A method for the synergistic control of PM2.5 and ozone through the use of recycled solid waste materials for VOCs degradation.
By preparing composite materials of fly ash, red mud, steel slag, and modified waste lithium-ion battery cathode materials, the problems of single function and low utilization rate of solid waste resources in VOCs treatment were solved. This achieved complete mineralization of VOCs, efficient interception of PM2.5, and catalytic decomposition of ozone, thus improving the synergistic control effect of multiple pollutants.
Patent Information
- Application Number
- CN202611611820.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing VOCs treatment technologies are limited in function, lack the ability to synergistically control PM2.5 and ozone, and have low solid waste resource utilization rates, high costs, and difficulties in industrialization and promotion.
Using fly ash, red mud, steel slag, and modified waste lithium-ion battery cathode materials as raw materials, a multifunctional composite material was prepared through pretreatment, alkaline fusion activation, acid etching pore formation, and transition metal doping. This composite material can achieve VOCs adsorption and enrichment, catalytic oxidation degradation, PM2.5 filtration and interception, and ozone catalytic decomposition.
It achieves complete mineralization of VOCs, efficient interception of PM2.5, and catalytic decomposition of ozone, improving the synergistic control of multiple pollutants, reducing costs, and increasing the resource utilization rate of solid waste.
Smart Images

Figure CN123102089A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the intersection of air pollution control technology and solid waste resource utilization, and in particular to a method for using recycled solid waste materials to synergistically control PM2.5 and ozone through VOCs degradation. Background Technology
[0002] Volatile organic compounds (VOCs) are a significant class of gaseous pollutants in the atmospheric environment, originating from a wide range of industries including petrochemicals, coating and printing, pharmaceutical manufacturing, waste incineration, and vehicle exhaust. VOCs readily undergo photochemical reactions under ultraviolet radiation from sunlight, making them a major contributor to complex air pollution, including increased PM2.5 and near-surface ozone concentrations, posing a significant threat to the ecological environment and human health. Studies have shown that VOCs are not only a major component of photochemical smog but also a crucial precursor to PM2.5, and under sunlight conditions, they can react with nitrogen oxides to generate secondary pollutants such as ozone. Therefore, VOC emission reduction and control are key breakthroughs for achieving synergistic governance of PM2.5 and ozone.
[0003] Currently, mainstream VOCs treatment technologies include adsorption, catalytic combustion, photocatalytic oxidation, low-temperature plasma, and biodegradation. Among these, adsorption is widely used due to its high efficiency, adaptability, and recyclability. Catalytic combustion catalysts primarily use noble metals such as platinum, palladium, and ruthenium as active components, loading these components onto high specific surface area supports. However, existing technologies still have the following problems:
[0004] First, it has limited functionality and lacks collaborative governance capabilities.
[0005] Second, the resource utilization rate of solid waste is low.
[0006] Third, there is insufficient attention paid to the synergistic control of ozone.
[0007] CN105642333B discloses a multifunctional environmental purification composite material, which is a catalyst comprising a molecular sieve support, TiO2, and a small amount of transition metal oxides, wherein the TiO2 and transition metal oxides are supported on the molecular sieve support. This invention also discloses a method for preparing the aforementioned multifunctional environmental purification composite material. The prepared catalyst exhibits characteristics such as high specific surface area, high catalytic oxidation activity, highly dispersed active components, and stable and efficient purification. Furthermore, this invention discloses the application of the aforementioned multifunctional environmental purification composite material in the synergistic purification of pollutants through photocatalytic oxidation and ozone catalytic oxidation. The multifunctional composite material not only absorbs ultraviolet light to generate good photocatalytic oxidation activity but also efficiently decomposes ozone and utilizes ozone decomposition to generate highly active oxygen to oxidize pollutants, achieving synergistic purification of pollutants through photocatalytic oxidation and ozone catalytic oxidation, resulting in thorough degradation and high purification efficiency. However, the prepared material is costly, employing an organic titanium source and the sol-gel method, which involves complex processes, high-temperature calcination energy consumption, and high consumption of auxiliary reagents, posing significant obstacles to industrialization. Summary of the Invention
[0008] To address the shortcomings of the existing technologies, this invention provides a method for using solid waste recycling materials to synergistically control PM2.5 and ozone through VOCs degradation. This method prepares a composite functional material that combines VOCs adsorption and enrichment, catalytic oxidation degradation, PM2.5 filtration and interception, and ozone catalytic decomposition, achieving the technical goal of "treating waste with waste and synergistic control of multiple pollutants".
[0009] This invention provides a method for using recycled solid waste materials to synergistically control PM2.5 and ozone through VOCs degradation, comprising the following steps:
[0010] S1. Pretreatment of solid waste recycling materials: Fly ash is calcined at 550-650℃ for 2-4 hours and then ball-milled to 200-400 mesh to obtain pretreated fly ash; red mud is dried at 105-120℃ for 12-24 hours and then pulverized through a 100-200 mesh sieve to obtain pretreated red mud; steel slag is ball-milled to 200-400 mesh and then dried at 105-120℃ for 12-24 hours to obtain pretreated steel slag; waste lithium-ion battery cathode material powder is mixed with recycled iron oxide and alumina in a certain proportion, and then processed using waste lithium-ion battery cathode material powder. The modified waste lithium-ion battery cathode material powder is obtained by mechanical and chemical activation with 0.5 times its mass of sodium hydroxide for 2-4 hours and calcined at 600-800℃ for 4-8 hours. The molar ratio of Co, Ni, Mn, Fe and Al in the modified waste lithium-ion battery cathode material powder is (0.2-0.4):(0.2-0.4):(0.2-0.4):(0.05-0.2):(0.05-0.2). The modified waste lithium-ion battery cathode material powder provides abundant acidic and alkaline sites that can adsorb organic substances such as alcohols, aldehydes, esters and hydrocarbons.
[0011] S2. Alkali fusion activation treatment: The pretreated fly ash obtained in step S1 is mixed with sodium hydroxide at a mass ratio of 1:0.8, activated at 500~700℃ for 1~3 hours, cooled and pulverized, then added to deionized water for leaching, filtered to obtain a silicon-aluminum rich leachate, the pH is adjusted to 10~11 and then hydrothermally crystallized at 70~90℃ for 6~24 hours, and after separation, washing and drying, modified fly ash is obtained;
[0012] S3. Composite carrier molding: The modified fly ash obtained in S2 is mixed with the pretreated red mud, pretreated steel slag and modified waste lithium-ion battery cathode material powder obtained in S1 at a mass ratio of (5~8):(1~3):(1~2):(1~2), a pore-forming agent and water are added, and the mixture is extruded into a green body. After drying, a composite carrier green body is obtained.
[0013] S4. Acid etching to create pores: Immerse the composite carrier preform obtained in S3 in 0.5~2.0 mol / L nitric acid solution, acid etch at 40~80℃ for 0~1 hours, wash until neutral and dry to obtain acid-etched composite carrier;
[0014] S5. Transition Metal Doping Loading: The acid-etched composite support obtained in S4 was impregnated in a mixed solution containing manganese nitrate, cerium nitrate, and cobalt nitrate, with a molar ratio of (3~6):(2~4):(1~2), and a total metal ion concentration of 0.1~0.5 mol / L. After impregnation for 6~24 hours, it was dried to obtain the metal-loaded precursor. In the Mn-Ce-Co ternary system, Mn provides the main catalytic activity, Ce provides oxygen storage and dispersion functions, and Co provides ozone decomposition specific activity and selective regulation functions. The composite oxide formed by the three can partially form a Mn-Ce-Co solid solution during calcination. The strong interaction between different metal ions significantly increases the oxygen vacancy concentration of the catalyst.
[0015] S6. High-temperature calcination molding: The metal-loaded precursor obtained in S5 is heated to 400-600℃ in air at a rate of 2-5℃ / min and calcined for 2-6 hours to obtain a solid waste recycling material-based composite functional material.
[0016] S7. Application: The solid waste recycling material-based composite functional material obtained in S6 is filled into a reactor, and the VOCs-containing waste gas is discharged at a space velocity of 1000~10000 h⁻¹. - ¹VOCs are adsorbed and catalytically oxidized and degraded through the material bed at a temperature of 20~200℃. At the same time, the material intercepts and filters PM2.5 in the exhaust gas and catalytically decomposes ozone.
[0017] Furthermore, the chemical composition of the fly ash, converted to oxides by mass percentage, is: SiO2 45~60%, Al2O3 20~35%, Fe2O3 3~8%, CaO 1~5%, MgO 0.5~2%. The role of fly ash in this invention is threefold: First, as a source of silica and alumina for zeolite molecular sieves. Through alkali fusion activation treatment, the inert aluminosilicate mineral phase in the fly ash is destroyed by NaOH, transforming into soluble silicates and aluminates. After hydrothermal crystallization, these are reconstructed into Na-X type zeolites with a regular microporous structure, providing sufficient active sites for VOCs adsorption. Second, as a structural framework for composite carriers. Fly ash-based zeolites possess excellent thermal and hydrothermal stability, providing structural support for red mud and steel slag, preventing structural collapse of the composite material during high-temperature calcination and use. Third, synergistically enhancing mass transfer efficiency. The microporous structure of zeolite, together with the mesopores and macropores introduced by subsequent acid etching, forms a multi-level pore system, which is conducive to the rapid diffusion of VOCs molecules and the timely desorption of product gases, thus avoiding the decrease in activity caused by pore blockage.
[0018] Further, the chemical composition of the red mud, converted to oxides by mass percentage, is: Fe2O3 30~50%, Al2O3 15~25%, SiO2 5~15%, CaO 1~5%, Na2O 5~10%, and loss on ignition ≤10%. The functions of the red mud are: First, to provide catalytic ozonation active components. The iron oxides in the red mud can catalyze the decomposition of ozone to generate highly active hydroxyl radicals and superoxide radicals, oxidizing and degrading VOCs molecules adsorbed on the material surface into CO2 and H2O. Second, to synergize with Mn-Ce-Co active components. The Fe in the red mud... 3+ / Fe 2+ Redox pairs form multi-metal oxide solid solutions with added Mn, Ce, and Co transition metal ions. The electron transfer effect between different metal ions can significantly increase the oxygen vacancy concentration and lattice oxygen mobility of the catalyst, enhancing its low-temperature catalytic activity. Third, they contribute alkaline sites to promote ozone decomposition. The alkaline substances remaining in red mud can provide an alkaline microenvironment for ozone decomposition, accelerating the conversion of ozone into reactive oxygen species.
[0019] Furthermore, the chemical composition of the steel slag, converted to oxides by mass percentage, is as follows: CaO 35-50%, FeO 15-25%, SiO2 10-20%, MgO 5-10%, MnO 1-3%, P2O5 1-3%. The functions of the steel slag are: First, to enhance the mechanical strength of the composite material. The high density and high hardness of the steel slag make it an ideal reinforcing phase for the composite material, significantly improving the crushing strength and wear resistance of the molded material particles and extending the service life of the material. Second, to provide auxiliary catalytic components beyond Mn-Ce-Co. The transition metal oxides such as FeO and MnO in the steel slag themselves possess certain catalytic oxidation activity, forming a multi-component catalytic system with the added Mn, Ce, and Co active components, broadening the catalyst's adaptability to VOCs components. Third, to adjust the surface acidity and alkalinity of the composite material. The abundant CaO in steel slag provides alkaline surface sites, which is beneficial for the chemical adsorption of acidic groups (such as carboxyl and phenolic hydroxyl groups) in VOCs molecules, thus enhancing the material's ability to capture oxygen-containing VOCs. Fourth, it synergistically promotes the filtration and interception of PM2.5. The irregular morphology and rough surface of steel slag particles help to form tortuous flow channels in the material bed, enhancing the inertial collision and interception effect on submicron particles.
[0020] Furthermore, in step S2, the hydrothermal crystallization temperature is 80℃, the crystallization time is 12 hours, and the resulting modified fly ash has a specific surface area of 400~600 m² / g and a pore volume of 0.25~0.40 cm³ / g.
[0021] Furthermore, in step S3, the mass ratio of modified fly ash, pretreated red mud, pretreated steel slag, and modified waste lithium-ion battery cathode material powder is 6:2:2:2.
[0022] Furthermore, in step S3, the pore-forming agent is sodium carboxymethyl cellulose, and the amount added is 3-5% of the mass of the modified fly ash.
[0023] Furthermore, in step S5, the molar ratio of Mn, Ce, and Co is 4:3:1.5, the total metal ion concentration is 0.3 mol / L, and the immersion time is 12 hours.
[0024] Further, in step S6, the calcination temperature is 500℃, the heating rate is 3℃ / min, and the holding time is 4 hours; in step S7, the exhaust gas treatment temperature is 80~150℃, and the space velocity is 3000~6000 h⁻¹. - ¹.
[0025] Furthermore, the molding method in step S3 employs a three-layer composite carrier molding process. This process utilizes a three-layer co-extrusion technology, using modified fly ash as the outer layer, modified waste lithium-ion battery cathode material powder as the middle layer, and pretreated red mud and pretreated steel slag as the inner layers. The mixture is extruded into a three-layer structure green body. The modified fly ash, pretreated red mud, pretreated steel slag, and modified waste lithium-ion battery cathode material powder obtained in S1 are mixed in a mass ratio of 6:2:2:2, with the pore-forming agent evenly distributed throughout the three layers. During the green body extrusion process, three layers of mud with different compositions are sequentially fed in. After drying and calcination, a layered structure with distinct interface partitions is formed. Each layer is independently optimized, allowing for independent optimization of its composition and structure, unaffected by the functions of other layers. This synergistic design aims to improve the material's utilization efficiency.
[0026] The present invention has the following significant advantages:
[0027] The mechanism by which this invention achieves VOCs degradation and synergistic control of PM2.5 and ozone can be summarized as a four-fold function of "adsorption enrichment - catalytic oxidation - physical filtration - catalytic decomposition": The microporous structure has a selective adsorption capacity for VOCs molecules, enriching low-concentration VOCs in the gas phase on the material surface and inside the pores, increasing the local concentration and creating favorable conditions for catalytic oxidation reactions; The adsorbed and enriched VOCs molecules are deeply oxidized to CO2 and H2O by active oxygen at the active sites of Mn-Ce-Co composite oxides, achieving complete mineralization of VOCs and avoiding secondary pollution; The multi-level pore structure of the composite material and the tortuous channels formed by irregular particle accumulation achieve multiple filtration mechanisms such as inertial collision, direct interception and diffusion deposition for fine particulate matter of 0.1~2.5μm in the exhaust gas, effectively reducing PM2.5 emissions; The ozone generated in the exhaust gas is catalytically decomposed into O2 at the active sites of red mud iron oxides and Co3O4. This process not only eliminates the toxicity of ozone itself, but also generates reactive oxygen species for the oxidative degradation of VOCs, realizing the innovative idea of "treating VOCs with ozone". Attached Figure Description
[0028] Figure 1 The image shows the SEM image of the composite carrier preform in step S3 of Example 1.
[0029] Figure 2 The image shows the SEM image of the acid-etched composite carrier in step S4 of Example 1.
[0030] Figure 3 The image shows the SEM image of the metal-loaded precursor in step S5 of Example 1.
[0031] Figure 4 The image shows the SEM image of the solid waste recycling material-based composite functional material in step S6 of Example 1. Detailed Implementation
[0032] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0033] Example 1
[0034] A method for using recycled solid waste materials to synergistically control PM2.5 and ozone through VOCs degradation includes the following steps:
[0035] S1. Pretreatment of solid waste recycling materials: Fly ash is calcined at 585℃ for 3 hours and then ball-milled to 250-300 mesh to obtain pretreated fly ash; red mud is dried at 110℃ for 20 hours and then pulverized through a 150-mesh sieve to obtain pretreated red mud; steel slag is ball-milled to 300-350 mesh and then dried at 110℃ for 16 hours to obtain pretreated steel slag; waste lithium-ion battery cathode material powder is mixed with recycled iron oxide and aluminum oxide in a certain proportion, and then mechanically activated with sodium hydroxide at 0.5 times the mass of the waste lithium-ion battery cathode material powder for 3 hours, and then calcined at 700℃ for 6 hours to obtain modified waste lithium-ion battery cathode material powder. The molar ratio of Co, Ni, Mn, Fe, and Al in the modified waste lithium-ion battery cathode material powder is 0.3:0.3:0.3:0.1:0.15.
[0036] S2. Alkali fusion activation treatment: The pretreated fly ash obtained in step S1 is mixed with sodium hydroxide at a mass ratio of 1:0.8, activated at 650℃ for 2 hours, cooled and pulverized, then added to deionized water for leaching, filtered to obtain a silicon-aluminum rich leachate, the pH is adjusted to 10~11 and then hydrothermally crystallized at 80℃ for 12 hours, and after separation, washing and drying, modified fly ash is obtained. The specific surface area of the obtained modified fly ash is 500 m² / g and the pore volume is 0.32 cm³ / g.
[0037] S3. Composite carrier molding: The modified fly ash obtained in S2 is mixed with the pretreated red mud, pretreated steel slag and modified waste lithium-ion battery cathode material powder obtained in S1 at a mass ratio of 6:2:2:2. A pore-forming agent and water are added, and the mixture is extruded into a green body. After drying, a composite carrier green body is obtained. The pore-forming agent is sodium carboxymethyl cellulose, and the amount added is 4% of the mass of the modified fly ash.
[0038] S4. Acid etching to create pores: The composite carrier preform obtained in S3 was immersed in a 1 mol / L nitric acid solution and acid etched at 60℃ for 0.3 hours. After washing until neutral, it was dried to obtain the acid-etched composite carrier.
[0039] S5. Transition metal doping loading: The acid-etched composite support obtained in S4 was immersed in a mixed solution containing manganese nitrate, cerium nitrate and cobalt nitrate in a molar ratio of 4:3:1.5 and a total metal ion concentration of 0.3 mol / L. After immersion for 12 hours, it was dried to obtain the metal-loaded precursor.
[0040] S6. High-temperature calcination molding: The metal-loaded precursor obtained in S5 is heated to 500°C at 3°C / min in air atmosphere and calcined for 4 hours to obtain solid waste recycling material-based composite functional material.
[0041] S7. Application: The solid waste recycling material-based composite functional material obtained in S6 is filled into a reactor, and the VOCs-containing waste gas is discharged at a space velocity of 5000 h⁻¹. - ¹VOCs are adsorbed and catalytically oxidized and degraded through the material bed at a temperature of 100℃. At the same time, the material intercepts and filters PM2.5 in the exhaust gas and catalytically decomposes ozone.
[0042] The chemical composition of the fly ash, converted to oxides by mass percentage, is: SiO2 58%, Al2O3 32%, Fe2O3 6%, CaO 3%, MgO 1%.
[0043] The chemical composition of the red mud, converted to oxides by mass percentage, is as follows: Fe2O3 48%, Al2O3 27%, SiO2 12%, CaO 4%, Na2O 9%, and loss on ignition 6%.
[0044] The chemical composition of the steel slag, converted to oxides by mass percentage, is as follows: CaO 48%, FeO 22%, SiO2 18%, MgO 8%, MnO 2%, P2O5 2%.
[0045] Example 2
[0046] A method for using recycled solid waste materials to synergistically control PM2.5 and ozone through VOCs degradation includes the following steps:
[0047] S1. Pretreatment of solid waste recycling materials: Fly ash is calcined at 585℃ for 3 hours and then ball-milled to 250-300 mesh to obtain pretreated fly ash; red mud is dried at 110℃ for 20 hours and then pulverized through a 150-mesh sieve to obtain pretreated red mud; steel slag is ball-milled to 300-350 mesh and then dried at 110℃ for 16 hours to obtain pretreated steel slag; waste lithium-ion battery cathode material powder is mixed with recycled iron oxide and aluminum oxide in a certain proportion, and then mechanically activated with sodium hydroxide at 0.5 times the mass of the waste lithium-ion battery cathode material powder for 3 hours, and then calcined at 700℃ for 6 hours to obtain modified waste lithium-ion battery cathode material powder. The molar ratio of Co, Ni, Mn, Fe, and Al in the modified waste lithium-ion battery cathode material powder is 0.3:0.3:0.3:0.1:0.15.
[0048] S2. Alkali fusion activation treatment: The pretreated fly ash obtained in step S1 is mixed with sodium hydroxide at a mass ratio of 1:0.8, activated at 650℃ for 2 hours, cooled and pulverized, then added to deionized water for leaching, filtered to obtain a silicon-aluminum rich leachate, the pH is adjusted to 10~11 and then hydrothermally crystallized at 80℃ for 12 hours, and after separation, washing and drying, modified fly ash is obtained. The specific surface area of the obtained modified fly ash is 500 m² / g and the pore volume is 0.32 cm³ / g.
[0049] S3. Composite Carrier Molding: A three-layer composite carrier molding process is adopted, which uses a three-layer co-extrusion technology: modified fly ash is used as the outer layer, modified waste lithium-ion battery cathode material powder is used as the middle layer, and pretreated red mud and pretreated steel slag are used as the inner layer. The mixture is extruded into a three-layer structure blank. The modified fly ash, the pretreated red mud, the pretreated steel slag obtained in S1, and the modified waste lithium-ion battery cathode material powder are mixed in a mass ratio of 6:2:2:2. The pore-forming agent is evenly distributed into the three-layer structure. The pore-forming agent is sodium carboxymethyl cellulose, and the amount added is 4% of the mass of the modified fly ash.
[0050] S4. Acid etching to create pores: The composite carrier preform obtained in S3 was immersed in a 1 mol / L nitric acid solution and acid etched at 60℃ for 0.3 hours. After washing until neutral, it was dried to obtain the acid-etched composite carrier.
[0051] S5. Transition metal doping loading: The acid-etched composite support obtained in S4 was immersed in a mixed solution containing manganese nitrate, cerium nitrate and cobalt nitrate in a molar ratio of 4:3:1.5 and a total metal ion concentration of 0.3 mol / L. After immersion for 12 hours, it was dried to obtain the metal-loaded precursor.
[0052] S6. High-temperature calcination molding: The metal-loaded precursor obtained in S5 is heated to 500°C at 3°C / min in air atmosphere and calcined for 4 hours to obtain solid waste recycling material-based composite functional material.
[0053] S7. Application: The solid waste recycling material-based composite functional material obtained in S6 is filled into a reactor, and the VOCs-containing waste gas is discharged at a space velocity of 5000 h⁻¹. - ¹VOCs are adsorbed and catalytically oxidized and degraded through the material bed at a temperature of 100℃. At the same time, the material intercepts and filters PM2.5 in the exhaust gas and catalytically decomposes ozone.
[0054] The chemical composition of the fly ash, converted to oxides by mass percentage, is: SiO2 58%, Al2O3 32%, Fe2O3 6%, CaO 3%, MgO 1%.
[0055] The chemical composition of the red mud, converted to oxides by mass percentage, is as follows: Fe2O3 48%, Al2O3 27%, SiO2 12%, CaO 4%, Na2O 9%, and loss on ignition 6%.
[0056] The chemical composition of the steel slag, converted to oxides by mass percentage, is as follows: CaO 48%, FeO 22%, SiO2 18%, MgO 8%, MnO 2%, P2O5 2%.
[0057] Example 3
[0058] A method for using recycled solid waste materials to synergistically control PM2.5 and ozone through VOCs degradation includes the following steps:
[0059] S1. Pretreatment of solid waste recycling materials: Fly ash is calcined at 585℃ for 3 hours and then ball-milled to 250-300 mesh to obtain pretreated fly ash; red mud is dried at 110℃ for 20 hours and then pulverized through a 150-mesh sieve to obtain pretreated red mud; steel slag is ball-milled to 300-350 mesh and then dried at 110℃ for 16 hours to obtain pretreated steel slag; waste lithium-ion battery cathode material powder is mixed with recycled iron oxide and aluminum oxide in a certain proportion, and then mechanically activated with sodium hydroxide at 0.5 times the mass of the waste lithium-ion battery cathode material powder for 3 hours, and then calcined at 700℃ for 6 hours to obtain modified waste lithium-ion battery cathode material powder. The molar ratio of Co, Ni, Mn, Fe, and Al in the modified waste lithium-ion battery cathode material powder is 0.3:0.3:0.3:0.1:0.15.
[0060] S2. Alkali fusion activation treatment: The pretreated fly ash obtained in step S1 is mixed with sodium hydroxide at a mass ratio of 1:0.8, activated at 650℃ for 2 hours, cooled and pulverized, then added to deionized water for leaching, filtered to obtain a silicon-aluminum rich leachate, the pH is adjusted to 10~11 and then hydrothermally crystallized at 80℃ for 12 hours, and after separation, washing and drying, modified fly ash is obtained. The specific surface area of the obtained modified fly ash is 500 m² / g and the pore volume is 0.32 cm³ / g.
[0061] S3. Composite carrier molding: The modified fly ash obtained in S2 is mixed with the pretreated red mud, pretreated steel slag and modified waste lithium-ion battery cathode material powder obtained in S1 at a mass ratio of 6:2:2:2. A pore-forming agent and water are added, and the mixture is extruded into a green body. After drying, a composite carrier green body is obtained. The pore-forming agent is sodium carboxymethyl cellulose, and the amount added is 4% of the mass of the modified fly ash.
[0062] S4. Acid etching to create pores: The composite carrier preform obtained in S3 was immersed in a 1 mol / L nitric acid solution and acid etched at 60℃ for 0.3 hours. After washing until neutral, it was dried to obtain the acid-etched composite carrier.
[0063] S5. Transition metal doping loading: The acid-etched composite support obtained in S4 was immersed in a mixed solution containing manganese nitrate, cerium nitrate and cobalt nitrate in a molar ratio of 4:3:1.5 and a total metal ion concentration of 0.3 mol / L. After immersion for 12 hours, it was dried to obtain the metal-loaded precursor.
[0064] S6. High-temperature calcination molding: The metal-loaded precursor obtained in S5 is heated to 500°C at 3°C / min in air atmosphere and calcined for 4 hours to obtain solid waste recycling material-based composite functional material.
[0065] S7. Application: The solid waste recycling material-based composite functional material obtained in S6 is filled into a reactor, and the VOCs-containing waste gas is discharged at a space velocity of 5000 h⁻¹. - ¹VOCs are adsorbed and catalytically oxidized and degraded through the material bed at a temperature of 100℃. At the same time, the material intercepts and filters PM2.5 in the exhaust gas and catalytically decomposes ozone.
[0066] The chemical composition of the fly ash, converted to oxides by mass percentage, is: SiO2 58%, Al2O3 32%, Fe2O3 6%, CaO 3%, MgO 1%.
[0067] The chemical composition of the red mud, converted to oxides by mass percentage, is as follows: Fe2O3 48%, Al2O3 27%, SiO2 12%, CaO 4%, Na2O 9%, and loss on ignition 6%.
[0068] The chemical composition of the steel slag, converted to oxides by mass percentage, is as follows: CaO 48%, FeO 22%, SiO2 18%, MgO 8%, MnO 2%, P2O5 2%.
[0069] Comparative Example 1
[0070] The modified waste lithium-ion battery cathode material powder component in Example 1 was removed, and corresponding modifications were made in subsequent steps. Other aspects are the same as in Example 1, and will not be repeated here.
[0071] Comparative Example 2
[0072] The red mud component in Example 1 was removed, and corresponding modifications were made in subsequent steps. The rest is the same as in Example 1, and will not be repeated here.
[0073] The solid waste recycling material-based composite functional materials prepared in the above embodiments and comparative examples were applied, and the results are shown in Table 1.
[0074] The test method was as follows: Composite functional materials were packed into a fixed-bed reactor (bed height 50 cm, inner diameter 5 cm), and simulated exhaust gas containing toluene (initial concentration 500 ppm), ozone (initial concentration 50 ppm), and PM2.5 (initial concentration 200 μg / m³) was introduced at a space velocity of 5000 h⁻¹. - ¹Passing through the bed, the reaction temperature is 100℃ and the relative humidity is 50%.
[0075] (1) VOCs degradation rate: The concentration of toluene at the inlet and outlet of the reactor was detected online by gas chromatography, and the degradation rate was calculated.
[0076] (2) Ozone decomposition rate: The ozone concentration at the inlet and outlet was detected by an ozone analyzer using ultraviolet absorption method, and the decomposition rate was calculated.
[0077] (3) PM2.5 interception rate: The mass concentration of PM2.5 at the inlet and outlet was detected by an aerosol particle size analyzer, and the interception rate was calculated.
[0078] (4) Crushing resistance: The crushing resistance of a single particle was measured using a particle strength tester.
[0079] Table 1 Test Project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Toluene degradation rate (%) 92.6 94.1 93.0 88.2 86.4 Ozone decomposition rate (%) 97.6 98.2 97.2 96.9 95.2 PM2.5 interception rate (%) 91.0 91.3 90.8 86.4 89.3 Crushing strength (N / piece) 38.5 40.1 38.4 38.4 39.1
[0080] Table 1 shows that the products prepared in Examples 1-3 exhibit good application effects, with a toluene degradation rate >92.5%, an ozone decomposition rate >97.1%, a PM2.5 interception rate >90.8%, and a crushing strength >38.3 N / particle. A comparison of the data from Examples 1 and 2 indicates that the product prepared using a three-layer composite carrier exhibits superior performance. Comparative Example 1 shows that modified waste lithium-ion battery cathode material powder can improve the toluene degradation rate and PM2.5 interception rate, while Comparative Example 2 shows that red mud can significantly improve the toluene degradation rate, PM2.5 interception rate, and ozone decomposition rate.
Claims
1. A method for using solid waste recycling materials to synergistically control PM2.5 and ozone through VOCs degradation, characterized in that, Includes the following steps: S1. Pretreatment of solid waste recycling materials: Fly ash is calcined at 550-650℃ for 2-4 hours and then ball-milled to 200-400 mesh to obtain pretreated fly ash; red mud is dried at 105-120℃ for 12-24 hours and then pulverized through a 100-200 mesh sieve to obtain pretreated red mud; steel slag is ball-milled to 200-400 mesh and then dried at 105-120℃ for 12-24 hours to obtain pretreated steel slag; waste lithium-ion battery cathode material powder is mixed with recycled iron oxide and alumina according to... After mixing in the specified proportions, the mixture is mechanically activated for 2-4 hours using sodium hydroxide at 0.5 times the mass of the waste lithium-ion battery cathode material powder, and then calcined at 600-800℃ for 4-8 hours to obtain modified waste lithium-ion battery cathode material powder. The molar ratio of Co, Ni, Mn, Fe, and Al in the modified waste lithium-ion battery cathode material powder is (0.2-0.4):(0.2-0.4):(0.2-0.4):(0.05-0.2):(0.05-0.2). S2. Alkali fusion activation treatment: The pretreated fly ash obtained in step S1 is mixed with sodium hydroxide at a mass ratio of 1:0.8, activated at 500~700℃ for 1~3 hours, cooled and pulverized, then added to deionized water for leaching, filtered to obtain a silicon-aluminum rich leachate, the pH is adjusted to 10~11 and then hydrothermally crystallized at 70~90℃ for 6~24 hours, and after separation, washing and drying, modified fly ash is obtained; S3. Composite carrier molding: The modified fly ash obtained in S2 is mixed with the pretreated red mud, pretreated steel slag and modified waste lithium-ion battery cathode material powder obtained in S1 at a mass ratio of (5~8):(1~3):(1~2):(1~2), a pore-forming agent and water are added, and the mixture is extruded into a green body. After drying, a composite carrier green body is obtained. S4. Acid etching to create pores: Immerse the composite carrier preform obtained in S3 in 0.5~2.0 mol / L nitric acid solution, acid etch at 40~80℃ for 0~1 hours, wash until neutral and dry to obtain acid-etched composite carrier; S5. Transition metal doping loading: The acid-etched composite support obtained in S4 is immersed in a mixed solution containing manganese nitrate, cerium nitrate and cobalt nitrate, with a molar ratio of (3~6):(2~4):(1~2), and a total metal ion concentration of 0.1~0.5 mol / L. After immersion for 6~24 hours, it is dried to obtain the metal-loaded precursor. S6. High-temperature calcination molding: The metal-loaded precursor obtained in S5 is heated to 400-600℃ in air at a rate of 2-5℃ / min and calcined for 2-6 hours to obtain a solid waste recycling material-based composite functional material. S7. Application: The solid waste recycling material-based composite functional material obtained in S6 is filled into a reactor, and the VOCs-containing waste gas is discharged at a space velocity of 1000~10000 h⁻¹. - ¹VOCs are adsorbed and catalytically oxidized and degraded through the material bed at a temperature of 20~200℃. At the same time, the material intercepts and filters PM2.5 in the exhaust gas and catalytically decomposes ozone.
2. The method for using solid waste recycling materials according to claim 1 for VOCs degradation and synergistic control of PM2.5 and ozone, characterized in that, The chemical composition of the fly ash, expressed as a percentage of oxides by mass, is as follows: SiO2 45~60%, Al2O3 20~35%, Fe2O3 3~8%, CaO 1~5%, MgO 0.5~2%.
3. The method for using solid waste recycling materials according to claim 1 for the synergistic control of PM2.5 and ozone through VOCs degradation, characterized in that, The chemical composition of the red mud, converted to oxides by mass percentage, is as follows: Fe2O3 30~50%, Al2O3 15~25%, SiO2 5~15%, CaO 1~5%, Na2O 5~10%, and loss on ignition ≤10%.
4. The method for using solid waste recycling materials according to claim 1 for the synergistic control of PM2.5 and ozone through VOCs degradation, characterized in that, The chemical composition of the steel slag, converted to oxides by mass percentage, is as follows: CaO 35~50%, FeO 15~25%, SiO2 10~20%, MgO 5~10%, MnO 1~3%, P2O5 1~3%.
5. The method for using solid waste recycling materials according to claim 1 for VOCs degradation and synergistic control of PM2.5 and ozone, characterized in that, In step S2, the hydrothermal crystallization temperature is 80℃, the crystallization time is 12 hours, and the resulting modified fly ash has a specific surface area of 400~600 m² / g and a pore volume of 0.25~0.40 cm³ / g.
6. The method for using solid waste recycling materials according to claim 1 for the synergistic control of PM2.5 and ozone through VOCs degradation, characterized in that, In step S3, the mass ratio of modified fly ash, pretreated red mud, pretreated steel slag, and modified waste lithium-ion battery cathode material powder is 6:2:2:
2.
7. The method for using solid waste recycling materials according to claim 1 for VOCs degradation and synergistic control of PM2.5 and ozone, characterized in that, In S3, the pore-forming agent is sodium carboxymethyl cellulose, and the amount added is 3-5% of the mass of the modified fly ash.
8. The method for using solid waste recycling materials according to claim 1 for VOCs degradation and synergistic control of PM2.5 and ozone, characterized in that, In step S5, the molar ratio of Mn, Ce, and Co is 4:3:1.5, the total metal ion concentration is 0.3 mol / L, and the immersion time is 12 hours.
9. The method for using solid waste recycling materials according to claim 1 for VOCs degradation and synergistic control of PM2.5 and ozone, characterized in that, In step S6, the calcination temperature is 500℃, the heating rate is 3℃ / min, and the holding time is 4 hours; in step S7, the waste gas treatment temperature is 80~150℃, and the space velocity is 3000~6000 h⁻¹. - ¹.
10. The method for using solid waste recycling materials according to claim 1 for VOCs degradation and synergistic control of PM2.5 and ozone, characterized in that, The molding method in step S3 adopts a three-layer composite carrier molding process. The process involves using a three-layer co-extrusion technology, with modified fly ash as the outer layer, modified waste lithium-ion battery cathode material powder as the middle layer, and pretreated red mud and pretreated steel slag as the inner layer. The mixture is extruded into a three-layer structure blank. The modified fly ash, pretreated red mud, pretreated steel slag, and modified waste lithium-ion battery cathode material powder obtained in S1 are mixed in a mass ratio of 6:2:2:2, and the pore-forming agent is evenly distributed into the three-layer structure.
Citation Information
Patent Citations
A multifunctional environmental purification composite material, its preparation method and application
CN105642333B