Preparation and application of a BiOI / CdS heterojunction photocatalytic material
By preparing BiOI/CdS heterojunction photocatalytic materials and combining solvothermal and coprecipitation methods, the problem of excessively fast recombination rates of photogenerated electron-hole pairs in BiOI and CdS photocatalysts was solved, achieving efficient photocatalytic degradation of malachite green and improving photocatalytic efficiency.
Patent Information
- Application Number
- CN202510623443.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
BiOI exhibits a high electron-hole recombination rate during photocatalysis, which affects catalytic efficiency. Single BiOI and CdS photocatalysts show excessively rapid photogenerated electron-hole recombination rates, making it difficult to effectively degrade organic pollutants.
By preparing BiOI/CdS heterojunction photocatalytic materials, and combining solvothermal and coprecipitation methods, BiOI nanosheets are grown in situ on the surface of CdS microspheres to form an irregular spherical structure, thereby constructing a heterostructure to enhance charge transport characteristics.
The BiOI/CdS heterojunction photocatalytic material significantly improved the photocatalytic degradation rate of malachite green, with a degradation rate 2.69 times that of CdS and 2.14 times that of BiOI. Superoxide radicals played a dominant role in the degradation process.
Smart Images

Figure CN123102387A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocatalytic materials for the degradation of organic pollutants, specifically relating to the preparation and application of a BiOI / CdS heterojunction photocatalytic material. Background Technology
[0002] With the rapid development of industry, the resulting severe water pollution has become a major global concern. The textile and dyeing industry, in particular, is a primary source of organic dye wastewater, resulting in a particularly significant environmental impact. These industries use a wide variety of dyes, adding color to fabrics and textiles while also causing environmental pollution. Photocatalysis, as a novel and sustainable application technology, has received considerable attention in recent years. Due to its green, efficient, and safe characteristics, it has been widely applied in the field of photocatalytic degradation of organic pollutants.
[0003] Cadmium sulfide (CdS), a typical II-VI group semiconductor, possesses a narrow bandgap, low cost, excellent performance, and diverse morphologies. These advantages have made it a focus of attention in various fields such as solar energy utilization, photocatalytic degradation of pollutants, and electrocatalytic water splitting. However, CdS has a significant drawback: its photogenerated electron-hole recombination rate is too fast, severely affecting catalytic efficiency. Bismuth oxide compounds (BiOX, X = Cl, Br, I) have become research hotspots in materials science and environmental science due to their unique layered crystal structure, high solar energy utilization efficiency, and excellent photocatalytic activity. Among the many BiOX compounds, BiOI stands out due to its narrow bandgap. This characteristic gives BiOI excellent solar energy absorption for visible light. However, it is undeniable that individual BiOIs face the challenge of a high electron-hole recombination rate during photocatalysis. Therefore, it is necessary to construct heterojunctions and introduce co-catalysts to effectively improve photocatalytic performance. Summary of the Invention
[0004] To address the shortcomings of the photocatalytic properties of the aforementioned single materials, this invention provides a method for preparing a BiOI / CdS heterojunction photocatalytic material, thereby improving the photocatalytic rate of malachite green degradation.
[0005] To effectively implement the above invention, the present invention is carried out through the following technical means:
[0006] The preparation of a BiOI / CdS heterojunction photocatalytic material includes the following steps:
[0007] (1) Preparation of CdS
[0008] Cadmium acetate was dispersed in a mixed solution of water and isopropanol and stirred until completely dissolved. Thiourea was then added to the solution, and stirring continued to obtain a precursor solution. This solution was then transferred to a lined high-temperature reactor. A hydrothermal reaction was carried out in an electrically heated constant-temperature drying oven. After the reaction was complete, the mixture was allowed to cool naturally and finally washed several times with ethanol and water to obtain CdS powder.
[0009] (2) Preparation of BiOI / CdS:
[0010] Cadmium sulfide was dispersed in a mixed solution of water and glycerol and stirred thoroughly until completely dissolved. Then, bismuth nitrate and potassium iodide were added simultaneously to the mixture, and stirring continued until an orange-yellow solution was obtained. The solution was then allowed to stand to allow for natural precipitation. Finally, the solution was washed several times with ethanol and water to obtain BiOI / CdS powder.
[0011] (3) Preparation of BiOI
[0012] Based on the original step (2), the addition of cadmium sulfide is removed, and then the operation is carried out in the same manner as the other steps after step (2) to finally obtain BiOI powder.
[0013] Preferably, the molar ratio of dissolved cadmium acetate and thiourea in step (1) is (1-2):(1-3), and the volume ratio of water to isopropanol in the mixed solution is 1:1.
[0014] Preferably, the stirring time of cadmium acetate in step (1) is 10 min, the stirring time of cadmium acetate and thiourea together is 20 min, the hydrothermal temperature is 120-180℃, and the standing time is 12 h.
[0015] Preferably, in step (2), the volume ratio of water to glycerol in the mixed solvent is 1:1, and the molar ratio of cadmium sulfide, bismuth nitrate, and potassium iodide is 0.276:(0.0125-0.2):(0.0125-0.2).
[0016] Preferably, the stirring time for cadmium sulfide in step (2) is 10 min, and the stirring time for adding bismuth nitrate and thiourea is 50 min.
[0017] Compared with the current technical solutions, the technical advantages of this invention are reflected in:
[0018] A BiOI / CdS heterojunction photocatalytic material was successfully prepared by combining a solvothermal method with a coprecipitation method. BiOI nanosheets were grown in situ on the surface of CdS microspheres to form an irregular spherical structure, constructing a heterostructure with excellent charge transport properties. Compared to single photocatalysts, the BiOI / CdS heterostructure not only exhibits superior visible light response but also effectively suppresses the recombination of photogenerated carriers, thereby significantly improving photocatalytic efficiency.
[0019] The photocatalytic degradation rate of malachite green by the BiOI / CdS heterojunction is 2.69 times that of CdS and 2.14 times that of BiOI, significantly improving the degradation rate of malachite green. Further free radical scavenging experiments revealed that superoxide radicals play a dominant role in the degradation process of malachite green. Attached Figure Description
[0020] Figure 1 The XRD patterns of CdS, BiOI / CdS, and BiOI prepared in Example 1 are shown.
[0021] Figure 2 The image shows an SEM image of CdS prepared in Example 1.
[0022] Figure 3 SEM image of BiOI / CdS prepared in Example 1.
[0023] Figure 4 SEM image of BiOI prepared in Example 1.
[0024] Figure 5 TEM image of BiOI / CdS prepared in Example 1.
[0025] Figure 6 The fluorescence spectra of CdS, BiOI / CdS, and BiOI prepared in Example 1 are shown.
[0026] Figure 7 The photocatalytic degradation curves of CdS, BiOI / CdS, and BiOI prepared in Example 1 are shown.
[0027] Figure 8 The photocatalytic degradation curves of CdS, BiOI / CdS, and BiOI after capture of active species prepared in Example 1 are shown. Detailed Implementation
[0028] To further clarify the technical details and implementation process of the present invention, the core content of the present invention will be explained and described in detail below with reference to specific embodiments:
[0029] Example 1
[0030] (1) Preparation of CdS
[0031] Accurately weigh 1 mmol of cadmium acetate and add it to a mixed solution of 10 ml deionized water and 10 ml isopropanol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Then, accurately weigh 1 mmol of thiourea and slowly add it to the above solution, continuing to stir for 20 min to obtain a stable precursor solution. Transfer the prepared precursor solution to a high-temperature reactor with a 30 ml liner, seal it, and place it in a preheated 120°C drying oven for 4 h. After the reaction, allow the reactor to cool naturally to room temperature, remove the product, and wash it repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry it in a 60°C electric thermostatic drying oven for 6 h to obtain CdS powder.
[0032] (2) Preparation of BiOI / CdS
[0033] Accurately weigh 0.276 mmol of cadmium sulfide and add it to a mixed solution consisting of 10 ml of deionized water and 10 ml of glycerol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Next, accurately weigh 0.05 mmol of bismuth nitrate and 0.05 mmol of potassium iodide and add them to the above mixed solution, and continue stirring for 50 min to obtain a homogeneous precursor solution. After stirring, let the solution stand for 12 h to allow BiOI precipitate to form naturally and precipitate completely. Finally, wash repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry in an electric thermostatic drying oven at 60 °C for 6 h to obtain BiOI / CdS powder.
[0034] (3) Preparation of BiOI
[0035] Based on the original step (2), the addition of cadmium sulfide is removed, and then the operation is carried out in the same manner as the other steps after step (2) to finally obtain BiOI powder.
[0036] Figure 1The XRD patterns of CdS, BiOI / CdS, and BiOI prepared in Example 1 are shown. The CdS sample exhibits distinct characteristic diffraction peaks at 25.325°, 26.766°, 28.283°, 44.139°, and 52.181°. These diffraction peaks correspond one-to-one with the (001), (002), (101), (200), and (212) crystal planes of the hexagonal CdS crystal, respectively. For the BiOI sample, the characteristic diffraction peaks appear at 29.497°, 31.546°, 37.084°, 45.201°, 51.119°, and 54.988°, respectively, corresponding to the (102), (110), (004), (200), (114), and (212) crystal planes of the tetragonal BiOI crystal, respectively. For the BiOI / CdS heterojunction, the characteristic diffraction peaks of CdS predominate. This is mainly attributed to the relatively low content of BiOI in the composite material, which weakens its crystal structure signal during overall characterization. Furthermore, the introduction of BiOI did not cause a significant shift in the position of the CdS diffraction peaks, confirming the good composite properties of CdS and BiOI.
[0037] Figure 2 The image shows a SEM image of CdS prepared in Example 1. The CdS particles are spherical with a diameter of about 1 μm, and the surface of the spheres is covered with a large number of tiny protrusions. Due to their high surface energy, the CdS particles are prone to agglomeration, forming clusters.
[0038] Figure 3 The image shows a SEM image of the BiOI / CdS prepared in Example 1. The BiOI / CdS heterojunction retains a clustered appearance similar to CdS. This indicates that BiOI nanosheets are directly grown on the surface of the CdS cluster structure, forming a unique heterostructure.
[0039] Figure 4 The image shows a SEM image of the BiOI prepared in Example 1. BiOI exhibits an irregular spherical structure assembled from nanosheets, with an average diameter of approximately 1 μm. Furthermore, BiOI demonstrates good dispersibility, with virtually no particle adhesion.
[0040] Figure 5 The image shows a TEM image of the BiOI / CdS prepared in Example 1. The central region is a solid structure, with BiOI nanosheets growing orderly on the surface of CdS microspheres. High-resolution transmission electron microscopy revealed that a lattice spacing of 0.299 nm corresponds to the (102) crystal plane of BiOI, while a lattice spacing of 0.318 nm corresponds to the (101) crystal plane of CdS. This demonstrates the successful preparation of the BiOI / CdS heterojunction.
[0041] Figure 6The fluorescence spectra of CdS, BiOI / CdS, and BiOI prepared in Example 1 are shown. The emission diffraction peak intensity of the BiOI / CdS heterojunction is significantly lower than that of pure CdS and BiOI. Therefore, it can be reasonably inferred that the addition of BiOI can effectively suppress the recombination of photogenerated carriers.
[0042] Figure 7 The photocatalytic degradation curves of CdS, BiOI / CdS, and BiOI prepared in Example 1 show that, with an irradiation time of 20 min, BiOI achieved a degradation rate of 84.74% for malachite green, CdS achieved a degradation rate of 82.83% for malachite green, while the BiOI / CdS heterojunction achieved a degradation rate as high as 96.06% for malachite green, which is 2.69 times that of CdS and 2.14 times that of BiOI.
[0043] Figure 8 The photocatalytic degradation curves of CdS, BiOI / CdS, and BiOI prepared in Example 1 after capturing active species were obtained. Disodium ethylenediaminetetraacetate, isopropanol, and p-benzoquinone were introduced to capture h, respectively. + ·OH and ·O2 - When disodium ethylenediaminetetraacetate and p-benzoquinone were added to the system, the degradation efficiency of malachite green by the BiOI / CdS composite material showed a significant decreasing trend; among them, p-benzoquinone had a particularly prominent inhibitory effect, leading to a significant reduction in the degradation rate. In stark contrast, the photocatalytic activity of the material remained basically unchanged after the addition of isopropanol, a phenomenon that fully demonstrates the influence of O2. - It is the key active species that dominates the degradation of malachite green in BiOI / CdS heterojunction and plays a decisive role in the photocatalytic reaction.
[0044] Example 2
[0045] (1) Preparation of CdS
[0046] Accurately weigh 2 mmol of cadmium acetate and add it to a mixed solution of 10 ml deionized water and 10 ml isopropanol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Then, accurately weigh 3 mmol of thiourea and slowly add it to the above solution, continuing to stir for 20 min to obtain a stable precursor solution. Transfer the prepared precursor solution to a high-temperature reactor with a 30 ml liner, seal it, and place it in a preheated 180°C drying oven for 4 h. After the reaction, allow the reactor to cool naturally to room temperature, remove the product, and wash it repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry it in a 60°C electric thermostatic drying oven for 6 h to obtain CdS powder.
[0047] (2) Preparation of BiOI / CdS
[0048] Accurately weigh 0.276 mmol of cadmium sulfide and add it to a mixed solution consisting of 10 ml of deionized water and 10 ml of glycerol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Next, accurately weigh 0.2 mmol of bismuth nitrate and 0.2 mmol of potassium iodide and add them to the above mixed solution, and continue stirring for 50 min to obtain a homogeneous precursor solution. After stirring, let the solution stand for 12 h to allow BiOI precipitate to form naturally and precipitate completely. Finally, wash repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry in an electric thermostatic drying oven at 60 °C for 6 h to obtain BiOI / CdS powder.
[0049] (3) Preparation of BiOI
[0050] Based on the original step (2), the addition of cadmium sulfide is removed, and then the operation is carried out in the same manner as the other steps after step (2) to finally obtain BiOI powder.
[0051] Example 3
[0052] (1) Preparation of CdS
[0053] Accurately weigh 1 mmol of cadmium acetate and add it to a mixed solution of 10 ml deionized water and 10 ml isopropanol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Then, accurately weigh 1 mmol of thiourea and slowly add it to the above solution, continuing to stir for 20 min to obtain a stable precursor solution. Transfer the prepared precursor solution to a high-temperature reactor with a 30 ml liner, seal it, and place it in a preheated 120°C drying oven for 4 h. After the reaction, allow the reactor to cool naturally to room temperature, remove the product, and wash it repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry it in a 60°C electric thermostatic drying oven for 6 h to obtain CdS powder.
[0054] (2) Preparation of BiOI / CdS
[0055] Accurately weigh 0.276 mmol of cadmium sulfide and add it to a mixed solution consisting of 10 ml of deionized water and 10 ml of glycerol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Next, accurately weigh 0.1 mmol of bismuth nitrate and 0.1 mmol of potassium iodide and add them to the above mixed solution, and continue stirring for 50 min to obtain a homogeneous precursor solution. After stirring, let the solution stand for 12 h to allow BiOI precipitate to form naturally and precipitate completely. Finally, wash repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry in an electric thermostatic drying oven at 60 °C for 6 h to obtain BiOI / CdS powder.
[0056] (3) Preparation of BiOI
[0057] Based on the original step (2), the addition of cadmium sulfide is removed, and then the operation is carried out in the same manner as the other steps after step (2) to finally obtain BiOI powder.
[0058] Example 4
[0059] (1) Preparation of CdS
[0060] Accurately weigh 1 mmol of cadmium acetate and add it to a mixed solution of 10 ml deionized water and 10 ml isopropanol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Then, accurately weigh 1 mmol of thiourea and slowly add it to the above solution, continuing to stir for 20 min to obtain a stable precursor solution. Transfer the prepared precursor solution to a high-temperature reactor with a 30 ml liner, seal it, and place it in a preheated 120°C drying oven for 4 h. After the reaction, allow the reactor to cool naturally to room temperature, remove the product, and wash it repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry it in a 60°C electric thermostatic drying oven for 6 h to obtain CdS powder.
[0061] (2) Preparation of BiOI / CdS
[0062] Accurately weigh 0.276 mmol of cadmium sulfide and add it to a mixed solution consisting of 10 ml of deionized water and 10 ml of glycerol. Stir with a magnetic stirrer at an appropriate speed for 10 min. Next, accurately weigh 0.0125 mmol of bismuth nitrate and 0.0125 mmol of potassium iodide and add them to the above mixed solution, and continue stirring for 50 min to obtain a homogeneous precursor solution. After stirring, let the solution stand for 12 h to allow BiOI precipitate to form naturally and precipitate completely. Finally, wash repeatedly with alternating ethanol and deionized water to thoroughly remove residual impurities. Finally, dry in an electric thermostatic drying oven at 60 °C for 6 h to obtain BiOI / CdS powder.
[0063] (3) Preparation of BiOI
[0064] Based on the original step (2), the addition of cadmium sulfide is removed, and then the operation is carried out in the same manner as the other steps after step (2) to finally obtain BiOI powder.
Claims
1. A method for preparing a BiOI / CdS heterojunction photocatalytic material, characterized in that, Includes the following steps: (1) Preparation of CdS: Cadmium acetate was dispersed in a mixed solution of water and isopropanol and stirred until it was completely dissolved. Thiourea was then added to the solution and stirring was continued to obtain a stable precursor solution. The solution was then transferred to a high-temperature reactor with a liner and subjected to hydrothermal reaction in an electrically heated constant-temperature drying oven. After the reaction was complete, the solution was allowed to cool naturally and washed several times with ethanol and water. Finally, the solution was dried to obtain CdS powder. (2) Preparation of BiOI / CdS: Cadmium sulfide was dispersed in a mixed solution of water and glycerol and stirred thoroughly until completely dissolved. Then, bismuth nitrate and potassium iodide were added to the mixed solution simultaneously and stirred continuously until a homogeneous precursor solution was obtained. The solution was allowed to stand for a period of time to facilitate the natural formation of precipitate. The solution was washed several times with ethanol and water and finally dried to obtain BiOI / CdS powder. (3) Preparation of BiOI: Based on the original step (2), the addition of cadmium sulfide is removed, and then the operation is carried out in the same manner as the other steps after step (2) to finally obtain BiOI powder. 2.The method for preparing BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: In step (1), the molar ratio of dissolved cadmium acetate and thiourea is (1-2):(1-3), and the volume ratio of water and isopropanol in the mixed solution is 1:
1.
3. The method for preparing the BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: In step (1), the stirring time of cadmium acetate is 10 min, the stirring time of cadmium acetate and thiourea is 20 min, the hydrothermal temperature is 120-180℃, and the standing time is 12 h.
4. The method for preparing the BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: In step (2), the volume ratio of water to glycerol in the mixed solvent is 1:1, and the molar ratio of cadmium sulfide, bismuth nitrate, and potassium iodide is 0.276:(0.0125-0.2):(0.0125-0.2). 5.The method for preparing BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: In step (2), the stirring time for cadmium sulfide is 10 min, and the stirring time for adding bismuth nitrate and thiourea is 50 min. 6.The method for preparing BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: • O2 - is the main active species in photocatalysis.
7. The method for preparing the BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: CdS particles were synthesized by hydrothermal method, and then BiOI was grown in situ on the CdS particles by co-precipitation method. 8.The method for preparing the BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: Application of BiOI / CdS heterojunction photocatalytic materials in the photocatalytic degradation of malachite green.
9. The method for preparing the BiOI / CdS heterojunction photocatalytic material according to claim 1, characterized in that: The photocatalytic degradation rate of malachite green by BiOI / CdS is 2.69 times that of CdS and 2.14 times that of BiOI.