] There are no particular restrictions on the thickness of the porous substrate, but it can be 5 to 50 μm. There are also no particular restrictions on the pore size and porosity present in the porous substrate, but they can be 0.01 to 50 μm and 10% to 95%, respectively.

[0121] On the other hand, in order to improve the mechanical strength of the diaphragm made of porous substrate and suppress short circuits between the positive and negative electrodes, a porous coating containing inorganic particles and binder polymer can also be included on at least one surface of the porous substrate.

[0122] On the other hand, in lithium secondary batteries, the electrolyte can contain organic solvents and lithium salts commonly used in electrolytes, and there are no particular restrictions.

[0123] As an organic solvent, any medium capable of facilitating the movement of ions participating in the battery's electrochemical reaction can be used without particular limitation. Specifically, as organic solvents, the following can be used: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene, fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), etc.

[0124] Among them, carbonate solvents are preferred, and a mixture of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) with high ionic conductivity and high dielectric constant that can improve the charging and discharging performance of the battery and low viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is even more preferred.

[0125] Lithium salts can be used without particular restrictions, as long as they are compounds that can provide lithium ions for use in lithium secondary batteries. Specifically, lithium salts can be: LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, etc. Preferably, lithium salts are contained in the electrolyte at a concentration of about 0.6 mol% to 2 mol%.

[0126] To improve battery life characteristics, suppress battery capacity degradation, and improve battery discharge capacity, in addition to the electrolyte component, the electrolyte may also contain one or more additives, such as: pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, (condensed) glycol dimethyl ethers, hexamethylphosphoric triamine, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted sulfadiazine, N,N-substituted imidazolidine, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, based on the total weight of the electrolyte, the content of the additives can be from 0.1 to 5% by weight.

[0127] Because the lithium secondary battery according to the present invention stably exhibits excellent resistance characteristics, discharge capacity, output characteristics and capacity retention, it can be used in portable devices such as mobile phones, laptops, digital cameras, energy storage systems (ESS), and electric vehicles such as hybrid electric vehicles (HEVs).

[0128] The present invention will be described in more detail below through embodiments. However, the following embodiments are for illustrative purposes only, and the scope of the invention is not limited thereto.

[0129] Example 1: Manufacturing of Lithium Secondary Batteries

[0130] (Preparation of the first positive electrode slurry)

[0131] Li(Ni) as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder are added to N-methyl-2-pyrrolidone (NMP) as a solvent, and mixed and stirred to prepare a first positive electrode slurry. At this time, the weight ratio of the positive electrode active material, conductive material, and binder in the solids is 96:2:2, and the solids content of the first positive electrode slurry is adjusted to 50% by weight.

[0132] (Preparation of the second cathode slurry)

[0133] Li(Ni) as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, carbon black as a conductive material, polyvinylidene fluoride (PVdF) as a binder, and 1,3-propane sulpholactone (PS) as a film-forming additive were added to N-methyl-2-pyrrolidone (NMP) as a solvent, mixed, and stirred to prepare a second positive electrode slurry. At this point, the weight ratio of the positive electrode active material, conductive material, and binder in the solids was 96:2:2. Based on the weight of the second positive electrode slurry, the content of the film-forming additive was 0.5% by weight, and the solids content of the second positive electrode slurry was adjusted to 40% by weight.

[0134] (Preparation process for the positive electrode)

[0135] First and second positive electrode pastes are coated onto aluminum foil using a nozzle printer, such as... Figure 5 The shape is shown in the figure. At this time, the loading ratio of the first positive electrode slurry to the second positive electrode slurry is adjusted to 9:1.

[0136] Subsequently, the positive electrode is dried, thereby achieving... Figure 6 The patterned positive electrode is manufactured using the shape shown in (B). The patterned positive electrode thus manufactured has a loading capacity of 4.25 mAh / cm³. 2 .

[0137] (Manufacturing of lithium secondary batteries)

[0138] Artificial graphite (particle size: 20 μm) as the negative electrode active material, carbon black as the conductive material, and styrene-butadiene rubber (SBR) as the binder were mixed and stirred in water at a weight ratio of 90:5:5 to prepare a negative electrode slurry. This slurry was then coated onto copper foil to prepare the negative electrode.

[0139] Electrode assemblies are fabricated by inserting a porous polyethylene separator between patterned positive and negative electrodes. The electrode assemblies are then inserted into a pouch cell casing, and an electrolyte is injected to create a full cell. The electrolyte used here is an electrolyte in which 1M LiPF6 is dissolved in an organic solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 3:4:3.

[0140] The assembled full cells were left to stand at 23°C for 24 hours for pre-aging. Afterward, the full cells were charged until they reached 30% SOC. High-temperature aging was performed by standing at 60°C for 12 hours, and room-temperature aging was performed by standing at 23°C for 24 hours. Subsequently, a portion of the battery casing was cut to vent the gases generated during the activation process, and the cut portion was sealed to complete the activation process.

[0141] Example 2: Manufacturing of Lithium Secondary Batteries

[0142] The lithium secondary battery was manufactured in the same manner as in Example 1, except that the film-forming additive was changed to be 1 wt% based on the weight of the second positive electrode slurry during the preparation of the second positive electrode slurry.

[0143] Example 3: Manufacturing of Lithium Secondary Batteries

[0144] The lithium secondary battery was manufactured in the same manner as in Example 1, except that the film-forming additive was changed to 2% by weight based on the weight of the second positive electrode slurry during the preparation of the second positive electrode slurry.

[0145] Example 4: Manufacturing of Lithium Secondary Batteries

[0146] The lithium secondary battery was manufactured in the same manner as in Example 1, except that the film-forming additive was changed to lithium difluorophosphate (LiF2O2P) during the preparation of the second positive electrode slurry.

[0147] Example 5: Manufacturing of Lithium Secondary Batteries

[0148] The lithium secondary battery was manufactured in the same manner as in Example 1, except that, in the preparation of the second positive electrode slurry, the film-forming additive was changed to lithium difluorophosphate (LiF2O2P) and the film-forming additive was changed to be 1 wt% based on the weight of the second positive electrode slurry.

[0149] Example 6: Manufacturing of Lithium Secondary Batteries

[0150] The lithium secondary battery was manufactured in the same manner as in Example 1, except that, in the preparation of the second positive electrode slurry, the film-forming additive was changed to lithium difluorophosphate (LiF2O2P) and the film-forming additive was changed to 2% by weight based on the weight of the second positive electrode slurry.

[0151] Comparative Example 1: Manufacturing of Lithium-ion Secondary Batteries

[0152] Li(Ni) as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder are added to N-methyl-2-pyrrolidone (NMP) as a solvent, and mixed and stirred to prepare a first positive electrode slurry. At this time, the weight ratio of the positive electrode active material, conductive material, and binder in the solids is 96:2:2, and the solids content of the first positive electrode slurry is adjusted to 50% by weight.

[0153] The positive electrode slurry was coated onto aluminum foil using a slot die coater and then dried. The resulting positive electrode had a loading capacity of 4.25 mAh / cm³. 2 .

[0154] Subsequently, a lithium secondary battery was manufactured in the same manner as in Example 1.

[0155] Comparative Example 2: Manufacturing of Lithium-ion Secondary Batteries

[0156] The lithium secondary battery was manufactured in the same manner as in Example 1, except that no film-forming additives were added during the preparation of the second positive electrode slurry.

[0157] Experimental Example 1: Performance Evaluation After High-Temperature Storage

[0158] The lithium secondary batteries manufactured in Examples 1 to 6 and the lithium secondary batteries manufactured in Comparative Examples 1 to 2 were each charged to 4.25 V / 55 mA at 0.33 C under constant current / constant voltage (CC / CV) conditions, and then discharged to 2.5 V at 0.33 C under constant current (CC) conditions.

[0159] The initial discharge capacity was measured using a PNE-0506 charge / discharge device (manufacturer: PNE Solution Co., Ltd., 5V, 6A). Additionally, after adjusting the SOC to 50%, a 2.5C pulse was applied for 10 seconds, and the initial resistance was calculated by the difference between the voltage before and after the pulse application.

[0160] Then, each secondary battery was left to stand at 60°C for 8 weeks.

[0161] Subsequently, after 8 weeks, CC-CV charge-discharge was performed using a CC current of 0.33 C, and the discharge capacity after high-temperature storage was measured using a PNE-0506 charge-discharge device (manufacturer: PNE Solution Co., Ltd., 5V, 6A).

[0162] Substitute the measured initial discharge capacity and the discharge capacity measured after 8 weeks of storage at high temperature into the following mathematical formula (1) to calculate the discharge capacity retention rate after high temperature storage. The results are shown in Table 1 below.

[0163] Subsequently, the resistance after 8 weeks of storage at high temperature was calculated by substituting the voltage drop that occurred under a 2.5 C discharge pulse applied for 10 seconds at 50% SOC into the following mathematical formula (2) to calculate the resistance increase rate (%), which is shown in Table 1 below. At this time, the voltage drop was measured using a PNE-0506 charge / discharge device (manufacturer: PNE Solution Co., Ltd., 5V, 6A).

[0164] The values ​​listed in Table 1 represent relative ratios when the calculated value of Comparative Example 1 is taken as 100%.

[0165] Mathematical formula (1): Capacity retention rate (%) = (Discharge capacity after 8 weeks of high-temperature storage / Initial discharge capacity) × 100

[0166] Mathematical formula (2): Resistance increase rate (%) = {(Resistance after 8 weeks of high-temperature storage - Initial resistance) / Initial resistance} × 100

[0167] Experiment Example 2: Evaluation of Gas Generation After High-Temperature Storage

[0168] The lithium secondary batteries manufactured in Examples 1 to 6 and the lithium secondary batteries manufactured in Comparative Examples 1 to 2 were left to stand at 60°C for 8 weeks, and then the amount of gas generated was measured. The results are shown in Table 1 below.

[0169] The values ​​listed in Table 1 represent relative ratios when the value of Comparative Example 1 is taken as 100%.

[0170] [Table 1]

[0171] Referring to Table 1, compared to the lithium secondary battery of Comparative Example 1, the lithium secondary battery of the Examples exhibits superior initial resistance due to its patterned electrodes. Although both the lithium secondary battery of the Examples and the lithium secondary battery of Comparative Example 2 contain patterned electrodes, the batteries of the Examples show a smaller rate of increase in resistance after high-temperature storage, less gas generation after high-temperature storage, and significantly better capacity retention after high-temperature storage. This is attributed to the uniform formation of film-forming additives on the electrode surface.

[0172] The present invention has been described in more detail with reference to the accompanying drawings and embodiments. However, it should be understood that the configurations described in the drawings or embodiments are merely one embodiment of the present invention and do not represent all the technical ideas of the present invention. Furthermore, it should be understood that various equivalents and modifications may exist as of the time of filing this application.

[0173] [Explanation of reference numerals in the attached figures]

[0174] 10, 100: Electrodes

[0175] 11, 110: Electrode current collector

[0176] 12, 120: Electrode active material layer

[0177] 130: Membrane layer

[0178] 21: First electrode paste

[0179] 22: Second electrode slurry

[0180] PE: Patterned electrode

[0181] CC: Concave

[0182] NC: non-concave

[0183] CCB: bottom of concave part

[0184] 30: Nozzle Printer

Claims

1. A method for manufacturing a lithium secondary battery, the method comprising the following steps: Prepare the electrodes; Use the electrodes to assemble lithium secondary batteries; and Activate the assembled lithium secondary battery. in, The electrode preparation process includes: The process of preparing a first electrode slurry containing a first electrode active material; The process of preparing a second electrode slurry containing a second electrode active material and a film-forming additive; The coating process of applying the first electrode paste and the second electrode paste onto the electrode current collector; and Drying process, In the coating process, The first electrode paste is coated into a shape having two or more recesses arranged at predetermined intervals facing the current collector recess, and The second electrode paste is coated into a shape that fills the interior of the recess.

2. The method for manufacturing a lithium secondary battery according to claim 1, wherein, The film-forming additive is selected from any one or a mixture of two or more of the following substances: cyclic carbonate compounds containing unsaturated bonds; cyclic or chain carbonate compounds containing halogen atoms; lithium salts having oxalate complexes as anions; imide lithium salts; fluorophosphate lithium salts; six-membered aromatic heterocyclic compounds containing two or more nitrogen atoms in their molecules; and sulfonyl lactone compounds.

3. The method for manufacturing a lithium secondary battery according to claim 1, wherein, The film-forming additive is selected from any one or a mixture of two or more of the following substances: lithium difluorophosphate (LiF2O2P) or lithium monofluorophosphate (Li2PO3F), 1,3-propane sulfonyl lactone (PS), 1,4-butane sulfonyl lactone, and 1,3-propene sulfonyl lactone.

4. The method for manufacturing a lithium secondary battery according to claim 1, wherein, Based on the total weight of the second electrode slurry, the content of the film-forming additive is less than 3% by weight.

5. The method for manufacturing a lithium secondary battery according to claim 1, wherein, The solid content of the second electrode slurry is lower than that of the first electrode slurry.

6. The method for manufacturing a lithium secondary battery according to claim 1, wherein, The first electrode slurry has a composition in which the film-forming additives are excluded from the second electrode slurry.

7. The method for manufacturing a lithium secondary battery according to claim 1, wherein, In the coating process, the first electrode paste and the second electrode paste are each coated by a nozzle printer, and The nozzle printer includes: two or more first nozzles configured to discharge the first electrode slurry; and two or more second nozzles configured to discharge the second electrode slurry. The first nozzle and the second nozzle are alternately arranged along the first direction.

8. The method for manufacturing a lithium secondary battery according to claim 1, wherein, In the coating process, based on the total loading of the first electrode slurry and the second electrode slurry, the loading of the second electrode slurry is less than 20% by weight.

9. The method for manufacturing a lithium secondary battery according to claim 1, wherein, The activation process includes a formation process that charges the assembled lithium secondary battery until it reaches a predetermined state of charge. During the formation process, a film layer is formed at the bottom of the recess.

10. The method for manufacturing a lithium secondary battery according to claim 1, wherein, The width (W), depth (H), and spacing of the recesses are controlled by adjusting the ratio of the loading amount of the first electrode slurry to the loading amount of the second electrode slurry, or by adjusting the ratio of the solid content of the first electrode slurry to the solid content of the second electrode slurry.

11. A lithium secondary battery, the lithium secondary battery comprising: a positive electrode; a negative electrode; a separator; and an electrolyte. in, The positive electrode and / or the negative electrode comprises: Electrode current collector; An electrode active material layer is disposed on the electrode current collector and has: a recessed portion facing the current collector; and non-recessed portions other than the recessed portion, wherein the electrode active material layer has a structure in which the recessed portion and the non-recessed portion are arranged alternately. and A film layer is formed along the surface of the electrode active material layer. The film layer is also present at the bottom of the recess.

12. The lithium secondary battery according to claim 11, wherein, The cross-section of the electrode active material layer has a shape in which the width on the surface side of the electrode active material layer is longer than the width on the current collector side.

13. The lithium secondary battery according to claim 11, wherein, The loading of the electrode active material layer is 4 mAh / cm². 2 above.

Citation Information

Patent Citations

  • Beoljibkkul sobiui ttukkeong,

    KR1020240136629A