A low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent, its preparation method, and its application.

By introducing Mg2+ and Sr2+ co-substitution and oxygen vacancy engineering into the calcium aluminum oxide lattice, a low-crystallinity, oxygen-vacancy-rich calcium aluminum-based defluorinating agent was prepared, which solved the problems of low active site density and narrow pH range of existing calcium aluminum oxides, and achieved efficient and low-cost fluoride ion removal effect.

CN123102294APending Publication Date: 2026-11-17JIANGSU UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202611558040.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing calcium aluminum oxide defluorinating agents have low surface active site density, few oxygen vacancies, and a narrow pH range, making it difficult to efficiently remove fluoride ions. Furthermore, the preparation process is energy-intensive and costly, hindering large-scale application.

Method used

By introducing Mg2+ and Sr2+ into the Ca-Al-O lattice to form low-crystallinity oxygen-rich vacancies, and combining this with inert atmosphere medium-temperature calcination and sodium borohydride etching, a low-crystallinity oxygen-rich calcium-aluminum-based fluoride remover was prepared, which enhanced the density of active sites and oxygen vacancies, and improved the fluoride ion removal rate and pH range.

Benefits of technology

It achieves efficient and low-cost fluoride ion removal, has a wide applicable pH range, good anti-interference ability and circulation regeneration performance, and is suitable for various water quality conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102294A_ABST
    Figure CN123102294A_ABST
Patent Text Reader

Abstract

This invention discloses a low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent, its preparation method, and its application. This defluorinating agent uses a calcium-aluminum hydrotalcite precursor as a matrix and achieves Mg removal through co-precipitation. 2+ 、Sr 2+ For Ca 2+ Co-substitution, followed by inert atmosphere calcination at medium temperature and liquid-phase reduction with NaBH4, creates a high-density oxygen vacancy on the surface; Mg 2+ It causes lattice shrinkage distortion and inhibits Ca-Al-O overcrystallization, Sr 2+ This causes localized lattice expansion and the formation of coordination-unsaturated sites. The defluorination process is carried out synergistically through surface electrostatic attraction, oxygen vacancy capture, surface hydroxyl ion exchange, and the reaction of calcium ions released by the defluorinating agent with fluoride ions to form CaF2 precipitate. The preparation process of this defluorinating agent is simple, mild, and inexpensive, and it also has high defluorination efficiency, a wide applicable pH range, strong anti-interference ability, and strong regeneration capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent, its preparation method, and its application, belonging to the technical field of water treatment and environmental functional material preparation. Background Technology

[0002] Fluorine is an essential trace element for the human body, but long-term excessive fluoride intake can lead to health problems such as dental fluorosis and skeletal fluorosis. The "Integrated Wastewater Discharge Standard" (GB 8978-1996) stipulates that the upper limit for fluoride in the first-class standard is 10 mg / L, while the "Standards for Drinking Water Quality" (GB 5749-2022) stipulates that the limit for fluoride content in drinking water is 1.0 mg / L. The concentration of fluoride ions in wastewater generated by industries such as photovoltaics and semiconductors often far exceeds the discharge standards, making the advanced treatment of fluoride-containing wastewater an important issue in environmental protection. Therefore, developing efficient and economical fluoride removal materials is of significant practical importance.

[0003] Currently, commonly used defluorination technologies include chemical precipitation, coagulation precipitation, ion exchange, membrane separation, and adsorption. Among these, adsorption is widely studied and applied due to its advantages such as simple operation, low cost, and suitability for deep removal of fluoride ions. Commonly used adsorbents include activated alumina, hydroxyapatite, layered double hydroxides, and metal oxides. Activated alumina is the most commonly used defluorination adsorbent, but its equilibrium adsorption capacity is typically only 2-5 mg / g, and its optimal operating pH range is narrow. In recent years, novel adsorbents such as aluminum-based rare earth materials, zirconium-based materials, and metal-organic frameworks have shown higher capacities, but their expensive raw materials and demanding preparation conditions hinder their engineering application.

[0004] Calcium aluminum oxides have attracted widespread attention in the field of fluoride removal due to their advantages such as wide availability of raw materials, low preparation cost, and environmental friendliness. Calcium ions in calcium aluminum oxides can react with fluoride ions to form slightly soluble CaF2, and the hydroxyl groups on the surface of aluminum ions can adsorb fluoride ions through ligand exchange, theoretically making them ideal low-cost fluoride removal materials. However, existing calcium aluminum oxides are mostly prepared using high-temperature solid-state sintering or hydrothermal crystallization methods, resulting in products with high crystallinity and few active sites. Fluoride ions can only react with a limited number of active sites on the surface, and the adsorption capacity is far from the theoretical level. Furthermore, the highly crystalline particles obtained by conventional high-temperature solid-state sintering are dense and hard, resulting in large mass transfer resistance and slow adsorption kinetics, making it difficult to further improve the fluoride removal capacity. The fluoride removal mechanism of calcium aluminum oxides involves the participation of surface active sites, and the degree of crystallinity of the material directly affects the surface hydroxyl density and the number of active sites. Low-crystallinity materials, due to their incomplete crystal lattice development, have more defect sites and unsaturated surface coordination structures, and are expected to provide a richer number of active sites for fluoride ion adsorption.

[0005] In addition, existing patents CN102389769A discloses a method for preparing a calcium-aluminum-lanthanum-based composite defluorination material; CN103071450A discloses a defluorination adsorbent, its preparation method, and its application; CN103274539A discloses a method for removing fluoride from water by complexation-coagulation-adsorption of a defluorination adsorbent based on an aluminum-based composite metal oxide; CN118681533A discloses a material and its application for treating fluoride in wastewater; and CN119390220B discloses a highly efficient defluorination agent suitable for photovoltaic wastewater and its application. Preparation processes: CN119771335A discloses an adsorption-type defluorinating agent, its preparation method, and its application; CN121402054A discloses a preparation method and application of a calcium-aluminum-lanthanum high-efficiency composite defluorinating agent; CN119869467B discloses a composite adsorbent, its preparation method, and its application, and a method for removing fluoride ions from photovoltaic wastewater; CN122682542A discloses a water defluorinating agent, its preparation method, and its application; CN122702404A discloses a calcium-aluminum-based defluorinating material derived from solid waste, its preparation method, and its application. However, none of the above-mentioned existing technologies simultaneously achieve the following technical features: introducing oxygen vacancies within the calcium-aluminum oxide-based framework; introducing two ions with significantly different radii at the same lattice position to form a "small ion contraction + large ion expansion" bi-site co-substitution, constructing a size screening effect for fluoride ions; and preparing low-crystallinity oxygen-rich vacancy calcium-aluminum oxides by medium-temperature calcination combined with chemical reduction under inert conditions. Therefore, developing a low-crystallinity, oxygen-vacancy-rich, wide-pH-range, low-cost, and highly efficient calcium-aluminum oxide defluorinating agent and its scalable preparation method is of significant practical value. Summary of the Invention

[0006] To overcome the problems of low surface active site density, few oxygen vacancies, and narrow pH range of existing calcium aluminum oxide defluorinating agents, this invention provides a low-crystallinity, oxygen-vacancy-rich calcium aluminum-based defluorinating agent, its preparation method, and its application. Through the synergy of bi-site co-substitution ("small ion shrinkage + large ion expansion") and oxygen vacancy engineering, the active site density of the material is increased and oxygen vacancies are increased. The resulting material maintains excellent removal rate and high selectivity for fluoride ions, has a wide pH range, and excellent recyclability.

[0007] In the Ca-Al-O lattice, with Mg 2+ 、Sr 2+ Replace part of Ca 2+ This results in a bi-substitution process characterized by "small ion contraction + large ion expansion." Mg 2+ radius compared to Ca 2+ Smaller size compresses locally coordinated octahedra, enhancing Al-O bond polarity and reducing F. - Embedding energy barrier; Sr 2+ radius compared to Ca 2+The size of the cage is increased, making the size matching degree of the cage to tetrahedral / near-spherical small anions better than that to large-volume tetrahedra, thereby establishing size repulsion selectivity at the structural level.

[0008] Oxygen vacancies are important anionic defect sites on the surface of metal oxides, possessing localized electron-rich and Lewis acid properties, and are important for F - Hard Lewis base anions possess strong coordination trapping capabilities. However, existing calcium-aluminum based defluorination materials are rarely designed from an oxygen vacancy engineering perspective: calcium-aluminum oxides prepared by conventional air calcination have low surface oxygen vacancy density.

[0009] This invention uses calcium aluminum hydrotalcite compounds as precursors and leverages the exchangeability of metal ions in their lamellar plates to co-precipitate Mg. 2+ 、Sr 2+ Introducing a layered structure achieves lattice co-substitution; after medium-temperature calcination in an inert atmosphere, the precursor is transformed into calcium-aluminum-based oxides, Mg 2+ Radius smaller than Ca 2+ This causes lattice shrinkage distortion and inhibits the over-crystallization of Ca-Al-O, Sr 2+ Radius greater than Ca 2+ This causes local lattice expansion and the formation of coordination unsaturated sites; under an inert atmosphere, oxygen is removed from the surface lattice to form oxygen vacancies, and then sodium borohydride reduction further etches out high-density surface oxygen vacancies and hydroxylates the surface.

[0010] The technical solution adopted in this invention is as follows: A method for preparing a low-crystallinity, oxygen-vacancy-rich calcium-aluminum-based defluorinating agent includes the following steps: S1. Dissolve calcium salt, magnesium salt, strontium salt and aluminum salt to obtain a mixed salt solution; S2. Adjust the pH of the mixed salt solution to 9-10, then react at 40-60℃ for 2-4 hours, and then raise the temperature to 70-80℃ for aging for 2-4 hours; S3. The aged solution is subjected to solid-liquid separation. The solid phase is washed and dried to obtain precursor powder. S4. Place the precursor powder in an inert atmosphere, calcine at 300-500℃ for 2-3 hours, and then cool (while still in an inert atmosphere during cooling). After grinding, obtain magnesium-strontium co-substituted calcium-aluminum oxide powder. S5. Disperse the magnesium strontium co-substituted calcium aluminum oxide powder in a sodium borohydride solution, stir, and then separate the solid and liquid phases. The solid phase is then washed, dried, and ground.

[0011] Preferably, the calcium salt, magnesium salt, strontium salt, and aluminum salt are the corresponding chlorides or nitrates.

[0012] Preferably, among the calcium salt, magnesium salt, strontium salt, and aluminum salt, the molar ratio of Ca to Al is (0.5-0.6):1, Mg accounts for 5%-10% of the total molars of Ca and Al, and Sr accounts for 3%-8% of the total molars of Ca and Al.

[0013] Preferably, the alkaline solution used to adjust the pH of the mixed salt solution is sodium hydroxide solution or ammonia water.

[0014] Preferably, the heating rate during calcination is 3-8°C / min.

[0015] Preferably, the concentration of the sodium borohydride solution is 0.2-1.0 mol / L.

[0016] A low-crystallinity, oxygen-vacancy-rich calcium-aluminum-based defluorinating agent is prepared by any of the methods described above.

[0017] Application of low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agents prepared by any of the above methods in the defluorination of fluoride-containing water bodies.

[0018] Preferably, the pH of the fluoride-containing water is 4-9.

[0019] The application of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent prepared by any of the above methods in the defluorination of water containing interfering anions and fluoride ions, wherein the interfering anions are chloride ions, sulfate ions, carbonate ions, bicarbonate ions, or dihydrogen phosphate ions.

[0020] The low-crystallinity, oxygen-rich, vacancy-enriched magnesium-strontium co-substituted calcium-aluminum oxide defluorinating agent provided by this invention relies on multiple synergistic processes such as surface electrostatic attraction, oxygen vacancy Lewis acid site coordination capture, surface hydroxyl ion exchange, and calcium ion precipitation to remove fluoride ions from water. It has high adsorption capacity and good anti-interference ability, specifically manifested as follows: (1) Surface hydroxyl groups enrich F through electrostatic interaction. - (2) Coordination unsaturated Ca at surface oxygen vacancies 2+ Al 3+ Mg 2+ 、Sr 2+ The cation acts as the Lewis acid center, with F - Coordination occurs to form a metal-F bond, which in turn bonds F... - Firmly fixed in the vacancy, Mg 2+ 、Sr 2+ Co-substitutional aberration site, strong bond solid fluorine, Sr 2+ Provides strong fluorine affinity sites; (3) Surface metal-OH groups and F - Ligand exchange occurs, releasing OH - To achieve chemical adsorption; Sr 2+ Due to its high softness and F -It has a strong effect and significantly improves selectivity. (4) The calcium ions and fluoride ions released by the material can form CaF2 precipitate, which further contributes to the fluoride removal capacity.

[0021] The beneficial effects of this invention are as follows: (1) The preparation process is simple, the raw materials are widely available and inexpensive, no special equipment is required, energy consumption is low, and it is easy to industrialize. (2) Through Mg 2+ 、Sr 2+ The synergy between lattice co-substitution distortion sites and oxygen vacancies keeps the calcium aluminum oxide products in a low crystallinity state, retaining abundant surface hydroxyl groups and unsaturated coordination active sites, which significantly improves the removal capacity of fluoride ions. (3) The obtained defluoridating agent has a wide applicable pH range and strong anti-interference ability against coexisting anions (chloride ions, sulfate ions, etc.). It can maintain a high defluoridation efficiency under a wide range of water quality conditions. Attached Figure Description

[0022] Figure 1 Flowchart for the preparation of a low-crystallinity, oxygen-rich, vacancy-enriched magnesium-strontium co-substituted calcium-aluminum oxide defluorinating agent; Figure 2 XRD patterns of the defluorinating agents prepared in Examples 1-3; Figure 3 The XRD pattern of the defluorinating agent prepared in Example 4; Figure 4 The XRD patterns of the defluorinating agents prepared in Examples 5-6 are shown below. Figure 5 SEM image of the defluorinating agent prepared in Example 1; Figure 6 The cyclic regeneration performance of the defluorinating agent prepared in Example 1. Detailed Implementation

[0023] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0024] Example 1: This example provides a method for preparing a low-crystallinity, oxygen-rich, vacant magnesium-strontium co-substituted calcium-aluminum oxide defluorinating agent. The process is as follows: Figure 1 As shown, the specific steps include: S1. Weigh 2.22g of anhydrous calcium chloride, 15.00g of aluminum nitrate nonahydrate, 0.29g of anhydrous magnesium chloride, and 0.80g of strontium chloride hexahydrate, and dissolve them in 200mL of deionized water to obtain Mg 2+ -Sr 2+ -Ca 2+ -Al 3+ Mixed salt (ionic) solutions; S2. Under stirring conditions at 40°C, add 8 g / L sodium hydroxide solution dropwise to the mixed salt solution obtained in step S1, adjust the pH value to 9.5, continue the reaction for 4 hours, and then raise the temperature to 70°C and age for 3 hours. S3. Separate the solid and liquid phases of the aged product obtained in step S2. Wash the solid phase with deionized water three times and then dry it in a drying oven at 80°C for 6 hours to obtain the precursor powder. S4. The precursor powder obtained in step S3 is calcined at 400°C for 3 hours under a nitrogen atmosphere, with the heating rate controlled at 5°C / min. After calcination, it is cooled to room temperature under a nitrogen atmosphere and then ground to obtain magnesium-strontium co-substituted calcium-aluminum oxide powder. S5. The powder obtained in step S4 is dispersed in a 0.2 mol / L sodium borohydride solution and stirred for 0.5 h. After solid-liquid separation, the solid phase is washed three times with deionized water, dried at 60 °C for 8 h, and then ground to obtain a magnesium-strontium co-substituted calcium-aluminum-based defluorinating agent with low crystallinity and a surface rich in oxygen vacancies.

[0025] Examples 2-6.

[0026] The steps of Examples 2-6 are basically the same as those of Example 1, except that the roasting temperatures in Examples 2, 3, 4, 5 and 6 are 300℃, 500℃, 200℃, 600℃ and 700℃, respectively.

[0027] Comparative Example 1: The steps are basically the same as those in Example 1, except that magnesium chloride and strontium chloride hexahydrate were not added in step S1, and sodium borohydride solution treatment was not performed in step S5.

[0028] Comparative Example 2: The steps are basically the same as those in Example 1, except that magnesium chloride and strontium chloride hexahydrate were not added in step S1.

[0029] Comparative Example 3: The steps are basically the same as those in Example 1, except that step S5, sodium borohydride solution treatment, is omitted.

[0030] Material characterization and defluorination performance testing.

[0031] 1. XRD characterization: The defluorinating agents prepared in Examples 1-6 were subjected to phase analysis using XRD. Figure 2 The figures show the XRD patterns of the defluorinating agents prepared in Examples 1-3. As can be seen from the figures, the samples prepared in Examples 1-3 only exhibit broadened diffuse diffraction peaks in the 20~40° range, without sharp crystalline diffraction peaks, indicating that low-crystallinity magnesium strontium co-substituted calcium aluminum oxide defluorinating agents were successfully prepared. Figure 3The image shows the XRD pattern of the defluorinating agent prepared in Example 4. As can be seen from the figure, the diffraction peaks of the sample prepared after calcination at 200℃ can all be indexed as the diffraction peaks of CaAl(OH)6Cl(H2O)2, indicating that the product still retains the precursor Fred salt structure at this temperature. Figure 4 The XRD patterns of the defluorinating agents prepared in Examples 5-6 are shown. As can be seen from the figures, significant crystal transformations occurred in the samples after calcination at 600℃ and 700℃. The calcined products mainly consist of Ca. 12 Al 14 O 33 It consists of a small amount of CaO and Ca(Al4O7). The XRD results above show that by controlling the calcination temperature at 300~500℃, a low-crystallinity magnesium-strontium co-substituted calcium-aluminum oxide defluorinating agent can be obtained.

[0032] 2. SEM morphological characterization: The surface morphology of the defluorinating agent prepared in Example 1 was observed using a scanning electron microscope. Figure 5 This is a SEM image of the defluorinating agent prepared in Example 1. The SEM image shows that the defluorinating agent is composed of stacked flake-like fragments and polyhedral particles. The particle edges are blunted, the crystallinity is low, and the interlacing of the flakes forms abundant interstitial pores and surface defect sites. This microstructure provides a large number of active sites brought about by Mg and Sr doping and oxygen vacancies. The hierarchical porosity is conducive to the mass transfer and diffusion of fluoride ions. The material can efficiently capture fluoride ions through electrostatic attraction and surface complexation. At the same time, the calcium-aluminum matrix ensures chemical stability, giving the defluorinating agent excellent water defluorination performance.

[0033] 3. Defluorination performance test: (1) The effect of the dosage of defluorinating agent; The prepared defluorinating agent (prepared in Example 1 and Comparative Examples 1-3) was added to 50.0 mL of an aqueous solution with an initial fluoride ion concentration of 20.0 mg / L. After reacting at room temperature for 4 h, the fluoride ion concentration was measured using a fluoride ion meter. The effect of the amount of defluorinating agent added (0.2-2.0 g / L) on the fluoride ion concentration after treatment was tested. The results of the fluoride ion concentration in the treated aqueous solution are shown in Table 1.

[0034] Table 1. Effect of defluorinating agent dosage on defluorination performance

[0035] As shown in Table 1, when the dosage of the defluorinating agent is 2.0 g / L, the fluoride ion concentration in the system after defluorination treatment with the defluorinating agent prepared in Example 1 is less than 1 mg / L, which meets the limit for fluoride content in drinking water specified in the "Standards for Drinking Water Quality" (GB 5749-2022). However, the fluoride ion concentration in the systems prepared with the defluorinating agents prepared in Comparative Examples 1, 2, and 3 is all higher than 1 mg / L after defluorination treatment. The results in Table 1 fully demonstrate that the low-crystallinity, oxygen-rich, vacant magnesium strontium co-substituted calcium aluminum oxide defluorinating agent prepared in Example 1 has good defluorination performance.

[0036] (2) Effect of calcination temperature on defluorination performance; 100 mg of a defluorinating agent (prepared in Examples 1-6) was added to 50.0 mL of an aqueous solution with an initial fluoride ion concentration of 20.0 mg / L. After reacting at room temperature for 4 h, the fluoride ion concentration was measured using a fluoride ion meter. The test results are shown in Table 2.

[0037] Table 2 Effect of calcination temperature on defluorination performance

[0038] As shown in Table 2, calcination temperature has a direct impact on fluoride ion concentration. The performance of defluorinating agents prepared at 200℃, 600℃, and 700℃ decreased significantly, confirming the retention effect of the low crystallinity state on active sites. Among them, the defluorinating agent prepared after calcination at 400℃ had the lowest residual fluoride ion concentration after treating fluoride-containing wastewater.

[0039] (3) The effect of pH value on defluorination performance; Fluorine-containing aqueous solutions with an initial fluoride ion concentration of 20.0 mg / L and pH values ​​of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, and 13 were prepared. The defluorinating agent prepared in Example 1 was added at a dosage of 2.0 g / L. After reacting at room temperature for 4 h, the defluorination efficiency under each pH condition was measured. The results are shown in Table 3.

[0040] Table 3 Effect of pH value on defluorination performance

[0041] The results in Table 3 show that the defluorinating agent prepared in Example 1 maintained good fluoride ion removal effect in the pH range of 4 to 9, indicating that the prepared defluorinating agent has strong pH adaptability.

[0042] (4) The effect of interfering with anions; In actual fluoride-containing wastewater, multiple anions often coexist. To evaluate the selective adsorption performance of the defluorinating agent, 50 mL of an aqueous solution with an initial fluoride ion concentration of 20.0 mg / L and containing 20.0 mg / L of chloride, sulfate, carbonate, bicarbonate, and dihydrogen phosphate ions were prepared. Then, 100 mg of the defluorinating agent prepared in Example 1 was added. After reacting at room temperature for 4 h, the fluoride ion concentration was measured, and the results are shown in Table 4.

[0043] Table 4. Effects of interfering ions on defluorination performance

[0044] Table 4 shows that the effects of chloride and sulfate ions on fluoride ion concentration are almost negligible; carbonate and bicarbonate ions show a small degree of influence; and dihydrogen phosphate ions show a relatively significant inhibitory effect. Overall, however, the prepared low-crystallinity, oxygen-vacancy-rich magnesium-strontium co-substituted calcium-aluminum oxide defluorinating agent exhibits good selectivity for fluoride ions.

[0045] (5) Regeneration and recycling performance; 100 mg of a fluoride removal agent (prepared in Example 1) was added to 50.0 mL of an aqueous solution with an initial fluoride ion concentration of 20.0 mg / L, and the reaction was carried out at room temperature for 4 h. The saturated fluoride removal agent was then regenerated by soaking in a 1 mol / L NaOH solution for 4 h, washed with water until neutral, and recycled 5 times. The fluoride ion removal rate only decreased from 95.1% to 90.3% (see...). Figure 6 It exhibits superior recyclability.

[0046] In summary, the preparation method of the low-crystallinity oxygen-rich vacancy magnesium strontium co-substituted calcium aluminum oxide defluorinating agent provided by the present invention is feasible. The obtained defluorinating agent has excellent defluorination effect and a wide pH adaptability range, and has good application prospects in the field of defluorination of fluoride-containing wastewater.

[0047] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a low-crystallinity, oxygen-vacancy-rich calcium-aluminum-based defluorinating agent, characterized in that, Includes the following steps: S1. Dissolve calcium salt, magnesium salt, strontium salt and aluminum salt to obtain a mixed salt solution; S2. Adjust the pH of the mixed salt solution to 9-10, then react at 40-60℃ for 2-4 hours, and then raise the temperature to 70-80℃ for aging for 2-4 hours; S3. The aged solution is subjected to solid-liquid separation. The solid phase is washed and dried to obtain precursor powder. S4. Place the precursor powder under an inert atmosphere, calcine at 300-500℃ for 2-3 hours, cool, and grind to obtain magnesium strontium co-substituted calcium aluminum oxide powder; S5. Disperse the magnesium strontium co-substituted calcium aluminum oxide powder in a sodium borohydride solution, stir, and then separate the solid and liquid phases. The solid phase is then washed, dried, and ground.

2. The preparation method of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent according to claim 1, characterized in that, Calcium salts, magnesium salts, strontium salts, and aluminum salts are the corresponding chlorides or nitrates, respectively.

3. The preparation method of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent according to claim 1, characterized in that, Among calcium, magnesium, strontium, and aluminum salts, the molar ratio of Ca to Al is (0.5-0.6):1, Mg accounts for 5%-10% of the total molars of Ca and Al, and Sr accounts for 3%-8% of the total molars of Ca and Al.

4. The preparation method of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent according to claim 1, characterized in that, The alkaline solution used to adjust the pH of the mixed salt solution is sodium hydroxide solution or ammonia water.

5. The preparation method of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent according to claim 1, characterized in that, The heating rate for roasting is 3-8℃ / min.

6. The preparation method of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent according to claim 1, characterized in that, The concentration of sodium borohydride solution is 0.2-1.0 mol / L.

7. A low-crystallinity, oxygen-vacancy-rich calcium-aluminum-based defluorinating agent, characterized in that, Prepared by the method according to any one of claims 1-6.

8. The application of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluorinating agent prepared by the method according to any one of claims 1-6 in the defluorination of fluoride-containing water bodies.

9. The application according to claim 8, characterized in that, The pH of fluoride-containing water is 4-9.

10. The application of the low-crystallinity, oxygen-rich, vacancy-enriched calcium-aluminum-based defluoridator prepared by the method according to any one of claims 1-6 in the defluoridation of water containing interfering anions and fluoride ions, characterized in that, The interfering anions are chloride, sulfate, carbonate, bicarbonate, or dihydrogen phosphate.

Citation Information

Patent Citations

  • Preparation method of calcium-aluminum-lanthanum-based compound fluorine-removing material

    CN102389769A

  • Defluorination adsorbent as well as preparation method and application thereof

    CN103071450A

  • Method for removing fluoride in drinking water by complexation-coacervation-adsorption with defluorination adsorption material based on aluminium base composite metal oxide

    CN103274539A

  • Material for treating fluoride in sewage and application

    CN118681533A

  • A high-efficiency defluorination agent suitable for photovoltaic wastewater and its preparation process

    CN119390220B