A catalyst preparation process for use in microchannel ammonia decomposition reactors
By coating the inner wall of the microreactor with an inorganic oxide film carrier and loading it with Ru and K additives, the problems of temperature drop and heat transfer efficiency in the ammonia decomposition equipment were solved, and a highly efficient ammonia decomposition hydrogen production reaction was achieved.
Patent Information
- Application Number
- CN202510604056.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ammonia decomposition hydrogen production equipment is large in size, and the uneven temperature distribution in the catalyst bed caused by temperature drop results in low utilization of precious metal active components and low heat transfer efficiency, making it difficult to meet the requirements of efficient ammonia decomposition.
An inorganic oxide film carrier is formed on the inner wall of the microreactor using a coating process, and the active component Ru and the additives K and Cs are loaded to form a catalyst coating, which improves the uniformity of the distribution of active components and the heat transfer efficiency.
The uniformly distributed catalyst coating improves catalyst utilization and operational flexibility of ammonia decomposition equipment, reduces the impact of temperature drop, and is suitable for efficient ammonia decomposition to hydrogen production reactions.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of ammonia decomposition for hydrogen production technology, and in particular to a catalyst preparation process for use in a microchannel ammonia decomposition reactor. Background Technology
[0002] Hydrogen energy is a widely available, clean, carbon-free, flexible, efficient, and versatile secondary energy source, making it an ideal interconnecting medium for promoting the clean and efficient utilization of traditional fossil fuels and supporting the large-scale development of renewable energy. However, the primary challenge to achieving large-scale hydrogen energy application is the storage and transportation of hydrogen. Hydrogen is highly flammable, has a wide range of explosion limits, and is prone to "hydrogen embrittlement." Furthermore, hydrogen has a low volumetric energy density, making its storage and transportation a pressing issue that needs to be addressed.
[0003] Ammonia possesses high energy density and a high hydrogen storage capacity by weight, with hydrogen comprising 17.7% by mass. Its decomposition produces only nitrogen and hydrogen, without generating COx greenhouse gases. Ammonia is highly compressible, ensuring safe storage and transportation. Its lower density than air means that leaks do not accumulate and diffuse rapidly, offering significant safety. Furthermore, ammonia synthesis technology is mature, and ammonia is inexpensive. Therefore, ammonia, as a hydrogen carrier, represents a promising application for converting hydrogen storage and transportation into ammonia storage and transportation, particularly through ammonia decomposition for hydrogen production.
[0004] Current research on ammonia decomposition catalysts mainly focuses on metals such as ruthenium (Ru), iridium (Ir), nickel (Ni), cobalt (Co), and iron (Fe). Among these, Ru-based catalysts exhibit the highest activity, with their catalytic performance at low temperatures far exceeding that of other non-precious metal-based catalysts. Currently, the Ru-based catalysts developed all maintain high loading levels. However, as Ru is a precious metal, high loading undoubtedly increases the cost of the catalyst. Therefore, how to improve the low-temperature activity of low Ru loading is a problem that needs to be solved in the field of ammonia decomposition.
[0005] Current research on ammonia decomposition catalysts mainly focuses on low-temperature, high-activity catalysts. These catalysts primarily use Ru as the active component, with most having a loading of around 100 mg. Their thermal effect is relatively small. However, for future applications of ammonia decomposition to be practically viable, a hydrogen production rate of at least 10–50 kg / h is required. Therefore, minimizing the temperature drop caused by the endothermic reaction and maximizing the catalytic efficiency of the active component Ru is crucial. The reaction equation for the decomposition of ammonia into hydrogen is as follows:
[0006] NH3→1 / 2N2+3 / 2H2ΔH 25℃ =46kJ / mol
[0007] Existing ammonia decomposition hydrogen production reactors mostly employ pyrolysis furnaces. For example, Chinese patent document CN205011382U discloses an ammonia decomposition hydrogen production device, including a shell, a heat exchanger, and a decomposition furnace. By exchanging heat between a high-temperature hydrogen-nitrogen mixture and gaseous ammonia in the heat exchanger, the temperature of the ammonia entering the decomposition furnace is increased, which is beneficial for the decomposition of gaseous ammonia. Another example is Chinese patent document CN210528460U, which discloses an ammonia decomposition hydrogen production apparatus, including a heat exchanger, a pyrolysis furnace, a cooler, and two dryers. The dryers can be regenerated using either hydrogen purging or nitrogen, offering greater flexibility. However, using a pyrolysis furnace has disadvantages such as large size and low heat transfer efficiency.
[0008] Microreactors have broad application prospects due to their small size, high heat transfer efficiency, short response time, and uniform temperature distribution. How to provide a microchannel reactor for ammonia decomposition with simple structure, high uniformity of flow rate and concentration distribution, and low fluid flow pressure has become a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0009] In view of the aforementioned deficiencies in the prior art, the technical problem to be solved by the present invention is to address the issues of large volume and uneven temperature distribution in the catalyst bed due to temperature drop, which in turn affects the low utilization rate of precious metal active components in existing ammonia decomposition hydrogen production reactors. The present invention provides a modular component integrating an ammonia decomposition microchannel reactor and catalyst, improving the utilization rate of existing catalysts and the operational flexibility of ammonia decomposition equipment. Due to limitations in pipe diameter and gas velocity, commonly used fixed-bed catalyst loading methods result in excessive pressure drop, affecting long-term operation of the equipment and are unsuitable for microreactor conditions. Therefore, the present invention employs a coating process for catalyst addition.
[0010] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0011] This invention provides a method for preparing a catalyst for use in a microchannel ammonia decomposition reactor, comprising the following steps:
[0012] S1 Select a microreactor inner tube of appropriate specifications as needed; calculate the amount of inorganic oxide film carrier to be coated based on the inner surface area of the inner tube, and then calculate the amount of active component based on the mass of the inorganic oxide film carrier.
[0013] S2 is used for pretreatment of the microreactor to remove impurities such as dust and grease from the tube wall;
[0014] S3 prepares a coating solution, then coats the coating solution onto the inner wall of the pretreated microreactor metal tube and then calcines it to grow an inorganic oxide film carrier.
[0015] S4 is obtained by impregnating the loaded active component on an inorganic oxide membrane support to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0016] Preferably, the coating amount of the inorganic oxide film carrier in step S1 is 140-180 g / m³. 2 .
[0017] Preferably, the microreactor in step S2 is made of metal; more preferably, the microreactor is made of a single metal or a composite metal; the single metal includes copper and aluminum; the composite metal includes stainless steel; selecting a metal microreactor can improve the heat transfer efficiency of the reaction process.
[0018] Preferably, the reactor is a hollow microchannel reactor, and more preferably a metal tubular reactor. The inner diameter is determined based on the required heat calculated according to the space velocity and conversion rate during the ammonia decomposition process, and the appropriate tube diameter is determined according to the heat transfer area and thermal conductivity. The inner diameter ranges from 0.5 to 3.0 mm, preferably from 1.0 to 2.0 mm.
[0019] Preferably, the pretreatment method in step S2 is one of chemical corrosion or sandblasting.
[0020] Preferably, the pretreatment method is chemical corrosion, which involves cleaning the tube wall with hot alkaline solution, rinsing it with deionized water, corroding the inner wall of the tube with acid solution, rinsing it with deionized water, and then drying it. This pretreatment step can improve the bonding strength between the catalyst and the tube wall of the microreactor.
[0021] More preferably, the hot alkaline solution is one of a hot sodium hydroxide aqueous solution or a hot potassium hydroxide aqueous solution; the concentration of the alkaline solution is 0.1 to 1.0 mol / L, and most preferably 0.2 to 0.5 mol / L.
[0022] More preferably, the acid solution is one of dilute nitric acid aqueous solution and dilute hydrochloric acid aqueous solution; the concentration of the acid solution is 0.01-0.2 mol / L, and most preferably 0.05-0.1 mol / L.
[0023] Preferably, the coating solution in step S2 is one or a mixture of aluminum sol, silica sol, and titanium dioxide sol.
[0024] Preferably, the coating solution is an aluminum sol, more preferably an acidic aluminum sol or a neutral aluminum sol; the pH value of the acidic aluminum sol is 2-3; the pH value of the neutral aluminum sol is 7-8; the most preferred coating solution is a neutral aluminum sol; the solid content of the neutral aluminum sol is 2-10%; if the aluminum sol concentration is too high, the coating solution is too viscous and is not suitable for coating the capillary tube, and an appropriate aluminum sol concentration can be selected according to the diameter of the micro-reaction metal tube.
[0025] Preferably, the coating process in step S3 is as follows: high-pressure gas is used to spray the coating liquid onto the inner wall of the metal tube of the microreactor. During the coating process, the gas is continuously purged. The total amount of coating liquid is added in batches according to the calculated total amount. During the spraying process, the coating liquid at the outlet is recovered and reused. After the coating is completed, the coating liquid is dried by gas.
[0026] Preferably, the calcination process in step S3 is as follows: first, the coated microreactor metal tube is dried at 80-150°C for 2-6 hours, and then the dried metal tube is calcined at 450-600°C in an inert atmosphere for 2-6 hours; more preferably, the drying temperature is 100-120°C and the drying time is 3-5 hours; the calcination temperature is 500-550°C and the tube is calcined for 3-5 hours; after calcination, the tube is cooled and weighed to calculate the actual mass of the carrier.
[0027] Preferably, the impregnation loading of the active component in step S4 is as follows: the precursor of the active component is dissolved in water to obtain an impregnation solution. During the impregnation process, the impregnation solution is sprayed onto the inner wall of the metal tube using gas. Excess impregnation solution is recovered and re-sprayed during the impregnation process until the impregnation solution is completely loaded onto the inorganic oxide carrier. Then, the carrier is dried by gas, and then dried and calcined.
[0028] More preferably, the active component includes the noble metal Ru and the non-noble metal Ni; the amount of the active component is 1.5-2.5% of the carrier mass.
[0029] More preferably, the active component further includes an active adjuvant, which is a compound containing K, N, and Cs elements, and the amount of the active adjuvant is 4-6% of the carrier mass; the active adjuvant can improve the activity of the active component.
[0030] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0031] 1. In this invention, an inorganic oxide film generated by coating is uniformly distributed on the inner wall of a metal tube as a carrier for the active components of the catalyst. Compared with a single hollow microreactor, the high specific surface area of the inorganic oxide film can effectively improve the distribution of active components and prevent the agglomeration of active components of the catalyst during high-temperature reaction. At the same time, since there are no gaps between the inorganic oxide film and the metal tube wall, its heat transfer efficiency is significantly higher than that of the fixed-bed catalytic system with traditional packing method. For the ammonia decomposition reaction with significant endothermic effect, the reaction process can minimize the situation where some catalysts fail to exert their due catalytic effect due to temperature drop.
[0032] 2. This invention improves the utilization rate of existing catalysts and the operational flexibility of ammonia decomposition equipment by integrating a microchannel reactor and catalyst coating. It can be applied to ammonia decomposition hydrogen production reaction systems, as well as other reaction systems with large thermal effects. Detailed Implementation
[0033] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0034] In practical use, the metal tubes in the microreactor have plasticity in shape, so they can be shaped into any shape as needed, including straight tubes, annular spiral bends, and S-shaped winding methods. The present invention will be further described below with reference to a straight tube example.
[0035] Example 1
[0036] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0037] S1 uses a stainless steel tube with an inner diameter of 1.0 mm and a length of 2.0 m, with an inner surface area of 6.28 × 10⁻⁶. -3 m 2 The theoretical value for coating an alumina film is calculated as 1.0 g, and the Ru loading is 2% of the alumina content, specifically 2.0 × 10⁻⁶ g. -2 g, the loading of K2O is 5% of alumina, specifically 5 × 10 g. -2 g;
[0038] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 0.2mol / L sodium hydroxide solution was used for 5 irrigations and cleanings. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.1mol / L nitric acid was used for 5 irrigations and acid washings. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Finally, the tube was dried by gas purging.
[0039] S3 prepares 20g of neutral aluminum sol with an alumina content of 5%, and then sprays the prepared aluminum sol solution onto the inner wall of stainless steel through gas. The outlet of the stainless steel pipe is equipped with a recovery device to recover the excess aluminum sol solution from a single coating and re-spray it until the entire inner wall of the pipe is coated. The pipe is then dried with air. After coating, the stainless steel pipe is dried at 120℃ for 4 hours and calcined at 500℃ for 4 hours, resulting in a uniform active alumina film on the inner wall.
[0040] S4 weighed 0.0517g of hydrated ruthenium trichloride (containing 37% ruthenium) and determined that the water absorption rate of alumina was 0.6gH2O / gAl2O3. The weighed hydrated ruthenium trichloride was dissolved in 1.2g of deionized water. After being dissolved evenly, the solution of the active component ruthenium was sprayed onto the inner wall of the stainless steel tube multiple times through gas. Excess solution was sprayed repeatedly until it was completely loaded onto the alumina film. It was then dried with gas, dried at 120℃ for 4 hours, and calcined at 500℃ for 4 hours.
[0041] S5 Weigh 0.0734g K2CO3, dissolve it in 1.2g water to prepare K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times by gas. Repeat the spraying of excess solution until the entire solution is loaded onto the coating of the precious metal ruthenium. Then dry it with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0042] Example 2
[0043] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0044] S1 uses a stainless steel tube with an inner diameter of 3.0mm and a length of 2.0m, with an inner surface area of 18.84×10. -3 m 2 The theoretical value for coating an alumina film is 3.0g, and the Ru loading is 2% of the alumina, specifically 6.0 × 10⁻⁶. -2 g, the loading of K2O is calculated as 5% of alumina, specifically 0.15g;
[0045] For the cleaning and pretreatment of the inner wall of the S2 metal tube, firstly, 0.1L of 0.2mol / L sodium hydroxide solution was used for 5 irrigations. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.1mol / L nitric acid was used for 5 irrigations. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was dried by gas purging.
[0046] S3 prepared 30g of neutral aluminum sol with an alumina content of 10%, and then sprayed the prepared aluminum sol solution onto the inner wall of stainless steel through gas. The stainless steel pipe outlet is equipped with a recovery device to recover the excess aluminum sol solution from a single coating and re-spray until the entire inner wall of the pipe is coated. The pipe is then dried with air. The coated stainless steel pipe is dried at 150°C for 4 hours and then calcined at 600°C for 4 hours, resulting in a uniform active alumina film on the inner wall.
[0047] S4 weighed 0.1551g of hydrated ruthenium trichloride (containing 37% ruthenium) and determined that the water absorption rate of alumina was 0.6gH2O / gAl2O3. The weighed hydrated ruthenium trichloride was dissolved in 3.6g of deionized water. After being dissolved evenly, the solution of the active component ruthenium was sprayed onto the inner wall of the stainless steel tube multiple times by gas. Excess solution was sprayed repeatedly until it was completely loaded onto the alumina film. It was then dried with gas, dried at 120℃ for 4 hours, and calcined at 500℃ for 4 hours.
[0048] S5 Weigh 0.2201g K2CO3, dissolve it in 3.6g water to prepare a K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times using gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the ruthenium coating. Then dry it with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0049] Example 3
[0050] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0051] S1 uses a stainless steel tube with an inner diameter of 1.5mm and a length of 2.0m, with an inner surface area of 9.42×10⁻⁶. -3 m 2 The theoretical value for coating an alumina film is calculated as 1.5g, and the Ru loading is calculated as 2% of the alumina content, specifically 3.0 × 10⁻⁶. -2 The K₂O loading is calculated as 5% of the alumina content, specifically 7.5 × 10⁻⁶ g. -2 g;
[0052] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 1.0mol / L sodium hydroxide solution was used for 5 irrigations and cleanings. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.2mol / L nitric acid was used for 5 irrigations and acid washings. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was dried by gas purging.
[0053] S3 prepared 15g of neutral aluminum sol with an alumina content of 10%, and then sprayed the prepared aluminum sol solution onto the inner wall of stainless steel through gas. The stainless steel pipe outlet is equipped with a recovery device to recover the excess aluminum sol solution from a single coating and re-spray until the entire inner wall of the pipe is coated. The pipe is then dried with air. The coated stainless steel pipe is dried at 120℃ for 4 hours and then calcined at 500℃ for 4 hours, resulting in a uniform active alumina film on the inner wall.
[0054] S4 weighed 0.0776g of hydrated ruthenium trichloride (containing 37% ruthenium) and determined that the water absorption rate of alumina was 0.6gH2O / gAl2O3. The weighed hydrated ruthenium trichloride was dissolved in 1.8g of deionized water. After being dissolved evenly, the solution of the active component ruthenium was sprayed onto the inner wall of the stainless steel tube multiple times by gas. Excess solution was sprayed repeatedly until it was completely loaded onto the alumina film. It was then dried with gas, dried at 120℃ for 4 hours, and calcined at 500℃ for 4 hours.
[0055] S5 Weigh 0.1101g K2CO3, dissolve it in 1.8g water to prepare a K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times using gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the ruthenium coating. Then, blow it dry with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0056] Example 4
[0057] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0058] S1 uses a stainless steel tube with an inner diameter of 0.5mm and a length of 2.0m, with an inner surface area of 3.14×10⁻⁶. -3 m 2 The theoretical value for coating an alumina film is calculated as 0.5g, and the Ru loading is calculated as 2% of the alumina content, specifically 1.0 × 10⁻⁶. -2 The K₂O loading is calculated as 5% of the alumina content, specifically 2.5 × 10⁻⁶ g. -2 g;
[0059] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 0.2mol / L potassium hydroxide solution was used for 5 irrigations and cleanings. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.1mol / L hydrochloric acid was used for 5 irrigations and acid washings. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was dried by gas purging.
[0060] S3 prepared 20g of neutral aluminum sol with an alumina content of 2.5%, and then sprayed the prepared aluminum sol solution onto the inner wall of stainless steel through gas. The stainless steel pipe outlet is equipped with a recovery device to recover the excess aluminum sol solution from a single coating and re-spray it until the entire inner wall of the pipe is coated. The pipe is then dried with air. After coating, the stainless steel pipe is dried at 120℃ for 5 hours and then calcined at 500℃ for 5 hours, resulting in a uniform active alumina film on the inner wall.
[0061] S4 Weigh 0.0259g of hydrated ruthenium trichloride (containing 37% ruthenium) and determine that the water absorption rate of alumina is 0.6gH2O / gAl2O3. Dissolve the weighed hydrated ruthenium trichloride in 0.6g of deionized water. After the solution is evenly dissolved, spray the solution of the active component ruthenium multiple times onto the inner wall of a stainless steel tube through gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the alumina film. Then, blow dry with gas, dry at 120℃ for 4 hours, and calcine at 500℃ for 4 hours.
[0062] S5 Weigh 0.0367g K2CO3, dissolve it in 0.6g water to prepare a K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times using gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the ruthenium coating. Then dry it with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0063] Example 5
[0064] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0065] S1 uses a stainless steel tube with an inner diameter of 3.0mm and a length of 2.0m, with an inner surface area of 18.84×10. -3 m 2 The theoretical value for coating an alumina film is 3.0g, and the Ru loading is 2% of the alumina, specifically 6.0 × 10⁻⁶. -2 g, the loading of K2O is 5% of alumina, specifically 15 × 10 g. -2 g, the specific steps include:
[0066] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 0.5mol / L sodium hydroxide solution was used for 5 irrigations and cleanings. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.2L of 0.2mol / L nitric acid was used for 5 irrigations and acid washings. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was dried by gas purging.
[0067] S3 prepared 30g of neutral aluminum sol with an alumina content of 10%, and then sprayed the prepared aluminum sol solution onto the inner wall of stainless steel through gas. The stainless steel pipe outlet is equipped with a recovery device to recover the excess aluminum sol solution from a single coating and re-spray until the entire inner wall of the pipe is coated. The pipe is then dried with air. After coating, the stainless steel pipe is dried at 120℃ for 6 hours and calcined at 600℃ for 5 hours, resulting in a uniform active alumina film on the inner wall.
[0068] S4 weighed 0.1551g of hydrated ruthenium trichloride (containing 37% ruthenium) and determined that the water absorption rate of alumina was 0.6gH2O / gAl2O3. The weighed hydrated ruthenium trichloride was dissolved in 3.6g of deionized water. After being dissolved evenly, the solution of the active component ruthenium was sprayed onto the inner wall of the stainless steel tube multiple times using gas. Excess solution was sprayed repeatedly until it was completely loaded onto the alumina film. The solution was then dried with gas, dried at 120℃ for 6 hours, and calcined at 500℃ for 6 hours.
[0069] S5 Weigh 0.2201g K2CO3 and dissolve it in 3.6g water to prepare a K2O aqueous solution. Spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times using gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the ruthenium coating. Then, blow it dry with gas, dry it at 120°C for 6 hours, and calcine it at 500°C for 6 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0070] Example 6
[0071] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0072] S1 uses a stainless steel tube with an inner diameter of 1.0 mm and a length of 2.0 m, with an inner surface area of 6.28 × 10⁻⁶. -3 m 2 The theoretical value for coating with silica film is calculated as 1.0g, and the Ru loading is calculated as 2% of the silica, specifically 2.0 × 10⁻⁶. -2 g, the loading of K2O is 5% of alumina, specifically 5 × 10 g. -2 g,
[0073] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 0.5mol / L sodium hydroxide solution was used for 5 irrigations and cleanings. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.2mol / L nitric acid was used for 5 irrigations and acid washings. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was dried by gas purging.
[0074] S3 prepares 20g of silica sol with a silica content of 5%, and then sprays the prepared silica sol solution onto the inner wall of stainless steel through gas. The outlet of the stainless steel pipe is equipped with a recovery device to recover the excess silica sol solution from a single coating and re-spray it until the entire inner wall of the pipe is coated. Then it is dried with air. The coated stainless steel pipe is dried at 120°C for 4 hours and calcined at 500°C for 4 hours, resulting in a uniform silica film on the inner wall.
[0075] S4 weighed 0.0517g of hydrated ruthenium trichloride (containing 37% ruthenium) and determined that the water absorption rate of silica was 0.7gH2O / gSiO2. The weighed hydrated ruthenium trichloride was dissolved in 1.4g of deionized water. After being dissolved evenly, the solution of the active component ruthenium was sprayed onto the inner wall of the stainless steel tube multiple times using gas. Excess solution was sprayed repeatedly until it was completely loaded onto the silica film. It was then dried with gas, dried at 120℃ for 4 hours, and calcined at 500℃ for 4 hours.
[0076] S5 Weigh 0.0734g K2CO3, dissolve it in 1.4g water to prepare a K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times using gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the ruthenium coating. Then dry it with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0077] Example 7
[0078] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0079] S1 uses a stainless steel tube with an inner diameter of 1.0 mm and a length of 2.0 m, with an inner surface area of 6.28 × 10⁻⁶. -3 m 2 The theoretical value for coating a titanium dioxide film is calculated as 1.0 g, and the Ru loading is 2% of the titanium dioxide, specifically 2.0 × 10⁻⁶ g. -2 g, the loading of K2O is 5% of titanium dioxide, specifically 5 × 10 g. -2 g, the specific steps include:
[0080] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 0.2mol / L sodium hydroxide solution was used for 5 irrigations and cleanings. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.1mol / L nitric acid was used for 5 irrigations and acid washings. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was dried by gas purging.
[0081] S3 prepared 20g of titanium sol with a titanium dioxide content of 5%, and then sprayed the prepared titanium sol solution onto the inner wall of stainless steel through gas. The stainless steel pipe outlet is equipped with a recovery device to recover the excess titanium sol solution from a single coating and re-spray it until the entire inner wall of the pipe is coated. The pipe is then dried with air. The coated stainless steel pipe is dried at 120°C for 4 hours and calcined at 500°C for 4 hours, resulting in a uniform active titanium dioxide film on the inner wall.
[0082] S4 weighed 0.0517g of hydrated ruthenium trichloride (containing 37% ruthenium) and determined that the water absorption rate of titanium dioxide was 0.5gH2O / gTiO2. The weighed hydrated ruthenium trichloride was dissolved in 1.0g of deionized water. After being dissolved evenly, the solution of the active component ruthenium was sprayed onto the inner wall of the stainless steel tube multiple times using gas. Excess solution was sprayed repeatedly until it was completely loaded onto the alumina film. The solution was then dried with gas, dried at 120℃ for 4 hours, and calcined at 500℃ for 4 hours.
[0083] S5 Weigh 0.0734g K2CO3, dissolve it in 1.0g water to prepare a K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times using gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the ruthenium coating. Then, blow it dry with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0084] Example 8
[0085] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0086] S1 uses a copper tube with an inner diameter of 1.0 mm and a length of 2.0 m, with an inner surface area of 6.28 × 10⁻⁶. -3 m 2 The theoretical value for coating an alumina film is calculated as 1.0 g, and the Ru loading is 2% of the alumina content, specifically 2.0 × 10⁻⁶ g. -2 g, the loading of K2O is 5% of alumina, specifically 5 × 10 g. -2 g, the specific steps include:
[0087] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 0.1mol / L sodium hydroxide solution was used for 5 irrigations and cleanings. The cleaning solution was injected into the tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.01mol / L nitric acid was used for 5 irrigations and acid washings. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was purged and dried by gas purging.
[0088] S3 prepares 20g of neutral aluminum sol with an alumina content of 5%, and then sprays the prepared aluminum sol solution onto the inner wall of the tube through gas. The tube outlet is equipped with a recovery device to recover the excess aluminum sol solution from a single coating and re-spray it until the entire inner wall of the tube is coated. The tube is then dried with air. The coated aluminum tube is dried at 120℃ for 4 hours and then calcined at 500℃ for 4 hours, resulting in a uniform active alumina film on the inner wall.
[0089] S4 weighed 0.0517g of hydrated ruthenium trichloride (containing 37% ruthenium) and determined that the water absorption rate of alumina was 0.6gH2O / gAl2O3. The weighed hydrated ruthenium trichloride was dissolved in 1.2g of deionized water. After being dissolved evenly, the solution of the active component ruthenium was sprayed onto the inner wall of the tube multiple times using gas. Excess solution was sprayed repeatedly until it was completely loaded onto the alumina film. The film was then dried with gas, dried at 120℃ for 4 hours, and calcined at 500℃ for 4 hours.
[0090] S5 Weigh 0.0734g K2CO3, dissolve it in 1.2g water to prepare K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times by gas. Repeat the spraying of excess solution until the entire solution is loaded onto the coating of the precious metal ruthenium. Then dry it with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0091] Example 9
[0092] A method for preparing a catalyst for use in a microchannel ammonia decomposition reactor includes the following steps:
[0093] S1 uses an aluminum tube with an inner diameter of 1.0mm and a length of 2.0m, with an inner surface area of 6.28×10. -3 m 2 The theoretical value for coating an alumina film is calculated as 1.0 g, and the Ru loading is 2% of the alumina content, specifically 2.0 × 10⁻⁶ g. -2 g, the loading of K2O is 5% of alumina, specifically 5 × 10 g. -2 g, the specific steps include:
[0094] For the pretreatment of the inner wall of the metal tube of the S2 microreactor, firstly, 0.1L of 0.1mol / L sodium hydroxide solution was used for 4 irrigations. The cleaning solution was added to the stainless steel tube by gas purging. Then, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, 0.1L of 0.01mol / L nitric acid was used for 5 irrigations. After acid washing, deionized water was used for cleaning until the pH value of the washing solution was neutral. Then, the tube was dried by gas purging.
[0095] S3 prepares 20g of neutral aluminum sol with an alumina content of 5%, and then sprays the prepared aluminum sol solution onto the inner wall of the aluminum tube through gas. The aluminum tube outlet is equipped with a recovery device to recover the excess aluminum sol solution from a single coating and re-spray it until the entire inner wall of the tube is coated. The tube is then dried with air. The coated aluminum tube is dried at 120℃ for 4 hours and then calcined at 500℃ for 4 hours, resulting in a uniform active alumina film on the inner wall.
[0096] S4 Weigh 0.0517g of hydrated ruthenium trichloride (containing 37% ruthenium) and determine that the water absorption rate of alumina is 0.6gH2O / gAl2O3. Dissolve the weighed hydrated ruthenium trichloride in 1.2g of deionized water. After the solution is evenly dissolved, spray the solution of the active component ruthenium multiple times onto the inner wall of the aluminum tube using gas. Repeat the spraying process for any excess solution until the entire solution is loaded onto the alumina film. Then, blow dry with gas, dry at 120℃ for 4 hours, and calcine at 500℃ for 4 hours.
[0097] S5 Weigh 0.0734g K2CO3, dissolve it in 1.2g water to prepare K2O aqueous solution, and spray the K2O aqueous solution onto the inner wall of a stainless steel tube multiple times by gas. Repeat the spraying of excess solution until the entire solution is loaded onto the coating of the precious metal ruthenium. Then dry it with gas, dry it at 120℃ for 4 hours, and calcine it at 500℃ for 4 hours to obtain the catalyst used in the microchannel ammonia decomposition reactor.
[0098] Test case
[0099] To compare the effects of the microreactor and catalyst coating composite process of this invention with conventional particle packing on the ammonia decomposition reaction process, a particle-supported catalyst with a consistent ratio of support to active component was prepared as a reference. Its ammonia decomposition activity was evaluated in a quartz tube reactor with an inner diameter of 8 mm. The specific ratios are as follows:
[0100] Reference catalyst 1
[0101] The specific steps in the preparation of this agent include: weighing 10g of spherical alumina carrier with a diameter of 1.0mm, loading it by equal volume impregnation, and dissolving 0.5172g of ruthenium trichloride hydrate (containing 37% Ru) in 6g of deionized water in the impregnation solution. After impregnation, air-dry at room temperature, dry at 120℃ for 4 hours, and calcine at 500℃ for 4 hours. The addition ratio of K2O is 5% of the alumina carrier, and the same equal volume impregnation method is used. The impregnation solution is 0.7336g of K2CO3 dissolved in 6g of deionized water. The air-drying, drying, and calcination processes after impregnation are the same as the Ru loading process.
[0102] Reference catalyst 2
[0103] The specific steps in the preparation of this agent include: weighing 10g of spherical silica carrier with a diameter of 1.0mm, loading it by equal volume impregnation, and dissolving 0.5172g of ruthenium trichloride hydrate (containing 37% Ru) in 7g of deionized water in the impregnation solution. After impregnation, air-dry at room temperature, dry at 120℃ for 4 hours, and calcine at 500℃ for 4 hours. The addition ratio of K2O is 5% of the alumina carrier, and the same equal volume impregnation method is used. The impregnation solution is 0.7336g of K2CO3 dissolved in 6g of deionized water. The air-drying, drying, and calcination processes after impregnation are the same as the Ru loading process.
[0104] Reference catalyst 3
[0105] The specific steps in the preparation of this agent include: weighing 10g of spherical titanium dioxide carrier with a diameter of 1.0mm, loading it by equal volume impregnation, and dissolving 0.5172g of ruthenium trichloride hydrate (containing 37% Ru) in 5g of deionized water in the impregnation solution. After impregnation, air-dry at room temperature, dry at 120℃ for 4 hours, and calcine at 500℃ for 4 hours. The addition ratio of K2O is 5% of that of the alumina carrier, and the same equal volume impregnation method is used. The impregnation solution is 0.7336g of K2CO3 dissolved in 6g of deionized water. The air-drying, drying, and calcination processes after impregnation are the same as those for Ru loading.
[0106] Ammonia decomposition conversion rate test:
[0107] The activity evaluation of Examples 1-9 and Reference Catalysts 1-3 in the ammonia decomposition reaction process was carried out by comparing the ammonia decomposition conversion rate per unit mass of catalyst at different temperatures. The reaction pressure was atmospheric pressure, and the flow rate of the reactant ammonia and the mass of the catalyst (including the support and active components) were uniformly 300 ml NH3 / g catalyst. Since the Ru and K2O contents were consistent in all examples and references, the ratio of the flow rate of the reactant ammonia gas to Ru was 6 ml NH3 / g Ru in all activity evaluation examples. The specific activity data comparison is shown in Table 1:
[0108] Table 1 Results of ammonia decomposition conversion rate test
[0109]
[0110]
[0111] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not intended to limit the present invention.
[0112] The above embodiments are merely preferred technical solutions of the present invention and should not be considered as limitations on the present invention. The scope of protection of the present invention should be limited to the technical solutions described in the claims, including equivalent substitutions of the technical features described in the claims. That is, equivalent substitutions and improvements within this scope are also within the scope of protection of the present invention.
Claims
1. A catalyst preparation process for use in a microchannel ammonia decomposition reactor, characterized in that, The process includes the following steps: S1 Select a microreactor inner tube of appropriate specifications as needed; calculate the amount of inorganic oxide membrane carrier to be coated based on the inner surface area of the inner tube, and then calculate the amount of active component based on the mass of the inorganic oxide membrane carrier. S2 is used for pretreatment of the microreactor to remove impurities such as dust and grease from the tube wall; S3 prepares a coating solution, then coats the coating solution onto the inner wall of the pretreated microreactor metal tube and then calcines it to grow an inorganic oxide film carrier. S4 is obtained by impregnating the loaded active component on an inorganic oxide membrane support to obtain the catalyst used in the microchannel ammonia decomposition reactor.
2. The preparation process according to claim 1, characterized in that: In step S1, the coating amount of the inorganic oxide film carrier is 140-180 g / m³. 2 .
3. The preparation process according to claim 1, characterized in that: The pretreatment method in step S2 is either chemical corrosion or sandblasting.
4. The preparation process according to claim 3, characterized in that: The pretreatment method is a chemical corrosion method, which involves cleaning the pipe wall with hot alkaline solution, rinsing it with deionized water, corroding the inner wall of the pipe with acid solution, rinsing it with deionized water, and then drying it.
5. The preparation process according to claim 1, characterized in that: In step S2, the coating solution is one or a mixture of aluminum sol, silica sol, and titanium dioxide sol.
6. The preparation process according to claim 5, characterized in that: The coating solution is aluminum sol.
7. The preparation process according to claim 1, characterized in that, The coating process in step S3 is as follows: high-pressure gas is used to spray the coating liquid onto the inner wall of the metal tube of the microreactor. During the coating process, the gas is continuously purged. During the spraying process, the coating liquid at the outlet is recovered and reused. After the coating is completed, the liquid is dried by gas.
8. The preparation process according to claim 1, characterized in that, The specific steps of impregnating and loading the active component in step S4 are as follows: the precursor of the active component is dissolved in water to obtain an impregnation solution. During the impregnation process, the impregnation solution is sprayed onto the inner wall of the metal tube using gas. Excess impregnation solution is recovered and re-sprayed during the impregnation process until the impregnation solution is completely loaded onto the inorganic oxide carrier. Then, the impregnation solution is dried by gas, and then dried and calcined.
9. The preparation process according to claim 1, characterized in that: The active components include the noble metal Ru and the non-noble metal Ni.
10. The preparation process according to claim 9, characterized in that: The active component also includes an active adjuvant, which is a compound containing K, N and Cs elements.
Citation Information
Patent Citations
Ammonia decomposition hydrogen producer
CN205011382U
Ammonia decomposition hydrogen production device
CN210528460U