A selective liberation pre-enrichment and comprehensive recovery method for ultra-low grade, high-calcium complex tungsten ore
By using selective grinding and stepped cyclone classification, tungsten-bearing minerals and fluorite in ultra-low grade high-calcium complex tungsten ores are separated from calcium-bearing gangue, solving the problems of large feed volume and high reagent consumption in existing technologies, and achieving efficient comprehensive recovery of tungsten minerals and fluorite.
Patent Information
- Application Number
- CN202611483143.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are difficult to effectively process ultra-low grade, high-calcium complex tungsten ores, resulting in large feed volumes, high reagent consumption, poor flotation selectivity, and limited effectiveness of gravity separation or heavy media routes for fine-grained separation, making it difficult to achieve selective liberation and comprehensive recovery of tungsten minerals and calcium-bearing gangue.
Tungsten-bearing minerals and fluorite are enriched in the particle size greater than 38 μm by selective grinding, while calcium-bearing gangue and easily mud-forming gangue are enriched in the particle size less than 30 μm. Fine-grained calcium-bearing gangue is removed by primary and secondary cyclone classification, followed by flotation of scheelite and fluorite to form a stepped enhanced classification system.
It significantly improved the grade of scheelite and fluorite, reduced the calcium-bearing gangue load, and decreased the consumption of subsequent flotation reagents, thus realizing the economical and comprehensive utilization of ultra-low grade high-calcium complex tungsten ores.
Smart Images

Figure CN123102496A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of mineral processing, and in particular to a selective liberation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore. Background Technology
[0002] Ultra-low grade, high-calcium complex tungsten ores typically exhibit extremely low WO3 grades, high calcium gangue content, and complex mineral composition. For example, a polymetallic mine in Hunan province has a WO3 grade of approximately 0.015%, CaF2 of approximately 14.23%, and CaCO3 of approximately 30.63%. If these ores are directly fed into the grinding and flotation process, a large amount of waste rock and calcium gangue will enter the system with the slurry, resulting in a large feed volume, high reagent consumption, and poor flotation selectivity.
[0003] The main challenge with this type of ore lies in the fact that scheelite itself is a calcium-bearing mineral, and gangue or associated minerals such as calcite, fluorite, and dolomite also contain calcium. Their surface properties are similar, making it easy for problems such as accidental flotation of calcite, suppression of scheelite, and interference between fluorite and scheelite to occur during flotation. Simply relying on collectors, depressants, or pulp conditioning for separation is insufficient to fundamentally reduce the calcium-bearing gangue load entering the flotation system.
[0004] Existing scheelite flotation technologies primarily rely on direct flotation after grinding, using a combination of reagents such as water glass, modified water glass, oxalic acid, lignin inhibitors, and hydroxamic acid or fatty acid collectors to regulate the flotation behavior of scheelite, calcite, and fluorite. The objective drawbacks of this approach are: for ultra-low-grade ores with approximately 0.015% WO3, the entire ore enters the flotation process, resulting in excessively low feed grade; high loading of calcium-bearing gangue such as calcite makes it difficult to balance concentrate grade and recovery; and a large amount of fine slime deteriorates the flotation environment, leading to sticky froth, enhanced entrainment, and increased reagent consumption.
[0005] Existing pre-enrichment technologies typically rely on density differences for tailings removal. For complex ores containing multiple minerals such as scheelite, wolframite, fluorite, calcite, and dolomite, simple gravity separation or heavy media routes have limited effectiveness in fine-grained separation and are prone to causing loss of fine tungsten particles. While single-stage cyclone or empirical classification can remove some fine mud, it does not construct a stepwise enrichment process based on the differences in mineral selective liberation, making it difficult to sufficiently reduce the calcium-bearing gangue load.
[0006] Patent document CN112827658A discloses a process where grinding undersize is mixed with flotation reagents and then subjected to hydrocyclone classification. The undersize is then fed into a flash or jet flotation machine for flotation, and the overflow is used for scheelite flotation. This process reduces the need for repeated grinding of liberated scheelite. The document also describes the effect of the overflow carrying away fine mud and calcium-containing minerals, and the relative enrichment of the undersize. This application proposes to use a two-stage hydrocyclone pre-enrichment process after selective grinding, followed by tungsten and fluorite recovery. The technical effectiveness should be evaluated in conjunction with the suitability of the ore sample, the distribution indicators of each stage, and the subsequent flotation results.
[0007] In summary, there is an urgent need to develop a selective dissociation pre-enrichment and comprehensive recovery method suitable for ultra-low grade, high-calcium complex tungsten ores, so as to achieve comprehensive resource utilization. Summary of the Invention
[0008] The purpose of this application is to provide a selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore, in order to solve the above-mentioned problems.
[0009] To achieve the above objectives, this application provides a selective liberation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore. The ultra-low-grade high-calcium complex tungsten ore contains tungsten-bearing minerals, calcium-bearing gangue, associated recoverable minerals, and easily mud-forming gangue. The tungsten-bearing minerals include scheelite, the calcium-bearing gangue includes calcite and dolomite, the associated recoverable minerals include fluorite, and the easily mud-forming gangue includes clay minerals. The WO3 grade in the ultra-low-grade high-calcium complex tungsten ore is not higher than 0.05%, and the combined mass fraction of calcite and dolomite is not less than 25%. The method includes the following steps: Selective grinding is performed on the ultra-low grade high-calcium complex tungsten ore to obtain selectively ground slurry. In the selectively ground slurry, calcium-containing gangue and easily mud-forming gangue are enriched in a particle size of less than 30 μm, and the tungsten-containing minerals and fluorite are enriched in a particle size of greater than 38 μm in the form of individual particles or rich intergrowths. The slurry after selective grinding is subjected to primary cyclone classification to obtain primary sand rich in tungsten-containing minerals and fluorite; The secondary sediment is slurried to obtain a slurry; the slurry is then subjected to scheelite flotation and fluorite flotation to obtain scheelite concentrate and fluorite concentrate.
[0010] Optionally, the WO3 grade in the ultra-low grade high-calcium complex tungsten ore is 0.005%-0.05%, the total mass fraction of calcite and dolomite is 25%-50%, and quartz and silicate gangue minerals are associated with it.
[0011] Optionally, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) The selective grinding adopts at least one of ball milling, rod milling, semi-autogenous milling and staged grinding; (2) The mass concentration of the selective grinding is 25%-40%.
[0012] Optionally, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) The first-stage cyclone classification is performed using a first-stage classification device, and the second-stage cyclone classification is performed using a second-stage classification device; Both the primary and secondary grading devices independently include hydrocyclones. (2) The secondary cyclone classification and slurry adjustment also include a third or higher cyclone classification. Each level uses the first-level sedimentation and slurry adjustment as feed and collects the overflow separately.
[0013] Optionally, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) The diameter of the underflow nozzle of the primary classifier is 0.08-0.15 of the diameter of the hydrocyclone cylinder, and the feed pressure is 0.06-0.15 MPa; (2) The diameter of the underflow nozzle of the secondary classification equipment is 0.15-0.25 of the diameter of the hydrocyclone cylinder, and the feed pressure is 0.05-0.12 MPa.
[0014] Optionally, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) When the tungsten-bearing minerals also include wolframite, the slurry is subjected to physical beneficiation to obtain wolframite and beneficiated slurry, and the beneficiated slurry is subjected to flotation of the scheelite; The physical beneficiation includes one of gravity separation, magnetic separation, combined gravity-magnetic separation and combined gravity-flotation; (2) The first-stage cyclone classification also yields a first-stage overflow, and the second-stage cyclone classification also yields a second-stage overflow; when the tungsten content in the first-stage overflow and the second-stage overflow is low, it is removed after scavenging, concentration or classification; when the tungsten content in the first-stage overflow and the second-stage overflow is high, it is returned to the grinding or the first-stage cyclone classification.
[0015] Optionally, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) Prior to the flotation of the scheelite, regrinding is also performed; (2) The flotation reagents for scheelite flotation include pH adjuster, scheelite inhibitor, activator and scheelite collector; the pH adjuster includes sodium carbonate, the scheelite inhibitor includes water glass, the activator includes lead nitrate and the scheelite collector includes benzohydroxyxamic acid.
[0016] Optionally, the flotation reagent for fluorite flotation includes gangue inhibitors and fluorite collectors; The gangue inhibitor comprises water glass, and the fluorite collector comprises oleic acid.
[0017] Optionally, the WO3 grade in the scheelite concentrate is ≥30%, and the CaF2 grade in the fluorite concentrate is ≥90%.
[0018] Compared with the prior art, the beneficial effects of this application include: The selective liberation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore provided in this application utilizes the differences in hardness and brittleness between high-calcium gangues such as calcite and dolomite, clay minerals, and target minerals such as scheelite and fluorite. Selective grinding preferentially finely crushes and mudsizes the high-calcium gangues and clay minerals into fine-grained particles, while the target tungsten-bearing minerals and fluorite remain in a medium-to-coarse-grained state of liberation or enrichment. Then, through the synergistic effect of primary and secondary cyclone classification, a large amount of calcium-bearing gangue and fine mud are removed before flotation, allowing the ore to enter the final stage of flotation. The flotation system significantly reduces the amount of ore, significantly increases the WO3 grade, and effectively reduces the CaCO3 load, thus reconstructing the composition of the feed minerals from the source. This fundamentally improves the flotation selectivity between scheelite and calcite, ultimately yielding high-grade scheelite and fluorite concentrates. It achieves comprehensive recovery of tungsten minerals and fluorite from ultra-low-grade, high-calcium complex tungsten ores. At the same time, due to the significant reduction in the amount of feed ore and the calcium-bearing gangue load, the reagent consumption and energy consumption of subsequent flotation operations are correspondingly reduced, resulting in significant economic benefits and comprehensive resource utilization value. Attached Figure Description
[0019] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation on the scope of this application.
[0020] Figure 1 This is a schematic flowchart of the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore provided in Example 2. Detailed Implementation
[0021] Understandably, this application is the first to propose a selective liberation pre-enrichment and comprehensive recovery method for "ultra-low grade, high-calcium complex tungsten ore," and clarifies the technical characteristics of this ore as follows: WO3 grade ≤ 0.05%, total calcium-bearing gangue (calcite + dolomite) ≥ 25%, and simultaneously containing scheelite, fluorite, and various calcium-bearing gangue minerals. This type of ore has not been studied as an independent processing target in existing technologies, primarily because current beneficiation technologies cannot economically and effectively process such extremely low-grade, high-calcium-load complex ores. The primary contribution of this application lies in identifying the unique characteristics of this type of ore and revealing its selective liberation pattern during grinding—tungsten-bearing minerals and fluorite tend to remain in the medium-to-coarse grain size, while calcium-bearing gangue preferentially undergoes fine crushing and mudification into the fine grain size. Based on this discovery, this application proposes a novel approach of "selective liberation pre-enrichment before flotation," breaking through the traditional "direct flotation after grinding" technical route.
[0022] First, the solution provided in this application will be explained in more detail as follows: This application provides a selective liberation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore. The ultra-low-grade high-calcium complex tungsten ore contains tungsten-bearing minerals, calcium-bearing gangue, associated recoverable minerals, and easily mud-forming gangue. The tungsten-bearing minerals include scheelite, the calcium-bearing gangue includes calcite and dolomite, the associated recoverable minerals include fluorite, and the easily mud-forming gangue includes clay minerals. The WO3 grade in the ultra-low-grade high-calcium complex tungsten ore is not higher than 0.05%, and the combined mass fraction of calcite and dolomite is not less than 25%. Optionally, the WO3 grade in ultra-low grade high-calcium complex tungsten ore can be any value between 0.005%, 0.01%, 0.015%, 0.02%, 0.025%, 0.03%, 0.035%, 0.04%, 0.045%, 0.05%, or 0.005%-0.05%, and the total mass fraction of calcite and dolomite can be any value between 25%, 30%, 35%, 40%, 45%, 50%, or 25%-50%. It should be noted that the above mass fractions are all based on the dry raw ore mass; calcite and dolomite are the target calcium-bearing gangues in this application, fluorite is an associated recoverable mineral, and clay minerals are separately classified as easily mud-forming gangues. It is understandable that, in addition to tungsten-bearing minerals mainly composed of scheelite, this application is also applicable to complex tungsten mines containing wolframite, scheelite, fluorite, and high-content calcite, dolomite, and clay, as well as tungsten-fluorite associated mines and low-grade tungsten tailings reprocessing materials. The method includes the following steps: selectively grinding ultra-low grade high-calcium complex tungsten ore to obtain selectively ground slurry; The calcium-bearing gangue and easily mud-forming gangue in the slurry after selective grinding are enriched in a particle size of less than 30 μm, and the tungsten-bearing minerals and fluorite are enriched in a particle size of greater than 38 μm in the form of monomers or intergrowths. It should be noted that this particle size difference should be confirmed through particle size yield, fractional particle size analysis, and mineral liberation analysis, rather than requiring all minerals to enter the corresponding particle size. Selective grinding controls the grinding intensity and endpoint according to the fractional mineral distribution and liberation status to avoid over-grinding caused by repeated grinding of liberated tungsten-bearing minerals and fluorite. The slurry after selective grinding is subjected to primary cyclone classification to obtain primary sand rich in tungsten-bearing minerals and fluorite. The primary sediment is subjected to secondary cyclone classification to obtain secondary sediment enriched with tungsten-containing minerals and fluorite; Understandably, before flotation, the selective liberation differences between scheelite, wolframite, fluorite and calcium-bearing gangue such as calcite, dolomite, and clay during the grinding process are utilized to allow fine-grained calcium-bearing gangue to preferentially enter the classification overflow and be removed, while tungsten-bearing minerals and fluorite are retained in the sediment and gradually enriched, thereby reconstructing the composition of the flotation minerals and improving the beneficiation of low-grade complex tungsten ore. The secondary sediment is slurried to obtain a slurry; the slurry is then subjected to scheelite flotation and fluorite flotation to obtain scheelite concentrate and fluorite concentrate.
[0023] In some embodiments, this application employs a tungsten-first, then fluorite flotation sequence: scheelite flotation is performed on the scheelite feed to obtain scheelite concentrate and scheelite flotation tailings; then, the tailings are subjected to fluorite flotation to obtain fluorite concentrate and final flotation tailings. For ore samples containing wolframite, wolframite can be recovered first, and then the beneficiated slurry can be fed into the above flotation process.
[0024] In some embodiments, the WO3 grade in the ultra-low grade high-calcium complex tungsten ore is 0.005%-0.05%, the total mass fraction of calcite and dolomite is 25%-50%, and it is associated with quartz and silicate gangue minerals.
[0025] Optionally, the WO3 grade in ultra-low grade high-calcium complex tungsten ore can be any value between 0.005%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, or 0.005-0.05%, and the total mass fraction of calcite and dolomite can be any value between 25%, 30%, 35%, 40%, 45%, 50%, or 25-50%.
[0026] In some embodiments, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) The selective grinding adopts at least one of ball milling, rod milling, semi-autogenous milling and staged grinding; (2) The mass concentration of the selective grinding is 25%-40%; Optionally, the mass concentration of selective grinding can be any value between 25%, 28%, 30%, 33%, 35%, 38%, 40%, or 25%-40%.
[0027] It is understandable that the classification particle size of selective grinding can be comprehensively adjusted based on the differences in mineral liberation particle size, the enrichment particle size of fine calcium-bearing gangue, the retention particle size of tungsten-bearing minerals, as well as the structural parameters and operating conditions of the on-site cyclone equipment, so that fine calcium-bearing gangue mainly enters the overflow and tungsten-bearing minerals mainly enter the sediment.
[0028] In some embodiments, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) The first-stage cyclone classification is performed using a first-stage classification device, and the second-stage cyclone classification is performed using a second-stage classification device; The primary grading device and the secondary grading device each independently include a hydrocyclone; Understandably, the role of primary hydrocyclone classification is to perform preliminary classification of the slurry after selective grinding. By utilizing the particle size separation effect of the hydrocyclone, the calcite, clay, and fine-grained calcium gangue that are preferentially crushed and muddied during selective grinding are removed with the overflow and discarded as tailings. Meanwhile, the coarser particles rich in scheelite, wolframite, and fluorite are retained in the sediment, achieving the first large-scale removal of calcium gangue and obtaining primary pre-enriched products, thus initially reducing the gangue load in subsequent operations. The purpose of the secondary cyclone classification is to enhance the classification of the primary sediment. Its purpose is not to simply repeat the primary classification, but to further remove the residual fine-grained calcium-containing gangue on the basis that the primary classification has already significantly reduced the fine-grained gangue load. This allows the tungsten-containing minerals and fluorite to be significantly enriched in the sediment, resulting in a pre-enriched tungsten ore product with higher grade and lower gangue content, thus providing higher-quality feed material for subsequent flotation operations. The combined effect of primary and secondary cyclone classification is that they form a tiered, enhanced classification system. Through a progressively advancing decalcification mechanism, they achieve stepwise and in-depth removal of calcium-containing gangue. Primary classification handles the main tailings removal, eliminating most of the fine-grained gangue; secondary classification focuses on refinement and enrichment, further purifying the feed material. Their synergistic effect significantly reduces the amount of ore entering the flotation system, substantially increases the WO3 grade, and effectively reduces the CaCO3 load, thus reconstructing the composition of the feed minerals before flotation. In the overall scheme of this application, the primary cyclone classification and the secondary cyclone classification together constitute the core link of selective liberation pre-enrichment, and are the key bridge connecting selective grinding with subsequent scheelite flotation and fluorite flotation. Their function is to transform the mineral particle size differences formed by selective grinding into actual material diversion effects, allowing fine-grained calcium-bearing gangue to systematically enter the overflow tailings, and allowing the target tungsten-bearing minerals and fluorite to be systematically retained in the sediment and enriched step by step. This transforms the originally extremely low-grade ore with an extremely high calcium-bearing gangue load into a pre-enriched product with industrial processing value, fundamentally improving the selectivity and economy of subsequent flotation operations. It is a key technological support for realizing the economical and comprehensive utilization of ultra-low-grade, high-calcium complex tungsten ores. (2) The secondary cyclone classification and the slurry conditioning also include a third or higher cyclone classification. Each level uses the first-level sedimentation and slurry conditioning as feed and collects the overflow separately.
[0029] Understandably, third- or higher vortex grading is used to further reduce the calcium-containing gangue load.
[0030] In some embodiments, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) The diameter of the underflow nozzle of the primary classifier is 0.08-0.15 of the diameter of the hydrocyclone cylinder, and the feed pressure is 0.06-0.15 MPa; Optionally, the ratio of the underflow nozzle diameter to the hydrocyclone cylinder diameter of the primary classifier can be any value between 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, or 0.08-0.15; and the feed pressure of the primary classifier can be any value between 0.06MPa, 0.07MPa, 0.08MPa, 0.09MPa, 0.10MPa, 0.11MPa, 0.12MPa, 0.13MPa, 0.14MPa, 0.15MPa, or 0.06-0.15MPa. (2) The diameter of the underflow nozzle of the secondary classification equipment is 0.15-0.25 of the diameter of the hydrocyclone cylinder, and the feed pressure is 0.05-0.12 MPa.
[0031] Optionally, the ratio of the underflow nozzle diameter to the hydrocyclone cylinder diameter of the secondary classifier can be any value between 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, or 0.15-0.25. The feed pressure of the secondary classifier can be any value between 0.05MPa, 0.06MPa, 0.07MPa, 0.08MPa, 0.09MPa, 0.10MPa, 0.11MPa, 0.12MPa, or 0.05-0.12MPa.
[0032] In some embodiments, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) When the tungsten-bearing minerals also include wolframite, the slurry is subjected to physical beneficiation to obtain wolframite and beneficiated slurry, and the beneficiated slurry is subjected to flotation of the scheelite; The physical beneficiation includes one of gravity separation, magnetic separation, combined gravity-magnetic separation and combined gravity-flotation; Understandably, when the pre-enriched product contains wolframite, the wolframite can be recovered first by physical beneficiation, based on its high density, weak magnetism, or differences in physical properties with gangue minerals, to obtain wolframite concentrate or wolframite rough concentrate. The tailings obtained from physical beneficiation are then put into subsequent flotation. For ores with low wolframite content, this step may not be necessary. (2) The first-stage cyclone classification also yields a first-stage overflow, and the second-stage cyclone classification also yields a second-stage overflow; when the tungsten content in the first-stage overflow and the second-stage overflow is low, it is removed after scavenging, concentration or classification; when the tungsten content in the first-stage overflow and the second-stage overflow is high, it is returned to the grinding or the first-stage cyclone classification.
[0033] In some embodiments, the selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore satisfies at least one of the following conditions: (1) Prior to the flotation of the scheelite, regrinding is also performed; (2) The flotation reagents for scheelite flotation include pH adjuster, scheelite inhibitor, activator and scheelite collector; the pH adjuster includes sodium carbonate, the scheelite inhibitor includes water glass, the activator includes lead nitrate and the scheelite collector includes benzohydroxyxamic acid.
[0034] Understandably, since a large amount of calcium-containing fine mud such as calcite and clay has been removed before flotation, the amount of ore entering the scheelite flotation and the load of calcium-containing gangue are significantly reduced, the target of the flotation reagents is more concentrated, and the selective separation conditions between scheelite and calcite are improved.
[0035] In some embodiments, the flotation reagent for fluorite flotation includes gangue inhibitors and fluorite collectors; The gangue inhibitor comprises water glass, and the fluorite collector comprises oleic acid.
[0036] It is understandable that, since fluorite is retained in the sediment along with tungsten-containing minerals during the selective liberation pre-enrichment process, and a large amount of calcite has already been removed before flotation, the interference of CaCO3 in the subsequent fluorite recovery is reduced, which is conducive to obtaining high-grade fluorite products.
[0037] In some embodiments, the WO3 grade in the scheelite concentrate is ≥30%, and the CaF2 grade in the fluorite concentrate is ≥90%.
[0038] Optionally, the WO3 grade in the scheelite concentrate can be any value between 30%, 32%, 34%, 36%, 38%, 40%, or 30%-40%, and the CaF2 grade in the fluorite concentrate can be any value between 90%, 92%, 94%, 96%, 97%, 98%, or 90%-98%.
[0039] The implementation schemes of this application will be described in detail below with reference to specific embodiments. However, those skilled in the art will understand that the following embodiments are only for illustrating this application and should not be regarded as limiting the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments used without specified manufacturers are all conventional products that can be purchased commercially.
[0040] Example 1 This embodiment provides a selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade, high-calcium complex tungsten ore. The chemical multi-element analysis and mineral composition of the raw ore used are shown in Table 1. Table 1. Multi-element chemical analysis of raw ore (mass fraction / %)
[0041] Mineral composition: scheelite, fluorite, calcite, quartz, garnet, diopside, wollastonite, feldspar, mica, chlorite, dolomite, apatite and minor sulfide minerals.
[0042] Mineralogical analysis shows that calcite and clay minerals, after dissociation and mudification, are mainly enriched in the -30μm grain size; scheelite and fluorite mainly exist as single entities or intergrowths in the +38μm grain size.
[0043] The specific steps are as follows: S1: The raw ore is ground and slurry adjusted to a mass concentration of approximately 30% to obtain the ground slurry. The grinding process uses a ball mill (φ1.05m × 1.5m), with steel ball media (φ60mm, φ40mm, φ25mm in a 3:2:1 ratio), a media filling rate of 28%, a ball-to-material ratio of 4:1, and a grinding mass concentration of 30%. The grinding control objectives are: to preferentially finely crush calcite and clay minerals into a -30μm particle size, and to maintain scheelite and fluorite in a +38μm particle size, either as single or intergrowths. S2: The slurry after grinding is subjected to primary hydrocyclone classification. The diameter of the primary hydrocyclone cylinder is φ350mm, the diameter of the underflow nozzle is 0.12 of the cylinder diameter, the feed pressure is 0.10 MPa, the actual classification d50 is about 30μm, and primary overflow and primary underflow are obtained; the primary overflow is discarded as tailings 1. S3: The primary sediment is used as a pre-enriched product for secondary hydrocyclone classification. The secondary hydrocyclone has a cylinder diameter of φ250 mm, the sediment nozzle diameter is 0.20 of the cylinder diameter, the feed pressure is 0.08 MPa, and the actual classification d50 is about 45 μm, resulting in secondary overflow and secondary sediment. The secondary overflow is discarded as tailings 2, and the secondary sediment is used as a tungsten-fluorite pre-enriched product. The grades and recovery rates of primary overflow tailings 1, secondary overflow tailings 2, secondary sedimentation pre-enrichment products and raw ore are shown in Table 2.
[0044] Table 2 Grade and Recovery Rate
[0045] Through selective dissociation pre-enrichment, WO3 increased from 0.015% to 0.118%, an enrichment of approximately 7.9 times; CaCO3 decreased from 30.63% to 6.50%, and the calcium-containing gangue load entering subsequent flotation was significantly reduced, indicating that this method has achieved the transformation of low-grade resources into flotable resources; S4: The pre-enriched secondary sediment product is regrinded and slurry-adjusted before being subjected to scheelite flotation. The flotation reagents include sodium carbonate (pH adjuster, dosage 1000 g / t raw ore), water glass (scheelite inhibitor, dosage 1000 g / t raw ore), lead nitrate (activator, dosage 400 g / t raw ore), and benzoic acid (scheelite collector, dosage 300 g / t raw ore). The flotation process of "one roughing, two cleaning, and two scavenging" is adopted to obtain scheelite concentrate and scheelite tailings. S5: Fluorite flotation is carried out on the scheelite tailings. The flotation reagents include fluorite inhibitor water glass (500 g / t raw ore) and fluorite collector oleic acid (300 g / t raw ore). The flotation process of "one rougher, two cleaners and two scavengers" is adopted to obtain fluorite concentrate.
[0046] The grades and recoveries of scheelite concentrate, fluorite concentrate, and raw ore are shown in Table 3.
[0047] Table 3 Grade and Recovery Rate
[0048] Example 2 This embodiment provides a selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore, which is a mixed black and white tungsten ore from Hunan Province. The raw ore has a WO3 grade of 0.022%, of which scheelite accounts for approximately 70% of the total tungsten minerals and wolframite accounts for approximately 30%; the CaF2 content is 12.80%, the CaCO3 content is 32.40%, and it also contains dolomite, quartz, mica, clay minerals, and a small amount of sulfide minerals.
[0049] Mineralogical analysis showed that scheelite, wolframite, and fluorite were mainly distributed in the +38 μm size after moderate grinding, while calcite and clay minerals were mainly enriched in the -30 μm size.
[0050] This embodiment provides a flowchart illustrating a selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore, as shown below. Figure 1 As shown, the specific steps are as follows: S1: Grinding and cyclone classification conditions are the same as in Example 1; The grades and recovery rates of the pre-enriched tailings (primary overflow tailings 1 and secondary overflow tailings 2), secondary sedimentation pre-enriched products, and raw ore are shown in Table 4.
[0051] Table 4 Grade and Recovery Rate
[0052] S2: After the secondary sand pre-enriched product is slurryed, it is subjected to magnetic separation to obtain wolframite concentrate and beneficiated slurry. Magnetic separation operation conditions: The magnetic separation operation conditions are: vertical ring pulsating high gradient magnetic separator, magnetic induction intensity 0.9 T, pulsation stroke 18 mm, pulsation frequency 250 r / min, feed particle size -74μm accounts for 70%, and a one-stage roughing and one-stage cleaning process is adopted. S3: After beneficiation, the slurry is regrinded to 80% of its thickness at -38μm before scheelite and fluorite flotation are carried out. The reagent system is the same as in Example 1.
[0053] The grades and recoveries of wolframite concentrate, scheelite concentrate, fluorite concentrate, and raw ore are shown in Table 5.
[0054] Table 5 Grade and Recovery Rate
[0055] This embodiment shows that the present invention is applicable to complex tungsten ores containing both wolframite and scheelite, and achieves comprehensive recovery of multiple valuable components through pre-enrichment followed by gravity separation-flotation.
[0056] Example 3 The only difference between this embodiment and Embodiment 1 is that a rod mill is used instead of a ball mill for grinding.
[0057] The grades and recovery rates of primary overflow tailings 1, secondary overflow tailings 2, secondary sedimentation pre-enrichment products, and raw ore are shown in Table 6.
[0058] Table 6 Grade and Recovery Rate
[0059] The reagent systems for scheelite flotation and fluorite flotation are the same as in Example 1. The grades and recoveries of scheelite concentrate, fluorite concentrate, and raw ore are shown in Table 7.
[0060] Table 7 Grade and Recovery Rate
[0061] This embodiment demonstrates that rod milling can also achieve selective dissociation.
[0062] Example 4 This embodiment provides a selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade, high-calcium complex tungsten ore with a WO3 grade close to the 0.05% threshold. The raw ore has a WO3 grade of 0.048%, a CaF2 content of 10.60%, a CaCO3 content of 27.80%, and contains scheelite, fluorite, calcite, dolomite, quartz, clay minerals, and a small amount of calcium-containing silicate minerals.
[0063] The specific steps are the same as in Example 1, except that the feed pressure of the first-stage hydrocyclone is 0.11 MPa and the feed pressure of the second-stage hydrocyclone is 0.09 MPa. After two-stage hydrocyclone classification, the yield of the pre-enriched secondary sediment is 18.00%, the WO3 grade is 0.25%, the WO3 recovery rate is 94.50%, and the CaCO3 grade is reduced to 7.40%.
[0064] After the secondary sediment pre-enriched product was regrinded to -38μm (82%), scheelite and fluorite were subjected to flotation using the same reagents as in Example 1. This yielded scheelite concentrate with a WO3 grade of 38.10% and a WO3 recovery rate of 75.40%, and fluorite concentrate with a CaF2 grade of 95.60% and a CaF2 recovery rate of 52.30%.
[0065] This embodiment shows that when the WO3 grade of the raw ore is close to the upper limit of 0.05%, this application can still significantly reduce the calcium-bearing gangue load through selective dissociation and two-stage cyclone pre-enrichment, and obtain qualified scheelite concentrate and fluorite concentrate.
[0066] Comparative Example 1 This comparative example uses the same raw ore as in Example 1, without selective liberation pre-enrichment. The raw ore is directly ground to -200 mesh (80%), followed by scheelite flotation and fluorite flotation. The reagent system is exactly the same as in Example 1.
[0067] The grades and recovery rates of scheelite concentrate and fluorite concentrate are shown in Table 8.
[0068] Table 8 Grade and Recovery Rate
[0069] Analysis: Because all the raw ore is directly fed into the flotation process, the calcium-bearing gangue and fine slime have a high load, and a large amount of calcite and fine slime seriously interfere with the flotation process. This comparative example illustrates that for ultra-low grade, high-calcium complex tungsten ores, direct flotation without pre-enrichment cannot yield a qualified concentrate product.
[0070] Comparative Example 2 This comparative example uses the same raw ore and grinding conditions as Example 1, but only performs primary cyclone classification (parameters are the same as primary cyclone in Example 1). The primary sediment is directly used as a pre-enriched product for scheelite flotation and fluorite flotation, without secondary cyclone classification.
[0071] The grades and recovery rates of primary overflow tailings 1, primary sedimentation pre-enrichment products, and raw ore are shown in Table 9.
[0072] Table 9 Grade and Recovery Rate
[0073] Analysis: Although single-stage vortexing removed some fine-grained calcite, the calcium-containing gangue load remained high. The CaCO3 content was still high, failing to adequately reconstruct the mineral composition before flotation. This comparative example demonstrates that single-stage classification is insufficient to significantly reduce the calcium-containing gangue load, and a two-stage enhanced classification is necessary.
[0074] Comparative Example 3 This comparative example uses the same raw ore as in Example 2. After selective grinding, no stepwise cyclone pre-enrichment is performed; instead, a shaking table or spiral sluice gravity separation is used directly. Due to the extremely low WO3 grade, large quantity, and high amount of fine mud in the raw ore, and the low separation efficiency of fine-grained scheelite, wolframite, and gangue such as calcite, traditional gravity separation can recover some of the coarser wolframite, but the loss of scheelite and fine-grained tungsten is significant, and fluorite is also difficult to enrich simultaneously.
[0075] The differences between this comparative example and Example 2 are shown in Table 10.
[0076] Table 10. Differences between Comparative Example 3 and Example 2
[0077] Comparative Example 4 This comparative example uses the same raw ore, grinding equipment, media regime, and slurry solids mass fraction as Example 1, but does not use the particle size distribution and mineral liberation degree as the grinding endpoint; instead, it uses the raw ore as a whole to grind to... 74 μm was used as the grinding endpoint, accounting for 80%. The remaining two stages of cyclone classification and flotation conditions were the same as in Example 1. The grades and recoveries of the primary overflow tailings 1, secondary overflow tailings 2, secondary sediment pre-enrichment products, and raw ore are shown in Table 11.
[0078] Table 11 Grade and Recovery Rate
[0079] The grades and recoveries of scheelite concentrate, fluorite concentrate, and raw ore are shown in Table 12.
[0080] Table 12 Grade and Recovery Rate
[0081] Analysis: Conventional grinding causes a large amount of scheelite and fluorite to enter the fine-grained fraction, resulting in a significant loss of valuable minerals to the overflow during the two-stage cyclone classification, and a substantial decrease in removal efficiency. This comparative example illustrates that selective grinding is a key prerequisite for this application; conventional grinding cannot create particle size differences between minerals, and even using the same classification and flotation process, it is impossible to obtain a qualified product.
[0082] Comparative Example 5 This comparative example uses the same raw ore and grinding conditions as Example 1, but the diameter of the hydrocyclone underflow nozzle exceeds the limits specified in this application.
[0083] First-stage cyclone: φ350mm, sand discharge nozzle diameter 105mm (0.30 times the cylinder diameter, exceeding the range of 0.08-0.15), feed pressure 0.10MPa.
[0084] Secondary cyclone: φ250mm, sand discharge nozzle diameter 75mm (0.30 times the cylinder diameter, exceeding the range of 0.15-0.25), feed pressure 0.08MPa.
[0085] The grades and recovery rates of primary overflow tailings 1, secondary overflow tailings 2, secondary sedimentation pre-enrichment products and raw ore are shown in Table 13.
[0086] Table 13 Grade and Recovery Rate
[0087] The grades and recoveries of scheelite concentrate, fluorite concentrate, and raw ore are shown in Table 14.
[0088] Table 14 Grade and Recovery Rate
[0089] Analysis: An excessively large underflow nozzle diameter leads to coarser particle size during classification, resulting in a large amount of calcium-containing gangue not entering the overflow but mixing into the underflow, rendering pre-enrichment almost ineffective. This comparative example illustrates that the underflow nozzle diameter of the hydrocyclone needs to be controlled within the range specified in this application to achieve effective selective decalcification.
[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
[0091] Furthermore, those skilled in the art will understand that although some embodiments herein include certain features included in other embodiments but not others, combinations of features from different embodiments are intended to be within the scope of this application and form different embodiments. For example, any of the claimed embodiments can be used in any combination. The information disclosed in this background section is intended only to enhance the understanding of the general background of this application and should not be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
Claims
1. A method for selective liberation pre-enrichment and comprehensive recovery of ultra-low-grade, high-calcium complex tungsten ore, characterized in that, The ultra-low grade, high-calcium complex tungsten ore contains tungsten-bearing minerals, calcium-bearing gangue, associated recoverable minerals, and easily mud-forming gangue; wherein, the tungsten-bearing minerals include the scheelite, the calcium-bearing gangue includes the calcite and the dolomite, the associated recoverable minerals include the fluorite, and the easily mud-forming gangue includes the clay minerals; the WO3 grade in the ultra-low grade, high-calcium complex tungsten ore is not higher than 0.05%, and the combined mass fraction of calcite and dolomite is not less than 25%; The method includes the following steps: Selective grinding is performed on the ultra-low grade high-calcium complex tungsten ore to obtain selectively ground slurry. In the selectively ground slurry, calcium-containing gangue and easily mud-forming gangue are enriched in a particle size of less than 30 μm, and the tungsten-containing minerals and fluorite are enriched in a particle size of greater than 38 μm in the form of individual particles or rich intergrowths. The slurry after selective grinding is subjected to primary cyclone classification to obtain primary sand rich in tungsten-containing minerals and fluorite; The primary sediment is subjected to secondary cyclone classification to obtain secondary sediment enriched with tungsten-containing minerals and fluorite; The secondary sediment is slurried to obtain a slurry; the slurry is then subjected to scheelite flotation and fluorite flotation to obtain scheelite concentrate and fluorite concentrate.
2. The selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore according to claim 1, characterized in that, The ultra-low grade high-calcium complex tungsten ore has a WO3 grade of 0.005%-0.05%, a total mass fraction of calcite and dolomite of 25%-50%, and is associated with quartz and silicate gangue minerals.
3. The selective dissociation pre-enrichment and comprehensive recovery method for ultra-low grade high-calcium complex tungsten ore according to claim 1, characterized in that, At least one of the following conditions must be met: (1) The selective grinding adopts at least one of ball milling, rod milling, semi-autogenous milling and staged grinding; (2) The mass concentration of the selective grinding is 25%-40%.
4. The selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore according to claim 1, characterized in that, At least one of the following conditions must be met: (1) The first-stage cyclone classification is performed using a first-stage classification device, and the second-stage cyclone classification is performed using a second-stage classification device; The primary and secondary grading devices each independently include hydrocyclones; (2) The secondary cyclone classification and the slurry conditioning also include a third or higher cyclone classification. Each level uses the first-level sedimentation and slurry conditioning as feed and collects the overflow separately.
5. The selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore according to claim 4, characterized in that, At least one of the following conditions must be met: (1) The diameter of the underflow nozzle of the primary classifier is 0.08-0.15 of the diameter of the hydrocyclone cylinder, and the feed pressure is 0.06-0.15 MPa; (2) The diameter of the underflow nozzle of the secondary classification equipment is 0.15-0.25 of the diameter of the hydrocyclone cylinder, and the feed pressure is 0.05-0.12 MPa.
6. The selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore according to claim 1, characterized in that, At least one of the following conditions must be met: (1) When the tungsten-bearing minerals also include wolframite, the slurry is subjected to physical beneficiation to obtain wolframite and beneficiated slurry, and the beneficiated slurry is subjected to flotation of the scheelite; The physical beneficiation includes one of gravity separation, magnetic separation, combined gravity-magnetic separation and combined gravity-flotation; (2) The first-stage cyclone classification also yields a first-stage overflow, and the second-stage cyclone classification also yields a second-stage overflow; when the tungsten content in the first-stage overflow and the second-stage overflow is low, it is removed after scavenging, concentration or classification; when the tungsten content in the first-stage overflow and the second-stage overflow is high, it is returned to the grinding or the first-stage cyclone classification.
7. The selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore according to claim 1, characterized in that, At least one of the following conditions must be met: (1) Prior to the flotation of the scheelite, regrinding is also performed; (2) The flotation reagents for scheelite flotation include pH adjuster, scheelite inhibitor, activator and scheelite collector; the pH adjuster includes sodium carbonate, the scheelite inhibitor includes water glass, the activator includes lead nitrate and the scheelite collector includes benzohydroxyxamic acid.
8. The selective dissociation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore according to claim 1, characterized in that, The flotation reagents for fluorite flotation include gangue inhibitors and fluorite collectors; The gangue inhibitor comprises water glass, and the fluorite collector comprises oleic acid.
9. The selective liberation pre-enrichment and comprehensive recovery method for ultra-low-grade high-calcium complex tungsten ore according to any one of claims 1-8, characterized in that, The WO3 grade in the scheelite concentrate is ≥30%, and the CaF2 grade in the fluorite concentrate is ≥90%.