Composite hollow fiber membrane fibers and their preparation methods
By using a composite hollow fiber membrane preparation method, a porous support layer and a dense separation layer are formed by mixing polytetramethylpentene, inorganic powder and liquid additives. This solves the problems of low air permeability and separation efficiency of existing hollow fiber membranes, and achieves efficient nitrogen and oxygen separation and improved stability.
Patent Information
- Application Number
- CN202611511402.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polytetramethylpentene hollow fiber membranes have low air permeability and separation efficiency, and the preparation process is complex, making it difficult to meet the stability requirements for large-scale production.
A composite hollow fiber membrane preparation method is adopted, which prepares a support layer and a separation layer melt by melting and mixing polytetramethylpentene, inorganic powder and liquid additives, and thermally composites them to form nascent hollow fiber membranes. The porous structure is formed by elution, which adjusts the porosity and pore size, improves the bonding strength between the support layer and the separation layer, reduces gas mass transfer resistance and improves separation efficiency.
It improves the nitrogen and oxygen separation efficiency, air permeability and strength of composite hollow fiber membrane fibers, reduces interfacial peeling and interfacial defects, enhances the stability and application range of membrane fibers, and is suitable for both internal and external air intake modes.
Smart Images

Figure CN123102168A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fiber separation membrane technology, specifically to a composite hollow fiber membrane filament and its preparation method. Background Technology
[0002] Hollow fiber membranes, due to their adjustable separation precision and high separation efficiency, have been widely used in wastewater treatment, battery separators, medical materials, and gas separation. Membrane separation is also a low-energy, high-efficiency separation technology. Polytetramethylpentene, as a polymer material with excellent chemical resistance, weather resistance, and processability, has been widely used in gas membrane separation.
[0003] Polytetramethylpentene hollow fiber membrane fibers can be prepared by melt spinning and stretching. Melt spinning and stretching involves melting and spinning the raw material, cooling and crystallizing it, and then stretching and shaping it to form stable porous polytetramethylpentene hollow fiber membrane fibers. However, the prepared polytetramethylpentene hollow fiber membrane fibers have homogeneity, which results in low air permeability and separation efficiency. Summary of the Invention
[0004] In order to at least partially solve the problems existing in the prior art, according to one aspect of the present invention, a method for preparing composite hollow fiber membrane filaments is provided, the technical solution of which is as follows.
[0005] The method for preparing composite hollow fiber membrane includes the following steps: melting and mixing polytetramethylpentene, inorganic powder and liquid additives to prepare a support layer melt; melting and mixing polytetramethylpentene, toughening agent and nucleating agent to prepare a separation layer melt; thermally combining the support layer melt and the separation layer melt to form nascent hollow fiber membrane; and eluting the nascent hollow fiber membrane to form composite hollow fiber membrane.
[0006] The method for preparing composite hollow fiber membrane fibers of the present invention involves a support layer melt obtained by melt mixing polytetramethylpentene, inorganic powder, and liquid additives. Polytetramethylpentene possesses chemical resistance and weather resistance, and can provide support. The inorganic powder and liquid additives can be used to create pores in the support layer. After elution, pores are formed, allowing the support layer to maintain high strength under conditions of high porosity. The liquid additives, as elutable diluents for pore formation, help reduce the viscosity of the support layer melt, promote the dispersion of inorganic powder, and, after elution, synergistically form interconnected channels with the inorganic powder, thereby adjusting the porosity and pore size of the support layer. The final support layer can form a porous structure, allowing it to primarily provide support and reduce gas mass transfer resistance. The separation layer melt is obtained by melt mixing polytetramethylpentene, a toughening agent, and a nucleating agent. Polytetramethylpentene... Polytetramethylpentene possesses high air permeability and nitrogen-oxygen separation rate. Toughening agents help improve the flexibility and crack resistance of the separation layer, reducing defects in the composite hollow fiber membrane during the forming process. Nucleating agents help regulate the crystallization behavior of polytetramethylpentene, influencing the density, microporous structure, and nitrogen-oxygen separation rate of the separation layer through crystallinity and crystalline region structure, thereby forming a separation layer with separation function. The nascent hollow fiber membrane is eluted to finally form a polytetramethylpentene composite hollow fiber membrane with a dense separation layer and a porous support layer. Since both the separation layer melt and the support layer melt are based on polytetramethylpentene, the high compatibility between the separation layer melt and the support layer melt results in high bonding strength, which helps reduce the interface peeling and interface defects commonly found in heterogeneous composite membranes, and improves the nitrogen-oxygen separation efficiency, air permeability, and strength of the composite hollow fiber membrane.
[0007] For example, in the step of preparing the support layer melt, the following raw materials are used by weight percentage: 30%~40% polytetramethylpentene, 40%~50% inorganic powder, and 10%~30% liquid additive. With this configuration, polytetramethylpentene possesses chemical and weather resistance and can provide support; the inorganic powder and liquid additive can be used to create pores in the support layer, forming pores after elution, allowing the support layer to maintain high strength under conditions of high porosity while reducing gas mass transfer resistance; the liquid additive helps reduce the viscosity of the support layer melt, promotes the dispersion of inorganic powder, and synergistically forms interconnected channels with the inorganic powder after elution, thereby adjusting the porosity and pore size of the support layer and reducing gas mass transfer resistance; by controlling the weight percentage of polytetramethylpentene, inorganic powder, and liquid additive in the support layer, the strength and stability of the composite hollow fiber membrane filaments can be effectively improved.
[0008] For example, the inorganic powder includes nano-calcium carbonate, nano-silica, or a mixture thereof; and / or the liquid additive includes synthetic plant esters, trimellitic acid, citrate ester plasticizers, or a mixture thereof. With this configuration, when nano-calcium carbonate, nano-silica, or a mixture thereof are used for pore formation, elution is easier and less costly, and gas transmembrane resistance is reduced. The synthetic plant esters, trimellitic acid, citrate ester plasticizers, or a mixture thereof, as elutable diluents for pore formation, help reduce the melt viscosity of the support layer, promote the dispersion of inorganic powders, and synergistically form interconnected channels with the inorganic powders after elution, thereby adjusting the porosity and pore size of the support layer and reducing gas mass transfer resistance.
[0009] For example, in the step of preparing the separator layer melt, the following raw materials are used by weight percentage: 90%~95% polytetramethylpentene, 3%~8% toughening agent, and 0.5%~2% nucleating agent. With this configuration, polytetramethylpentene exhibits high air permeability and nitrogen-oxygen separation rate; the toughening agent helps improve the flexibility and crack resistance of the separator layer, reducing defects in the composite hollow fiber membrane during the molding process; the nucleating agent helps regulate the crystallization behavior of polytetramethylpentene, influencing the density, microporous structure, and nitrogen-oxygen separation rate of the separator layer through crystallinity and crystalline region structure; by controlling the weight percentages of polytetramethylpentene, toughening agent, and nucleating agent in the separator layer, the crystallization and separation performance of the separator layer can be adjusted, thereby improving air permeability and separation efficiency.
[0010] For example, the toughening agent includes polyolefin elastomers, high molecular weight polyethylene, polypropylene, or mixtures thereof; and / or the nucleating agent includes sorbic acid or organophosphate nucleating agents. This configuration allows the polyolefin elastomer or polypropylene to improve the flexibility and crack resistance of the release layer, reducing defects in the composite hollow fiber membrane filaments during the molding process; the sorbic acid or organophosphate nucleating agent helps regulate the crystallization behavior of polytetramethylpentene, influencing the density, microporous structure, and nitrogen-oxygen separation rate of the release layer through crystallinity and crystalline region structure.
[0011] For example, the step of preparing the support layer melt includes: uniformly mixing polytetramethylpentene, inorganic powder, and liquid additives using a high-speed mixer or kneader; and homogenizing the uniformly mixed raw materials using a screw extruder to form the support layer melt. This configuration ensures uniform mixing of the polytetramethylpentene, inorganic powder, and liquid additives using a high-speed mixer or kneader, guaranteeing consistent feeding into the screw extruder. The homogenization of the uniformly mixed raw materials using the screw extruder to form the support layer melt results in a uniform and stable composition of the support layer melt, improving the uniformity of the pore distribution in subsequent molding.
[0012] For example, in the step of forming a support layer melt by mixing and homogenizing the uniformly mixed raw materials using a screw extruder, the mixing temperature is 210℃~250℃. This setting facilitates the full plasticization of polytetramethylpentene under the action of liquid additives, and the formation of a uniform homogeneous or near-homogeneous melt with the liquid additives, promoting the uniform dispersion and wetting of inorganic powders, thereby ensuring uniform mixing of the raw materials.
[0013] For example, the step of preparing the separator layer melt includes: uniformly mixing polytetramethylpentene, toughening agent, and nucleating agent using a high-speed mixer or kneader; and homogenizing the uniformly mixed raw materials using a screw extruder to form the separator layer melt. This configuration ensures uniform mixing of the polytetramethylpentene, toughening agent, and nucleating agent using a high-speed mixer or kneader, guaranteeing consistent feeding into the screw extruder. The homogenization of the uniformly mixed raw materials using the screw extruder to form the separator layer melt results in a separator layer melt with uniform composition, crystallinity, and thickness, thereby improving air permeability and separation efficiency.
[0014] For example, in the step of homogenizing and mixing the uniformly mixed raw materials using a screw extruder to form the release layer melt, the mixing temperature is 240℃~290℃. This setting facilitates the full plasticization of polytetramethylpentene under the action of liquid additives, and avoids the agglomeration of nucleating agents and the local enrichment of toughening agents, thereby ensuring the uniformity of the composition, crystallization behavior, and wall thickness of the final release layer.
[0015] For example, in the step of thermally combining the support layer melt and the separator layer melt to form nascent hollow fiber membrane filaments, the process includes: the support layer melt and the separator layer melt are quantitatively delivered to a composite annular die by metering pumps, and the support layer melt and the separator layer melt are extruded together through the composite annular die and cooled to form nascent hollow fiber membrane filaments. This configuration, with the support layer melt and the separator layer melt being quantitatively delivered by metering pumps, allows for independent and precise control of the extrusion flow rate and thickness ratio of the two layers. This helps ensure uniform separator layer thickness, stable support layer structure, and that the separator layer primarily provides separation selectivity while the support layer primarily provides support. The composite extrusion of the two melts after entering the composite annular die allows the separator layer melt to adhere to the inner or outer side of the support layer melt, achieving thermal bonding in a high-temperature molten state. This helps reduce interfacial delamination and interfacial defects commonly found in heterogeneous composite membranes.
[0016] For example, in the step of eluting nascent hollow fiber membrane filaments to form composite hollow fiber membrane filaments, the nascent hollow fiber membrane filaments are soaked and extracted to remove inorganic powder and liquid additives, resulting in composite hollow fiber membrane filaments. This setup allows the extractant to penetrate the support layer through soaking and extraction of the nascent hollow fiber membrane filaments, removing the inorganic powder and liquid additives. These, together with the pores formed by thermal phase separation during the cooling stage, constitute a porous structure, improving the porosity, pore size, and pore connectivity of the support layer.
[0017] According to another aspect of the present invention, a composite hollow fiber membrane filament is provided, which is prepared by the method described above, wherein a separation layer is attached to the inner or outer surface of a support layer. When the separation layer of the composite hollow fiber membrane filament of the present invention is attached to the inner surface of the support layer, an internal air intake mode can be achieved; when the separation layer is attached to the outer surface of the support layer, an external air intake mode can be achieved. This allows for selection based on the application scenario, expanding the scope of application and reducing interfacial peeling and defects common in heterogeneous composite membranes. Furthermore, it improves the nitrogen and oxygen separation efficiency, permeability, and strength of the composite hollow fiber membrane filament.
[0018] For example, the support layer has a thickness D1, which is 0.1 mm to 0.2 mm. With the thickness D1 in this range, the support layer still has sufficient wall thickness and structural integrity after being eluted to form a high porosity and large pore size. It also ensures that the mass transfer path length of the gas through the support layer is moderate, which helps to reduce the resistance of the support layer to gas transmission and maintain a high air permeability.
[0019] For example, the separation layer has a thickness D2, which is 4 to 8 micrometers. This configuration, with a thickness D2 within this range and a relatively small thickness, will improve the nitrogen and oxygen separation rate while ensuring air permeability.
[0020] A series of simplified concepts are introduced in the description of the invention, which will be further explained in detail in the detailed description section. This description is not intended to limit the key features and essential technical features of the claimed technical solution, nor is it intended to determine the scope of protection of the claimed technical solution.
[0021] The advantages and features of the present invention will be described in detail below with reference to the accompanying drawings. Attached Figure Description
[0022] The following figures are included as part of this invention for understanding its principles. The figures illustrate embodiments of the invention and their descriptions, serving to explain the principles of the invention. In the figures,
[0023] Figure 1 This is a cross-sectional view of a composite hollow fiber membrane filament, which is an exemplary embodiment of the present invention.
[0024] The above figures include the following reference numerals:
[0025] 10. Composite hollow fiber membrane filaments; 110. Support layer; 120. Separation layer. Detailed Implementation
[0026] In the following description, numerous details are provided to enable a thorough understanding of the invention. However, those skilled in the art will appreciate that the following description merely illustrates preferred embodiments of the invention, and that the invention can be practiced without one or more of these details. Furthermore, to avoid obscuring the invention, some technical features well-known in the art have not been described in detail.
[0027] To fully understand the embodiments of the present invention, detailed structures will be presented in the following description. Obviously, the implementation of the embodiments of the present invention is not limited to the specific details familiar to those skilled in the art. Preferred embodiments of the present invention are described in detail below; however, in addition to these detailed descriptions, the present invention may have other embodiments.
[0028] This invention provides a method for preparing composite hollow fiber membrane filaments. The following will describe in detail a method for preparing composite hollow fiber membrane filaments according to an embodiment of the present invention, with reference to the accompanying drawings.
[0029] The preparation method of composite hollow fiber membrane filament 10 includes the following steps: preparing a support layer melt by melt mixing polytetramethylpentene, inorganic powder, and liquid additives; preparing a separation layer melt by melt mixing polytetramethylpentene, toughening agent, and nucleating agent; thermally bonding the support layer melt and the separation layer melt to form nascent hollow fiber membrane filaments; and eluting the nascent hollow fiber membrane filaments to form composite hollow fiber membrane filament 10. It should be noted that the support layer 110 can be made of high molecular weight polytetramethylpentene resin, which ensures high strength while maintaining high porosity and large pore size. The separation layer 120 can be made of low molecular weight polytetramethylpentene, which can improve air permeability and nitrogen-oxygen separation rate.
[0030] The method for preparing the composite hollow fiber membrane 10 of the present invention involves a support layer melt obtained by melt mixing polytetramethylpentene, inorganic powder, and liquid additives. Polytetramethylpentene possesses chemical resistance and weather resistance, and can provide support. The inorganic powder and liquid additives can be used to create pores in the support layer 110. After elution, pores are formed, allowing the support layer 110 to maintain high strength under conditions of high porosity. The liquid additives, as elutable diluents for creating pores, help reduce the viscosity of the support layer melt, promote the dispersion of inorganic powder, and, after elution, synergistically form interconnected channels with the inorganic powder, thereby adjusting the porosity and pore size of the support layer 110. The resulting support layer 110 can form a porous structure, enabling it to primarily provide support and reduce gas mass transfer resistance. The separation layer melt is obtained by melt mixing polytetramethylpentene, a toughening agent, and a nucleating agent. Polytetramethylpentene... With high air permeability and nitrogen-oxygen separation rate, the toughening agent helps improve the flexibility and crack resistance of the separation layer 120, reducing defects in the composite hollow fiber membrane 10 during the molding process. The nucleating agent helps regulate the crystallization behavior of polytetramethylpentene, influencing the density, microporous structure, and nitrogen-oxygen separation rate of the separation layer 120 through crystallinity and crystalline region structure, thereby forming a separation layer 120 with separation function. The nascent hollow fiber membrane filaments are eluted to finally form a polytetramethylpentene composite hollow fiber membrane filament with a dense separation layer 120 and a porous support layer 110. Since both the separation layer melt and the support layer melt are based on polytetramethylpentene, the high compatibility between the separation layer melt and the support layer melt results in high bonding strength, which helps reduce the interface peeling and interface defects common in heterogeneous composite membranes, and improves the nitrogen-oxygen separation efficiency, air permeability rate, and strength of the composite hollow fiber membrane filament 10.
[0031] For example, in the step of preparing the support layer melt, the following raw materials are used by weight percentage: 30%~40% polytetramethylpentene, 40%~50% inorganic powder, and 10%~30% liquid additive. Specifically, the weight percentage of polytetramethylpentene can be 30%, 32%, 35%, or 40%, etc. The weight percentage of inorganic powder can be 40%, 42%, 45%, or 50%, etc. The weight percentage of liquid additive can be 10%, 15%, 20%, or 30%, etc. Thus, polytetramethylpentene possesses chemical and weather resistance and can provide support; inorganic powder and liquid additives can be used to create pores in the support layer 110, forming pores after elution, allowing the support layer 110 to maintain high strength under conditions of large porosity, while reducing gas mass transfer resistance; liquid additives help reduce the melt viscosity of the support layer, promote the dispersion of inorganic powder, and synergistically form interconnected channels with inorganic powder after elution, thereby adjusting the porosity and pore size of the support layer 110 and reducing gas mass transfer resistance; by controlling the mass percentage of polytetramethylpentene, inorganic powder, and liquid additives in the support layer 110, the strength and stability of the composite hollow fiber membrane filament 10 can be effectively improved.
[0032] For example, the inorganic powder includes nano-calcium carbonate, nano-silica, or a mixture thereof; and / or the liquid additive includes synthetic plant esters, trimellitic acids (e.g., trioctyl trimellitate), citrate esters (e.g., trioctyl citrate), plasticizers, or mixtures thereof. Thus, when nano-calcium carbonate, nano-silica, or a mixture thereof is used for pore formation, elution is easier, costs are lower, and gas transmembrane resistance is reduced. Synthetic plant esters, trimellitic acids, citrate esters, or mixtures thereof, as elutable diluents for pore formation, help reduce the melt viscosity of the support layer, promote the dispersion of inorganic powders, and synergistically form interconnected channels with the inorganic powders after elution, thereby adjusting the porosity and pore size of the support layer 110 and reducing gas mass transfer resistance.
[0033] For example, in the step of preparing the separator layer melt, the following raw materials are used by weight percentage: 90%~95% polytetramethylpentene, 3%~8% toughening agent, and 0.5%~2% nucleating agent. Specifically, the weight percentage of polytetramethylpentene can be 90%, 92%, 94%, or 95%, etc. The weight percentage of the toughening modifier can be 3%, 5%, 6%, or 8%, etc. The weight percentage of the nucleating agent can be 0.5%, 1%, 1.5%, or 2%, etc. Thus, polytetramethylpentene has high air permeability and nitrogen-oxygen separation rate; the toughening agent helps improve the flexibility and crack resistance of the separation layer 120 and reduces defects in the composite hollow fiber membrane filament 10 during the molding process; the nucleating agent helps regulate the crystallization behavior of polytetramethylpentene, affecting the compactness, microporous structure and nitrogen-oxygen separation rate of the separation layer 120 through crystallinity and crystalline region structure; by controlling the mass percentage of polytetramethylpentene, toughening agent and nucleating agent in the separation layer 120, the crystallization and separation performance of the separation layer 120 can be adjusted, thereby improving air permeability and separation efficiency.
[0034] For example, the toughening agent includes polyolefin elastomer (POE), high molecular weight polyethylene, polypropylene (PP), or mixtures thereof; and / or the nucleating agent includes sorbic acid or organophosphate nucleating agents. Thus, the polyolefin elastomer or polypropylene helps improve the flexibility and crack resistance of the release layer 120, reducing defects in the composite hollow fiber membrane filament 10 during the molding process; the sorbic acid or organophosphate nucleating agent helps regulate the crystallization behavior of polytetramethylpentene, influencing the density, microporous structure, and nitrogen-oxygen separation rate of the release layer 120 through crystallinity and crystalline region structure.
[0035] For example, the step of preparing the support layer melt includes: uniformly mixing polytetramethylpentene, inorganic powder, and liquid additives using a high-speed mixer or kneader; and homogenizing the uniformly mixed raw materials using a screw extruder to form the support layer melt. Thus, uniformly mixing polytetramethylpentene, inorganic powder, and liquid additives using a high-speed mixer or kneader ensures uniform mixing and stable feeding into the screw extruder. Homogenizing the uniformly mixed raw materials using the screw extruder to form the support layer melt results in a uniform composition and stable dispersion of the support layer melt, improving the uniformity of pore distribution in subsequent molding.
[0036] For example, in the step of forming a support layer melt by homogenizing and mixing the uniformly mixed raw materials using a screw extruder, the mixing temperature is 210℃~250℃. Specifically, the mixing temperature can be 210℃, 220℃, 240℃, or 250℃, etc. This facilitates the full plasticization of polytetramethylpentene under the action of liquid additives, and the formation of a uniform homogeneous or near-homogeneous melt with the liquid additives, promoting the uniform dispersion and wetting of inorganic powders, thereby ensuring uniform mixing of the raw materials.
[0037] For example, the step of preparing the separator layer melt includes: uniformly mixing polytetramethylpentene, toughening agent, and nucleating agent using a high-speed mixer or kneader; and homogenizing the uniformly mixed raw materials using a screw extruder to form the separator layer melt. Thus, uniformly mixing polytetramethylpentene, toughening agent, and nucleating agent using a high-speed mixer or kneader ensures uniform mixing and stable feeding into the screw extruder. Homogenizing the uniformly mixed raw materials using the screw extruder to form the separator layer melt results in a separator layer melt with uniform composition, crystallinity, and thickness, thereby improving air permeability and separation efficiency.
[0038] For example, in the step of homogenizing and mixing the uniformly mixed raw materials using a screw extruder to form the release layer melt, the mixing temperature is 240℃~290℃. Specifically, the mixing temperature can be 240℃, 260℃, 280℃, or 290℃, etc. This facilitates the full plasticization of polytetramethylpentene under the action of liquid additives and avoids the agglomeration of nucleating agents and the local enrichment of toughening agents, thereby ensuring the uniformity of the composition, crystallization behavior, and wall thickness of the final release layer 120.
[0039] For example, in the step of thermally combining the support layer melt and the separator layer melt to form nascent hollow fiber membrane filaments, the process includes: the support layer melt and the separator layer melt are quantitatively fed to a composite annular die by metering pumps, and the support layer melt and the separator layer melt are extruded together through the composite annular die and cooled to form nascent hollow fiber membrane filaments. It should be noted that the delivery rate of the metering pumps can be adjusted according to requirements to achieve a suitable thickness. The extruded support layer melt and separator layer melt are cooled at a certain spinning speed. Thus, the support layer melt and the separator layer melt are quantitatively fed by metering pumps, allowing independent and precise control of the extrusion flow rate and thickness ratio of the two layers. This helps ensure the uniform thickness of the separator layer 120 and the structural stability of the support layer 110, and ensures that the separator layer 120 mainly provides separation selectivity and the support layer 110 mainly provides support. The composite extrusion of the two melts after entering the composite annular die allows the separator layer melt to adhere to the inner or outer side of the support layer melt, achieving thermal composite in a high-temperature molten state, which helps reduce interface delamination and interface defects common in heterogeneous composite membranes.
[0040] For example, in step 10 of eluting nascent hollow fiber membrane filaments to form composite hollow fiber membrane filaments, the nascent hollow fiber membrane filaments are soaked and extracted to remove inorganic powder and liquid additives, resulting in composite hollow fiber membrane filaments 10. Specifically, when nano-calcium carbonate is used as the inorganic powder and synthetic vegetable oil is used as the liquid additive, hydrochloric acid and ethanol can be used for soaking and extraction. In this way, by soaking and extracting the nascent hollow fiber membrane filaments, the extractant penetrates into the support layer 110, removing the inorganic powder and liquid additives, thereby forming a porous structure together with the pores formed by thermal phase separation during the cooling stage, improving the porosity, pore size, and pore connectivity of the support layer 110.
[0041] In existing technologies, thermally induced phase separation involves dissolving polytetramethylpentene in a latent solvent at high temperature to form a homogeneous melt, followed by phase separation after cooling to form porous polytetramethylpentene hollow fiber membrane filaments. This method allows for easy control of pore size and porosity, resulting in a relatively narrower pore size distribution and the ability to produce membrane filaments with a stepped pore size distribution. However, due to the complexity of the process and the numerous control parameters, the stability of the stepped layer used for nitrogen and oxygen separation is difficult to guarantee, making it challenging to meet the stability requirements of large-scale production. Therefore, to address these issues, the present invention provides a method for preparing the composite hollow fiber membrane filament 10, comprising the following steps:
[0042] S1. Polytetramethylpentene, inorganic powder and liquid additives are mixed evenly using a high-speed mixer or kneader; polytetramethylpentene, toughening agent and nucleating agent are mixed evenly using a high-speed mixer or kneader.
[0043] S2. The two uniformly mixed raw materials are mixed and homogenized using different screw extruders. The mixture is then mixed at a temperature of 210℃~250℃ to form a support layer melt, and at a temperature of 240℃~290℃ to form a separation layer melt.
[0044] S3. The support layer melt and the separation layer melt are quantitatively delivered to the composite annular die by metering pumps, and the delivery volume and spinning speed of each metering pump are adjusted. After the support layer melt and the separation layer melt are extruded and thermally combined through the composite annular die, they are cooled to cause thermal phase separation of the support layer 110 and the separation layer 120 to cool and crystallize to form a dense or nearly dense layer, finally obtaining the nascent hollow fiber membrane filament.
[0045] S4. After soaking and extracting inorganic powder and liquid additives from the nascent hollow fiber membrane filaments, composite hollow fiber membrane filaments 10 are obtained.
[0046] This method involves thermally bonding a dense separation layer 120 of the required thickness onto a support layer 110. Simultaneously, the forming and pore-forming methods of the support layer 110 and the separation layer 120 can be individually controlled. This allows for the preparation of a composite hollow fiber membrane 10 with high separation efficiency and high air permeability. The support layer 110 is prepared using a combination of dissolution and thermal oxidization, while the separation layer 120 is processed using melt spinning. By controlling the thickness and crystallinity of the separation layer 120, its separation efficiency is adjusted. After thermal bonding, a polytetramethylpentene hollow fiber membrane with high separation efficiency, high air permeability, and high strength is formed.
[0047] According to another aspect of the present invention, a composite hollow fiber membrane filament 10 is provided, which is prepared by the method described above, wherein a separation layer 120 is attached to the inner or outer surface of a support layer 110. When the separation layer 120 of the composite hollow fiber membrane filament 10 of the present invention is attached to the inner surface of the support layer 110, an internal air intake mode can be achieved; when the separation layer 120 is attached to the outer surface of the support layer 110, an external air intake mode can be achieved. This allows for selection based on the application scenario, expanding the scope of application and reducing interface peeling and interface defects common in heterogeneous composite membranes. Furthermore, it improves the nitrogen and oxygen separation efficiency, permeability, and strength of the composite hollow fiber membrane filament 10.
[0048] For example, the support layer 110 has a thickness D1, which is 0.1 mm to 0.2 mm. Thus, with a thickness D1 within this range, the support layer 110, after being eluted to form a high porosity and large pore size, still maintains sufficient wall thickness and structural integrity, and ensures that the mass transfer path length of the gas through the support layer 110 is moderate. This helps to reduce the resistance of the support layer 110 to gas transmission and maintain a high permeability.
[0049] For example, the separation layer 120 has a thickness D2, which is 4 micrometers to 8 micrometers. Thus, the thickness D2 is within this range, and the thickness is relatively small, which will improve the nitrogen and oxygen separation rate while ensuring air permeability.
[0050] Example 1
[0051] 30% polytetramethylpentene, 50% nano-calcium carbonate, and 20% synthetic vegetable oil were uniformly mixed using a high-speed mixer, and 95% polytetramethylpentene, 4% POE, and 0.5% nucleating agent were also uniformly mixed using the same high-speed mixer. The two raw materials were then homogenized and compounded separately using different twin-screw extruders. The compounding temperature for the support layer melt was 250℃, and for the separation layer melt was 290℃. After homogenization using the twin-screw extruders, the support layer melt and separation layer melt were metered and pumped to a composite annular die for compound extrusion. By controlling the flow rates of the two metering pumps, the thicknesses of the support layer 110 and separation layer 120 of the prepared composite hollow fiber membrane filament 10 were controlled. After co-extrusion, the membrane filaments were water-cooled and formed to obtain nascent hollow fiber membrane filaments. The nascent hollow fiber membrane filaments were then extracted at room temperature using hydrochloric acid and ethanol to remove calcium carbonate and organic liquid, respectively. After drying, the composite hollow fiber membrane filament 10 was obtained. The separation layer 120 of the prepared composite hollow fiber membrane 10 is located outside the support layer 110. It is an externally compressed composite hollow fiber membrane 10. The separation layer 120 has a thickness of 4 μm, and the support layer 110 has a thickness of 0.15 mm.
[0052] Performance testing: Tensile breaking strength is 20 MPa, elongation at break is 100%, and air throughput under standard conditions is 300 ml / ( The nitrogen-oxygen separation efficiency is 1:2.2.
[0053] Example 2
[0054] 35% polytetramethylpentene, 40% nano-silica, and 25% trioctyl citrate were uniformly mixed using a high-speed mixer, and 95% polytetramethylpentene, 4% POE, and 0.5% nucleating agent were also uniformly mixed using the same high-speed mixer. The two raw materials were then homogenized and compounded separately using different twin-screw extruders. The mixing temperature for the support layer melt was 250℃, and for the separation layer melt was 280℃. After homogenization using the twin-screw extruders, the support layer melt and separation layer melt were metered and pumped to a composite annular die for compound extrusion. By controlling the flow rates of the two metering pumps, the thicknesses of the support layer 110 and separation layer 120 of the prepared composite hollow fiber membrane filament 10 were controlled. After co-extrusion, the membrane filaments were water-cooled and formed to obtain nascent hollow fiber membrane filaments. The nascent hollow fiber membrane filaments were then extracted at room temperature using sodium hydroxide aqueous solution and ethanol to remove silica and organic liquid, respectively. After drying, the composite hollow fiber membrane filament 10 was obtained. The separation layer 120 of the prepared composite hollow fiber membrane 10 is located outside the support layer 110. It is an externally compressed composite hollow fiber membrane 10. The separation layer 120 has a thickness of 8 μm, and the support layer 110 has a thickness of 0.15 mm.
[0055] Performance testing: Tensile breaking strength is 22 MPa, elongation at break is 105%, and air flux under standard conditions is 260 ml / ( The nitrogen-oxygen separation efficiency is 1:2.5.
[0056] Example 3
[0057] 40% polytetramethylpentene, 40% nano-calcium carbonate, and 20% trioctyl pyromellitic acid were uniformly mixed using a high-speed mixer, and 90% polytetramethylpentene, 8% POE, and 2% nucleating agent were uniformly mixed using the same high-speed mixer. The two raw materials were then homogenized and compounded separately using different twin-screw extruders. The compounding temperature for the support layer melt was 250℃, and for the separation layer melt was 270℃. After homogenization using the twin-screw extruders, the support layer melt and separation layer melt were metered and pumped to a composite annular die for compound extrusion. By controlling the flow rates of the two metering pumps, the thicknesses of the support layer 110 and separation layer 120 of the prepared composite hollow fiber membrane filament 10 were controlled. After co-extrusion, the membrane filaments were water-cooled and formed to obtain nascent hollow fiber membrane filaments. The nascent hollow fiber membrane filaments were then extracted at room temperature using hydrochloric acid and ethanol to remove calcium carbonate and organic liquid, respectively. After drying, the composite hollow fiber membrane filament 10 was obtained. The separation layer 120 of the prepared composite hollow fiber membrane 10 is located outside the support layer 110. It is an externally compressed composite hollow fiber membrane 10. The thickness of the separation layer 120 is 5 μm, and the thickness of the support layer 110 is 0.15 mm.
[0058] Performance testing: Tensile breaking strength is 25 MPa, elongation at break is 120%, and air flux under standard conditions is 320 ml / ( The nitrogen-oxygen separation efficiency is 1:2.
[0059] Comparative Examples
[0060] The granules of 40% polytetramethylpentene, 40% nano-calcium carbonate, and 20% trioctyl pyromellitic acid were melt-mixed by a twin-screw extruder and quantitatively extruded through a metering pump. After passing through a single-layer annular die, the hollow fiber membrane precursor was directly extruded to obtain the precursor. The calcium carbonate and organic liquid in the hollow fiber membrane precursor were extracted at room temperature using hydrochloric acid and ethanol, respectively. After drying, hollow fiber membrane fibers were obtained.
[0061] Performance testing: Tensile breaking strength is 23 MPa, elongation at break is 110%, and air throughput under standard conditions is 22000 ml / ( It does not have the ability to separate nitrogen and oxygen.
[0062] In summary, based on the performance test results of Examples 1-3, the composite hollow fiber membrane filament 10 meets the requirements for strength and elongation at break, and its dense separation layer improves nitrogen and oxygen separation efficiency. Furthermore, using Example 3 and the comparative example as control groups, the comparative example lacks a separation layer and therefore does not possess nitrogen and oxygen separation capability.
[0063] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, parts, components, and / or combinations thereof.
[0064] The present invention has been described through the above embodiments. However, it should be understood that the above embodiments are for illustrative purposes only and are not intended to limit the invention to the scope of the described embodiments. Furthermore, those skilled in the art will understand that the present invention is not limited to the above embodiments, and many more variations and modifications can be made based on the teachings of the present invention, all of which fall within the scope of protection claimed by the present invention. The scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for producing a composite hollow fiber membrane filament, characterized by, Including the following steps: A support layer melt was prepared by melt mixing polytetramethylpentene, inorganic powder and liquid additives; A separation layer melt was prepared by melt mixing polytetramethylpentene, toughening agent and nucleating agent; The support layer melt and the separation layer melt are thermally combined to form nascent hollow fiber membrane filaments; The nascent hollow fiber membrane fibers are eluted to form composite hollow fiber membrane fibers.
2. The composite hollow fiber membrane filament production method according to claim 1, characterized by, In the step of preparing the support layer melt, the following raw materials are used by weight percentage: 30%~40% polytetramethylpentene, 40%~50% inorganic powder, and 10%~30% liquid additive.
3. The composite hollow fiber membrane filament production method according to claim 2, characterized by, The inorganic powder includes nano-calcium carbonate, nano-silica, or a mixture of both; and / or The liquid additives include synthetic vegetable esters, trimesic acid, citrate plasticizers, or mixtures thereof.
4. The composite hollow fiber membrane filament production method according to claim 1, characterized by, In the step of preparing the separator layer melt, the following raw materials are used by weight percentage: 90%~95% polytetramethylpentene, 3%~8% toughening agent, and 0.5%~2% nucleating agent.
5. The composite hollow fiber membrane filament production method according to claim 4, characterized by, The toughening agent includes polyolefin elastomers, high molecular weight polyethylene, polypropylene, or mixtures thereof; and / or The nucleating agent includes sorbic acid or organophosphate nucleating agents.
6. The composite hollow-fiber membrane-silk production method according to claim 1, characterized by, The step of preparing the support layer melt includes: Polytetramethylpentene, inorganic powder and liquid additives are mixed evenly using a high-speed mixer or kneader; The support layer melt is formed by mixing and homogenizing the uniformly mixed raw materials using a screw extruder.
7. The composite hollow fiber membrane filament production method according to claim 6, characterized by, In the step of forming a support layer melt by mixing and homogenizing the uniformly mixed raw materials using a screw extruder, the mixing temperature is 210℃~250℃.
8. The composite hollow-fiber membrane-silk production method according to claim 1, characterized by, The step of preparing the separated layer melt includes: Polytetramethylpentene, toughening agent and nucleating agent are mixed evenly using a high-speed mixer or kneader; The raw materials are mixed and homogenized using a screw extruder to form a separate layer melt.
9. The composite hollow fiber membrane filament production method according to claim 8, characterized by, In the step of forming a separate layer melt by mixing and homogenizing the uniformly mixed raw materials using a screw extruder, the mixing temperature is 240℃~290℃.
10. The composite hollow-fiber membrane-silk production method according to claim 1, characterized by, The step of thermally bonding the support layer melt and the separation layer melt to form nascent hollow fiber membrane fibers includes: The support layer melt and the separation layer melt are respectively metered and pumped to the composite annular die, and the support layer melt and the separation layer melt are extruded together through the composite annular die and cooled to form the nascent hollow fiber membrane filament.
11. The method for preparing composite hollow fiber membrane filaments according to claim 1, characterized in that, In the step of eluting the nascent hollow fiber membrane filaments to form composite hollow fiber membrane filaments, the nascent hollow fiber membrane filaments are soaked and extracted to extract inorganic powder and liquid additives to obtain composite hollow fiber membrane filaments.
12. A composite hollow fiber membrane filament, characterized in that, The separation layer is prepared by any one of the preparation methods described in claims 1-11, and is attached to the inner or outer surface of the support layer.
13. The composite hollow fiber membrane filament of claim 12, wherein, The support layer has a thickness D1, which is 0.1 mm to 0.2 mm.
14. The composite hollow fiber membrane filament of claim 12, wherein, The separation layer has a thickness D2, which is 4 micrometers to 8 micrometers.