A material for high-temperature-resistant lining pipe of an oilfield production device and a preparation method thereof
By combining HNBR and PPS at the interface and reinforcing with nano-silica, the high-temperature resistant inner liner material for oilfield production equipment has solved the problems of heat resistance and toughness under high-temperature conditions in ultra-deep oilfields. It has achieved stability and wear resistance of the material at 180℃, is compatible with steel pipe composite processes, and extends the service life of the material.
Patent Information
- Application Number
- CN202611466093.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-13
AI Technical Summary
In existing oilfield production equipment operating under ultra-deep, high-temperature conditions, conventional ultra-high molecular weight polyethylene materials have insufficient heat resistance limits, metal pipelines are prone to corrosion in complex media environments and are costly, while high-performance polymer materials are too expensive and difficult to meet the requirements of composite processing.
By employing a dual modification mechanism of grafting reaction + self-crosslinking reaction during the pre-impregnation and extrusion process of HNBR, and through the interfacial bonding between HNBR and PPS and the reinforcement of nano-silica, a high-temperature resistant inner liner material for oilfield production equipment is prepared. This material is compatible with steel pipe composite processes and meets the requirements of long-term high-temperature operating conditions above 180℃.
The material does not soften or deform at 180℃, has a lower oil absorption rate at high temperatures, improved toughness, and significantly enhanced wear resistance. It can meet the tensile assembly process requirements of steel pipe lined composite pipes and extend their service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of modified materials for oilfield production pipes, specifically to a high-temperature resistant inner lining material for oilfield production equipment and its preparation method. Background Technology
[0002] In the field of oilfield pipeline technology, composite pipelines using ultra-high molecular weight polyethylene (UHMWPE) liners and steel pipes have gradually replaced traditional pure steel pipes, becoming the mainstream development trend for conventional onshore and offshore oilfield pipelines due to their excellent wear resistance, aging resistance, and corrosion resistance. UHMWPE materials have high toughness, low friction coefficient, and excellent resistance to media corrosion, significantly reducing pipeline wear and scaling problems. However, as oilfield extraction depths continue to increase, ultra-deep oil production conditions place extremely stringent high-temperature requirements on pipeline lining materials: at oil production depths above 3000 meters, downhole temperatures can reach 150℃; at depths above 5000 meters, long-term downhole operating temperatures generally exceed 180℃; and at depths above 8000 meters, long-term downhole operating temperatures generally exceed 220℃. Simultaneously, the media environment includes complex systems such as water, crude oil, acids and alkalis, and high-salt content. Conventional UHMWPE materials have a heat resistance limit of no more than 120℃, and under high-temperature environments, they soften, deform, and experience a sharp drop in strength, making them completely unsuitable for ultra-deep, high-temperature oilfield conditions.
[0003] In high-temperature operating conditions, the industry currently mainly adopts two types of alternative solutions: The first is metal pipes with various coatings or surface treatments. Although metal pipes are resistant to high temperatures, they suffer from severe wear, rapid corrosion, and short fatigue life under multi-media coupling conditions in oil fields, requiring frequent replacement and resulting in extremely high overall maintenance costs. The second is to use high-performance polymer materials that are corrosion-resistant, oil-resistant, high-temperature resistant, and hydrolysis-resistant as lining materials to form composite pipes with steel pipes. For example, PEEK has excellent corrosion resistance, oil resistance, high-temperature resistance, and hydrolysis resistance, and can withstand long-term high temperatures above 220℃. However, the material unit price is as high as 700-1000 yuan / kg, making the material cost extremely high and preventing large-scale application.
[0004] In the process of compositing a polymer liner tube with a steel pipe, the liner tube needs to be stretched until its outer diameter is smaller than the inner diameter of the steel pipe. After being pulled into the steel pipe, the traction force is removed, and the liner tube springs back to its original position, forming an interference fit with the steel pipe to achieve composite fixation. This process requires the liner material to have an elongation of no less than 15% at the processing temperature and to be able to stably and elastically recover after stress removal, ensuring that the liner tube deforms and fits snugly without cracking or delamination. Existing high-temperature engineering plastics generally have high rigidity and low elongation, making it difficult to meet the requirements of composite processing.
[0005] Therefore, the industry urgently needs to develop a new type of inner lining material that is low-cost, can withstand long-term high temperatures of 180°C, is resistant to complex oilfield media, is wear-resistant and anti-eccentric wear, and has an elongation rate that meets the requirements of steel pipe composite processes. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high-temperature resistant inner lining pipe material for oilfield production equipment and its preparation method. Through the dual modification mechanism of grafting reaction + self-crosslinking reaction during the pre-impregnation and extrusion process of HNBR, the material simultaneously achieves high heat resistance, high wear resistance, low high temperature oil absorption, high elongation, and high compatibility. It can be adapted to the stretching composite process of steel pipes and is used in the long-term high temperature and harsh working conditions above 180°C in ultra-deep oilfields.
[0007] To achieve the above technical effects, the following technical solution is adopted: A high-temperature resistant inner lining material for oilfield production equipment comprises, by mass percentage: 65%–85% polyphenylene sulfide (PPS) powder, 10%–35% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3%–1% grafted monomer, and 0.015%–0.03% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane. Furthermore, the PPS is a linear, low-crosslinking polyphenylene sulfide powder with a melt flow index (MFR) of 10–30 g / 10 min under conditions of 315°C and 5 kg load. The preferred commercial grades are Solvay Ryton PR28 and Ticona 1140L0. Furthermore, the HNBR has a saturation of ≥98% and an acrylonitrile content of 33-36%, preferably using commercial brands such as Zeon Zetpol 2010 and Zetpol 3010. Furthermore, the grafting monomer is ethylene-glycidyl methacrylate; Furthermore, it also includes nano-silica powder, wherein the amount of nano-silica powder added is 0.3% to 1% of the mass of HNBR powder; On the other hand, the present invention also provides a method for preparing a high-temperature resistant inner lining material for oilfield production equipment, comprising the following preparation steps: Step S1: Mix N-methyl-2-pyrrolidone, methyl isobutyl ketone, and acetone in a mass ratio of 8~4: 5~2: 3~1 to obtain a composite solvent; Step S2: Add the grafted monomer and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane to the composite solvent obtained in step S1, stir and dissolve evenly to obtain a modified functional solution with a mass fraction of 20~45%. Step S3: Add the modified functional solution prepared in step S2 to the HNBR powder, mix and stir for 1-5 min to fully wet the HNBR powder, then add nano silica powder, continue mixing and stirring until uniform, and then let stand at room temperature for 24-40 h for modification to allow the HNBR particles to fully adsorb the modified solution; the mass ratio of HNBR to modified functional solution and nano silica is: HNBR : modified functional solution : nano silica = 100 : 5-8 : 0.3-1; S4: Dry the mixture after step S3 (which has been allowed to stand and modified) to remove residual solvent and obtain modified HNBR composite powder. S5: The modified HNBR composite powder obtained in step S4 is premixed with polyphenylene sulfide (PPS) powder evenly, and then fed into a twin-screw extruder with a vent for melt blending and extrusion granulation. During the extrusion and melting process, the HNBR grafting reaction and self-crosslinking reaction are triggered simultaneously to prepare a high-temperature resistant inner lining pipe composite material. Furthermore, in step S2, the stirring speed is 300-500 r / min and the stirring time is 15-30 min to ensure that the material is completely dispersed and dissolved. Furthermore, in step S3, a modified functional solution is added to the HNBR powder, and the mixture is stirred for 2-3 minutes to complete the pre-impregnation. Then, nano-silica powder is added, and the mixture is stirred for another 20-40 minutes to ensure that the nano-silica, the modified solution, and the HNBR powder are mixed evenly. Furthermore, in step S4, the mixture after static modification is dried at 80~130℃; Furthermore, in step S5, the twin-screw extrusion temperature range is 260–300°C. Grafting and cross-linking reactions are initiated during the extrusion process, and the prepared composite material has an elongation at break of ≥15% and a mechanical retention rate of ≥90% after long-term thermo-oxidative aging at 180°C.
[0008] The beneficial effects of this invention are as follows: 1) This invention enables HNBR to undergo moderate self-crosslinking through an extrusion in-situ grafting + self-crosslinking dual reaction coupling mechanism, thereby constructing a stable molecular network. The material can withstand high temperatures of 180℃ for a long time without softening or deformation, with minimal strength loss. Its high-temperature wear resistance is greatly improved, and its high-temperature oil absorption rate is significantly reduced. This invention can completely solve the industry bottlenecks of insufficient heat resistance of ultra-high molecular weight polyethylene, uneven wear and corrosion of metal pipes, and high cost of PEEK.
[0009] 2) This invention strengthens the interface bonding between PPS and HNBR through grafting reaction, which can completely solve the problems of incompatibility between the two phases, easy delamination, and large performance fluctuations. The toughness of the material is significantly improved, and the elongation at tensile fracture at 250℃ is stable at ≥15%, which fully meets the tensile assembly process requirements of steel pipe lining composite pipe and can achieve tight bonding and composite with steel pipe.
[0010] 3) The composite material of this invention is suitable for the complex medium environment of ultra-deep oilfields. Under long-term working conditions at 180℃, it has excellent resistance to water, crude oil, acid and alkali and high salt corrosion. Its wear resistance and anti-eccentric wear ability are far superior to traditional metal pipes, and its service life is significantly extended.
[0011] 4) This invention can simultaneously trigger two reactions during melt extrusion: First, the grafting reaction between HNBR and PPS mediated by the grafted monomer forms chemical bonds at the interface between the two phases, significantly improving the interfacial bonding and compatibility, and substantially enhancing the material's toughness and tensile elongation. The ethylene-glycidyl methacrylate epoxy group has strong activity and can form efficient covalent bonds at the interface between PPS and HNBR, thoroughly improving the poor compatibility and easy phase separation problems caused by polarity differences, resulting in high interface modification efficiency and suitability for the modification requirements of this system. Second, peroxide 301 initiates a moderate self-crosslinking reaction of the HNBR molecular chain, constructing a dense and stable elastic crosslinking network, significantly improving the material's heat resistance, high-temperature dimensional stability, wear resistance, and reducing the oil absorption rate of high-temperature crude oil.
[0012] 5) During the pretreatment process, nano-silica can uniformly coat HNBR particles, avoiding powder wetting and swelling and agglomeration during standing, and ensuring uniform dispersion of modified components; at the same time, with the nano size effect, it can achieve wear-resistant reinforcement, crack toughening, thermal barrier and anti-aging, and improve the high-temperature stability and wear resistance of the material. Detailed Implementation
[0013] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0014] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0015] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments of the present invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, and / or combinations thereof.
[0016] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the art; unless otherwise specified, the experimental methods and techniques used are conventional methods and techniques in the art.
[0017] The technical solutions provided by the present invention will be described below with reference to the embodiments. The scope of protection of the present invention is not limited by the following embodiments.
[0018] All embodiments and comparative examples of this invention use the following raw material grades: PPS: Solvay Ryton PR28, HNBR: Zetpol 2010 (Japan).
[0019] Example 1 A high-temperature resistant inner lining material for oilfield production equipment, comprising, by weight percentage: 75% polyphenylene sulfide (PPS) powder, 24.685% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% glycidyl methacrylate (GMA), 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (i.e., peroxide 301), and 0.5% nano-silica by weight of HNBR powder; The preparation method is as follows: Step S1: Mix N-methyl-2-pyrrolidone, methyl isobutyl ketone, and acetone in a mass ratio of 5:3:2 to obtain a composite solvent; Step S2: Add ethylene-glycidyl methacrylate and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane to the composite solvent prepared in step S1, stir and dissolve evenly to obtain a modified functional solution with a mass fraction of 30%. The stirring speed is 400 r / min and the stirring time is 20 min to ensure that the materials are completely dispersed and dissolved. Step S3: Add the modified functional solution prepared in step S2 to the HNBR powder, mix and stir for 2 min to fully wet the HNBR powder, then add nano silica powder, continue mixing and stirring for 30 min to homogenize, and then let stand at room temperature for 30 h for modification to allow the HNBR particles to fully adsorb the modified solution; wherein, the mass ratio of HNBR to modified functional solution and nano silica is: HNBR : modified functional solution : nano silica = 100 : 5.3 : 0.5; Step S4: The mixture modified by standing in step S3 is dried at 120°C to remove residual solvent and obtain modified HNBR composite powder. Step S5: The modified HNBR composite powder obtained in step S4 is premixed with polyphenylene sulfide (PPS) powder evenly, and then fed into a twin-screw extruder with a vent for melt blending, extrusion granulation, and extrusion. The twin-screw extrusion temperature range is 260-300℃. During the extrusion melting process, the HNBR grafting reaction and self-crosslinking reaction are triggered simultaneously to prepare a high-temperature resistant inner lining pipe composite material.
[0020] Example 2 A high-temperature resistant inner lining material for oilfield production equipment, by mass percentage, comprises: 80% polyphenylene sulfide (PPS) powder, 18.97% hydrogenated nitrile butadiene rubber (HNBR) powder, 1% glycidyl methacrylate (GMA), 0.03% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, and 0.5% nano-silica by mass of HNBR powder; the preparation method is the same as in Example 1.
[0021] Example 3 A high-temperature resistant inner lining material for oilfield production equipment, by mass percentage, comprises: 65% polyphenylene sulfide (PPS) powder, 34.69% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% glycidyl methacrylate (GMA), 0.01% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, and 0.5% nano-silica by mass of HNBR powder; the preparation method is the same as in Example 1.
[0022] Example 4 A high-temperature resistant inner lining material for oilfield production equipment, by mass percentage, comprises: 70% polyphenylene sulfide (PPS) powder, 29.685% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% glycidyl methacrylate (GMA), 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, and 0.5% nano-silica by mass of HNBR powder; the preparation method is the same as in Example 1.
[0023] Comparative Example 1 (PPS-HNBR composite material) A PPS-HNBR composite material, by mass percentage, comprises: 75% polyphenylene sulfide (PPS) powder and 25% hydrogenated nitrile butadiene rubber (HNBR) powder; the PPS powder and HNBR powder are premixed uniformly, and then fed into a twin-screw extruder with a vent for melt blending, extrusion granulation, and the twin-screw extrusion temperature range is 260–300℃ to prepare the PPS-HNBR composite material.
[0024] Comparative Example 2 (without GMA grafted monomer) A composite material, by mass percentage, comprises: 75% polyphenylene sulfide (PPS) powder, 24.985% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, and 0.5% nano-silica by mass of HNBR powder; except that ethylene-glycidyl methacrylate (GMA) is not added in step S2, the other preparation steps are the same as in Example 1.
[0025] Comparative Example 3 (without 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane) A composite material, by mass percentage, comprises: 75% polyphenylene sulfide (PPS) powder, 24.7% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% ethylene-glycidyl methacrylate, and 0.5% nano-silica by mass of HNBR powder; except that 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane is not added in step S2, the rest of the preparation steps are the same as in Example 1.
[0026] Comparative Example 4 (Low HNBR High Rigidity Formulation) A composite material, by mass percentage, comprises: 90% polyphenylene sulfide (PPS) powder, 9.685% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% glycidyl methacrylate (GMA), 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (i.e., peroxide 301), and 0.5% nano-silica by mass of HNBR powder; the preparation process is the same as in Example 1.
[0027] Comparative Example 5 (High HNBR High Rigidity Formulation) A composite material, by mass percentage, comprises: 55% polyphenylene sulfide (PPS) powder, 43.685% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% glycidyl methacrylate (GMA), 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (i.e., peroxide 301), and 0.5% nano-silica by mass of HNBR powder; the preparation process is the same as in Example 1.
[0028] Comparative Example 6 (Solvent-free dry powder blend system) A composite material with the same raw material formulation as in Example 1, namely, by mass percentage, comprising: 75% polyphenylene sulfide (PPS) powder, 24.685% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% glycidyl methacrylate (GMA), 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (i.e., peroxide 301), and 0.5% nano-silica by mass of HNBR powder; The preparation method is as follows: the above raw materials are premixed evenly, and then put into a twin-screw extruder with a vent for melt blending, extrusion and granulation. The twin-screw extrusion temperature range is 260-300℃, and the composite material is prepared.
[0029] Comparative Example 7 (without nano-silica) A composite material, by mass percentage, comprises: 75% polyphenylene sulfide (PPS) powder, 24.685% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% ethylene-glycidyl methacrylate (GMA), and 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (i.e., peroxide 301); the preparation process is the same as in Example 1.
[0030] Comparative Example 8 (replace EMA with MAH) A composite material, by mass percentage, comprises: 75% polyphenylene sulfide (PPS) powder, 24.685% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3% maleic anhydride (MAH), 0.015% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (i.e., peroxide 301), and 0.5% nano-silica by mass of HNBR powder; the preparation process is the same as in Example 1.
[0031] The composite materials prepared in Examples 1-4 and Comparative Examples 1-8 were subjected to the following performance tests: The following tests were conducted: 2000 h of thermo-oxidative aging at 180℃; room temperature tensile properties; impact strength of a simply supported beam; oil absorption rate after 2000 h of immersion in crude oil at 180℃; mortar abrasion properties; and Vicat softening temperature test. The Vicat softening temperature test was performed according to GB / T 1633-2000 standard, with a heating rate of 120℃ / h and an applied load of 10 N. The impact strength test adopted GB / T 1043.1-2021 unnotched impact test for simply supported beams, conducted at room temperature. The results are shown in Table 1. Table 1. Performance test results of the composite materials prepared in Examples 1-4 and Comparative Examples 1-8
[0032] As shown in Table 1, the high-temperature resistant inner lining material for oilfield production equipment prepared in Example 1 exhibits the best overall performance, demonstrating a balance of rigidity and toughness, high-temperature resistance, oil resistance, and wear resistance, fully meeting the requirements of composite processes and long-term operation at 180℃. In Examples 1-4, the HNBR content was within the optimal range of 10%–35%. A horizontal comparison using the optimal formulation of Example 1 as a benchmark reveals the following: In Example 2, with a high PPS and high graft crosslinking ratio, the material's heat resistance and wear resistance slightly improved, while the yield elongation and impact toughness decreased slightly but still fully met the requirements; In Example 3, with a high HNBR ratio, the material exhibited the best elongation and impact resistance, while its heat resistance, oil resistance, and anti-aging properties slightly decreased but still met the operating conditions; In Example 4, the low GMA content system showed slight fluctuations in overall performance, with all indicators meeting the process and high-temperature service standards. The four sets of examples demonstrated balanced and stable performance, fully verifying the scientific validity and practicality of the formulation ratio range, dual-reaction modification process, and supporting additive system of this invention.
[0033] Comparative Example 1 uses only physical blending of pure dry powders of PPS and HNBR as raw materials, without any interface modification or cross-linking network structure. Compared with Example 1, the composite material system prepared in Comparative Example 1 has significantly lower yield elongation and unnotched impact strength, higher material brittleness, and extremely poor interfacial compatibility between the two phases. At the same time, the oil absorption rate of high-temperature crude oil is greatly increased, and the Vicat softening point, high-temperature thermo-oxidative aging strength retention rate, and wear resistance are significantly reduced. The PPS-HNBR composite material prepared in Comparative Example 1 cannot meet the requirements of steel pipe tensile composite process, nor can it be adapted to the long-term high-temperature oilfield service conditions of 180℃, and has no engineering application value.
[0034] Compared to Example 1, Comparative Example 2 discarded the GMA grafted monomer and only retained the peroxide 301 (3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane) crosslinking system and nano-silica additive. It could only achieve HNBR self-crosslinking and could not complete the chemical bonding modification of the PPS and HNBR two-phase interface. Compared to Example 1, the yield elongation and unnotched impact strength of this system were significantly lower, the two-phase interface bonding was weak, and it was prone to delamination and cracking under stress. At the same time, the high-temperature oil absorption rate was higher, and its high-temperature thermo-oxidative aging stability and wear resistance were significantly weaker. The material prepared in Comparative Example 2 did not meet the tensile elongation standard, making it unsuitable for the steel pipe tensile composite assembly process and unable to meet the long-term high-temperature service requirements of 180℃ in ultra-deep oilfields.
[0035] Compared to Example 1, Comparative Example 3 discarded the peroxide 301 crosslinking agent, retaining only the GMA grafted monomer and nano-silica additive. It only optimized the interfacial compatibility of the two phases and could not construct the HNBR crosslinked network structure. Compared to Example 1, although the yield point elongation of the system prepared in Comparative Example 3 basically met the requirements, the Vicat softening point, high-temperature thermo-oxidative aging strength retention rate, and wear resistance were significantly lower. The oil absorption rate of high-temperature crude oil was significantly increased, and the material's high-temperature deformation resistance and swelling resistance were weak. The material prepared in Comparative Example 3 could only meet the requirements of the steel pipe tensile composite process, and its high-temperature stability performance was severely lacking, making it unsuitable for the harsh operating conditions of long-term high-temperature oilfields at 180°C.
[0036] Compared to Example 1, Comparative Example 4 significantly reduced the amount of HNBR (below the critical threshold of 10%) and increased the proportion of rigid PPS resin. The grafted monomers, crosslinking agents, nano-additives, and preparation processes were all consistent with Example 1. Compared to Example 1, the yield point elongation and unnotched impact strength of the system prepared in Comparative Example 4 were significantly lower, indicating excessive rigidity and brittleness. Although it exhibited excellent Vicat softening point and high-temperature oil resistance, it severely lacked toughness. The material prepared in Comparative Example 4 could not meet the elongation requirements of the steel pipe tensile composite process, and was prone to brittle fracture and springback failure during assembly, thus lacking practical engineering value.
[0037] Compared to Example 1, Comparative Example 5 significantly increased the amount of HNBR (above the critical threshold of 35%) and reduced the proportion of PPS heat-resistant resin. The remaining additives, formulation ratios, and preparation processes were consistent with Example 1. Compared to Example 1, the system prepared in Comparative Example 5 exhibited excellent yield elongation, unnotched impact strength, and sufficient toughness; however, its Vicat softening point was significantly lower and below 180°C, resulting in a substantial increase in high-temperature crude oil absorption and a significant decrease in high-temperature thermo-oxidative aging retention and wear resistance. The composite material prepared in Comparative Example 5 could meet the requirements of the steel pipe tensile composite assembly process, but its heat resistance, oil resistance, and aging resistance were substandard, making it unsuitable for long-term high-temperature operation at 180°C in ultra-deep oilfields.
[0038] Comparative Example 6 uses the same complete raw material formula and additive dosage, but omits the solvent wetting pretreatment and room temperature static activation process, and adopts a direct dry powder blending extrusion process. Compared with Example 1, the system prepared in Comparative Example 6 has more microstructural defects due to the inability of the modified components to penetrate and adsorb uniformly, insufficient melt reaction, significantly lower yield point elongation and unnotched impact strength, higher high-temperature oil absorption rate, and significantly reduced high-temperature thermo-oxidative aging stability and wear resistance. The overall performance uniformity of the material is poor. The composite material prepared in Comparative Example 6 does not meet the comprehensive performance requirements and cannot simultaneously meet the dual requirements of steel pipe stretching composite process and long-term service in 180°C high-temperature oilfields.
[0039] Comparative Example 7 has the same complete formulation and preparation process, except that the nano-silica functional additive was omitted. Compared with Example 1, the yield point elongation and unnotched impact strength of the system prepared in Comparative Example 7 basically meet the requirements, and the basic mechanical properties can meet the requirements of the composite process; however, the dispersion, reinforcement, heat insulation and toughening effects of nanoparticles are lacking, resulting in a significant decrease in the high-temperature thermo-oxidative aging strength retention rate and wear resistance, a slight increase in the high-temperature crude oil absorption rate, and a significant weakening of the material's long-term high-temperature service stability, dimensional stability and anti-wear performance. The basic properties of the composite material prepared in Comparative Example 7 barely meet the requirements, but its long-term service performance is weak and cannot meet the long-term use requirements of the harsh high-temperature conditions in ultra-deep oilfields; this also further confirms that the ethylene-glycidyl methacrylate (GMA) grafted monomer selected in this invention can efficiently optimize the interfacial bonding between the two phases, which is the core key to ensuring the excellent mechanical properties and interfacial compatibility of the material.
[0040] Comparative Example 8 used the same formulation, crosslinking agent, nano-additives, and complete preparation process as Example 1, except that the GMA grafting monomer was replaced with an equal amount of maleic anhydride (MAH). Compared to Example 1, maleic anhydride exhibited lower interfacial reactivity and grafting efficiency with PPS and HNBR, resulting in weak interfacial bridging and an inability to effectively improve interfacial compatibility. This led to significantly lower yield point elongation, tensile strength, and unnotched impact strength, resulting in weak interfacial bonding and insufficient toughness. Simultaneously, the high-temperature oil absorption rate increased, and the high-temperature aging stability and wear resistance decreased significantly. The fracture elongation of the composite material prepared in Comparative Example 8 was far below the 15% standard, which could not meet the requirements of the steel pipe tensile composite assembly process, and its long-term high-temperature service performance was insufficient, thus lacking engineering application value. In other words, Comparative Example 8 shows that ethylene-glycidyl methacrylate (GMA) has higher interfacial reactivity and stronger grafting modification efficiency than traditional maleic anhydride grafted monomers. It can form stable chemical bonds between the PPS and HNBR phases, greatly improving interfacial compatibility and fundamentally solving the problems of incompatibility between the two phases, easy phase separation, and weak mechanical properties. It is the core preferred monomer for achieving high toughness and high stability in the material of this invention.
[0041] Combining the data from multiple gradient formulation examples and comparative experiments of this invention, it is clear that the mechanical toughness (elongation at break) and high-temperature heat resistance of the composite material exhibit a significant positive and negative correlation with the HNBR content. The HNBR rubber phase is mainly responsible for improving the elongation toughness of the material, while the PPS resin phase mainly provides high-temperature heat resistance, wear resistance, and structural stability. The ratio of the two phases has a strict compatibility critical range, directly determining whether the material meets the dual-use standards for oilfield inner lining pipes (tensile elongation ≥15%, long-term resistance to 180℃ high-temperature conditions). The performance variation law of the prepared composite material is as follows: 1. The variation of elongation at break with HNBR content As the HNBR content in the system gradually increases, the proportion of rubber flexibility in the composite material increases, the molecular chain slippage ability during yielding and tensile testing is enhanced, and the elongation at break shows a continuous and steady upward trend. Based on the critical values from experimental data, it can be determined that when the HNBR mass content is below 10%, the rubber toughening component in the system is severely insufficient, the material is excessively rigid and brittle, and the elongation at break of the composite material is below the critical standard of 15%, failing to meet the requirements of the tensile composite assembly process for steel pipe linings. It is prone to brittle fracture and springback failure during tensile testing, making interference fit with the steel pipe impossible. A typical example is Comparative Example 4 (HNBR content 9.685%), with an elongation of only 10.2%, completely unsuitable for composite processing conditions.
[0042] When the HNBR content is maintained within the optimal range of 10% to 35% as defined in this invention, the material elongation is stable at ≥15%, which can balance toughness and structural strength, and is perfectly suited for steel pipe stretching composite process; among them, Example 3 with high HNBR ratio (HNBR 34.69%) has an elongation of up to 18.6%, with sufficient toughness reserve.
[0043] 2. Variation of Vicat softening point with HNBR content Contrary to the trend in elongation, as the content of HNBR rubber phase continues to increase, the proportion of high-temperature rigid PPS resin in the system decreases, the overall high-temperature deformation resistance of the composite material gradually declines, and the Vicat softening point continues to decrease. Considering the requirements of long-term service in ultra-deep oilfields at 180℃, it can be determined that when the HNBR mass content is higher than 35%, the proportion of flexible rubber is too high, the support of the high-temperature resin skeleton is insufficient, and the Vicat softening point of the composite material is lower than 180℃, failing to meet the requirements of long-term high-temperature service at 180℃. Under high-temperature downhole conditions, it is prone to failure problems such as softening, collapse, deformation, and dimensional instability. A typical example is Comparative Example 5 (HNBR content 43.685%), with a Vicat softening point of only 178℃, lower than the critical temperature for high-temperature conditions, and its heat resistance performance is substandard.
[0044] Therefore, those skilled in the art will recognize that although embodiments of the present invention have been shown and described in detail herein, many other variations or modifications conforming to the principles of the present invention can be directly determined or derived from the disclosure of the present invention without departing from the spirit and scope of the invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.
Claims
1. A high-temperature resistant inner lining material for oilfield production equipment, characterized in that, By mass percentage, it includes the following components: 65%–85% polyphenylene sulfide (PPS) powder, 10%–35% hydrogenated nitrile butadiene rubber (HNBR) powder, 0.3%–1% grafted monomer, and 0.015%–0.03% 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane.
2. The high-temperature resistant inner lining material for oilfield production equipment according to claim 1, characterized in that, The PPS is a linear, low-crosslinked polyphenylene sulfide powder with a melt flow index (MFR) of 10–30 g / 10 min under conditions of 315°C and 5 kg load.
3. The high-temperature resistant inner lining material for oilfield production equipment according to claim 1, characterized in that, The HNBR has a saturation of ≥98% and an acrylonitrile content of 33-36%.
4. The high-temperature resistant inner lining material for oilfield production equipment according to claim 1, characterized in that, The grafting monomer is ethylene-glycidyl methacrylate.
5. The high-temperature resistant inner lining material for oilfield production equipment according to claim 1, characterized in that, It also includes nano-silica powder, wherein the amount of nano-silica powder added is 0.3% to 1% of the mass of HNBR powder.
6. A method for preparing a high-temperature resistant inner lining material for oilfield production equipment as described in any one of claims 1 to 5, characterized in that, The preparation steps include the following: Step S1: Mix N-methyl-2-pyrrolidone, methyl isobutyl ketone, and acetone in a mass ratio of 8~4: 5~2: 3~1 to obtain a composite solvent; Step S2: Add the grafted monomer and 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane to the composite solvent obtained in step S1, stir and dissolve evenly to obtain a modified functional solution with a mass fraction of 20~45%. Step S3: Add the modified functional solution prepared in step S2 to the HNBR powder, mix and stir for 1-5 min, then add nano-silica powder, continue to mix and stir evenly, and then let stand for 24-40 h for modification; the mass ratio of HNBR to modified functional solution and nano-silica is: HNBR : modified functional solution : nano-silica = 100 : 5-8 : 0.3-1; S4: Dry the mixture after step S3 (which has been allowed to stand and modified) to remove residual solvent and obtain modified HNBR composite powder. S5: The modified HNBR composite powder obtained in step S4 is premixed with polyphenylene sulfide (PPS) powder and then fed into a twin-screw extruder for melt blending and extrusion granulation. During the extrusion and melting process, the HNBR grafting reaction and self-crosslinking reaction are triggered simultaneously to prepare a high-temperature resistant inner lining pipe composite material.
7. The preparation method according to claim 6, characterized in that, In step S2, the stirring speed is 300-500 r / min and the stirring time is 15-30 min.
8. The preparation method according to claim 6, characterized in that, In step S3, the modified functional solution is added to the HNBR powder, and after mixing and stirring for 2-3 minutes, nano-silica powder is added, and mixing and stirring is continued for 20-40 minutes.
9. The preparation method according to claim 6, characterized in that, In step S4, the mixture after static modification is dried at 80~130℃.
10. The preparation method according to claim 6, characterized in that, In step S5, the twin-screw extrusion temperature range is 260-300℃, and the elongation at break of the prepared composite material is ≥15%, and the mechanical retention rate after long-term thermo-oxidative aging at 180℃ is ≥90%.