A method for deep degradation and debromination of resin powder from waste printed circuit boards
By combining mechanical ball milling with ultrasonic oscillation, and utilizing the synergistic effect of the catalytic activity of steel slag and hydrogen peroxide solution, the problem of incomplete debromination of waste printed circuit board resin powder was solved, achieving low-energy consumption and high-efficiency debromination, and obtaining high-purity debromination resin powder.
Patent Information
- Application Number
- CN202611440408.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for debromination of resin powder from waste printed circuit boards suffer from high energy consumption, incomplete debromination, and low efficiency. Furthermore, traditional methods are prone to causing environmental pollution and resource waste.
Mechanical ball milling combined with steel slag as a milling aid was employed to achieve deep degradation and debromination of resin powder through the synergistic effect of ultrasonic oscillation and hydrogen peroxide solution. Specific steps included: crushing and sorting, ball milling, settling, and filtration. The catalytic activity of steel slag and the ultrasonic cavitation effect were utilized to enhance reaction efficiency.
It achieves low-energy, high-efficiency debromination of resin powder, obtaining high-purity debromination resin powder, taking into account both environmental friendliness and resource utilization value, and reducing energy consumption and cost.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste conversion technology, and in particular to a method for deep degradation and debromination of waste printed circuit board resin powder. Background Technology
[0002] With the rapid development of electronic technology, the generation of waste printed circuit boards (WPCBs) has increased dramatically, making their treatment and recycling an urgent environmental problem. Waste WPCBs are mainly composed of resin, metal, and glass fiber, with resin making up a significant proportion and containing toxic polymers such as brominated epoxy resins. They possess high calorific value and potential recycling value. However, traditional treatment methods such as incineration and landfill not only result in severe resource waste but also easily cause environmental pollution.
[0003] Currently, mechanical ball milling shows promise in solid waste treatment due to its mild reaction conditions and lack of the need for high temperature and pressure. However, simple mechanical ball milling for debromination suffers from high energy consumption, limited damage to the polymer resin matrix, and incomplete debromination. Advanced oxidation processes (AOPs), particularly those based on persulfate (PDS / PMS) and hydrogen peroxide (H2O2), can generate strong oxidizing free radicals that can effectively degrade BFRs. However, when directly applied to waste circuit board (WPCB) resin powder, the results are unsatisfactory due to low mass transfer efficiency and easy catalyst deactivation. In summary, current research on debromination of waste circuit board resin powder is limited by low efficiency, high cost, or demanding conditions. Summary of the Invention
[0004] The purpose of this invention is to disclose a method for deep degradation and debromination of resin powder from waste printed circuit boards, in order to solve one or more technical problems existing in the existing methods and provide at least one beneficial option or create conditions.
[0005] To achieve the above objectives, the present invention provides the following technical solution: The first aspect of this invention is to provide a method for degrading and debrominating resin powder from waste printed circuit boards, characterized by comprising the following steps: 1) Remove the components from the waste printed circuit boards, crush and sort the rare and precious metals, and then dehydrate and dry the remaining components to obtain waste printed circuit board resin powder. 2) The waste printed circuit board resin powder is mixed with steel slag, ball-milled, and then allowed to stand at room temperature to obtain the ball-milled product; 3) Add H2O2 solution to the ball-milled product, sonicate, and after the reaction is complete, remove it and let it stand at room temperature; 4) After filtration, the filtrate is a high-concentration bromine-containing solution, and the filter residue is debromination resin powder.
[0006] The method first obtains high-purity resin powder in step 1) to avoid interference from impurities in the subsequent debromination reaction, ensuring the purity and controllability of the reaction system. Innovatively, steel slag is used as a ball milling aid coupled with mechanical ball milling pretreatment, replacing the traditional pure mechanical ball milling method. Steel slag combines mechanical grinding enhancement with catalytic activity, significantly reducing ball milling energy consumption. Simultaneously, it disrupts the dense polymer matrix structure of the resin and breaks the internal C-Br bonds through mechanochemical effects, solving the problems of limited damage to the resin matrix and incomplete debromination caused by traditional ball milling. Subsequently, ultrasonic oscillation with hydrogen peroxide is combined to achieve an advanced oxidation reaction. The ultrasonic cavitation effect enhances the mass transfer efficiency of the reaction system, overcoming the drawbacks of high mass transfer resistance and insufficient reaction contact in traditional advanced oxidation technologies. At the same time, steel slag can act as a stable solid-phase catalyst, avoiding the defects of easy deactivation and loss of conventional oxidation catalysts, significantly improving the efficiency of the oxidative debromination reaction. The entire process is characterized by mild conditions and a simple workflow. High-purity debrominated resin powder can be obtained through simple filtration, achieving efficient, low-energy, and thorough debromination of waste circuit board resin powder, while taking into account both harmless treatment and the resource utilization value of the resin matrix.
[0007] In a further embodiment of the first aspect of the present invention, the mass ratio of the waste printed circuit board resin powder to steel slag is 1:(1~4). When the ratio is within this range, the steel slag can be dispersed on the surface of the resin powder particles, which can refine the resin particles and fully break down the dense resin matrix through sufficient grinding media, and also provide sufficient active catalytic sites for the subsequent oxidative debromination reaction. This effectively avoids the problems of insufficient catalytic sites and poor grinding effect when the amount of steel slag is too low, resulting in incomplete matrix destruction and low debromination efficiency; at the same time, it avoids the problems of significantly increased ineffective grinding energy consumption, material agglomeration and blockage of mass transfer in the subsequent oxidation reaction when the amount of steel slag is too high, and the fact that excessive steel slag will coat the resin active sites, thereby reducing the debromination effect and increasing material treatment costs and solid waste residue. This preferred ratio can balance the debromination effect and energy consumption cost, achieving efficient and low-cost debromination.
[0008] In a further embodiment of the first aspect of the present invention, the ball-to-material ratio in the ball milling process is 1:50. When the ball-to-material ratio is 1:50, the frequency of contact and impact force between the grinding balls and the mixture are optimal. The grinding balls can exert uniform compression, impact, and shearing effects on the material, efficiently breaking down the polymer agglomerates of the resin, fully activating the catalytic activity of the steel slag, inducing mechanochemical reactions, and assisting in breaking the stable C-Br bonds within the resin. Under low energy consumption, this ensures uniform grinding and activation effects for batches of material, improving process stability and debromination uniformity.
[0009] In a further embodiment of the first aspect of the invention, the ball mill operates at a speed of 300-450 rpm. This limited speed provides sufficient mechanical impact and shear energy to effectively break the dense cross-linked structure of the resin polymer in waste circuit boards, exposing the bromine-containing functional groups encapsulated within the resin. Simultaneously, it stimulates the active sites on the steel slag surface, laying a good foundation for subsequent ultrasonic oxidation debromination. This avoids situations where the speed is too low, resulting in insufficient mechanical force, difficulty in effectively destroying the resin matrix, low activation of C-Br bonds, and only shallow surface debromination with poor debromination completeness. Conversely, it avoids situations where the speed is too high, leading to a sharp increase in equipment energy consumption, material overheating and agglomeration, and even excessive degradation of the resin matrix, damaging the resin's resource utilization properties, and exacerbating equipment wear and shortening its service life. This speed range achieves an optimal balance between debromination effect, energy consumption, and material integrity.
[0010] In a further embodiment of the first aspect of the invention, the ball milling time is 2–12 hours. As the ball milling proceeds, the resin particles are continuously refined, the dense matrix is continuously broken down, and the internal bromine-containing groups are fully exposed. This allows for sufficient mechanochemical interaction between the steel slag and the resin, stabilizing and activating the C-Br bonds, and significantly reducing the reaction energy barrier for subsequent oxidative debromination. Limiting the upper limit of the time avoids a continuous increase in ineffective energy consumption and a significant decrease in production efficiency. Furthermore, prolonged mechanical action can easily lead to resin powder agglomeration and the covering of active sites, which inhibits the debromination reaction. It also causes excessive damage to the resin matrix, affecting subsequent resource utilization. This time parameter balances debromination depth, production energy consumption, and process efficiency.
[0011] In a further embodiment of the first aspect of the present invention, the concentration of the H2O2 solution is 20%–30%. Under the catalytic and ultrasonic coupling effect of steel slag, this high concentration of H2O2 can stably and continuously generate a large number of highly oxidizing active groups such as hydroxyl radicals, which efficiently attack and break the activated C-Br bonds in the resin, converting organic bromine into soluble inorganic bromine for removal. Limiting the upper limit of the concentration avoids excessive active groups from easily initiating side reactions, damaging the effective matrix structure of the resin, and reducing the resource utilization quality of the debromination resin.
[0012] In a further embodiment of the first aspect of the present invention, the H2O2 solution is mixed with the ball-milled product at a liquid-to-solid ratio of 25:1.
[0013] In a further embodiment of the first aspect of the present invention, the ultrasonic oscillation power is 300~400 W.
[0014] In a further embodiment of the first aspect of the present invention, the duration of the ultrasonic oscillation is 10 to 60 minutes.
[0015] In a further embodiment of the first aspect of the invention, the filtration is performed using a 0.22 μm polyethersulfone membrane.
[0016] Compared with the prior art, the beneficial effects of the present invention are: This invention proposes a method for debromination of waste printed circuit board (PCB) resin powder based on mechanical ball milling and deep chemical oxidation. The method employs a step-by-step synergistic process combining mechanical ball milling activation with ultrasonic-enhanced oxidation. The high-energy mechanical force of the ball milling (for physical breakage and chemical bond breaking) and the cavitation effect of ultrasound (for activating peroxides, such as H₂O₂) produce a synergistic degradation effect. Mechanical ball milling first disrupts the structure of the waste PCB resin powder, and then ultrasound introduces free radicals (such as -OH) to enhance the oxidizing power of the peroxides, targeting and degrading brominated organic compounds, thereby achieving deep debromination of the waste PCB resin powder. Specifically, mechanical ball milling is used for physical breakage and chemical bond breaking of the waste PCB, while ultrasonic activation of the peroxides generates free radicals for oxidative degradation of brominated organic compounds, forming a combined physical and chemical attack to achieve efficient and low-consumption debromination. Detailed Implementation
[0017] The following embodiments further illustrate the content of the present invention, but should not be construed as limiting the present invention. Any modifications and substitutions made to the methods, steps, or conditions of the present invention without departing from the spirit and essence of the present invention are within the scope of the present invention.
[0018] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.
[0019] In the following examples and comparative examples, all raw materials used are commercially available products.
[0020] Example 1 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. Remove capacitors and other components from waste printed circuit boards, and after crushing, sorting and other steps, recover rare and precious metals. The remaining components are dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:1 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 1 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0021] Example 2 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. Remove capacitors and other components from waste printed circuit boards, and after crushing, sorting and other steps, recover rare and precious metals. The remaining components are dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:2 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 1 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400W and an ultrasonic reaction time of 30min; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0022] Example 3 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:3 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 1 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0023] Example 4 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:4 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 1 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0024] Example 5 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:4 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 300 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 1 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0025] Example 6 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:4 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 350 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 1 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0026] Example 7 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:4 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 0.5 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0027] Example 8 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:4 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 2 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0028] Example 9 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:4 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of ultrapure water, with a liquid-to-solid ratio of 25:1, and let it stand for 30 minutes. S4. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S3, pass it through a membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0029] Example 10 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. Thoroughly mix the waste printed circuit board resin powder (WPCBs) and steel slag mentioned in S1 at a ratio of 1:4 (by weight); S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 2 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0030] Example 11 A method for debromination of waste printed circuit board resin powder based on mechanical ball milling and deep chemical oxidation includes the following steps: S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. The waste printed circuit board resin powder (WPCBs) mentioned in S1 is thoroughly mixed with steel slag at a ratio of 1:4 (by weight), and placed in a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 2 mL. Let it stand for 30 minutes. S4. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S3, pass it through a membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0031] Comparative Example 1 S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. Place the waste circuit board resin powder (WPCBs) mentioned in S1 into a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 300 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 2 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0032] Comparative Example 2 S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. Place the waste circuit board resin powder (WPCBs) mentioned in S1 into a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 350 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 2 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0033] Comparative Example 3 S1. After removing capacitors and other components from waste printed circuit boards, and through crushing and sorting steps, rare and precious metals are recovered. The remaining components are then dehydrated and dried to obtain waste printed circuit board resin powder. S2. Place the waste circuit board resin powder (WPCBs) mentioned in S1 into a planetary ball mill with a ball-to-material ratio of 1:50 (by weight), a ball milling speed of 400 rpm, and a ball milling time of 6 hours. S3. Take 0.2 g of the sample from S2 and place it in a centrifuge tube. Add an appropriate amount of H2O2 solution with a liquid-to-solid ratio of 25:1. The concentration of H2O2 solution is 30%, and the volume is 2 mL. S4. Place the sample from S3 in an ultrasonic oscillator for reaction, with an ultrasonic power of 400 W and an ultrasonic reaction time of 30 minutes; S5. Take an appropriate amount of the solution from the centrifuge tube after the reaction in S4, pass it through a 0.22 μm polyethersulfone membrane, and use an ion chromatograph to detect the concentration of bromide ions in the solution.
[0034] The bromine content of Examples 1-11 and Comparative Examples 1-3 was detected by ion chromatography and the debromination rate was calculated. The results are shown in Table 1. The specific surface area of the samples before and after ball milling was measured by a specific surface area meter. The results are shown in Table 2.
[0035] Table 1. Results of debromination rate determination
[0036] Table 2. Specific surface area measurement results before and after ball milling (WPCBs: steel slag = 1:4)
[0037] Comparative analysis of Examples 1-6 and Comparative Examples 1-3 shows that, under the conditions of a fixed ball-to-material ratio (50:1) and milling time (6 hours), the debromination rate is significantly affected by both the steel slag addition ratio and the milling speed. As the steel slag ratio increases from 1:1 to 1:4, and the milling speed increases from 300 rpm to 400 rpm, the debromination rate exhibits a monotonically increasing trend, reaching its maximum value (approximately 50%) at a WPCBs:steel slag ratio of 1:4 and a milling speed of 400 rpm.
[0038] Comparative analysis of Examples 4, 7-8 and Comparative Examples 1-3 shows that for any fixed steel slag ratio, the debromination rate significantly increases as the H2O2 dosage increases from 0.5 mL to 2.0 mL. For example, at a 1:4 ratio, the debromination rate can be significantly increased from approximately 30% at 0.5 mL to nearly 60% at 2.0 mL.
[0039] Comparative analysis of Examples 4, 9-11 shows that the debromination rate of "ball milling alone" is only 15%, indicating that mechanical ball milling can activate non-metallic powders for debromination, but the effect is limited; the debromination rate of "ultrasound-H2O2 alone" is extremely low, indicating that the ultrasonic cavitation effect or the active free radicals generated by H2O2 decomposition in this system cannot effectively attack the C-Br bonds; the debromination efficiency of "ball milling-static oxidation" is increased to 60%, indicating that mechanical ball milling can "activate" non-metallic powders, thereby exposing the C-Br bonds and creating favorable conditions for subsequent oxidation reactions; finally, the debromination efficiency of the "ball milling-ultrasound-H2O2" synergistic system is as high as 95%, proving that there is a significant positive synergistic effect between mechanical ball milling and ultrasonic treatment.
[0040] This result confirms that, under the extreme conditions provided by ultrasonic cavitation, sufficient H2O2 is essential for generating enough hydroxyl radicals (•OH) to efficiently break C-Br bonds. The combined results of the examples and comparative examples show that mechanical activation of steel slag improves the mass transfer and contact efficiency of the reaction, while H2O2 provides sufficient oxidation capacity under ultrasonic drive. The synergistic effect of these two factors jointly determines the overall efficiency of the debromination reaction. Furthermore, in the synergistic system of "mechanical ball milling activation-ultrasonic enhanced oxidation," the debromination rate significantly increases with the increase of the steel slag ratio and the amount of H2O2, verifying the feasibility of this process. This system fully utilizes the physical crushing and activation effect of mechanical ball milling on brominated flame retardants in waste circuit boards, combined with ultrasonic-enhanced H2O2 decomposition to generate free radicals, achieving a highly efficient synergy between mechanical activation and ultrasonic chemical oxidation.
[0041] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.
Claims
1. A method for degrading and debrominating resin powder from waste printed circuit boards, characterized in that, Includes the following steps: 1) Remove the components from the waste printed circuit boards, crush and sort the rare and precious metals, and then dehydrate and dry the remaining components to obtain waste printed circuit board resin powder. 2) The waste printed circuit board resin powder is mixed with steel slag, ball-milled, and then allowed to stand at room temperature to obtain the ball-milled product; 3) Add H2O2 solution to the ball-milled product, sonicate, and after the reaction is complete, remove it and let it stand at room temperature; 4) After filtration, the filtrate is a high-concentration bromine-containing solution, and the filter residue is debromination resin powder.
2. The method according to claim 1, characterized in that, The mass ratio of the waste printed circuit board resin powder to the steel slag is 1:(1~4).
3. The method according to claim 1, characterized in that, The ball-to-material ratio for ball milling is 1:
50.
4. The method according to claim 1, characterized in that, The ball mill rotates at a speed of 300~450 rpm.
5. The method according to claim 4, characterized in that, The ball milling time is 2 to 12 hours.
6. The method according to claim 1, characterized in that, The concentration of the H2O2 solution is 20%–30%.
7. The method according to claim 6, characterized in that, H2O2 solution is mixed with the ball-milled product at a liquid-to-solid ratio of 25:
1.
8. The method according to claim 1, characterized in that, The ultrasonic oscillation power is 300~400 W.
9. The method according to claim 8, characterized in that, The duration of the ultrasonic oscillation is 10 to 60 minutes.
10. The method according to claim 1, characterized in that, The filtration is performed using a 0.22 μm polyethersulfone membrane.