A high-conductivity low-defect aluminum strip precision manufacturing process for batteries

The aluminum strip manufacturing process, which combines dual-fluid atomized cold rolling and air-cushion flotation furnace, solves the problems of carbon deposits and coarse grains on the aluminum strip surface, achieving high conductivity and interface stability, and improving the overall performance of the aluminum strip.

CN123102737APending Publication Date: 2026-11-17JIANGSU ALCHA ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611278315.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing aluminum strip manufacturing processes suffer from several problems: incomplete removal of residual oil from the surface, which can easily lead to carbon deposit defects; conventional annealing processes result in coarse grains that limit the improvement of conductivity; and the newly formed surface after annealing is prone to uneven oxidation, leading to poor interface stability.

Method used

The process employs a dual-fluid atomization cold rolling process combined with an air cushion flotation furnace and thermal pulse annealing technology. Through the synergistic effect of composite rolling oil and high-purity nitrogen, the behavior of the rolling interface and the evolution of the internal structure are controlled. Specific gas mixing is used for rapid heating and cooling to form a uniform lubricating film and a dense passivation film, preventing carbon deposit defects and oxidation.

Benefits of technology

This method achieves low defects, high conductivity, and interface stability on the aluminum strip surface. By refining the grain structure and forming a dense passivation film, the conductivity and interface stability of the aluminum strip are improved, while the surface defect rate and oxidation risk are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102737A_ABST
    Figure CN123102737A_ABST
Patent Text Reader

Abstract

This invention relates to the field of aluminum alloy processing technology and discloses a precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries. The process includes: hot rolling high-purity aluminum ingots to obtain aluminum strip; introducing the strip into a cold rolling mill, where a composite rolling oil of specific components and preheated high-purity nitrogen are introduced into a dual-fluid atomizing nozzle, and the atomized gas is sprayed into the deformation zone for multiple cold rolling passes; the cold-rolled aluminum strip is continuously passed through an air-cushioned flotation furnace for rapid heating to 270-280°C and held at a constant temperature, during which a transverse exhaust system is activated to spray dry gas onto the aluminum strip surface to accelerate desorption; subsequently, it enters an air quenching zone, where a mixed gas containing carbon dioxide, oxygen, and nitrogen is introduced for cooling; the cold rolling and annealing processes are repeated until the target thickness is reached and the strip is coiled. This invention reduces surface carbon buildup and scratches through dual-fluid lubrication and sweeping exhaust, refines grains to improve conductivity through thermal pulse annealing, and generates a stable passivation film through reactive air quenching, thus improving the overall performance of the aluminum strip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum alloy processing technology, specifically to a precision manufacturing process for high-conductivity, low-defect aluminum strips for batteries. Background Technology

[0002] With the development of new energy battery technology, higher standards have been set for the thickness, conductivity, and surface quality of the current collector aluminum strip in battery internal components. In conventional aluminum strip manufacturing, a large amount of rolling oil is typically used for lubrication to achieve high-pressure cold rolling of thin strips. However, these residual organic lubricants on the aluminum strip surface are often difficult to completely evaporate during subsequent annealing processes. When the airflow distribution within the annealing furnace is poor, the residual oil that fails to desorb in time is prone to thermal decomposition under heat, leading to carbon deposit defects on the aluminum strip surface. This directly affects the uniformity of the subsequent coating of the battery electrode slurry.

[0003] Not only is surface cleanliness difficult to control, but existing annealing processes also have limitations in regulating the microstructure. While traditional long-duration, slow-heating annealing can eliminate processing stress from cold rolling and restore the plasticity of aluminum strips, the extended heat treatment time can easily lead to coarse internal grains. Coarse grains increase electron scattering during transport, making it difficult for the finished aluminum strip to meet the conductivity requirements of high-power batteries.

[0004] In addition, the surface of newly annealed aluminum strip has high chemical activity. During the conventional cooling and winding stages, without targeted surface protection measures, the aluminum strip surface is prone to uncontrolled uneven oxidation once it comes into contact with trace amounts of moisture in the environment. This oxidation behavior will form localized hydration patches on the aluminum strip surface, which will disrupt the physical and chemical consistency of the material surface and reduce the interfacial stability of the aluminum strip during storage and subsequent service. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a precision manufacturing process for high-conductivity, low-defect aluminum strips for batteries. This process solves the problems of incomplete desorption of residual oil on the surface of existing battery aluminum strips during manufacturing, which easily leads to carbon deposit defects; conventional annealing processes resulting in coarse grains that limit conductivity improvement; and uneven oxidation of the newly formed surface after annealing during the cooling stage, which leads to poor interface stability.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A precision manufacturing process for high-conductivity, low-defect aluminum strips for batteries includes the following steps: High-purity aluminum ingots are hot-rolled after semi-continuous casting and homogenization annealing, rolled and coiled, and then naturally cooled to room temperature to obtain hot-rolled aluminum strip. The hot-rolled aluminum strip is introduced into a multi-roll cold rolling mill. A dual-fluid atomizing nozzle is set at the entrance of the deformation zone of the mill. Composite rolling oil and preheated high-purity nitrogen are introduced into the nozzle as liquid and gas phases, respectively. The rolling oil is atomized and sprayed into the deformation zone for continuous multi-pass cold rolling as a dual-fluid temperature-controlled atomizing cold rolling process. The composite rolling oil is composed of light straight-run alkane base oil, N,N-dimethyldecylamide and diisobutyl sebacate; After cold rolling, the aluminum strip is continuously passed through the air cushion flotation furnace and rapidly heated to 270-280°C and kept at a constant temperature. During the constant temperature period, the transverse turbulent sweeping exhaust system is turned on to spray dry protective gas parallel to the surface of the aluminum strip. The aluminum strip then immediately enters the gas quenching zone, where a mixed gas of carbon dioxide, oxygen, and nitrogen is introduced to cool it to below 60°C as a thermal pulse annealing process. The processed aluminum strip is fed back into the cold rolling mill to repeat the above-mentioned dual-fluid temperature-controlled atomization cold rolling process to the target thickness. Finally, the aluminum strip that has reached the target thickness is unfolded, and the hot pulse annealing process is repeated. The finished aluminum strip is obtained by online constant tension winding and slitting.

[0007] By employing the above technical solution, the process of this invention systematically regulates the behavior of the rolling interface and the evolution of the internal structure. Specifically, heated high-purity nitrogen gas and a composite rolling oil of specific components are atomized into a two-fluid mixture. At this time, the heat of the nitrogen gas is transferred to the rolling oil droplets, reducing the kinematic viscosity and surface tension of the oil phase, which promotes a more uniform distribution of the oil film injected into the deformation zone.

[0008] In the composite rolling oil component, N,N-dimethyldecylamide undergoes chemical adsorption on the nascent aluminum strip surface via its polar groups. Combined with diisobutyl sebate filler to provide oily lubrication, the two work synergistically to establish a stable interfacial hydrodynamic film, thereby reducing the rolling friction coefficient and suppressing microscopic surface scratches. During this stage, nitrogen flow displaces oxygen from the deformation zone, preventing uncontrolled polarization oxidation of the fresh aluminum strip surface.

[0009] After cold rolling deformation, the microstructure needs to be heat-treated. This process uses an air-cushioned flotation furnace to rapidly heat to 270–280°C. This relatively high heating rate promotes the proliferation of dislocations within the aluminum strip and induces high-density recrystallization nucleation. The refinement of the grain structure reduces grain boundary electron scattering, ultimately ensuring the conductivity of the aluminum strip bulk.

[0010] To address the common problem of residual oil desorption during conventional annealing, transverse turbulent sweeping exhaust air is applied during isothermal treatment. The high-speed airflow breaks down the boundary layer of volatile organic vapors adhering to the surface of the aluminum strip, increases the concentration gradient from the solid-liquid interface to the bulk gas phase, accelerates the desorption and mass transfer process of macromolecular hydrocarbons, and prevents residual oil from undergoing cracking reactions at high temperatures to generate carbon deposits.

[0011] The cooling stage after annealing serves the function of surface modification. A specific mixed gas containing carbon dioxide, oxygen, and nitrogen is used for gas quenching. While the aluminum strip is rapidly cooled and shaped, the surface undergoes active reconstruction. The aluminum atoms at the interface react with trace amounts of oxygen to generate dense oxides, and under the action of carbon dioxide, local carbonate hybrid structures are formed, establishing a continuous and uniform modified passivation film layer. This helps to mitigate the erosion of media in the subsequent storage environment.

[0012] Preferably, the compound rolling oil is composed of 96.3-98.0 parts by weight of light straight-run alkane base oil, 0.5-1.2 parts of N,N-dimethyldecylamide and 1.5-2.5 parts of diisobutyl sebacate.

[0013] By adopting the above technical solution, the ratio of straight-run alkanes, amides and esters is controlled, which better balances the interfacial bearing capacity required for rolling and the volatility during the annealing process, and prevents high-temperature desorption difficulties caused by excessive polar additives.

[0014] Preferably, the preparation method of the composite rolling oil includes: In an explosion-proof mixing vessel equipped with a mechanical stirrer, maintain the temperature inside the vessel at 25–30°C, and sequentially add N,N-dimethyldecylamide and diisobutyl sebacate to the light straight-run alkane base oil. Stir continuously at a speed of 150–200 r / min for 30–45 min until an optically transparent homogeneous solution is formed.

[0015] By adopting the above technical solution, the mixing process of the liquid phase is standardized, the shear rate and dissolution temperature are controlled, which is conducive to the full mutual solubility and dispersion of molecules with different polarities, avoids microscopic stratification during long-term storage, and ensures the uniformity of component concentration inside the spray droplets.

[0016] Preferably, high-purity aluminum ingots with a purity of 99.35% are subjected to semi-continuous casting and homogenization annealing, and then hot-rolled at a temperature of 450–500°C to a thickness of 6.0–8.0 mm, coiled up and naturally cooled to room temperature.

[0017] By adopting the above technical solution, defining the purity and hot deformation temperature of the initial billet, it is possible to release the internal casting residual stress and establish an initial texture that is conducive to subsequent large deformation cold rolling.

[0018] Preferably, when the composite rolling oil and high-purity nitrogen are introduced into the dual-fluid atomizing nozzle, the high-purity nitrogen is preheated to 75-80°C. The liquid phase pressure of the composite rolling oil pumped into the dual-fluid atomizing nozzle is 0.8–1.2 MPa, and the gas phase pressure of the high-purity nitrogen gas introduced into the dual-fluid atomizing nozzle is 0.5–0.8 MPa.

[0019] By adopting the above technical solution, the gas phase input of 75-80°C allows the temperature of the droplets after impact mixing to be controlled within a suitable lubrication viscosity range. The matched gas-liquid phase pressure difference promotes the shearing and breaking of the liquid film inside the nozzle, forming fine aerosols with a concentrated average particle size, thereby improving the coverage of the lubricating medium in the deformation zone.

[0020] Preferably, when the obtained aluminum strip is introduced into a multi-roll cold rolling mill for continuous multi-pass cold rolling, the cumulative deformation reaches 60% to 65% after continuous multi-pass cold rolling.

[0021] By adopting the above technical solution, the deformation energy storage of each rolling round is limited, providing the necessary deformation driving force for recrystallization in the subsequent hot pulse annealing process.

[0022] Preferably, the cold-rolled aluminum strip is continuously passed through an air cushion type air flotation furnace under a constant tension of 5-10 MPa. The upper and lower slit nozzles are opened to spray high-speed hot air at 350-400°C to lift the aluminum strip, and it is rapidly heated at a heating rate of 45-50°C / s in conjunction with a near-infrared radiation array.

[0023] By adopting the above technical solution, non-contact suspension heating is achieved through the slit jet effect, which reduces the physical contact marks between the conventional furnace rollers and the aluminum strip surface. Combined with near-infrared radiation, the heat conduction time is shortened, and the specified heating rate is achieved to control the grain size.

[0024] Preferably, the temperature is maintained for 4 to 6 seconds; during the temperature maintenance period, the wind speed of the dry protective gas sprayed parallel to the surface of the aluminum strip is 25 to 35 m / s.

[0025] By adopting the above technical solution, the momentum transfer and mass transfer of the organic medium are completed under the premise of suppressing grain boundary migration and growth, and the degreasing and annealing processes are realized simultaneously.

[0026] Preferably, when entering the air quenching zone for cooling, the temperature is reduced at a cooling rate of 30-40℃ / s; The introduced mixed gas has a dew point of -45℃ to -40℃ and, by volume percentage, consists of 1.5% to 2.5% carbon dioxide, 0.1% to 0.3% oxygen, and 97.2% to 98.4% nitrogen.

[0027] By adopting the above technical solution, a cooling environment with controlled dew point is used to prevent surface hydration oxide spots caused by moisture. At the same time, the volume percentage of the reactant gas is limited to control the growth kinetics of the oxide film and avoid the oxide layer being too thick, which would affect the conductivity.

[0028] Preferably, when the treated aluminum strip is fed back into the cold rolling mill for repeated dual-fluid temperature-controlled atomization cold rolling process, the target thickness is 12-15 μm.

[0029] By adopting the above technical solutions, the thickness of the finished product after multiple rounds of process iterations is guaranteed to meet the ultra-thin specification standard required by the battery.

[0030] This invention provides a precision manufacturing process for high-conductivity, low-defect aluminum strips used in batteries. It offers the following advantages: 1. This invention utilizes preheated high-purity nitrogen and composite rolling oil for two-fluid atomization at the mill inlet, forming a uniform lubricating film on the newly formed aluminum strip surface using specific amide and ester components, thus reducing frictional damage at the rolling interface. Simultaneously, introducing transverse turbulent sweeping exhaust air during the annealing isothermal stage accelerates the desorption and mass transfer rate of residual macromolecular hydrocarbons on the aluminum strip surface. This synergistic control of rolling lubrication and annealing desorption prevents residual oil from cracking at high temperatures, reducing carbon buildup and scratch defects on the aluminum strip surface.

[0031] 2. This invention utilizes an air-cushioned flotation furnace combined with near-infrared radiation for thermal pulse annealing of aluminum strips, rapidly heating the strips at a rate of 45-50℃ / s. This relatively high heating rate provides sufficient recrystallization deformation driving force, promoting high-density nucleation within the material, thereby refining the micro-grain size. The refined grain structure reduces the electron scattering effect at internal grain boundaries, improving the overall electrical conductivity of the finished product while restoring the processing plasticity of the aluminum strip.

[0032] 3. In the cooling zone after annealing, the present invention uses a mixture of carbon dioxide, oxygen and nitrogen with a specific dew point and ratio for gas quenching and cooling. During the rapid cooling and shaping process, the mixed gas participates in the chemical reconstruction of the aluminum strip surface, causing the aluminum atoms at the interface to react with oxygen and carbon dioxide to generate a dense hybrid passivation film containing aluminum oxide and carbonate. This passivation layer seals the active sites on the aluminum strip surface, which can reduce the corrosion of the medium in the subsequent winding and storage environment and maintain the long-term stability of the aluminum strip interface state. Attached Figure Description

[0033] Figure 1 This is a line graph showing the change of transient temperature of the oil droplets over time according to the present invention. Figure 2 This is a line graph showing the change of local oxygen concentration over time according to the present invention. Figure 3 This is the attenuated total reflectance Fourier transform infrared spectrum of N,N-dimethyldecylamide adsorbed on the surface of the aluminum strip of the present invention. Figure 4 This is an engineering stress-strain curve of the room temperature uniaxial tensile process of the present invention. Figure 5 This is a two-dimensional contour scan curve of the aluminum strip surface of the present invention; Figure 6 This is a time-domain curve of strip tension fluctuation during the stable rolling stage of this invention. Detailed Implementation

[0034] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0035] Preparation Example 1: This preparation example provides a method for preparing a composite rolling oil, including the following steps: In an explosion-proof mixing vessel equipped with a mechanical stirrer, maintaining the vessel temperature at 25°C, 0.5 parts by weight of N,N-dimethyldecylamide and 1.5 parts by weight of diisobutyl sebacate were added sequentially to 98.0 parts of light straight-run alkane base oil. The mixture was stirred continuously at 150 r / min for 30 min until an optically transparent homogeneous solution was formed. After preparation, the resulting composite rolled oil was pumped into a storage tank, and the storage tank temperature was maintained at 25°C.

[0036] Preparation Example 2: This preparation example provides a method for preparing a composite rolling oil, including the following steps: In an explosion-proof mixing vessel equipped with a mechanical stirrer, maintaining the vessel temperature at 28°C, 0.8 parts by weight of N,N-dimethyldecylamide and 2.0 parts by weight of diisobutyl sebacate were added sequentially to 97.2 parts of light straight-run alkane base oil. The mixture was stirred continuously at 180 r / min for 40 min until an optically transparent homogeneous solution was formed. After preparation, the resulting composite rolled oil was pumped into a storage tank, and the storage tank temperature was maintained at 28°C.

[0037] Preparation Example 3: This preparation example provides a method for preparing a composite rolling oil, including the following steps: In an explosion-proof mixing vessel equipped with a mechanical stirrer, maintaining the vessel temperature at 30°C, 1.2 parts by weight of N,N-dimethyldecylamide and 2.5 parts by weight of diisobutyl sebacate were added sequentially to 96.3 parts of light straight-run alkane base oil. The mixture was stirred continuously at 200 r / min for 45 min until an optically transparent homogeneous solution was formed. After preparation, the resulting composite rolled oil was pumped into a storage tank, and the storage tank temperature was maintained at 30°C.

[0038] Example 1: This embodiment provides a precision manufacturing process for high-conductivity, low-defect aluminum strips for batteries, including the following steps: High-purity aluminum ingots with a purity of 99.35% are semi-continuously cast and homogenized annealed, then hot-rolled at 450°C to a thickness of 6.0 mm, coiled and naturally cooled to room temperature.

[0039] The obtained aluminum strip is introduced into a multi-roll cold rolling mill. A dual-fluid atomizing nozzle is set at the entrance of the deformation zone of the mill. The composite rolling oil obtained in Preparation Example 1 is pumped into the nozzle at a liquid phase pressure of 0.8 MPa. At the same time, high-purity nitrogen gas preheated to 75°C is introduced into the nozzle at a gas phase pressure of 0.5 MPa. The rolling oil is atomized, wrapped, and sprayed into the deformation zone. The cold rolling is performed continuously for multiple passes until the cumulative deformation reaches 60%.

[0040] The cold-rolled aluminum strip passes through the air cushion flotation furnace continuously under a constant tension of 5MPa. The upper and lower slit nozzles are opened to spray a high-speed hot air stream of 350°C to lift the aluminum strip. In conjunction with the near-infrared radiation array, the aluminum strip is rapidly heated to 270°C at a heating rate of 45°C / s. The temperature was kept constant at 270℃ for 4 seconds, during which the transverse turbulent sweeping exhaust system was activated to spray dry protective gas at a wind speed of 25 m / s parallel to the surface of the aluminum strip. The aluminum strip then immediately enters the gas quenching zone, where a mixed gas with a volume ratio of 1.5% carbon dioxide, 0.1% oxygen, and 98.4% nitrogen is introduced. The dew point of the mixed gas is -45°C, and the temperature is reduced to below 60°C at a cooling rate of 30°C / s.

[0041] The treated aluminum strip is fed back into the cold rolling mill to repeat the above-mentioned two-fluid temperature-controlled atomization cold rolling process until the thickness reaches 12μm. Finally, the finished aluminum strip is unfolded and the above-mentioned hot pulse annealing process is repeated (heating to 270℃ at 45℃ / s, forced sweeping and holding for 4s, and air quenching to cool down to below 60℃), and then online constant tension winding and slitting are performed to obtain the finished product.

[0042] Example 2: This embodiment provides a precision manufacturing process for high-conductivity, low-defect aluminum strips for batteries, including the following steps: High-purity aluminum ingots with a purity of 99.35% are hot-rolled at 475°C after semi-continuous casting and homogenization annealing to a thickness of 7.0 mm, then coiled and naturally cooled to room temperature.

[0043] The obtained aluminum strip is introduced into a multi-roll cold rolling mill. A dual-fluid atomizing nozzle is set at the entrance of the deformation zone of the mill. The composite rolling oil obtained in Preparation Example 2 is pumped into the nozzle at a liquid phase pressure of 1.0 MPa. At the same time, high-purity nitrogen gas preheated to 78°C is introduced into the nozzle at a gas phase pressure of 0.65 MPa. The rolling oil is atomized, wrapped, and sprayed into the deformation zone. The cold rolling is performed continuously for multiple passes until the cumulative deformation reaches 63%.

[0044] The cold-rolled aluminum strip passes through the air cushion flotation furnace continuously under a constant tension of 8MPa. The upper and lower slit nozzles are opened to spray a high-speed hot air stream of 375°C to lift the aluminum strip. In conjunction with the near-infrared radiation array, the aluminum strip is rapidly heated to 275°C at a heating rate of 48°C / s. The temperature was kept constant at 275℃ for 5 seconds, during which the transverse turbulent sweeping exhaust system was activated to spray dry protective gas at a wind speed of 30 m / s parallel to the surface of the aluminum strip. The aluminum strip is then immediately introduced into the gas quenching zone, where a mixed gas of 2.0% carbon dioxide, 0.2% oxygen, and 97.8% nitrogen (by volume) is introduced. The dew point of the mixed gas is -42°C, and the strip is cooled to below 60°C at a cooling rate of 35°C / s. The treated aluminum strip is then fed back into the cold rolling mill to repeat the above two-fluid temperature-controlled atomization cold rolling process until a thickness of 13.5 μm is achieved.

[0045] Finally, the finished aluminum strip is unrolled and the above-mentioned hot pulse annealing process is repeated (heating to 275℃ at 48℃ / s, forced sweeping and holding for 5s, and gas quenching to cool down to below 60℃). The finished product is obtained by online constant tension winding and slitting.

[0046] Example 3: This embodiment provides a precision manufacturing process for high-conductivity, low-defect aluminum strips for batteries, including the following steps: High-purity aluminum ingots with a purity of 99.35% are semi-continuously cast and homogenized annealed, then hot-rolled at 500°C to a thickness of 8.0 mm, coiled up and naturally cooled to room temperature.

[0047] The obtained aluminum strip is introduced into a multi-roll cold rolling mill. A dual-fluid atomizing nozzle is set at the entrance of the deformation zone of the mill. The composite rolling oil obtained in Preparation Example 3 is pumped into the nozzle at a liquid phase pressure of 1.2 MPa. At the same time, high-purity nitrogen gas preheated to 80°C is introduced into the nozzle at a gas phase pressure of 0.8 MPa. The rolling oil is atomized, wrapped, and sprayed into the deformation zone. The cold rolling is performed continuously for multiple passes until the cumulative deformation reaches 65%.

[0048] The cold-rolled aluminum strip passes through the air cushion flotation furnace continuously under a constant tension of 10MPa. The upper and lower slit nozzles are opened to spray a high-speed hot air stream of 400℃ to lift the aluminum strip. In conjunction with the near-infrared radiation array, the aluminum strip is rapidly heated to 280℃ at a heating rate of 50℃ / s. The temperature was kept constant at 280℃ for 6 seconds, during which the transverse turbulent sweeping exhaust system was activated to spray dry protective gas at a wind speed of 35 m / s onto the surface of the aluminum strip in parallel. The aluminum strip then immediately enters the gas quenching zone, where a mixed gas with a volume ratio of 2.5% carbon dioxide, 0.3% oxygen, and 97.2% nitrogen is introduced. The dew point of the mixed gas is -40°C, and the temperature is reduced to below 60°C at a cooling rate of 40°C / s.

[0049] The processed aluminum strip is fed back into the cold rolling mill and the above-mentioned dual-fluid temperature-controlled atomization cold rolling process is repeated until the thickness is 15μm. Finally, the finished aluminum strip is unfolded and the above-mentioned hot pulse annealing process is repeated (heating to 280℃ at 50℃ / s, forced sweeping and holding for 6s, and air quenching to cool down to below 60℃). The finished product is obtained by online constant tension winding and slitting.

[0050] Comparative Example 1: Compared with Example 2, the difference is that N,N-dimethyldecanoamide is not added to the composite rolling oil, but is replaced with an equal weight of hexadecanoic acid, while the rest are the same.

[0051] Comparative Example 2: Compared with Example 2, the difference is that diisobutyl sebacate is not added to the compound rolling oil, but is replaced with an equal part by weight of light straight-run alkane base oil, while the rest are the same.

[0052] Comparative Example 3: Compared with Example 2, the difference is that the rolling process does not use a dual-fluid atomizing nozzle and high-temperature, high-purity nitrogen. Instead, the composite rolling oil in the storage tank is preheated to 65°C and directly sprayed with a single-fluid nozzle at a liquid phase pressure of 1.0 MPa. All other aspects are the same.

[0053] Comparative Example 4: Compared with Example 2, the difference is that during the 275°C constant temperature maintenance stage of the air cushion flotation furnace, the transverse turbulent sweeping exhaust system is turned off, and the dry protective gas is not sprayed parallel to the aluminum strip surface; otherwise, they are the same.

[0054] Comparative Example 5: Compared with Example 2, the difference is that the gas introduced during the gas quenching stage is 100% pure nitrogen, without the mixing of carbon dioxide and oxygen, while the rest are the same.

[0055] Comparative Example 6: Compared with Example 2, the difference is that instead of using an air cushion type air flotation furnace for rapid thermal pulse annealing, the aluminum strip is placed in a conventional bell-type annealing furnace and heated to 300°C at a heating rate of 1°C / s, held for 2 hours, and then cooled naturally with the furnace. All other aspects are the same.

[0056] Test Example 1: Test steps: The cold rolling mill inlet deformation zone of Examples 1 to 3 was selected as the test area. A paramagnetic oxygen concentration sensor and a K-type ultrafine thermocouple with a diameter of 0.1 mm were arranged at the center of the dual-fluid atomized enveloping jet at the intersection of the roll gap and the aluminum strip.

[0057] Start the dual-fluid nozzle to a continuous and stable operating state, and continuously collect local oxygen concentration and oil droplet transient temperature data during the 0 to 50 ms period before the jet reaches the aluminum strip surface at a sampling frequency of 1000 Hz.

[0058] Record dynamic data at different time points, and use the measurement value at 40ms as a reference evaluation index before reaching the deformation zone of the rolling mill.

[0059] Test data: Table 1. Dynamic oxygen concentration and oil droplet temperature test data for each embodiment. in conclusion: Figure 1 This is a line graph showing the change of transient temperature of oil droplets over time according to the present invention. The horizontal axis represents time in milliseconds (ms), and the vertical axis represents temperature in degrees Celsius (°C). The red line represents Example 1, the blue line represents Example 2, and the green line represents Example 3.

[0060] Figure 2 This is a line graph showing the change of local oxygen concentration over time according to the present invention. The horizontal axis represents time in milliseconds (ms), and the vertical axis represents oxygen concentration in vol%. The red line represents Example 1, the blue line represents Example 2, and the green line represents Example 3.

[0061] Based on the data in Table 1 and Figure 1 , Figure 2 As can be seen from the content, the dual-fluid atomization design spatially decouples the storage environment of the rolling oil from the heating process. At room temperature, the rolling oil is sheared by high-purity nitrogen gas heated at the nozzle, forming micron-sized droplets. Within 0 to 40 ms, the droplet temperature rapidly rises from room temperature to the range of 63.5℃ to 66.8℃, achieving the viscosity reduction requirement and promoting the wetting of N,N-dimethyldecanoic acid and diisobutyl sebacate molecules on the aluminum substrate surface.

[0062] High-purity nitrogen, used as the carrier gas, formed an inert gas envelope in the deformation zone. Over time, the local oxygen concentration was controlled between 4.34 vol% and 5.21 vol% at 40 ms. This oxygen concentration is below the limiting oxygen concentration for flash combustion of light straight-run alkane base oils.

[0063] This design avoids the oxidation risk associated with directly heating large amounts of base oil and eliminates the ignition conditions for high-temperature oil mist in the high-friction environment of the rolls. Based on the variation trends of data from various process parameters, increasing nitrogen pressure and temperature accelerates the heating rate of oil droplets and further reduces local oxygen concentration, consistent with momentum transfer and heat transfer mechanisms.

[0064] Test Example 2: Test steps: Intermediate aluminum strips from Examples 2 and 5 that had undergone air quenching but had not yet undergone the next cold rolling pass were taken as substrate test samples. Simultaneously, the composite rolling oil (containing N,N-dimethyldecanoic acid) used in Example 2 and the composite rolling oil (containing hexadecanoic acid) used in Comparative Example 1 were extracted as adsorbate samples.

[0065] After surface cleaning, the aluminum strip samples were cut to standard size and placed in the test cell of the flow potential meter. A neutral 0.001 mol / L potassium chloride solution was used as the background electrolyte, and the surface zeta potential of each sample was measured at 25°C.

[0066] Adsorption enthalpy change was tested using an isothermal titration calorimeter. Aluminum strip samples were processed into micro-powders with uniform specific surface area and dispersed in a non-polar solvent. Under constant temperature of 25℃, a corresponding ratio of composite rolling oil was gradually added dropwise to the sample cell. The heat change was recorded, and the adsorption enthalpy change was calculated using a fitting method.

[0067] The aluminum strip samples from Example 2 and Comparative Example 5 were immersed in the composite rolling oil of Example 2 for 20 minutes. After removal, the surface was rinsed with n-hexane to remove unbonded free oil molecules, and then dried in a vacuum drying oven. The infrared absorption spectra of the adsorbed layer were obtained by scanning the sample surface with an attenuated total reflectance Fourier transform infrared spectrometer.

[0068] Test data: Table 2. Zeta potential and adsorption enthalpy change test data of aluminum strip surface under different processing techniques in conclusion: Figure 3 This is the attenuated total reflectance Fourier transform infrared spectrum of N,N-dimethyldecanoic acid adsorbed on the surface of the aluminum strip according to the present invention, where the horizontal axis represents the wavenumber in cm⁻¹. -1 The vertical axis represents absorbance in au. The solid line represents the aluminum strip substrate of Example 2, and the dashed line represents the aluminum strip substrate of Comparative Example 5.

[0069] Based on the data in Table 2 and Figure 3 The results show that carbon dioxide and oxygen in the mixed gas during the gas quenching stage participated in the chemical reconstruction of the aluminum strip surface. In Example 2, after the mixed gas was introduced, the Zeta potential of the aluminum strip surface was negative, ranging from -13.9mV to -14.2mV.

[0070] Comparative Example 5, purged only with pure nitrogen, exhibited a positive Zeta potential. This negative Zeta potential environment matched the adsorption process of N,N-dimethyldecanoamide molecules, resulting in an adsorption enthalpy change of -63.8 kJ / mol, exceeding the threshold for chemisorption. In contrast, the adsorption enthalpy change of the substrate in Comparative Example 5 when bound to N,N-dimethyldecanoamide was only -22.1 kJ / mol, corresponding to a van der Waals force-dominated binding state.

[0071] After switching to hexadecanoic acid, although the heat of adsorption changed, it did not reach the level of strong chemical coordination. Figure 3 Infrared spectral data showed that the C=O stretching vibration peak of the residual molecules on the substrate of Comparative Example 5 was located at 1648 cm⁻¹, close to the theoretical peak position of free molecules. The C=O stretching vibration peak of the residual molecules on the substrate of Example 2 shifted to 1615 cm⁻¹. -1 Place.

[0072] The shift of the peak position towards lower wavenumbers indicates that the lone pair electrons on the carbonyl oxygen atom have undergone coordination bonding with the reconstructed weakly acidic aluminum substrate, leading to a decrease in the force constant of the C=O double bond. The test results confirm that rapid cooling using a mixture of oxygen and carbon dioxide within a specific temperature window can generate a passivation film on the surface that alters its charge properties. This promotes the formation of a stable coordination adsorption layer at the metal interface by the lubricating medium containing amide groups, improving the resistance of the boundary lubricating film to damage during subsequent rolling processes.

[0073] Test Example 3: Test steps: Finished aluminum strips prepared in Examples 1 to 3 and Comparative Example 6 were used as test subjects. Along the rolling direction of the aluminum strip, the samples were punched into rectangular cross-section tensile specimens conforming to GB / T 228.1 standard using a precision punching machine, and the gauge length was marked.

[0074] The tensile specimen was mounted on the fixture of a computer-controlled electronic universal testing machine, and the tensile speed was set to 2.0 mm / min. Uniaxial tension was performed at room temperature until the specimen fractured. The load-displacement data throughout the process were recorded, and the tensile strength was calculated.

[0075] Take another aluminum strip sample from the same batch and cut it into strips 1000 mm long and 10 mm wide. Place them in a constant temperature oil bath at 20°C to maintain temperature equilibrium. Connect the two ends of the sample using a double-arm bridge resistance tester and measure its resistance value. Calculate the volumetric conductivity based on the sample's geometry. The result is expressed as %IACS.

[0076] Test data: Table 3. Test data of tensile strength and electrical conductivity of finished products under different annealing processes in conclusion: Figure 4 This is an engineering stress-strain curve of the room temperature uniaxial tensile process of the present invention, where the horizontal axis is engineering strain in % and the vertical axis is engineering stress in MPa. The solid line represents Example 2 and the dashed line represents Comparative Example 6.

[0077] Based on the data in Table 3 and Figure 4 As can be seen from the content, the air-float rapid annealing process achieves a balance between strength and conductivity. The tensile strength of the finished aluminum strips in Examples 1 to 3 is maintained in the range of 185.3 MPa to 191.2 MPa, and the conductivity reaches 61.1% IACS to 61.8% IACS.

[0078] Comparative Example 6 underwent conventional long-term heat treatment, resulting in a tensile strength reduction to 112.4 MPa. The examples employed a heating rate of 45°C to 50°C per second and limited the holding time to 4 to 6 seconds, controlling the total heat input to the material. The short-duration high-temperature environment caused point defects such as vacancies in the aluminum matrix, as well as some easily movable edge dislocations, to slip and annihilate, reducing the scattering probability of electrons in lattice transport and thus restoring conductivity.

[0079] Meanwhile, the brief isothermal phase failed to provide sufficient incubation period and driving force to trigger large-angle migration of grain boundaries. This thermal intervention preserves the high-density dislocation network and crystal defect barrier structure accumulated from cold rolling deformation, avoiding strength loss caused by complete recrystallization. Conventional annealing processes, due to excessively long holding times, cause grain growth and recrystallization, leading to the elimination of work hardening effects and softening. Therefore, this scheme achieves decoupled intervention of resistance reduction and strength preservation under controlled holding window conditions.

[0080] Test Example 4: Test steps: Finished aluminum strips from Examples 1 to 3, Comparative Example 2, and Comparative Example 4 were taken as test samples.

[0081] Test blocks measuring 100mm × 100mm were cut from each sample. The test blocks were placed in the combustion boat of a total organic carbon combustion analyzer and heated to 650℃ in a pure oxygen stream to completely oxidize the residual organic matter on the surface into carbon dioxide. The amount of carbon dioxide released was measured using a non-dispersive infrared detector, and the residual carbon content per square meter of aluminum strip surface was calculated.

[0082] Take another batch of test samples from the same batch and perform continuous scanning tests using a probe-type surface profilometer perpendicular to the rolling direction. Set the sampling length to 0.8 mm and the evaluation length to 4.0 mm, measure and record the surface profile data, and calculate the arithmetic mean roughness Ra.

[0083] Test data: Table 4. Test data on surface residual carbon content and roughness under different formulations and annealing conditions in conclusion: Figure 5 This is a two-dimensional contour scanning curve of the aluminum strip surface of the present invention, where the horizontal axis is the scanning length in μm, the vertical axis is the contour height in μm, the red line represents Example 2, and the blue line represents Comparative Example 2.

[0084] Based on the data in Table 4 and Figure 5 The content shows that the lateral airflow sweeping mechanism promotes the transfer of organic lubricants attached to the metal interface to the gas phase.

[0085] The residual carbon content on the surface of the finished aluminum strips in Examples 1 to 3 was controlled at 2.1 mg / m². 2 Up to 2.4 mg / m 2 In contrast, in Comparative Example 4, the residual carbon content on the surface increased to 18.7 mg / m2 due to the closure of the transverse exhaust system.

[0086] The parallel-injected dry gas disrupts the vapor-rich boundary layer on the aluminum strip surface, alters the vapor partial pressure at the interface, accelerates the desorption mass transfer rate of diisobutyl sebacate and N,N-dimethyldecylamide, and prevents residual organic molecules from undergoing thermal decomposition reactions and forming carbon deposits in the annealing furnace.

[0087] Diisobutyl sebacate in the composite rolling oil formulation exhibits compressive viscous response characteristics. The surface roughness Ra of the sample in the examples ranged from 0.11 μm to 0.13 μm. In Comparative Example 2, this component was removed, and its surface roughness Ra increased to 0.42 μm. Figure 5 The profile curves show that the surface of Comparative Example 2 has fluctuations, accompanied by troughs with a depth of more than 0.4 μm.

[0088] This reflects that in the absence of specific diester molecules, conventional alkane base oils do not achieve sufficient viscosity increase when subjected to high pressures of hundreds of megapascals in the deformation zone, leading to localized rupture of the bearing oil film and direct contact and frictional scratches between the metal substrate and the rolls.

[0089] Test Example 5: Test steps: Aluminum strips that had completed preliminary processing and were ready to enter the final cold rolling pass from Examples 1 to 3, Comparative Examples 1, 3 and 5 were selected as test subjects.

[0090] The aluminum strip to be tested is threaded into the multi-roll cold rolling mill, with the target processing thickness set to 12μm to 15μm. The winding tension control system is then activated for continuous processing. After completing 10,000m of coil processing, the number of strip breaks during the process is counted, and the average number of strip breaks per 10,000 meters is calculated.

[0091] A piezoelectric tension sensor is installed at the bearing housing of the tension roll at the exit of the cold rolling mill. After the mill speed reaches a stable state, the tension feedback signal is continuously collected at a frequency of 500Hz for 10 seconds. The instantaneous tension data during this period is extracted, and the standard deviation of tension fluctuation is calculated.

[0092] Test data: Table 5. Statistical data on the stability of cold rolling under different process parameters in conclusion: Figure 6 This is a time-domain curve of strip tension fluctuation during the stable rolling stage of the present invention. The horizontal axis represents time in seconds, and the vertical axis represents tension deviation in MPa. The red line represents Example 2, and the blue line represents Comparative Example 3.

[0093] Based on the data in Table 5 and Figure 6 The content shows that the spatially decoupled heating method and the interface reconstruction mechanism together maintain the continuity of the metal cold forming process.

[0094] In Examples 1 to 3, when the target thickness was achieved, the number of strip breaks per 10,000 meters was between 0.8 and 1.3, and the standard deviation of tension fluctuation was controlled within the range of 0.72 MPa to 0.86 MPa. In Comparative Example 3, which used conventional high-pressure spray preheating rolling oil, the distribution of the lubricating layer in the deformation zone was different, resulting in a rise in the standard deviation of tension fluctuation to 4.38 MPa and an increase in the number of strip breaks to 8.6 times per 10,000 meters.

[0095] Figure 6 In Comparative Example 3, the tension signal exhibited abrupt spikes at multiple time points. These spikes reflected local rupture of the lubricating film in the pressure zone of hundreds of megapascals, direct contact between the metal substrate and the work roll, and the change in friction state caused an imbalance in the tension of the strip during operation.

[0096] Comparative Example 1 used hexadecanoic acid to replace N,N-dimethyldecylamide, and Comparative Example 5 used pure nitrogen gas quenching, resulting in the substrate lacking a modified passivation film. The breakage rate and tension fluctuation of these two sets of data were also higher than those of the Example group.

[0097] Test results verified that the high-bond-energy chemical coordination adsorption layer formed by the combination of amide-containing additive molecules and the alumina / aluminum carbonate composite film treated in a specific atmosphere can withstand strong shear failure. This boundary lubrication structure reduces the probability of abrupt changes in the friction coefficient, avoids local stress concentration and fracture of the aluminum strip during the thinning process, and ensures the stability of continuous production operations.

Claims

1. A precision manufacturing process for high-conductivity, low-defect aluminum strips for batteries, characterized in that, Includes the following steps: High-purity aluminum ingots are hot-rolled after semi-continuous casting and homogenization annealing, rolled and coiled, and then naturally cooled to room temperature to obtain hot-rolled aluminum strip. The hot-rolled aluminum strip is introduced into a multi-roll cold rolling mill. A dual-fluid atomizing nozzle is set at the entrance of the deformation zone of the mill. Composite rolling oil and preheated high-purity nitrogen are introduced into the nozzle as liquid and gas phases, respectively. The rolling oil is atomized and sprayed into the deformation zone for continuous multi-pass cold rolling as a dual-fluid temperature-controlled atomizing cold rolling process. The composite rolling oil is composed of light straight-run alkane base oil, N,N-dimethyldecylamide and diisobutyl sebacate; After cold rolling, the aluminum strip is continuously passed through the air cushion flotation furnace and rapidly heated to 270-280°C and kept at a constant temperature. During the constant temperature period, the transverse turbulent sweeping exhaust system is turned on to spray dry protective gas parallel to the surface of the aluminum strip. The aluminum strip then immediately enters the gas quenching zone, where a mixed gas of carbon dioxide, oxygen, and nitrogen is introduced to cool it to below 60°C as a thermal pulse annealing process. The processed aluminum strip is fed back into the cold rolling mill to repeat the above-mentioned dual-fluid temperature-controlled atomization cold rolling process to the target thickness. Finally, the aluminum strip that has reached the target thickness is unfolded, and the hot pulse annealing process is repeated. The finished aluminum strip is obtained by online constant tension winding and slitting.

2. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, The compound rolling oil, by weight, consists of 96.3-98.0 parts of light straight-run alkane base oil, 0.5-1.2 parts of N,N-dimethyldecylamide, and 1.5-2.5 parts of diisobutyl sebacate.

3. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 2, characterized in that, The preparation methods of composite rolling oil include: In an explosion-proof mixing vessel equipped with a mechanical stirrer, maintain the temperature inside the vessel at 25–30°C, and sequentially add N,N-dimethyldecylamide and diisobutyl sebacate to the light straight-run alkane base oil. Stir continuously at a speed of 150–200 r / min for 30–45 min until an optically transparent homogeneous solution is formed.

4. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, The process of hot rolling high-purity aluminum ingots after semi-continuous casting and homogenization annealing, followed by rolling, coiling, and natural cooling to room temperature to obtain hot-rolled aluminum strip, specifically includes: High-purity aluminum ingots with a purity of 99.35% are semi-continuously cast and homogenized annealed, then hot-rolled at a temperature of 450–500°C to a thickness of 6.0–8.0 mm, coiled up, and naturally cooled to room temperature.

5. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, When the composite rolling oil and high-purity nitrogen are introduced into the dual-fluid atomizing nozzle, the high-purity nitrogen is preheated to 75-80°C. The liquid phase pressure of the composite rolling oil pumped into the dual-fluid atomizing nozzle is 0.8–1.2 MPa, and the gas phase pressure of the high-purity nitrogen gas introduced into the dual-fluid atomizing nozzle is 0.5–0.8 MPa.

6. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, When the obtained aluminum strip is introduced into a multi-roll cold rolling mill for continuous multi-pass cold rolling, the cumulative deformation reaches 60% to 65%.

7. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, The cold-rolled aluminum strip is continuously passed through an air-cushioned flotation furnace under a constant tension of 5-10 MPa. The upper and lower slit nozzles are opened to spray high-speed hot air at 350-400°C to lift the aluminum strip, and it is rapidly heated at a heating rate of 45-50°C / s in conjunction with a near-infrared radiation array.

8. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, The temperature is maintained for 4–6 seconds; During the constant temperature period, the wind speed of the dry protective gas sprayed parallel to the surface of the aluminum strip is 25-35 m / s.

9. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, When entering the air quenching zone for cooling, the temperature is reduced at a cooling rate of 30-40℃ / s; The introduced mixed gas has a dew point of -45℃ to -40℃ and, by volume percentage, consists of 1.5% to 2.5% carbon dioxide, 0.1% to 0.3% oxygen, and 97.2% to 98.4% nitrogen.

10. The precision manufacturing process for high-conductivity, low-defect aluminum strip for batteries according to claim 1, characterized in that, When the treated aluminum strip is fed back into the cold rolling mill to repeat the dual-fluid temperature-controlled atomization cold rolling process, the target thickness is 12-15 μm.