A superabsorbent resin-based water-retaining and root-promoting composite material for garden plants

By combining a modified superabsorbent polymer matrix, a water-retaining additive, and a root-promoting active component, the problems of decreased water absorption ratio and structural collapse of superabsorbent polymers in saline soils were solved, achieving high osmotic pressure difference and a stable network, promoting root growth, and avoiding pesticide damage.

CN123100475APending Publication Date: 2026-11-17郑州市园林绿化发展中心 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611268547.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing superabsorbent polymers exhibit reduced water absorption rates in saline soils, their three-dimensional network structure is prone to collapse, resulting in insufficient water retention capacity. Furthermore, the release of root-promoting active ingredients is uncontrollable, easily leading to root deformities and pesticide damage.

Method used

A composite material consisting of a modified superabsorbent resin matrix, a modified water-retaining functional additive, and a modified root-promoting active component is used. Through the synergistic effect of calcium phosphate crosslinking, chitosan crosslinking network, attapulgite activation and pore expansion, and α-naphthaleneacetic acid active component, the water absorption capacity and network stability of the material in a polyvalent salt ion environment are improved, and the sustained release of active ingredients is achieved through the phosphate ester structure.

Benefits of technology

Maintaining a high osmotic pressure difference and stable network structure under the coexistence of polyvalent salt ions enables the slow release and continuous supply of water, avoiding network collapse and root deformity, and improving the water retention rate and root promotion effect of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of garden plant cultivation technology, specifically to a water-retaining and root-promoting composite material based on superabsorbent resin for garden plants. The composite material comprises the following raw materials: a modified superabsorbent resin matrix, a modified water-retaining functional agent, and a modified root-promoting active component. In this invention, the modified superabsorbent resin matrix enhances the stability of the resin's three-dimensional network structure and gel strength, allowing the material to maintain structural integrity during repeated water absorption and release. The modified water-retaining functional agent increases surface active sites, specific surface area, and pore volume, improving the water absorption and retention performance of attapulgite soil in saline media. The modified root-promoting active component enhances biocompatibility, prevents premature degradation of active ingredients, and extends the effective period of root-promoting action. These three modified components collectively solve the problems of low water absorption ratio, poor salt tolerance, and excessively rapid release of root-promoting active ingredients in existing garden water-retaining materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of garden plant cultivation technology, specifically to a water-retaining and root-promoting composite material based on a highly absorbent resin for garden plants. Background Technology

[0002] Superabsorbent polymer (SAP)-based water-retaining and root-promoting composite materials are a type of functional horticultural material that integrates water retention and root growth promotion. This material utilizes the three-dimensional network structure of superabsorbent polymer to absorb and store a large amount of water, which is slowly released for plant absorption when the soil is dry. At the same time, it uses active components to regulate the level of endogenous hormones in plants, stimulate the division and elongation of root meristematic cells, and promote the occurrence and development of lateral roots and adventitious roots.

[0003] In existing technologies, sodium polyacrylate superabsorbent polymers exhibit a sharp decrease in water absorption rate in saline soil environments, and their three-dimensional network structure is prone to collapse after repeated water absorption and release, leading to decreased gel strength and low reusability, especially in Ca... 2+ Mg 2+ Under conditions where polyvalent salt ions coexist, carboxylate ions are coordinated and shielded, resulting in a sharp decrease in osmotic pressure difference and a weakening of water retention capacity.

[0004] Water-retaining materials often employ simple physical blending or single acid activation, resulting in insufficient opening of their nanopores, low specific surface area and pore volume utilization, poor interfacial compatibility with polymer resin matrices, and a tendency to undergo phase separation and aggregation.

[0005] The active ingredients that promote root growth have a short duration of action in the soil and are rapidly degraded by photosynthesis and microorganisms. The release curves of existing physical coating slow-release technologies are uncontrollable, and they are highly sensitive to concentration. Excessive use can easily lead to root malformation and phytotoxicity.

[0006] Based on this, the present invention provides a water-retaining and root-promoting composite material based on superabsorbent resin for garden plants. Summary of the Invention

[0007] The purpose of this invention is to provide a superabsorbent resin-based water-retaining and root-promoting composite material for garden plants. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants prepared by this invention simulates soil salinity solution (Ca). 2+ Mg 2+ A high water absorption ratio in (coexistence) indicates that the material has high Ca content. 2+ Mg 2+Under conditions of coexistence of polyvalent salt ions, it can still maintain a high osmotic pressure difference and network structure stability, and can effectively absorb and retain water; the high water retention rate of the composite material in soil after 10 days indicates that the material has a strong ability to slowly release the absorbed water and continuously supply the plant roots in a real soil environment; the high water retention rate after repeated water absorption and release 5 times indicates that the material can still maintain a high water retention capacity after multiple cycles of water absorption, drying and re-absorption, the three-dimensional network structure is not easy to collapse and the gel strength decays slowly.

[0008] To achieve the above objectives, the present invention provides the following technical solution: a superabsorbent resin-based water-retaining and root-promoting composite material for garden plants, which is composed of the following parts by weight of raw materials: 100 parts of modified superabsorbent resin matrix, 30-50 parts of modified water-retaining functional additive, and 3-5 parts of modified root-promoting active component.

[0009] The modified superabsorbent resin matrix is ​​prepared by treating sodium acrylate with an aqueous solution of calcium phosphate, ammonium persulfate, N,N'-methylenebisacrylamide, chitosan, and polyvinyl alcohol.

[0010] The modified water-retaining functional additive is prepared by treating attapulgite with citric acid, urea and zinc sulfate; the attapulgite is then subjected to thermal activation and acid activation pretreatment to obtain an activated pretreated attapulgite suspension.

[0011] The modified root-promoting active component is prepared by treating α-naphthaleneacetic acid with fulvic acid, phosphoric acid, and calcium phosphate; the α-naphthaleneacetic acid is then subjected to purification treatment and activation treatment by adsorption decolorization.

[0012] Further, the preparation method of the modified superabsorbent resin matrix is ​​as follows: Sodium acrylate is mixed with deionized water to prepare a sodium acrylate aqueous solution with a mass fraction of 20-30%. Zinc phosphate is added and stirred evenly, and nitrogen gas is passed through to remove oxygen. Ammonium persulfate and N,N'-methylenebisacrylamide are added, and a prepolymerization reaction is carried out at 50-70℃ to obtain product A. Chitosan is added to an acetic acid aqueous solution with a mass fraction of 1-3% to prepare a chitosan acetic acid solution with a mass fraction of 1-2%, and then added to product A. The reaction is carried out at 60-80℃ to obtain product B. A polyvinyl alcohol aqueous solution with a mass fraction of 5-15% is added to product B, and the reaction is carried out by stirring at 70-90℃. After cooling to room temperature, the product is filtered, washed, dried, and pulverized to obtain the modified superabsorbent resin matrix.

[0013] Further, the mass ratio of calcium phosphate to sodium acrylate is 1:8-12; the amount of ammonium sulfate added is 0.4-0.8% of the mass of sodium acrylate, and the amount of N,N'-methylenebisacrylamide added is 0.05-0.15% of the mass of sodium acrylate; the mass ratio of chitosan to sodium acrylate is 1:15-25; and the mass ratio of polyvinyl alcohol to sodium acrylate is 1:25-35.

[0014] Further, the preparation method of the activated pretreated attapulgite suspension is as follows: the raw attapulgite ore is crushed and sieved, and then calcined at 300-400℃ to obtain thermally activated attapulgite; the thermally activated attapulgite is dispersed in a hydrochloric acid solution with a mass fraction of 5-15% at a solid-liquid ratio of 1:5-10g / mL, and after acid activation treatment by stirring at 40-60℃, it is filtered, washed with water until neutral, and dried to obtain acid-thermal double-activated attapulgite; the acid-thermal double-activated attapulgite is dispersed in deionized water to prepare a suspension with a mass fraction of 10-20%, and ultrasonically dispersed to obtain the activated pretreated attapulgite suspension.

[0015] Further, the preparation method of the modified water-retaining functional additive is as follows: citric acid is added to the activated pretreated attapulgite suspension, and after stirring and reacting at 50-70℃, the mixture is filtered and washed to obtain citric acid complexed activated modified attapulgite; the citric acid complexed activated modified attapulgite is dispersed in a urea aqueous solution with a mass fraction of 5-15%, and after stirring and reacting at 60-80℃, the mixture is filtered and washed to obtain urea intercalated pore-expanding modified attapulgite; the urea intercalated pore-expanding modified attapulgite is dispersed in a zinc sulfate aqueous solution with a mass fraction of 4-8%, and after reacting at 40-60℃, the mixture is filtered, washed, and dried to obtain the modified water-retaining functional additive.

[0016] Furthermore, the mass ratio of citric acid to attapulgite is 1:10-15; the mass ratio of urea to attapulgite is 1:5-10; and the mass ratio of zinc sulfate to attapulgite is 1:12-18.

[0017] Further, the purification and activation treatment method for α-naphthaleneacetic acid is as follows: α-naphthaleneacetic acid raw material is dissolved in anhydrous ethanol to prepare a solution with a mass fraction of 10-20%, activated carbon is added, and the solution is stirred at 40-60℃ for adsorption and decolorization treatment, followed by filtration to obtain a purified α-naphthaleneacetic acid solution; sodium hydroxide ethanol solution is added to the purified α-naphthaleneacetic acid solution to adjust the pH to 8.0-9.0, and the solution is stirred at 50-70℃ to obtain an activated sodium α-naphthaleneacetic acid solution; the activated sodium α-naphthaleneacetic acid solution is concentrated under reduced pressure to remove part of the solvent to 40-50% of its original volume to obtain an activated concentrate, thus completing the purification and activation treatment.

[0018] Furthermore, the mass ratio of activated carbon to α-naphthaleneacetic acid is 1:20-30; the volume ratio of ethanol to water in the sodium hydroxide ethanol solution is 1-3:1, and the mass fraction of the sodium hydroxide ethanol solution is 6-10%.

[0019] Further, the preparation method of the modified root-promoting active component is as follows: α-naphthaleneacetic acid after purification and activation is dissolved in an aqueous ethanol solution to prepare a solution with a mass fraction of 6-10%, fulvic acid is added, and the mixture is stirred and reacted at 40-60℃ to obtain a fulvic acid synergistic modified product; phosphoric acid is added to the fulvic acid synergistic modified product, and the mixture is stirred and reacted at 50-70℃ to obtain a phosphate ester complex modified product; an aqueous solution of calcium phosphate is added to the phosphate ester complex modified product, and the mixture is stirred and reacted at 30-50℃, followed by vacuum distillation to remove the solvent, and freeze-drying to obtain the modified root-promoting active component.

[0020] Further, the volume ratio of ethanol to water in the ethanol-water solution is 1-3:1, the mass ratio of fulvic acid to α-naphthaleneacetic acid is 1:4-6, the mass ratio of phosphoric acid to α-naphthaleneacetic acid is 1:8-12, the mass fraction of the calcium phosphate aqueous solution is 3-5%, and the mass ratio of calcium phosphate to α-naphthaleneacetic acid is 1:15-25.

[0021] Compared with the prior art, the beneficial effects of the present invention are: 1. In this invention, the modified superabsorbent resin matrix uses sodium acrylate as the polymer backbone. Calcium ion crosslinking sites are introduced in situ through calcium phosphate. A dual-network structure is constructed using the interpenetrating crosslinking network of chitosan and the semi-interpenetrating network of polyvinyl alcohol, which reinforces the structure and inhibits network collapse during repeated water absorption and release. Simultaneously, the coordination shielding effect of calcium ions reduces the sensitivity of carboxylate groups to polyvalent salt ions, thus enhancing the composite material's ability to withstand calcium ions. 2+ Mg 2+ It maintains a high osmotic pressure difference and water absorption capacity in coexisting soil, solving the problem of the sharp drop in water absorption rate and short cycle life of conventional sodium polyacrylate resin in saline environment.

[0022] 2. In this invention, attapulgite is thermally activated to remove structural water and acid-activated to replace interlayer cations, making the pores fully interconnected. Then, it is activated by citric acid complexation to introduce carboxyl coordination groups to increase surface active sites. Urea intercalation expands the pores, increasing the specific surface area and pore volume. Zinc sulfate ion exchange anchors zinc ions in the interlayer or on the surface, giving attapulgite dual functionality of cation exchange and coordination adsorption. At the same time, zinc ions act as a bridge to improve the interfacial compatibility between attapulgite and the resin matrix, avoiding phase separation and agglomeration. This solves the problems of low pore utilization and poor interfacial bonding with polymer matrix in attapulgite activated by single acid.

[0023] 3. In this invention, the modified root-promoting active ingredient is first purified by adsorption and decolorization of α-naphthaleneacetic acid by activated carbon, and then converted into sodium salt by alkalization to improve water solubility. Then, it is enhanced with fulvic acid to form a molecular complex through hydrogen bonding and hydrophobic interaction to enhance biocompatibility. Phosphoric acid complexes with the hydroxyl groups of α-naphthaleneacetic acid to form a phosphate ester structure to prevent premature degradation of active groups. Calcium ions are combined through ionic bonds and coordination bonds to achieve slow release regulation, so that the release rate of active ingredients in the soil matches the growth period of plant roots, avoiding the problems of uncontrollable release and excessive application of pesticides caused by conventional physical coating. Detailed Implementation

[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0025] It should be noted that the raw materials used in the following embodiments are all commercially available.

[0026] Example 1: A water-retaining and root-promoting composite material based on superabsorbent resin for garden plants, composed of the following parts by weight of raw materials: 100 parts modified superabsorbent resin matrix, 30 parts modified water-retaining functional additive, and 3 parts modified root-promoting active component.

[0027] The modified superabsorbent resin matrix is ​​prepared by treating sodium acrylate with calcium phosphate, ammonium persulfate, N,N'-methylenebisacrylamide, chitosan and polyvinyl alcohol aqueous solution.

[0028] The modified water-retaining functional additive is prepared by treating attapulgite with citric acid, urea and zinc sulfate; the attapulgite is then subjected to thermal activation and acid activation pretreatment to obtain an activated pretreated attapulgite suspension.

[0029] The modified root-promoting active component was prepared by treating α-naphthaleneacetic acid with fulvic acid, phosphoric acid, and calcium phosphate. The α-naphthaleneacetic acid was then subjected to purification and activation treatments, including adsorption and decolorization.

[0030] The modified superabsorbent resin matrix is ​​prepared as follows: Sodium acrylate is dissolved in deionized water to prepare a 20% sodium acrylate aqueous solution. Zinc phosphate is added and stirred until homogeneous. Nitrogen gas is then purged for 20 minutes to remove oxygen. Ammonium persulfate and N,N'-methylenebisacrylamide are added, and the mixture is prepolymerized at 50°C for 30 minutes to obtain product A. Chitosan is added to a 1% acetic acid aqueous solution to prepare a 1% chitosan acetic acid solution, which is then added to product A. The mixture is reacted at 60°C for 2 hours to obtain a chitosan crosslinked network interpenetrating modified product. A 5% polyvinyl alcohol aqueous solution is added to the chitosan crosslinked network interpenetrating modified product, and the mixture is stirred at 70°C for 1 hour to allow the polyvinyl alcohol molecular chains to form an interpenetrating network structure with the resin network. The mixture is then cooled to room temperature, filtered, washed, dried, and pulverized to obtain the modified superabsorbent resin matrix.

[0031] The mass ratio of calcium phosphate to sodium acrylate is 1:8; the amount of ammonium sulfate added is 0.4% of the mass of sodium acrylate, and the amount of N,N'-methylenebisacrylamide added is 0.05% of the mass of sodium acrylate; the mass ratio of chitosan to sodium acrylate is 1:15; and the mass ratio of polyvinyl alcohol to sodium acrylate is 1:25.

[0032] The preparation method of the activated pretreated attapulgite suspension is as follows: attapulgite ore is crushed through a 100-mesh sieve, placed in a muffle furnace, and calcined at 300℃ for 1 hour to remove surface water and structural water, resulting in thermally activated attapulgite; the thermally activated attapulgite is dispersed in a 5% hydrochloric acid solution at a solid-liquid ratio of 1:5 g / mL, and acid-activated at 40℃ for 1 hour to allow hydrogen ions to replace the metal cations in the attapulgite crystals, increasing the specific surface area and pore volume; the solution is filtered, washed with water until neutral, and dried to obtain acid-thermal double-activated attapulgite; the acid-thermal double-activated attapulgite is dispersed in deionized water to prepare a 10% suspension, and ultrasonically dispersed at an ultrasonic frequency of 40kHz for 20 minutes to fully exfoliate and disperse the activated attapulgite, resulting in the activated pretreated attapulgite suspension.

[0033] The preparation method of the modified water-retaining functional additive is as follows: citric acid is added to the activated pretreated attapulgite suspension, and the mixture is stirred at 50°C for 1 hour to allow the citric acid to undergo a complexation reaction with calcium and magnesium ions on the surface of the attapulgite. After filtration and washing, citric acid complexed activated modified attapulgite is obtained. The citric acid complexed activated modified attapulgite is dispersed in a urea aqueous solution and stirred at 60°C for 2 hours to allow urea molecules to insert into the interlayer of the attapulgite for pore expansion treatment. After filtration and washing, urea-intercalated pore-expanding modified attapulgite is obtained. The urea-intercalated pore-expanding modified attapulgite is dispersed in a zinc sulfate aqueous solution and stirred at 40°C for ion exchange reaction for 1 hour to allow zinc ions to exchange into the interlayer of the attapulgite or adsorb onto the surface. After filtration, washing, and drying, the modified water-retaining functional additive is obtained.

[0034] The mass ratio of citric acid to attapulgite is 1:10; the mass ratio of urea to attapulgite is 1:5; and the mass ratio of zinc sulfate to attapulgite is 1:12.

[0035] The purification and activation methods for α-naphthaleneacetic acid are as follows: α-naphthaleneacetic acid raw material is dissolved in anhydrous ethanol to prepare a 10% (w / w) solution. Activated carbon is added, and the mixture is stirred at 40°C for 30 min for adsorption and decolorization. The activated carbon is then removed by filtration to obtain a purified α-naphthaleneacetic acid solution. Sodium hydroxide ethanol solution is added to the purified α-naphthaleneacetic acid solution to adjust the pH to 8.0. The mixture is stirred at 50°C for 30 min to convert α-naphthaleneacetic acid into sodium α-naphthaleneacetate, which has better water solubility, thus obtaining an activated sodium α-naphthaleneacetate solution. The activated sodium α-naphthaleneacetate solution is then concentrated under reduced pressure (0.04 MPa, 40°C) to remove some of the solvent to 40% of the original volume, yielding an activated concentrate, thus completing the purification and activation processes.

[0036] The mass ratio of activated carbon to α-naphthaleneacetic acid is 1:20; the volume ratio of ethanol to water in the sodium hydroxide ethanol solution is 1:1, and the mass fraction of the sodium hydroxide ethanol solution is 6%.

[0037] The preparation method of the modified root-promoting active component is as follows: α-naphthaleneacetic acid (NAA) after purification and activation is dissolved in an aqueous ethanol solution to prepare a 6% (w / w) solution. Fulvic acid is added, and the mixture is stirred and reacted at 40°C for 1 hour. This allows fulvic acid and NAA to form a molecular complex through hydrogen bonding and hydrophobic interactions, yielding a fulvic acid synergistic modified product. Phosphoric acid is added to the fulvic acid synergistic modified product, and the mixture is stirred and reacted at 50°C for 1 hour. This allows phosphoric acid to undergo a complexation reaction with the hydroxyl groups of NAA, forming a stable phosphate ester complex, yielding a phosphate ester complex modified product. A calcium phosphate aqueous solution is added to the phosphate ester complex modified product, and the mixture is stirred and reacted at 30°C for 30 minutes. This allows calcium ions to combine with the modified NAA molecules through ionic and coordinate bonds, forming a sustained-release complex. The solvent is then removed by vacuum distillation, and the mixture is freeze-dried to obtain the modified root-promoting active component.

[0038] In the ethanol-water solution, the volume ratio of ethanol to water is 1:1, the mass ratio of fulvic acid to α-naphthaleneacetic acid is 1:4, the mass ratio of phosphoric acid to α-naphthaleneacetic acid is 1:8, the mass fraction of calcium phosphate aqueous solution is 3%, and the mass ratio of calcium phosphate to α-naphthaleneacetic acid is 1:15.

[0039] Example 2: A water-retaining and root-promoting composite material based on superabsorbent resin for garden plants, composed of the following parts by weight of raw materials: 100 parts modified superabsorbent resin matrix, 40 parts modified water-retaining functional additive, and 4 parts modified root-promoting active component.

[0040] The modified superabsorbent resin matrix is ​​prepared by treating sodium acrylate with calcium phosphate, ammonium persulfate, N,N'-methylenebisacrylamide, chitosan and polyvinyl alcohol aqueous solution.

[0041] The modified water-retaining functional additive is prepared by treating attapulgite with citric acid, urea and zinc sulfate; the attapulgite is then subjected to thermal activation and acid activation pretreatment to obtain an activated pretreated attapulgite suspension.

[0042] The modified root-promoting active component was prepared by treating α-naphthaleneacetic acid with fulvic acid, phosphoric acid, and calcium phosphate. The α-naphthaleneacetic acid was then subjected to purification and activation treatments, including adsorption and decolorization.

[0043] The modified superabsorbent resin matrix is ​​prepared as follows: Sodium acrylate is dissolved in deionized water to prepare a 25% sodium acrylate aqueous solution. Zinc phosphate is added and stirred until homogeneous. Nitrogen gas is then purged for 25 minutes to remove oxygen. Ammonium persulfate and N,N'-methylenebisacrylamide are added, and the mixture is prepolymerized at 60°C for 45 minutes to obtain product A. Chitosan is added to a 2% acetic acid aqueous solution to prepare a 1.5% chitosan acetic acid solution, which is then added to product A. The mixture is reacted at 70°C for 3 hours to obtain a chitosan crosslinked network interpenetrating modified product. A 10% polyvinyl alcohol aqueous solution is added to the chitosan crosslinked network interpenetrating modified product, and the mixture is stirred at 80°C for 1.5 hours to allow the polyvinyl alcohol molecular chains to form an interpenetrating network structure with the resin network. The mixture is then cooled to room temperature, filtered, washed, dried, and pulverized to obtain the modified superabsorbent resin matrix.

[0044] The mass ratio of calcium phosphate to sodium acrylate is 1:10; the amount of ammonium sulfate added is 0.6% of the mass of sodium acrylate, and the amount of N,N'-methylenebisacrylamide added is 0.1% of the mass of sodium acrylate; the mass ratio of chitosan to sodium acrylate is 1:20; and the mass ratio of polyvinyl alcohol to sodium acrylate is 1:30.

[0045] The preparation method of the activated pretreated attapulgite suspension is as follows: attapulgite ore is crushed through a 150-mesh sieve, placed in a muffle furnace, and calcined at 350℃ for 1.5 hours to remove surface water and structural water, resulting in thermally activated attapulgite. The thermally activated attapulgite is dispersed in a 10% hydrochloric acid solution at a solid-liquid ratio of 1:7.5 g / mL, and acid-activated at 50℃ for 2 hours to allow hydrogen ions to replace the metal cations in the attapulgite crystals, increasing the specific surface area and pore volume. After filtration, washing with water until neutral, and drying, acid-thermal double-activated attapulgite is obtained. The acid-thermal double-activated attapulgite is dispersed in deionized water to prepare a 15% suspension, and ultrasonically dispersed at a frequency of 50 kHz for 30 minutes to fully exfoliate and disperse the activated attapulgite, resulting in the activated pretreated attapulgite suspension.

[0046] The preparation method of the modified water-retaining functional additive is as follows: citric acid is added to the activated pretreated attapulgite suspension, and the mixture is stirred at 60°C for 1.5 h to allow the citric acid to undergo a complexation reaction with calcium and magnesium ions on the surface of the attapulgite. After filtration and washing, citric acid complexed activated modified attapulgite is obtained. The citric acid complexed activated modified attapulgite is dispersed in a urea aqueous solution and stirred at 70°C for 2.5 h to allow urea molecules to insert into the interlayer of the attapulgite for pore expansion treatment. After filtration and washing, urea intercalated pore-expanding modified attapulgite is obtained. The urea intercalated pore-expanding modified attapulgite is dispersed in a zinc sulfate aqueous solution and stirred at 50°C for ion exchange reaction for 1.5 h to allow zinc ions to exchange into the interlayer of the attapulgite or adsorb onto the surface. After filtration, washing, and drying, the modified water-retaining functional additive is obtained.

[0047] The mass ratio of citric acid to attapulgite is 1:12.5; the mass ratio of urea to attapulgite is 1:7.5; and the mass ratio of zinc sulfate to attapulgite is 1:15.

[0048] The purification and activation treatment methods for α-naphthaleneacetic acid are as follows: α-naphthaleneacetic acid raw material is dissolved in anhydrous ethanol to prepare a 15% (w / w) solution. Activated carbon is added, and the mixture is stirred at 50°C for adsorption and decolorization treatment for 45 min. The activated carbon is then removed by filtration to obtain a purified α-naphthaleneacetic acid solution. Sodium hydroxide ethanol solution is added to the purified α-naphthaleneacetic acid solution to adjust the pH to 8.5. The mixture is stirred at 60°C for 45 min to convert α-naphthaleneacetic acid into sodium α-naphthaleneacetate, which has better water solubility, thus obtaining an activated sodium α-naphthaleneacetate solution. The activated sodium α-naphthaleneacetate solution is then concentrated under reduced pressure at a vacuum degree of 0.05 MPa and a temperature of 45°C. Part of the solvent is evaporated to 45% of the original volume to obtain an activated concentrate, thus completing the purification and activation treatment.

[0049] The mass ratio of activated carbon to α-naphthaleneacetic acid is 1:25; the volume ratio of ethanol to water in the sodium hydroxide ethanol solution is 2:1, and the mass fraction of the sodium hydroxide ethanol solution is 8%.

[0050] The preparation method of the modified root-promoting active component is as follows: α-naphthaleneacetic acid (NAA) after purification and activation is dissolved in an ethanol aqueous solution to prepare an 8% (w / w) solution. Fulvic acid is added, and the mixture is stirred and reacted at 50°C for 1.5 h to allow NAA and α-naphthaleneacetic acid to form a molecular complex through hydrogen bonding and hydrophobic interactions, resulting in a NAA-synergistic modified product. Phosphoric acid is added to the NAA-synergistic modified product, and the mixture is stirred and reacted at 60°C for 1.5 h to allow phosphoric acid to undergo a complexation reaction with the hydroxyl groups of NAA, forming a stable phosphate ester complex, resulting in a phosphate ester complex modified product. A calcium phosphate aqueous solution is added to the phosphate ester complex modified product, and the mixture is stirred and reacted at 40°C for 45 min to allow calcium ions to combine with the modified NAA molecules through ionic and coordinate bonds, forming a slow-release complex. The solvent is then removed by vacuum distillation, and the mixture is freeze-dried to obtain the modified root-promoting active component.

[0051] The volume ratio of ethanol to water in the ethanol-water solution is 2:1, the mass ratio of fulvic acid to α-naphthaleneacetic acid is 1:5, the mass ratio of phosphoric acid to α-naphthaleneacetic acid is 1:10, the mass fraction of the calcium phosphate aqueous solution is 4%, and the mass ratio of calcium phosphate to α-naphthaleneacetic acid is 1:20.

[0052] Example 3: A water-retaining and root-promoting composite material based on superabsorbent resin for garden plants, composed of the following parts by weight of raw materials: 100 parts modified superabsorbent resin matrix, 50 parts modified water-retaining functional additive, and 5 parts modified root-promoting active component.

[0053] The modified superabsorbent resin matrix is ​​prepared by treating sodium acrylate with calcium phosphate, ammonium persulfate, N,N'-methylenebisacrylamide, chitosan and polyvinyl alcohol aqueous solution.

[0054] The modified water-retaining functional additive is prepared by treating attapulgite with citric acid, urea and zinc sulfate; the attapulgite is then subjected to thermal activation and acid activation pretreatment to obtain an activated pretreated attapulgite suspension.

[0055] The modified root-promoting active component was prepared by treating α-naphthaleneacetic acid with fulvic acid, phosphoric acid, and calcium phosphate. The α-naphthaleneacetic acid was then subjected to purification and activation treatments, including adsorption and decolorization.

[0056] The modified superabsorbent resin matrix is ​​prepared as follows: Sodium acrylate is dissolved in deionized water to prepare a 30% sodium acrylate aqueous solution. Zinc phosphate is added and stirred until homogeneous. Nitrogen gas is then purged for 30 minutes to remove oxygen. Ammonium persulfate and N,N'-methylenebisacrylamide are added, and the mixture is prepolymerized at 70°C for 60 minutes to obtain product A. Chitosan is added to a 3% acetic acid aqueous solution to prepare a 2% chitosan-acetic acid solution, which is then added to product A. The mixture is reacted at 80°C for 4 hours to obtain a chitosan crosslinked network interpenetrating modified product. A 15% polyvinyl alcohol aqueous solution is added to the chitosan crosslinked network interpenetrating modified product, and the mixture is stirred at 90°C for 2 hours to allow the polyvinyl alcohol molecular chains to form an interpenetrating network structure with the resin network. The mixture is then cooled to room temperature, filtered, washed, dried, and pulverized to obtain the modified superabsorbent resin matrix.

[0057] The mass ratio of calcium phosphate to sodium acrylate is 1:12; the amount of ammonium sulfate added is 0.8% of the mass of sodium acrylate, and the amount of N,N'-methylenebisacrylamide added is 0.15% of the mass of sodium acrylate; the mass ratio of chitosan to sodium acrylate is 1:25; and the mass ratio of polyvinyl alcohol to sodium acrylate is 1:35.

[0058] The preparation method of the activated pretreated attapulgite suspension is as follows: attapulgite ore is crushed through a 200-mesh sieve, placed in a muffle furnace, and calcined at 400℃ for 2 hours to remove surface water and structural water, resulting in thermally activated attapulgite. The thermally activated attapulgite is dispersed in a 15% hydrochloric acid solution at a solid-liquid ratio of 1:10 g / mL, and acid-activated at 60℃ for 3 hours to allow hydrogen ions to replace the metal cations in the attapulgite crystals, increasing the specific surface area and pore volume. After filtration, washing with water until neutral, and drying, acid-thermal double-activated attapulgite is obtained. The acid-thermal double-activated attapulgite is dispersed in deionized water to prepare a 20% suspension, and ultrasonically dispersed at an ultrasonic frequency of 60kHz for 40 minutes to fully exfoliate and disperse the activated attapulgite, resulting in the activated pretreated attapulgite suspension.

[0059] The preparation method of the modified water-retaining functional additive is as follows: citric acid is added to the activated pretreated attapulgite suspension, and the mixture is stirred at 70°C for 2 hours to allow the citric acid to undergo a complexation reaction with calcium and magnesium ions on the surface of the attapulgite. After filtration and washing, citric acid complexed activated modified attapulgite is obtained. The citric acid complexed activated modified attapulgite is dispersed in a urea aqueous solution and stirred at 80°C for 3 hours to allow urea molecules to insert into the interlayer of the attapulgite for pore expansion treatment. After filtration and washing, urea-intercalated pore-expanding modified attapulgite is obtained. The urea-intercalated pore-expanding modified attapulgite is dispersed in a zinc sulfate aqueous solution and stirred at 60°C for ion exchange reaction for 2 hours to allow zinc ions to exchange into the interlayer of the attapulgite or adsorb onto the surface. After filtration, washing, and drying, the modified water-retaining functional additive is obtained.

[0060] The mass ratio of citric acid to attapulgite is 1:15; the mass ratio of urea to attapulgite is 1:10; and the mass ratio of zinc sulfate to attapulgite is 1:18.

[0061] The purification and activation methods for α-naphthaleneacetic acid are as follows: α-naphthaleneacetic acid raw material is dissolved in anhydrous ethanol to prepare a 20% (w / w) solution. Activated carbon is added, and the mixture is stirred at 60°C for 60 min for adsorption and decolorization. The activated carbon is then removed by filtration to obtain a purified α-naphthaleneacetic acid solution. Sodium hydroxide ethanol solution is added to the purified α-naphthaleneacetic acid solution to adjust the pH to 9.0. The mixture is stirred at 70°C for 60 min to convert α-naphthaleneacetic acid into sodium α-naphthaleneacetate, which has better water solubility, thus obtaining an activated sodium α-naphthaleneacetate solution. The activated sodium α-naphthaleneacetate solution is then concentrated under reduced pressure (0.06 MPa, 50°C) to remove some of the solvent to 50% of its original volume, yielding an activated concentrate, thus completing the purification and activation processes.

[0062] The mass ratio of activated carbon to α-naphthaleneacetic acid is 1:30; the volume ratio of ethanol to water in the sodium hydroxide ethanol solution is 3:1, and the mass fraction of the sodium hydroxide ethanol solution is 10%.

[0063] The preparation method of the modified root-promoting active component is as follows: α-naphthaleneacetic acid (NAA) after purification and activation is dissolved in an aqueous ethanol solution to prepare a 10% (w / w) solution. Fulvic acid is added, and the mixture is stirred and reacted at 60°C for 2 hours. This allows fulvic acid and NAA to form a molecular complex through hydrogen bonding and hydrophobic interactions, yielding a fulvic acid synergistic modified product. Phosphoric acid is added to the fulvic acid synergistic modified product, and the mixture is stirred and reacted at 70°C for 2 hours. This allows phosphoric acid to undergo a complexation reaction with the hydroxyl groups of NAA, forming a stable phosphate ester complex, yielding a phosphate ester complex modified product. A calcium phosphate aqueous solution is added to the phosphate ester complex modified product, and the mixture is stirred and reacted at 50°C for 60 minutes. This allows calcium ions to combine with the modified NAA molecules through ionic and coordinate bonds, forming a slow-release complex. The solvent is then removed by vacuum distillation, and the mixture is freeze-dried to obtain the modified root-promoting active component.

[0064] The volume ratio of ethanol to water in the ethanol-water solution is 3:1, the mass ratio of fulvic acid to α-naphthaleneacetic acid is 1:6, the mass ratio of phosphoric acid to α-naphthaleneacetic acid is 1:12, the mass fraction of calcium phosphate aqueous solution is 5%, and the mass ratio of calcium phosphate to α-naphthaleneacetic acid is 1:25.

[0065] Comparative Example 1: The difference between this comparative example and Example 1 is that the modified superabsorbent resin matrix in this comparative example is replaced with untreated sodium acrylate.

[0066] Comparative Example 2 differs from Example 1 in that the modified water-retaining functional additive is replaced with untreated attapulgite.

[0067] Comparative Example 3 differs from Example 1 in that the modified root-promoting active component in this comparative example is replaced with untreated α-naphthaleneacetic acid.

[0068] Performance testing: The relevant properties of the samples of superabsorbent resin-based water-retaining and root-promoting composite materials for garden plants provided in Examples 1 to 3 and Comparative Examples 1 to 3 were tested respectively, and the test data are recorded in Table 1 below: Table 1 - Performance Test Table of Superabsorbent Resin-Based Water-Retaining and Root-Promoting Composite Materials for Garden Plants Testing items <![CDATA[Simulated soil salt solution (Ca 2+ , Mg 2+ coexisting) water absorption capacity (g / g)]]> Water retention rate (%) of composite material in soil after 10 days Water retention rate (%) after 5 cycles of water absorption and release. Example 1 68 69.4 75.8 Example 2 71 72.5 77.9 Example 3 75 74.1 81.1 Comparative Example 1 30 38.6 45.9 Comparative Example 2 52 53.2 62.5 Comparative Example 3 60 60.1 68.1 Among them, the superabsorbent resin-based water-retaining and root-promoting composite materials for garden plants prepared according to the test methods in NY / T886-2022 (Examples 1, 2, 3, Comparative Examples 1, 2, and 3) simulated soil salinity solutions (Ca). 2+ Mg 2+ Water absorption ratio test in coexistence.

[0069] The 10-day water retention rate of the superabsorbent resin-based water-retaining and root-promoting composite material for garden plants prepared according to the test methods in NY / T886-2022 (Examples 1, 2, 3, Comparative Examples 1, 2, and 3) was tested in the soil.

[0070] The water retention rate of the superabsorbent resin-based water-retaining and root-promoting composite materials for garden plants prepared according to the test methods in NY / T886-2022 (Examples 1, 2, 3, Comparative Examples 1, 2, and 3) was tested after repeated water absorption and release five times.

[0071] By comparing and analyzing the relevant data in the table, it can be seen that the superabsorbent resin-based water-retaining and root-promoting composite material for garden plants prepared in this invention simulates soil salinity solution (Ca). 2+ Mg 2+ A high water absorption ratio in (coexistence) indicates that the material has high Ca content. 2+ Mg 2+Even under conditions of coexistence of polyvalent salt ions, the composite material maintains a high osmotic pressure difference and network structure stability, effectively absorbing and retaining moisture. The high 10-day water retention rate in soil indicates a strong ability to slowly release absorbed water and continuously supply it to plant roots in a real soil environment. The high water retention rate after five cycles of water absorption and release indicates that the material maintains a high water retention capacity even after multiple cycles of water absorption, drying, and reabsorption; the three-dimensional network structure is not easily collapsed, and the gel strength decays slowly. Therefore, the superabsorbent resin-based water-retaining and root-promoting composite material for garden plants provided by this invention has a broader market prospect and is more suitable for widespread application.

[0072] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0073] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A superabsorbent resin-based water-retaining and root-promoting composite material for garden plants, characterized in that, It is composed of the following raw materials in parts by weight: 100 parts modified superabsorbent resin matrix, 30-50 parts modified water-retaining functional additive, and 3-5 parts modified root-promoting active component; The modified superabsorbent resin matrix is ​​prepared by treating sodium acrylate with calcium phosphate, ammonium persulfate, N,N'-methylenebisacrylamide, chitosan and polyvinyl alcohol aqueous solution; The modified water-retaining functional additive is prepared by treating attapulgite with citric acid, urea and zinc sulfate; the attapulgite is then subjected to thermal activation and acid activation pretreatment to obtain an activated pretreated attapulgite suspension. The modified root-promoting active component is prepared by treating α-naphthaleneacetic acid with fulvic acid, phosphoric acid, and calcium phosphate; the α-naphthaleneacetic acid is then subjected to purification treatment and activation treatment by adsorption decolorization.

2. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 1, characterized in that, The modified superabsorbent resin matrix is ​​prepared by adding deionized water to sodium acrylate to prepare a sodium acrylate aqueous solution with a mass fraction of 20-30%, adding zinc phosphate and stirring evenly, and then purging with nitrogen to remove oxygen; adding ammonium persulfate and N,N'-methylenebisacrylamide, and prepolymerizing at 50-70℃ to obtain product A; adding chitosan to an acetic acid aqueous solution with a mass fraction of 1-3% to prepare a chitosan acetic acid solution with a mass fraction of 1-2%, and then adding it to product A, and reacting at 60-80℃ to obtain product B; adding a polyvinyl alcohol aqueous solution with a mass fraction of 5-15% to product B, stirring and reacting at 70-90℃, cooling to room temperature, filtering, washing, drying, and pulverizing to obtain the modified superabsorbent resin matrix.

3. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 2, characterized in that: The mass ratio of calcium phosphate to sodium acrylate is 1:8-12; the amount of ammonium sulfate added is 0.4-0.8% of the mass of sodium acrylate, and the amount of N,N'-methylenebisacrylamide added is 0.05-0.15% of the mass of sodium acrylate; the mass ratio of chitosan to sodium acrylate is 1:15-25; and the mass ratio of polyvinyl alcohol to sodium acrylate is 1:25-35.

4. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 1, characterized in that, The preparation method of the activated pretreated attapulgite suspension is as follows: attapulgite ore is crushed and sieved, then calcined at 300-400℃ to obtain thermally activated attapulgite; the thermally activated attapulgite is dispersed in a 5-15% hydrochloric acid solution at a solid-liquid ratio of 1:5-10 g / mL, and after acid activation treatment at 40-60℃, it is filtered, washed with water until neutral, and dried to obtain acid-thermal double-activated attapulgite; the acid-thermal double-activated attapulgite is dispersed in deionized water to prepare a suspension with a mass fraction of 10-20%, and ultrasonically dispersed to obtain the activated pretreated attapulgite suspension.

5. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 1, characterized in that, The preparation method of the modified water-retaining functional additive is as follows: citric acid is added to the activated pretreated attapulgite suspension, and the mixture is stirred and reacted at 50-70℃, then filtered and washed to obtain citric acid complexed activated modified attapulgite. Citric acid complex-activated modified attapulgite is dispersed in a urea aqueous solution with a mass fraction of 5-15%, stirred and reacted at 60-80℃, then filtered and washed to obtain urea intercalation pore-expanding modified attapulgite. Urea-intercalated pore-expanding modified attapulgite is dispersed in a 4-8% zinc sulfate aqueous solution, reacted at 40-60℃, filtered, washed, and dried to obtain a modified water-retaining functional additive.

6. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 6, characterized in that: The mass ratio of citric acid to attapulgite is 1:10-15; the mass ratio of urea to attapulgite is 1:5-10; and the mass ratio of zinc sulfate to attapulgite is 1:12-18.

7. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 1, characterized in that, The purification and activation treatment method of α-naphthaleneacetic acid is as follows: α-naphthaleneacetic acid raw material is dissolved in anhydrous ethanol to prepare a solution with a mass fraction of 10-20%, activated carbon is added, and the solution is stirred, adsorbed and decolorized at 40-60℃ and then filtered to obtain a purified α-naphthaleneacetic acid solution. Add sodium hydroxide ethanol solution to the purified α-naphthaleneacetic acid solution to adjust the pH to 8.0-9.0, and stir the reaction at 50-70℃ to obtain an activated α-naphthaleneacetic acid sodium salt solution; concentrate the activated α-naphthaleneacetic acid sodium salt solution under reduced pressure to remove part of the solvent to 40-50% of the original volume to obtain an activated concentrate, thus completing the purification and activation treatment.

8. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 7, characterized in that: The mass ratio of activated carbon to α-naphthaleneacetic acid is 1:20-30; the volume ratio of ethanol to water in the sodium hydroxide ethanol solution is 1-3:1, and the mass fraction of the sodium hydroxide ethanol solution is 6-10%.

9. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 1, characterized in that, The modified root-promoting active component is prepared by dissolving purified and activated α-naphthaleneacetic acid in an aqueous ethanol solution to prepare a solution with a mass fraction of 6-10%, adding fulvic acid, and stirring and dissolving at 40-60℃ to obtain the fulvic acid synergistic modified product. Phosphoric acid was added to the fulvic acid synergistic modified product, and the mixture was stirred at 50-70℃ to obtain a phosphate ester complex modified product. A calcium phosphate aqueous solution was added to the phosphate ester complex modified product, and the mixture was stirred at 30-50℃. The solvent was removed by vacuum distillation, and the product was freeze-dried to obtain the modified root-promoting active component.

10. The superabsorbent resin-based water-retaining and root-promoting composite material for garden plants according to claim 9, characterized in that: The volume ratio of ethanol to water in the ethanol-water solution is 1-3:1, the mass ratio of fulvic acid to α-naphthaleneacetic acid is 1:4-6, the mass ratio of phosphoric acid to α-naphthaleneacetic acid is 1:8-12, the mass fraction of the calcium phosphate aqueous solution is 3-5%, and the mass ratio of calcium phosphate to α-naphthaleneacetic acid is 1:15-25.