A method for controlling the springback instability of an arc-shaped flange
By adjusting the rounded corner forming path of the arc-shaped flange area, it first forms an intermediate rounded corner smaller than the product's rounded corner radius, and then presses back to the final rounded corner. This solves the problem of springback instability of the arc-shaped flange area on the planar area, improves the forming accuracy and stability of the parts, and reduces the number of mold repairs and trial moldings.
Patent Information
- Application Number
- CN202611193930.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-17
AI Technical Summary
In the cold stamping process of automotive parts, the springback instability of the arc-shaped flange area to the adjacent planar area is difficult to control stably, resulting in a decrease in the dimensional accuracy and assembly quality of the parts, which is difficult to effectively improve with existing methods.
By adjusting the rounded corner forming path of the arc-shaped flange area, an intermediate rounded corner smaller than the product's rounded corner radius is first formed, and then it is pressed back to the final product's rounded corner radius. The forming scheme is optimized using finite element simulation to reduce the impact of springback instability in the planar area.
Without altering the final product structure, the forming stress distribution in the arc-shaped flange area and its adjacent planar areas was improved, thereby enhancing the forming accuracy and stability of the parts and reducing the costs of subsequent mold repair and trial molding.
Smart Images

Figure CN123102813A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of cold stamping forming technology, and in particular to a method for controlling the springback instability of an arc-shaped flange. Background Technology
[0002] In the cold stamping process of automotive parts, some sheet metal parts typically require flanging, shaping, and other processes to form a predetermined three-dimensional structure. For parts with curved flanging areas and planar areas connected to these areas, the sheet metal is susceptible to material springback during forming and unloading, causing deviations between the actual formed state and the design state. Especially near the curved flanging area, stress release after forming may lead to localized depressions or surface instability in adjacent planar areas, thereby affecting the dimensional accuracy and assembly quality of the parts.
[0003] In existing processes, springback deviations are typically compensated for by adjusting the mold profile, increasing the pressure or support of the material, and repeatedly testing and repairing the mold. However, for the localized springback instability caused by the curved flange area affecting adjacent planar areas, simply relying on conventional springback compensation or localized strong pressure methods is often insufficient to reliably improve the collapse state of the planar areas, and can easily lead to extended debugging cycles, increased mold modifications, and higher production costs. Therefore, it is necessary to provide a method that can control the springback instability of planar areas caused by curved flange forming without altering the final product structure. Summary of the Invention
[0004] This application aims to address at least one of the technical problems existing in the prior art. To this end, this application proposes a method for controlling the springback instability of an arc-shaped flange, which can reduce the impact of the arc-shaped flange area on the planar area's springback instability.
[0005] The arc-shaped flange springback instability control method according to an embodiment of this application is applied to the processing of a part to be formed. The part to be formed has an arc-shaped flange region and a planar region connected to the arc-shaped flange region, and the arc-shaped flange region has a product fillet radius. The arc-shaped flange springback instability control method of the embodiment includes: obtaining the initial forming scheme and the maximum collapse tolerance of the part to be formed; performing initial springback simulation on the part to be formed based on the initial forming scheme to obtain an initial springback collapse value; determining a primary target back pressure radius smaller than the product fillet radius based on the initial springback collapse value and the product fillet radius, and determining the primary target back pressure radius based on the primary target back pressure radius. A back-pressure radius is generated to form a single-stage back-pressure forming scheme, wherein the single-stage back-pressure forming scheme is used to first form a rounded corner with the target back-pressure radius on the semi-finished sheet material, and then back-press the rounded corner with the target back-pressure radius into a rounded corner with the product rounded corner radius; based on the single-stage back-pressure forming scheme, a single-stage back-pressure springback simulation is performed on the part to be formed to obtain a first springback collapse value; if the first springback collapse value meets the maximum collapse tolerance, the single-stage back-pressure forming scheme is determined as the target forming scheme; based on the target forming scheme, the semi-finished sheet material is subjected to arc-shaped flanging forming to obtain the part to be formed.
[0006] The arc-shaped flange springback instability control method according to the embodiments of this application has at least the following beneficial effects: By first performing initial springback simulation based on the initial forming scheme, the initial springback collapse of the part to be formed in the planar area is obtained. Then, based on the initial springback collapse value and the product fillet radius, a target back-press radius smaller than the product fillet radius is determined, and a first-stage back-press forming scheme is generated, which first forms the fillet of the target back-press radius in the semi-finished sheet material, and then back-presses it into the fillet radius of the product fillet. This allows the forming path of the arc-shaped flange area to be adjusted without changing the final product structure of the part to be formed, thereby improving the forming stress distribution of the arc-shaped flange area and its adjacent planar areas. When the first springback collapse value obtained from the first-stage back-press springback simulation meets the maximum collapse tolerance, the first-stage back-press forming scheme is determined as the target forming scheme and used for actual arc-shaped flange forming. This reduces the impact of the arc-shaped flange area on the planar area, improves the local collapse in the planar area, increases the forming accuracy and forming stability of the part, and reduces the cost of subsequent repeated mold repairs and trial moldings. Attached Figure Description
[0007] The present application will be further described below with reference to the accompanying drawings and embodiments, wherein: Figure 1 This is a schematic diagram of the structure of the arc-shaped flange area and the planar area in the part to be formed in the embodiment; Figure 2 This is a schematic diagram of the springback instability region after the initial springback simulation of the part to be formed in the example embodiment; Figure 3 A schematic diagram of the initial springback displacement distribution of a part to be formed, provided for an embodiment; Figure 4 This is a schematic diagram of the first stress release and springback displacement distribution after performing a first stress release simulation on the arc-shaped flange area in an example embodiment; Figure 5 This is a schematic diagram of the second stress release and rebound displacement distribution after performing a second stress release simulation on the planar model area in the example embodiment; Figure 6 This is a schematic diagram showing the relationship between the fillet radius of the product and the target back-press radius in a single-stage back-press forming scheme, as illustrated in the example. Figure 7 This is a schematic diagram illustrating the relationship between the primary target back pressure radius, the secondary target back pressure radius, and the product fillet radius in the secondary back pressure forming scheme of the embodiment; Figure 8 This is a flowchart illustrating the springback instability control method for curved flanges in an embodiment. Figure 9 This is a flowchart illustrating the process of determining the secondary back-pressing forming scheme in an embodiment.
[0008] Figure label: Planar area 100; Planar shape area 110; Curved edge area 200; Rebound instability area 300. Detailed Implementation
[0009] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.
[0010] In the description of this application, it should be understood that the orientation descriptions, such as up, down, front, back, left, right, etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0011] In the description of this application, "several" means one or more, "multiple" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the stated number, while "above," "below," and "within" are understood to include the stated number. The use of "first" and "second" in the description is merely for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.
[0012] In the description of this application, unless otherwise expressly defined, terms such as "setup," "installation," and "connection" should be interpreted broadly, and those skilled in the art can reasonably determine the specific meaning of the above terms in this application in conjunction with the specific content of the technical solution.
[0013] In the description of this application, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0014] It should be noted that in all specific embodiments of this application, when processing data related to user identity or characteristics, such as user information, user behavior data, user historical data, and user location information, user permission or consent is obtained first. Furthermore, the collection, use, and processing of this data comply with relevant laws, regulations, and standards. In addition, when embodiments of this application require access to sensitive personal information of users, separate permission or consent from the user is obtained through pop-ups or redirection to confirmation pages. Only after obtaining the user's separate permission or consent is the necessary user-related data required for the proper functioning of these embodiments acquired.
[0015] This application provides a method for controlling springback instability of an arc-shaped flange. The method is applied to the processing of a part to be formed. The part to be formed can be an automotive body structural component, a reinforcing component, a connector, or other sheet metal parts formed by cold stamping. The part has an arc-shaped flange area and a planar area connected to the arc-shaped flange area. The arc-shaped flange area can be a sidewall, flange boundary, or transition area formed after the sheet metal is flanged along an arc trajectory; the planar area can be an area adjacent to the arc-shaped flange area that is planar or approximately planar in the product design state.
[0016] like Figure 1As shown, the part to be formed may include a planar region 100 and an arc-shaped flange region 200. The planar region 100 may be a plate-like region in the part to be formed that is generally planar or nearly planar, and may have mounting holes, positioning holes, shallow ribs, shallow concave and convex shapes or other stamping structures, or may not have obvious shapes. The arc-shaped flange region 200 is connected to the planar region 100 and extends in an arc shape along the boundary or local contour of the part to be formed. The arc-shaped flange region 200 may include flange sidewalls, flange rounded corners, and corner portions that transition and connect with the planar region 100.
[0017] exist Figure 1 In the example shown, the curved flange region 200 is located near one edge of the planar region 100, and there is a corner position with a large curvature change in the curved flange region 200. During the flange forming process, the material flow direction, flange line length, and local bending state will all change at this corner position, which can easily cause uneven residual stress distribution in the curved flange region 200 and its adjacent planar region 100. Especially near the position where the curved flange region 200 connects with the planar region 100, a large stress gradient may be formed in the thickness direction due to the different stress states of the upper and lower surfaces at the flange fillet, which may drive the planar region 100 to local depression or collapse after the part is removed from the mold.
[0018] Therefore, this embodiment does not improve springback instability by changing the final product structure of the planar region 100. Instead, it adjusts the forming path of the rounded corners in the arc-shaped flange region 200, so that the arc-shaped flange region 200 first forms an intermediate rounded corner with a radius different from that of the final product, and then is pressed back to the radius required by the final product. In this way, the residual stress distribution of the arc-shaped flange region 200 and its adjacent planar region 100 can be actively adjusted, thereby reducing the risk of local springback instability in the planar region 100.
[0019] It should be noted that the arc-shaped flanged area in this application embodiment may specifically include locations where the flanged trajectory has corners. For such parts, when flanged in the arc-shaped flanged area, the flanged line length, flanged direction, and material flow state change near the corner, which can easily cause local stress concentration in the planar area connected to the corner. This local stress concentration usually manifests as island-shaped or cluster-shaped stress distribution areas in simulation results, and may drive local depressions, collapses, or surface distortions in the planar area after the part leaves the mold, thereby causing springback instability in the planar area.
[0020] The curved flange area has a product fillet radius. The product fillet radius refers to the design radius that the rounded transition portion of the curved flange area should achieve in the final product state of the part to be formed. This product fillet radius can be understood as either the fitted radius of the corresponding rounded arc surface in the product design model, or the fitted radius of the arc surface of the mold used to finally form the rounded corner of the product. Similarly, the "radius" mentioned in this application, such as the primary target back pressure radius, can refer to the fitted radius of the corresponding arc surface on the forming mold, or the fitted radius of the intermediate rounded arc surface of the semi-finished sheet material during the forming process. Since there is a one-to-one correspondence between the rounded arc surface and its fitted radius in the specific forming process, this application can use "product fillet radius" or "primary target back pressure radius" to represent the corresponding rounded arc surface itself, or it can represent the radius value of the rounded arc surface; its specific meaning can be determined according to the context.
[0021] like Figure 8 As shown, the embodiment of the arc-shaped flange springback instability control method includes, but is not limited to, steps S100 to S600: S100: Obtain the initial molding scheme and maximum collapse tolerance of the part to be molded; S200. Based on the initial molding scheme, perform initial springback simulation on the part to be molded to obtain the initial springback collapse value. S300. Based on the initial springback collapse value and the product fillet radius, determine the primary target back pressure radius which is smaller than the product fillet radius, and generate a primary back pressure forming scheme based on the primary target back pressure radius. The primary back pressure forming scheme is used to first form the semi-finished sheet into a fillet with a primary target back pressure radius, and then back pressure the fillet with a primary target back pressure radius into a fillet with the product fillet radius. S400. Based on the one-time back pressure forming scheme, perform one-time back pressure springback simulation on the part to be formed to obtain the first springback collapse value. S500, if the first rebound collapse value meets the maximum collapse tolerance, the single-stage backpressure forming scheme is determined as the target forming scheme; S600: Based on the target forming scheme, the semi-finished sheet material is subjected to arc-shaped flanging to obtain the part to be formed.
[0022] In step S100, the initial forming scheme refers to the original stamping forming process scheme designed for the part to be formed. This initial forming scheme may include the product model of the part to be formed, sheet material parameters, sheet thickness, process layout, die surface, pressing conditions, flanging direction, flanging sequence, and process supplementary aspects. The initial forming scheme should at least define the process of forming the curved flanging area directly according to the product's fillet radius or according to an existing process, so that subsequent analysis can be conducted based on this initial forming scheme to determine whether springback instability exists in the planar area.
[0023] Maximum collapse tolerance characterizes the maximum allowable degree of indentation or the maximum negative springback displacement range in a planar region. Specifically, in springback simulation or product inspection, the springback displacement of the planar region relative to the reference surface can be calculated using the product's theoretical surface, fitting reference surface, three-point fitting surface, or other preset inspection reference. When the local displacement of the planar region deviates towards the indentation direction, this displacement can be defined as the springback collapse value. Maximum collapse tolerance can be the allowable collapse range based on product dimensional tolerances, surface quality requirements, assembly requirements, or internal process standards. For example, maximum collapse tolerance can be expressed as the springback collapse value should fall within a preset tolerance range, which can be determined based on the part's function, inspection requirements, and subsequent assembly needs. In other words, maximum collapse tolerance is used to determine whether the springback instability of the planar region obtained by the current forming scheme has been controlled to an acceptable level.
[0024] In step S200, based on the initial molding scheme, an initial springback simulation is performed on the part to be molded to obtain the initial springback collapse value.
[0025] Initial springback simulation refers to the unloading calculation of the formed part after stamping simulation to simulate the elastic recovery and residual stress release process of the part after it leaves the mold. Initial springback simulation can be implemented using finite element simulation software, such as sheet metal stamping simulation software, to simulate the forming and springback processes of the part. The initial springback collapse value indicates the maximum amount of indentation or maximum negative springback displacement in the planar region after forming and springback simulation under the initial forming scheme. This initial springback collapse value characterizes the severity of springback instability in the planar region when no backpressure control measures are adopted. Generally, the larger the absolute value of the initial springback collapse value, the more severe the local indentation in the planar region, corresponding to the need for stronger stress distribution adjustment measures.
[0026] like Figure 2 As shown, in an exemplary initial springback simulation result, the springback displacement distribution of the part to be formed after leaving the mold can be displayed by a springback displacement heat map. Figure 2 The rebound instability region 300 is located within the planar region 100 and near the corner of the curved flange region 200. This rebound instability region 300 appears as a localized color cluster in the heatmap, indicating a significant difference in rebound displacement compared to the surrounding planar regions. It should be noted that... Figure 2This is a springback displacement heatmap, where different colors represent the magnitude of springback displacement or the degree of surface deviation at different locations on the part to be molded. For example, a color change from red, yellow, green, cyan to blue can indicate that the springback displacement value in the corresponding area gradually transitions from a large positive deviation to a negative deviation or a large indentation deviation. The specific correspondence between colors and displacement values can be determined according to the color scale settings in the simulation software; this application does not limit the specific color scale range. Figure 2 As shown in the example, blue or dark blue areas can represent areas that deviate significantly in the concave direction relative to the evaluation benchmark, red or orange-red areas can represent areas that deviate significantly in the opposite direction relative to the evaluation benchmark, and green or cyan-green areas can represent areas with relatively small deviations or in a transitional state.
[0027] exist Figure 2 In the context of the planar region 100, the rebound instability region 300 appears as an island-shaped or cluster-shaped negative displacement area located slightly below the center. The local rebound displacement value in this region is significantly lower than that of the surrounding areas, indicating that a local depression or collapse has occurred in the planar region 100 at this location. By extracting the maximum depression amount within this rebound instability region 300, the initial rebound collapse value can be obtained. For example, when using the product's theoretical surface, the fitted plane, or a preset detection benchmark as the zero-point reference, and defining the depression direction as negative, the minimum displacement value in the rebound instability region 300 can be used as the initial rebound collapse value; when evaluating the degree of depression by absolute value, the absolute value of this minimum displacement value can be used as the initial maximum collapse amount.
[0028] Depend on Figure 2 It can be seen that the springback instability of planar region 100 is not manifested as a uniform shift across the entire planar region 100, but rather as a localized island-like collapse. This type of localized collapse is usually related to the corner flanging process of the curved flanging region 200. In particular, at the corner of the curved flanging region 200, the material is subjected to combined deformations such as bending, stretching, and compression during the flanging process, which easily leads to localized residual stress concentration in the adjacent planar region 100. When the part to be formed leaves the mold, this localized residual stress is released and rebalanced, causing the planar region 100 to exhibit a springback instability such as... Figure 2 The local depression shown.
[0029] Therefore, through Figure 2 The rebound displacement thermogram shown can identify the rebound instability region 300 within the planar region 100 and quantify the initial rebound collapse value of this instability region 300. This initial rebound collapse value can serve as an important basis for subsequently determining the primary target backpressure radius, primary target backpressure amount, secondary target backpressure radius, or secondary target backpressure amount. In other words, Figure 2The springback displacement heat map shown is not only used to judge whether there is springback instability under the initial forming scheme, but also to guide the subsequent springback instability control by adjusting the fillet forming path of the curved flanging area 200.
[0030] For example, the initial springback collapse value can be recorded as a . in which, a represents the springback collapse value of the planar area under the initial forming scheme, and in particular can represent the maximum depression amount of the springback unstable region in the planar area. If the theoretical product surface or the fitting reference surface is taken as the zero reference, and the depression direction is defined as the negative direction, then a can be a negative value; at this time, | a | represents the absolute magnitude of the initial springback collapse value, that is, the initial maximum collapse amount. It should be noted that the setting of the symbol direction can be adjusted according to the coordinate definition of the simulation software or the detection system. This application focuses on the collapse degree of the planar area relative to the target surface, rather than limiting a certain positive or negative coordinate direction.
[0031] After the initial springback collapse value is obtained through initial springback simulation, it can be judged whether there is springback instability exceeding the maximum collapse tolerance in the planar area under the initial forming scheme. If the initial springback collapse value already meets the maximum collapse tolerance, it indicates that the springback instability of the planar area under the initial forming scheme is within an acceptable range, and subsequent back pressure control measures may not be enabled; if the initial springback collapse value does not meet the maximum collapse tolerance, it is necessary to actively control the residual stress distribution state by adjusting the fillet forming process of the curved flanging area.
[0032] In step S300, a primary target back pressure radius smaller than the product fillet radius is determined according to the initial springback collapse value and the product fillet radius, and a primary back pressure forming scheme is generated according to the primary target back pressure radius, wherein the primary back pressure forming scheme is used to make the semi-finished sheet material first form a fillet with the primary target back pressure radius, and then back-press the fillet with the primary target back pressure radius into a fillet with the product fillet radius.
[0033] The primary target back pressure radius refers to the smaller fillet radius that the semi-finished sheet material is formed first before being back-pressed to the product fillet radius in the primary back pressure forming scheme. That is to say, the primary target back pressure radius is smaller than the product fillet radius. If the product fillet radius is denoted as R, and the primary target back pressure radius is denoted as R1, it satisfies: R1<R, where R represents the product fillet radius of the curved flanging area in the final product state, and R1 represents the intermediate state fillet radius that the semi-finished sheet material is first formed in the primary back pressure forming scheme.
[0034] as Figure 6 shown in, Figure 6shows the relative relationship between the product fillet radius R and the primary target coining radius R1 in a one-step coining forming scheme. Herein, R denotes the product fillet radius that the curved flanging region 200 of the to-be-formed part should reach in the final product state, and R1 denotes the intermediate state fillet radius formed first in the one-step coining forming scheme. R1 is smaller than R, that is, it satisfies: R1<R. In Figure 6 the illustrated one-step coining forming scheme, the semi-finished sheet is not directly formed into the final state in one step according to the product fillet radius R. Instead, the curved flanging region 200 is first formed into a fillet with the primary target coining radius R1, and then the fillet with the primary target coining radius R1 is coined into a fillet with the product fillet radius R through a subsequent coining or sizing process. That is to say, Figure 6 the fillet forming path corresponding to the illustrated one-step coining forming scheme can be expressed as: R1→R R1→R, wherein first forming the smaller primary target coining radius R1 allows the curved flanging region 200 to undergo a local bending deformation process different from that of directly forming to the product fillet radius R; then coining R1 to R can introduce reverse adjustment or stress redistribution effect in the curved flanging region 200. Through this fillet forming path, the residual stress distribution state in the curved flanging region 200 and its adjacent planar region 100 can be actively changed, thereby reducing the stress gradient difference in the thickness direction of the planar region 100, and lowering the tendency of the planar region 100 to form local dents or collapse after being separated from the die.
[0035] Specifically, in the initial forming scheme, if the curved flanging region is directly formed to the product fillet radius R, a state where the upper surface is dominated by compressive stress, the lower surface is dominated by tensile stress, and the stress gradient in the thickness direction is large may occur near the corner. This state is prone to cause dent-type springback instability in the planar region connected to the curved flanging region after demolding and unloading. In the one-step coining forming scheme, the semi-finished sheet is first formed to the smaller primary target coining radius R1, and then coined to the product fillet radius R. This coining process can introduce a reverse deformation effect into the original single tension-compression distribution state, so that the tensile stress and compressive stress in the local region are redistributed, the stress gradient difference in the thickness direction of the planar region is reduced, and then the tendency of the planar region to collapse driven by residual stress is lowered.
[0036] The target backpressure radius can be determined based on the initial springback collapse value and the product's fillet radius. Generally, the larger the absolute value of the initial springback collapse, the more pronounced the springback instability, requiring a larger backpressure action to change the stress distribution. In this case, the target backpressure radius can be relatively smaller. Conversely, the smaller the absolute value of the initial springback collapse, the weaker the required backpressure action, and the target backpressure radius can be relatively close to the product's fillet radius. In other words, determining the target backpressure radius should consider two aspects: firstly, it should ensure sufficient backpressure between the target backpressure radius and the product's fillet radius to improve springback instability; secondly, it should avoid an excessively small target backpressure radius, which could lead to cracking in the curved flange area, excessive thinning, wrinkling, or other forming problems.
[0037] A single-stage back-pressing forming scheme may include: mold surface parameters for forming the target back-pressing radius, mold surface parameters for back-pressing the target back-pressing radius to the product's fillet radius, the movement relationship of the pressure plate or support plate, the movement path of the flanging insert, the forming sequence, and the corresponding process parameters. Since the core objective of this application is to change the intermediate forming state of the fillet region, any process scheme that enables the semi-finished sheet material to first form the target back-pressing radius and then back-press it to the product's fillet radius can be considered an implementation of the single-stage back-pressing forming scheme.
[0038] In step S400, after generating a single back-pressure forming scheme, a single back-pressure springback simulation is performed on the part to be formed based on the single back-pressure forming scheme to obtain the first springback collapse value.
[0039] One-stage backpressure springback simulation refers to simulating the forming process of a part to be formed according to a one-stage backpressure forming scheme, and then calculating the springback after unloading to obtain the springback shape of the part after adopting the one-stage backpressure forming scheme. Compared with the initial springback simulation, the one-stage backpressure springback simulation has adjusted the rounded corner forming process in the arc-shaped flange area. That is, the simulation process needs to reflect that the semi-finished sheet material is first formed into a rounded corner with a target backpressure radius, and then backpressured into a rounded corner with the product rounded corner radius. When performing the one-stage backpressure springback simulation, the material parameters, mesh parameters, friction conditions, and springback evaluation benchmarks of the initial springback simulation can be used to ensure that the initial springback collapse value is comparable to the first springback collapse value. In other words, except for the adjustment of the rounded corner forming process in the arc-shaped flange area, other conditions affecting the springback evaluation are preferably kept consistent, so as to accurately determine the degree of improvement of the springback instability by the one-stage backpressure forming scheme itself.
[0040] The first springback collapse value refers to the springback collapse value generated in the planar area when the part to be formed is removed from the mold after a single-stage back-press forming process. The first springback collapse value is used to evaluate the improvement effect of the single-stage back-press forming process on springback instability in the planar area. If the first springback collapse value is smaller than the initial springback collapse value, it indicates that the single-stage back-pressing process has adjusted the stress state of the curved flange area and its adjacent planar areas; if the first springback collapse value further meets the maximum collapse tolerance, it indicates that the single-stage back-press forming process can meet the springback instability control requirements of the part to be formed.
[0041] In step S500, after obtaining the first springback collapse value, it is determined whether the first springback collapse value meets the maximum collapse tolerance. If the first springback collapse value meets the maximum collapse tolerance, the single-stage backpressure forming scheme is determined as the target forming scheme.
[0042] The target forming scheme refers to the final process scheme that, after simulation verification, can be used for actual production or trial molding verification. In this embodiment, when the first springback collapse value meets the maximum collapse tolerance, it indicates that the single-stage back-press forming scheme has been able to control the local depression or springback instability in the planar area within the allowable range, thus eliminating the need for a more complex back-press adjustment process. At this point, the single-stage back-press forming scheme can be used as the target forming scheme, and mold design, mold modification, trial molding debugging, or production processing can be carried out accordingly.
[0043] The first rebound collapse value meeting the maximum collapse tolerance can be understood as the maximum indentation corresponding to the first rebound collapse value not exceeding the preset allowable range. For example, when the indentation direction is negative, it can be determined whether the first rebound collapse value is within the preset collapse tolerance range. This judgment is not limited to the maximum value at a single point; it can also be based on a comprehensive judgment combining the area of the rebound instability region, the indentation gradient, the trend of surface difference changes, or the distribution of detection points. In other words, as long as it can be demonstrated that the surface quality of the planar area after using the one-time back-press forming scheme meets the preset requirements, the first rebound collapse value can be considered to meet the maximum collapse tolerance.
[0044] Once the single-stage back-pressure forming scheme is determined as the target forming scheme, the target back-pressure radius, product fillet radius, mold surface design, forming sequence, and related process parameters can be solidified as the basis for subsequent manufacturing. It should be noted that the final product fillet radius in the target forming scheme is still the product fillet radius. Therefore, the method of this application does not change the final product design state of the part to be formed, but rather adjusts the stress distribution by changing the intermediate fillet radius and back-pressure path during the forming process.
[0045] In step S600, after determining the target forming scheme, the semi-finished sheet metal is subjected to arc-shaped flanging forming based on the target forming scheme to obtain the part to be formed. The semi-finished sheet metal refers to the sheet metal that has completed part of the stamping process or is in the state of waiting to be flanged before executing the target forming scheme. Depending on the process layout of different parts, the semi-finished sheet metal can be the sheet metal after drawing, trimming, pre-flanging, punching, partial shaping or other preliminary processes, or it can be the initial sheet metal that directly enters the arc-shaped flanging process.
[0046] The embodiment of the arc-shaped flange springback instability control method adjusts the rounded corner forming path of the arc-shaped flange area without changing the final product state. This causes the arc-shaped flange area to undergo a process of initial small-radius forming followed by back pressing to the product's rounded corner radius. This process alters the residual stress distribution in the arc-shaped flange area and adjacent planar areas, reducing the stress gradient difference in the thickness direction of the planar areas. This weakens the driving effect of residual stress release on the surface shape of the planar areas, suppressing the formation of local depressions or collapses in the planar areas. Compared to simply applying strong pressure to the planar areas using a pressure plate or support plate, this embodiment does not merely constrain the shape of the planar areas externally, but rather addresses the root cause of springback instability by actively adjusting the stress distribution caused by the rounded corner flange. Therefore, it improves the stability of springback control and reduces the number of subsequent mold repairs and trials.
[0047] In some embodiments, after performing a single-stage backpressure springback simulation on the part to be formed based on a single-stage backpressure forming scheme and obtaining the first springback collapse value, if the first springback collapse value does not meet the maximum collapse tolerance, it indicates that the single-stage backpressure forming scheme alone cannot control the springback instability of the planar region within the allowable range. In this case, it can be further determined whether the target backpressure radius has reached the forming limit. If the target backpressure radius has reached the forming limit, a secondary backpressure forming scheme can be used to continue adjusting the stress distribution state of the arc-shaped flange region.
[0048] The first rebound collapse value not meeting the maximum collapse tolerance can be understood as the presence of localized depressions, collapses, or surface deviations exceeding the allowable range in the planar area after a single-stage back-pressing process. For example, in an evaluation system where the direction of the depression is negative, if the first rebound collapse value still exceeds the preset maximum collapse tolerance range, it indicates that the localized rebound instability in the planar area has not been sufficiently suppressed. This judgment can be based on the maximum depression amount or can be determined comprehensively by combining the depression area, depression gradient, key detection point deviations, or product surface quality requirements.
[0049] Reaching the forming limit of the target backpressure radius means that, under the current material characteristics, sheet thickness, arc-shaped flange area structure, and mold forming conditions of the part to be formed, the target backpressure radius can no longer be reduced, or further reduction will lead to unacceptable formability problems in the arc-shaped flange area of the semi-finished sheet. Formability problems can include cracking, excessive thinning, wrinkling, localized material accumulation, excessive risk of tearing in the rounded corner area, or inability to stably form the flange contour. Since a smaller target backpressure radius usually results in a stronger backpressure effect when backpressured from the target backpressure radius to the product's rounded corner radius, process engineers often try to gradually reduce the target backpressure radius during the first backpressure optimization process to increase the ability of the first backpressure forming scheme to adjust the residual stress distribution. However, when the target backpressure radius continues to decrease, the localized plastic deformation in the rounded corner area increases, making the sheet more prone to cracking or excessive thinning. Therefore, when the target backpressure radius has been reduced to the lower limit of formability, and the first springback collapse value still does not meet the maximum collapse tolerance, it means that relying solely on one backpressure is no longer sufficient to balance springback control and forming safety. In this case, a secondary backpressure forming scheme needs to be introduced.
[0050] Therefore, as Figure 9 As shown, in some embodiments, step S500 determines the single-stage backpressure forming scheme as the target forming scheme if the first rebound collapse value meets the maximum collapse tolerance. This step also includes, but is not limited to, steps S700 to S900: S700: When the first springback collapse value does not meet the maximum collapse tolerance and the primary target back pressure radius reaches the forming limit, a secondary target back pressure radius greater than the product fillet radius is determined based on the initial springback collapse value, the primary target back pressure radius, and the product fillet radius. A secondary back pressure forming scheme is generated based on the secondary target back pressure radius. The secondary back pressure forming scheme is used to sequentially form the semi-finished sheet into fillets with the primary target back pressure radius, fillets with the secondary target back pressure radius, and fillets with the product fillet radius. S800: Based on the secondary back pressure forming scheme, perform secondary back pressure springback simulation on the part to be formed to obtain the second springback collapse value. S900, if the second rebound collapse value meets the maximum collapse tolerance, the secondary backpressure forming scheme is determined as the target forming scheme.
[0051] In step S700, if the first springback collapse value does not meet the maximum collapse tolerance and the primary target back pressure radius reaches the forming limit, a secondary target back pressure radius greater than the product fillet radius is determined based on the initial springback collapse value, the primary target back pressure radius, and the product fillet radius.
[0052] The secondary target back-press radius refers to the larger intermediate fillet radius formed by the back-pressing of the semi-finished sheet material before it is finally pressed back to the product fillet radius from the primary target back-press radius in the secondary back-pressing forming scheme. If the product fillet radius is denoted as R, the primary target back-press radius as R1, and the secondary target back-press radius as R2, then the following condition must be met: R2 > R > R1. The purpose of having a secondary target back-press radius larger than the product fillet radius is to ensure that the curved flange area undergoes a process of back-pressing from a small fillet radius to an intermediate fillet radius larger than the product fillet radius, and then back-pressing from that intermediate fillet radius to the product fillet radius. Compared with the primary back-pressing forming scheme, the secondary back-pressing forming scheme can increase the overall back-pressing effect of the fillet area without further reducing the primary target back-press radius, thereby further changing the residual stress distribution in the curved flange area and its adjacent planar areas.
[0053] like Figure 7 As shown, Figure 7 This paper illustrates the relative relationship between the primary target back-press radius R1, the secondary target back-press radius R2, and the product fillet radius R in a two-stage back-press forming scheme. Here, R represents the fillet radius that the curved flange area 200 of the part to be formed should achieve in the final product state; R1 represents the smaller intermediate fillet radius formed first in the two-stage back-press forming scheme; and R2 represents the larger intermediate fillet radius formed before the final back-press from R1 to R. Figure 7 In the example shown, R1, R, and R2 satisfy: R2>R>R1. That is, in the secondary back-pressing forming scheme, the arc-shaped flange area 200 of the semi-finished sheet material first forms a rounded corner with a primary target back-pressing radius R1; subsequently, this rounded corner with the primary target back-pressing radius R1 is back-pressed or adjusted to a rounded corner with a secondary target back-pressing radius R2; finally, the rounded corner with the secondary target back-pressing radius R2 is back-pressed to the final rounded corner with the product rounded corner radius R. Thus, Figure 7 The fillet forming path corresponding to the secondary back-press forming scheme shown can be represented as: R1→R2→R. Figure 6 Compared to the single-stage back-press forming scheme shown, Figure 7 The illustrated secondary back-pressure forming scheme adds a secondary target back-pressure radius R2, larger than the product fillet radius R, between R1 and R. This secondary target back-pressure radius R2 allows for increased back-pressure effect even when the primary target back-pressure radius R1 has reached its forming limit and cannot be further reduced. In other words, the secondary back-pressure forming scheme does not rely on further reducing R1 to improve springback control; instead, it allows for a more thorough stress redistribution in the curved flange region 200 by making the fillet undergo a multi-stage forming path from a smaller radius R1 to a larger radius R2, and then back to the product radius R.
[0054] Specifically, if the primary target back-press radius has reached the forming limit, further reduction of the primary target back-press radius may lead to cracking, excessive thinning, or other failure risks in the curved flange area. However, by determining a secondary target back-press radius larger than the product's fillet radius, the semi-finished sheet material can undergo a more thorough reverse adjustment from the primary target back-press radius to the secondary target back-press radius while maintaining the primary target back-press radius from decreasing further, before being back-pressed to the fillet radius required for the final product. This process is equivalent to increasing the degree of stress redistribution by changing the intermediate fillet path, thereby improving the ability to mitigate springback instability in planar areas.
[0055] When determining the secondary target backpressure radius, the initial springback collapse value can be used to characterize the severity of springback instability in the part to be formed without backpressure control measures. Generally, the larger the absolute value of the initial springback collapse value, the more severe the springback instability in the planar area, requiring a larger secondary backpressure effect. The primary target backpressure radius is used to define the initial fillet state of the secondary backpressure process, and the product fillet radius is used to define the final product state of the part to be formed. Therefore, the determination of the secondary target backpressure radius should, on the basis of satisfying the final backpressure to the product fillet radius, ensure that a sufficient geometric backpressure amount is formed between the primary target backpressure radius and the secondary target backpressure radius.
[0056] In some implementations, the secondary target backpressure amount can be determined based on the initial springback collapse value, and then the secondary target backpressure radius can be determined based on the secondary target backpressure amount and the primary target backpressure radius. The secondary target backpressure amount represents the radial distance or geometric adjustment between the fillet corresponding to the secondary target backpressure radius and the fillet corresponding to the primary target backpressure radius. This secondary target backpressure amount can be positively correlated with the absolute value of the initial springback collapse value. For example, the weight of the secondary backpressure amount can be determined based on the material strength, elongation, work hardening index, sheet thickness, arc flange height, product fillet radius, and simulation experience of similar parts of the semi-finished sheet metal, and the secondary target backpressure amount can be determined based on the weight of the secondary backpressure amount and the initial springback collapse value. The weight of the secondary backpressure amount can be an empirical value or can be corrected by simulation results of multiple candidate secondary target backpressure radii. For common automotive cold stamping sheet metal, the weight of the secondary backpressure amount can be pre-established based on existing experimental data or simulation data; for new materials or special structural parts, it can be determined through finite element simulation iteration.
[0057] A secondary back-pressing forming scheme is generated based on the secondary target back-pressing radius. This scheme sequentially forms rounded corners from the semi-finished sheet material, creating rounded corners with the primary target back-pressing radius, rounded corners with the secondary target back-pressing radius, and rounded corners with the final product rounded corner radius. In other words, the rounded corner forming process corresponding to the secondary back-pressing forming scheme can be represented as: semi-finished sheet material → R1 → R2 → R.
[0058] In step S800, after generating the secondary backpressure forming scheme, the secondary backpressure springback simulation is performed on the part to be formed based on the secondary backpressure forming scheme to obtain the second springback collapse value.
[0059] Secondary backpressure springback simulation refers to simulating the forming process of a part to be formed according to a secondary backpressure forming scheme, and performing unloading springback calculations after forming to obtain the springback shape of the part after the secondary backpressure forming scheme is adopted. Compared with primary backpressure springback simulation, secondary backpressure springback simulation needs to reflect the process of the semi-finished sheet material being formed sequentially into rounded corners with primary target backpressure radius, rounded corners with secondary target backpressure radius, and rounded corners with product rounded corner radius.
[0060] The second springback collapse value refers to the springback collapse value of the part to be formed in the planar area after it leaves the mold following the secondary back-press forming process. The second springback collapse value is used to evaluate the control effect of the secondary back-press forming process on springback instability in the planar area. If the second springback collapse value is less than the absolute value of the first springback collapse value, or if the depression range of the planar area corresponding to the second springback collapse value is significantly reduced, it indicates that the secondary back-press forming process further improves the residual stress release state in the planar area. If the second springback collapse value meets the maximum collapse tolerance, it indicates that the secondary back-press forming process can meet the forming quality requirements of the part to be formed.
[0061] In the secondary backpressure springback simulation, it is preferable to maintain the same or comparable evaluation benchmarks as the initial springback simulation and the primary backpressure springback simulation. For example, using the same product theoretical surface, the same detection points, the same three-point fitting method, or the same springback displacement output method. This makes the initial springback collapse value, the first springback collapse value, and the second springback collapse value comparable, thus facilitating the determination of whether the secondary backpressure forming scheme has a further improvement effect compared to the initial forming scheme and the primary backpressure forming scheme.
[0062] Secondary backpressure springback simulation can also be combined with formability results for comprehensive evaluation. In actual process design, secondary backpressure forming schemes should also avoid formability problems such as wrinkling in rounded corner areas, material accumulation, or local crushing. If the secondary target backpressure radius is too large, local material accumulation or wrinkling may occur in the semi-finished sheet when it changes from the primary target backpressure radius to the secondary target backpressure radius. Therefore, the secondary target backpressure radius needs to provide sufficient stress redistribution while also remaining within the formable range.
[0063] In step S900, after obtaining the second springback collapse value, it is determined whether the second springback collapse value meets the maximum collapse tolerance. If the second springback collapse value meets the maximum collapse tolerance, the secondary backpressure forming scheme is determined as the target forming scheme.
[0064] The second rebound collapse value meeting the maximum collapse tolerance means that after adopting the secondary back-pressing forming scheme, the maximum amount of indentation, the degree of local collapse, or the surface shape deviation in the planar area is within the preset allowable range. For example, it can be determined whether the second rebound collapse value falls within the allowable range corresponding to the maximum collapse tolerance; for systems evaluated by absolute deviation, it can also be determined whether the absolute value of the second rebound collapse value is less than or equal to the allowable threshold.
[0065] After determining the secondary back-press forming scheme as the target forming scheme, the final part to be formed still retains the product's fillet radius. In other words, the secondary target back-press radius exists only as an intermediate forming state and does not change the final product structure of the part to be formed. In this way, springback instability control in planar areas can be achieved by adjusting the forming path without changing the product design or adding additional product features.
[0066] The secondary back-press forming scheme is suitable for parts with a large initial springback collapse value, where the target back-press radius has approached or reached the forming limit, but the first springback collapse value still does not meet the maximum collapse tolerance. For such parts, if the conventional strong pressure method is continued to be used on the planar area, it is often difficult to change the internal residual stress state of the springback instability area; however, by using the secondary back-press forming scheme, the stress clusters originally concentrated in the planar area can be weakened or redistributed through the multi-stage back-press path in the rounded corner area, reducing the stress gradient difference in the thickness direction of the planar area, thereby reducing the driving force for the formation of local depressions after demolding.
[0067] In some embodiments, step S200 performs initial springback simulation on the part to be molded based on the initial molding scheme to obtain the initial springback collapse value, and further includes, but is not limited to, steps S210 to S240: S210. Based on the initial molding scheme, perform initial springback simulation on the part to be molded to obtain the initial molding form of the part after it leaves the mold. S220. Based on the initial forming state, obtain the initial springback displacement distribution of the planar region; S230. Based on the initial rebound displacement distribution, the initial rebound instability region of the planar area is obtained; S240. Extract the maximum indentation in the initial rebound instability region as the initial rebound collapse value.
[0068] In step S210, based on the initial molding scheme, an initial springback simulation is performed on the part to be molded to obtain the initial molding shape of the part after it leaves the mold.
[0069] The initial forming scheme refers to the original stamping process scheme before adopting a single-stage or double-stage back-press forming scheme. It may include the product model of the part to be formed, sheet material parameters, sheet thickness, process layout, die surface, blanking conditions, flanging direction, flanging sequence, and springback compensation settings. When performing initial springback simulation based on the initial forming scheme, finite element simulation of the stamping process of the part to be formed can be performed first. Then, after forming is completed, the die constraints can be released to simulate the elastic recovery and residual stress release process of the part after it leaves the die.
[0070] The initial forming shape refers to the simulated geometric shape of the part to be formed after it has been shaped according to the initial forming scheme and removed from the mold. This initial forming shape differs from the constrained shape under mold closure; it reflects the actual trend of the part after unloading due to the rebalancing of residual stress. Therefore, the initial forming shape can be used to determine whether local depressions, local warping, abrupt changes in surface shape, or other springback instability phenomena occur in planar areas. In the specific simulation process, stamping simulation software can be used, such as AutoForm, PAM-STAMP, Dynaform, LS-DYNA, or other finite element software capable of sheet metal forming and springback analysis.
[0071] In step S220, after obtaining the initial forming shape, the initial springback displacement distribution of the planar region is obtained according to the initial forming state.
[0072] Initial springback displacement distribution refers to the set of springback displacements of each point or finite element node in a planar region relative to a reference datum. This reference datum can be the theoretical surface of the product, the die surface, the target surface before springback compensation, the fitted plane, or a datum surface established based on detection points. In the evaluation of the surface shape of automotive stamping parts, a three-point fitting or multi-point fitting method is often used to establish an evaluation datum for the planar region, and then the normal deviation or specified direction deviation of each point in the planar region in the initial forming shape relative to this evaluation datum is calculated.
[0073] In one implementation, the initial springback displacement distribution can be obtained from the nodal displacement cloud map output by finite element simulation software. Specifically, a planar region connected to the arc-shaped flange area can be selected in the initial forming shape, and the displacement values of each node in this planar region in the normal direction or a preset detection direction can be extracted. If the theoretical surface of the product is used as a reference, the initial springback displacement distribution can reflect the degree of deviation of the planar region from the product design state; if a fitted plane is used as a reference, the initial springback displacement distribution can reflect the local unevenness changes inside the planar region, thus making it easier to identify local springback instability.
[0074] In step S230, the initial rebound instability region of the planar region is obtained based on the initial rebound displacement distribution.
[0075] The initial springback instability region refers to the area in a planar region where localized depressions, collapses, or abnormal surface shapes occur under the initial forming scheme. This region typically exhibits a significant concentration of negative displacement relative to the surrounding planar region, and its outline may appear as an island, cluster, or partially closed. For parts with corners in the curved flange area, the initial springback instability region is often located in the planar region adjacent to the corner of the curved flange area. This is because the material flow direction and stress state change drastically during the corner flange process, easily leading to localized residual stress concentration at this location.
[0076] In one implementation, the initial springback instability region can be identified by setting a displacement threshold. For example, when the negative displacement of certain points or nodes in the initial springback displacement distribution exceeds a preset threshold, the continuous area containing these points or nodes can be defined as the initial springback instability region. This preset threshold can be determined based on the maximum collapse tolerance, product inspection requirements, or surface finish requirements of the planar area. For parts with high surface finish requirements, a stricter threshold can be used; for parts primarily requiring assembly functionality, the threshold can be set in conjunction with assembly clearance and welding positioning requirements.
[0077] In step S240, the maximum indentation in the initial rebound instability region is extracted as the initial rebound collapse value.
[0078] The maximum indentation refers to the maximum displacement relative to the reference datum in the indentation direction within the initial rebound instability region. If the indentation direction is considered negative, the maximum indentation corresponds to the minimum rebound displacement value within the initial rebound instability region; if expressed as the absolute value of the indentation degree, the maximum indentation corresponds to the value with the largest absolute value of the negative displacement. To facilitate connection with the subsequent determination of backpressure, the initial rebound collapse value can be denoted as 'a', where 'a' represents the maximum indentation within the initial rebound instability region. When the indentation direction is negative in the simulation coordinate system, 'a' can be negative; its absolute magnitude can be represented by |a| when the degree of collapse needs to be measured later.
[0079] The initial rebound collapse value quantifies the severity of rebound instability in the planar region under the initial forming scheme. When determining the target backpressure radius, the required backpressure intensity can be judged based on the initial rebound collapse value. Generally, the larger the absolute value of the initial rebound collapse value, the more severe the collapse in the planar region, requiring a larger backpressure amount or stronger corner stress redistribution measures; conversely, the smaller the absolute value of the initial rebound collapse value, the smaller the backpressure amount can be used to reduce unnecessary forming risks.
[0080] In some embodiments, the planar area of the part to be formed has a planar shaping area. The planar shaping area refers to a local reinforcing rib, shallow rib, shallow concave-convex shape (such as product markings), local embossed structure, or other stamping shape formed on the planar area connected to the arc-shaped flange area to meet the product's rigidity, assembly, clearance, or appearance requirements. For this type of part to be formed, the springback instability of the planar area may be affected by multiple factors, such as the flange forming of the arc-shaped flange area, or the forming of the planar shaping area itself. For parts to be formed with a planar shaping area, the initial forming scheme also corresponds to a mold structure for forming this planar shaping area. Therefore, before determining the target springback radius based on the initial springback collapse value and the product's fillet radius, the cause of the springback instability in the initial springback instability area can be confirmed to avoid misjudging springback instability caused by non-arc-shaped flange areas as springback instability caused by arc-shaped flange areas.
[0081] Correspondingly, in some embodiments, after performing initial springback simulation on the part to be molded based on the initial molding scheme in step S200 to obtain the initial springback collapse value, steps S251 to S256 may also be included, but are not limited to: S251. Perform a first stress release simulation on the arc-shaped flange area of the initial forming shape to obtain the first release springback displacement distribution of the planar area. S252. Perform a second stress release simulation on the planar modeling area of the initial formed shape to obtain the second release springback displacement distribution of the planar area. S253. Based on the first release rebound displacement distribution, extract the first release rebound instability region and the first release rebound collapse value; S254. Based on the second release rebound displacement distribution, extract the second release rebound instability region and the second release rebound collapse value; S255. Based on the first release rebound instability area and the second release rebound instability area, and / or the first release rebound collapse value and the second release rebound collapse value, determine whether the cause of the rebound instability of the initial rebound instability area originates from the arc-shaped flange area. S256. If it is determined that the cause of the rebound instability is from the arc-shaped flange area, perform the step of determining a primary target back pressure radius smaller than the product's fillet radius based on the initial rebound collapse value and the product's fillet radius.
[0082] In step S251, a first stress release simulation is performed on the arc-shaped flange area of the initial forming shape to obtain the first release springback displacement distribution of the planar area.
[0083] The initial forming morphology refers to the simulated geometric shape of the part after it has been formed according to the initial forming scheme and removed from the mold. It retains the residual stress state caused by the initial forming scheme. During the forming process, the curved flange area experiences changes in material flow direction, bending direction, and degree of plastic deformation in localized areas due to the curved flange line and potential corners. This can easily lead to uneven stress on the upper and lower surfaces or a large stress gradient in the thickness direction. Therefore, by performing a first stress release simulation on the curved flange area of the initial forming morphology, the springback response after partially releasing or weakening the residual stress in the curved flange area can be simulated.
[0084] The first stress relief simulation can be achieved through the stress relief module in stamping simulation software or through finite element post-processing. For example, it can locally clear the stress, reduce the residual stress, and reset the material state of elements or nodes in the curved flange region. Alternatively, the regional stress relief function provided by the software can partially or completely eliminate the driving effect of the curved flange region on the subsequent springback. It should be noted that the purpose of the first stress relief simulation is not to simulate an independent process that necessarily exists in actual production, but rather to use a simulation diagnostic method to analyze and confirm the source of springback instability.
[0085] The first release springback displacement distribution refers to the springback displacement distribution of the planar region relative to a reference datum after the first stress release simulation of the curved flange area. This reference datum can be consistent with the reference datum used for the initial springback displacement distribution, such as the product's theoretical surface, fitting plane, three-point fitting surface, or a preset detection datum. To ensure the reliability of the comparison results, the first release springback displacement distribution preferably uses the same detection direction, the same evaluation area, and the same data processing method as the initial springback displacement distribution.
[0086] By observing the first release and rebound displacement distribution, it can be determined whether the local depression in the planar area decreases and whether the initial rebound instability area shrinks or disappears after the residual stress in the arc-shaped flange area is released or weakened. If the first release and rebound displacement distribution shows a significant improvement in the collapse of the planar area, it indicates that the arc-shaped flange area has a strong influence on the initial rebound instability area.
[0087] In step S252, after completing or performing the first stress release simulation in parallel, a second stress release simulation can be performed on the planar modeling area of the initial forming shape to obtain the second release springback displacement distribution of the planar area.
[0088] The second stress relief simulation can employ the same or similar simulation methods as the first stress relief simulation. The difference lies in that the stress relief object is a planar shape region, rather than a curved edge region. Specifically, local stress zeroing, residual stress reduction, or material state reset can be performed on elements, nodes, or material integration points in the planar shape region to simulate the influence of residual stress in the planar shape region on the rebound response after release. To ensure the comparability of the first and second stress relief simulations, both preferably use the same stress relief ratio, the same rebound calculation settings, and the same evaluation benchmark.
[0089] The second-release rebound displacement distribution refers to the rebound displacement distribution of the planar region relative to the reference datum after performing a second stress release simulation on the planar region. By analyzing the second-release rebound displacement distribution, it can be determined whether the planar region is the main cause of the initial rebound instability region. If the second-release rebound displacement distribution shows that the collapse of the planar region has not been improved, or even if the collapse range has expanded or the collapse value has increased, it indicates that the planar region is not the main source of the initial rebound instability region, or that the planar region actually has a certain local support or stiffness enhancement effect on the planar region.
[0090] In some implementations, the first stress relief simulation and the second stress relief simulation can be executed sequentially or in parallel within different simulation models. Regardless of the order, as long as the first and second stress relief springback displacement distributions can be obtained separately and used for subsequent comparative analysis, it is acceptable.
[0091] In step S253, after obtaining the first release rebound displacement distribution, the first release rebound instability region and the first release rebound collapse value are extracted based on the first release rebound displacement distribution. The first release rebound instability region refers to the area in the planar region that still exhibits local depression or rebound instability after the first stress release simulation of the arc-shaped flange region. The first release rebound collapse value refers to the maximum depression amount in the first release rebound instability region, used to quantify the degree of collapse that still exists in the planar region after stress release of the arc-shaped flange region. The extraction method of the first release rebound instability region and the first release rebound collapse value can be consistent with the extraction method of the initial rebound instability region and the initial rebound collapse value.
[0092] In step S254, after obtaining the second release rebound displacement distribution, the second release rebound instability region and the second release rebound collapse value are extracted based on the second release rebound displacement distribution. The second release rebound instability region refers to the region in the planar region that still exhibits local depression or rebound instability after performing the second stress release simulation on the planar modeling region. The second release rebound collapse value refers to the maximum depression amount in the second release rebound instability region, used to quantify the degree of collapse of the planar region after stress release. For ease of comparison, the extraction method of the second release rebound instability region and the second release rebound collapse value is preferably consistent with the extraction method of the initial rebound instability region, the initial rebound collapse value, the first release rebound instability region, and the first release rebound collapse value. That is, after performing the first stress release simulation and the second stress release simulation, the corresponding rebound instability region and rebound collapse value can be extracted respectively under the same planar region, the same reference datum, the same detection direction, and the same threshold rule.
[0093] In steps S255 and S256, after obtaining the first release rebound instability region, the first release rebound collapse value, the second release rebound instability region, and the second release rebound collapse value, respectively, it is determined whether the cause of the rebound instability in the initial rebound instability region originates from the arc-shaped flange region, based on the first and second release rebound instability regions and / or the first and second release rebound collapse values. Here, "and / or" indicates that the judgment can be made based solely on region changes, solely on collapse value changes, or a comprehensive judgment based on both region changes and collapse value changes. Region changes are mainly used to evaluate whether the scope of rebound instability influence has changed, while collapse value changes are mainly used to evaluate whether the severity of rebound instability has changed. Combining both can improve the reliability of cause confirmation.
[0094] In one implementation, when the first release rebound instability region is significantly smaller or disappears compared to the initial rebound instability region, and the first release rebound collapse value is significantly reduced compared to the initial rebound collapse value, it can be determined that the rebound instability of the initial rebound instability region originates from the arc-shaped flange region. Here, "significantly smaller" or "significantly reduced" can be determined based on a preset ratio, a preset threshold, or process experience. For example, it can be set that when the improvement in the first release rebound collapse value relative to the initial rebound collapse value reaches a preset ratio, the arc-shaped flange region is considered the main cause; alternatively, it can be determined based on whether the concave region in the simulation cloud diagram is eliminated or whether it changes from a continuous island-like region to scattered small regions.
[0095] In another implementation, the first release rebound instability region and the second release rebound instability region can be compared. If the first release rebound instability region is significantly smaller than the second release rebound instability region, or the first release rebound collapse value is significantly smaller than the second release rebound collapse value, it indicates that releasing the stress in the curved flange region is more effective in improving the collapse of the planar region than releasing the stress in the planar shape region. This suggests that the cause of the rebound instability in the initial rebound instability region originates from the curved flange region.
[0096] In another implementation, reverse verification can be performed by combining the changing trend of the second release rebound displacement distribution. If, after performing the second stress release simulation on the planar shape region, the second release rebound instability region does not improve or further expands, and the second release rebound collapse value does not decrease or further increases, while after performing the first stress release simulation on the curved flange region, the first release rebound instability region significantly improves, then it can be more reliably determined that the rebound instability of the initial rebound instability region originates from the curved flange region. This situation indicates that the planar shape region is not the main factor causing the rebound instability of the planar region, and may even have a certain effect on local stiffness enhancement or stress balancing of the planar region.
[0097] It should be noted that determining whether the cause of springback instability in the initial springback instability region originates from the curved flange area does not require the curved flange area to be the sole influencing factor. In actual stamping, springback instability in planar areas may be influenced by multiple factors, including material properties, sheet thickness, blanking state, planar shaping area, and flange height. The phrase "originating from the curved flange area" in this application can be understood as the residual stress state in the curved flange area being the primary factor leading to the formation of the initial springback instability region, or that adjusting the rounded corner forming path of the curved flange area can have a dominant effect on improving the initial springback instability region.
[0098] To further illustrate the process of confirming the cause of rebound instability through stress relief simulation, the following will combine... Figures 3 to 5 An exemplary implementation will be described.
[0099] like Figure 3 As shown, Figure 3 This illustration shows the initial springback displacement distribution of a part to be formed after initial springback simulation under an initial forming scheme in one embodiment. A planar shaping area 110 may be provided on the planar region 100 of the part to be formed. The planar shaping area 110 may include local convex bulges, grooves, reinforcing ribs, embossed structures, positioning shapes, or other shallow shaping structures. Since the planar shaping area 110 itself will also generate local plastic deformation and residual stress during the forming process, when springback instability occurs in the planar region 100, it is necessary to determine whether the springback instability mainly originates from the curved flange region 200 or mainly from the planar shaping area 110. Figure 3This is a springback displacement heatmap, where different colors represent the magnitude of springback displacement or the degree of surface deviation at different locations of the part to be formed relative to the evaluation datum. For example, red or orange-red areas can represent regions with large positive deviations relative to the evaluation datum, yellow and green areas can represent regions with smaller deviations or in a transitional state, and cyan, blue, or purple areas can represent regions with negative deviations or a tendency to concave relative to the evaluation datum. The specific correspondence between colors and displacement values can be determined according to the color scale settings in the simulation software; this application does not limit the specific color scale range.
[0100] exist Figure 3 In the initial rebound displacement distribution shown, there are localized blue or purple clusters within planar region 100, which can be identified as initial rebound instability regions. These initial rebound instability regions are located near the influence area between planar shaping region 110 and curved flange region 200; therefore, based solely on… Figure 3 The initial rebound displacement distribution shown may not be sufficient to directly determine whether the rebound instability is mainly caused by the residual stress of the rounded corner of the curved flange region 200 or by the residual stress of the planar shaping region 110. Therefore, stress release simulations can be performed on the curved flange region 200 and the planar shaping region 110 respectively, and the changes in rebound displacement distribution before and after stress release can be compared.
[0101] like Figure 4 As shown, Figure 4 The diagram shows the first stress-relief springback displacement distribution obtained after performing a first stress-relief simulation on the arc-shaped flange region 200 in the initial forming shape. The first stress-relief simulation can be understood as weakening or releasing the residual stress influence of the arc-shaped flange region 200 in the simulation analysis to observe whether the springback displacement distribution of the planar region 100 improves. Specifically, the stress-relief module of the simulation software can be used to perform regional residual stress relief, local stress zeroing, or residual stress reduction on the elements, nodes, or material integration points of the arc-shaped flange region 200, and the springback displacement distribution of the planar region 100 can be recalculated under the same evaluation criteria. Figure 4 It can be seen that after performing the first stress relief simulation on the curved flange region 200, Figure 3 The localized blue or purple clusters within the planar region 100 significantly weakened, shrank, or nearly disappeared, resulting in a smoother overall color distribution in the planar region 100. In other words, the first release rebound displacement distribution was significantly improved compared to the initial rebound displacement distribution, indicating that the residual stress state of the arc-shaped flange region 200 has a significant impact on the local depressions or collapses of the planar region 100. Therefore, it can be determined that in this embodiment, the formation of the initial rebound instability region is mainly related to the flange forming process of the arc-shaped flange region 200, particularly to the residual stress distribution at the rounded corners of the arc-shaped flange region 200.
[0102] like Figure 5 As shown, Figure 5 The diagram shows the second stress-relief springback displacement distribution obtained after performing a second stress-relief simulation on the planar shaping region 110 in the initial molding form. The second stress-relief simulation can be understood as weakening or releasing the residual stress influence of the planar shaping region 110 in the simulation analysis to observe whether the springback displacement distribution of the planar region 100 is improved. To ensure the reliability of the comparison results, the second stress-relief simulation preferably uses the same or comparable stress-relief method, springback calculation conditions, evaluation criteria, detection direction, and color code rules as the first stress-relief simulation. Figure 5 It can be seen that after performing the second stress relief simulation on the planar modeling region 110, there is still a large area of blue or purple negative deviation region within the planar region 100, and this negative deviation region is even relative to... Figure 3 The initial rebound displacement distribution shown further expands or deepens. In other words, after releasing the residual stress in the planar shaping region 110, the local collapse of the planar region 100 is not effectively improved; instead, there may be a trend of expansion of the rebound instability region or an increase in the rebound collapse value. This result indicates that the planar shaping region 110 is not the main cause of the formation of this initial rebound instability region; conversely, in some embodiments, the planar shaping region 110 may also have a certain inhibitory effect on the rebound instability of the planar region 100 through local structural stiffness or local stress balance.
[0103] Through the Figures 3 to 5 A comparison reveals that releasing the residual stress in the curved flange region 200 significantly improves the springback instability of the planar region 100; however, releasing the residual stress in the planar shaping region 110 does not improve the springback instability or even exacerbates it. Therefore, it can be determined that the initial springback instability in this embodiment is primarily caused by the curved flange region 200, rather than primarily by the planar shaping region 110.
[0104] Furthermore, Figures 3 to 5The comparison results also illustrate that if only the pressure plate, support plate, or shaping insert is used to apply localized strong pressure to the planar region 100, although it may temporarily constrain the shape of the planar region 100 when the mold is closed, it cannot effectively change the residual stress distribution state in the arc-shaped flange region 200 that leads to springback instability. Therefore, this embodiment of the application adjusts the rounded corner forming path of the arc-shaped flange region 200 so that the arc-shaped flange region 200 first forms a rounded corner corresponding to the target back pressure radius, and then back pressures it to the rounded corner corresponding to the product rounded corner radius, or further through a rounded corner corresponding to the target back pressure radius and then back pressures it to the rounded corner corresponding to the product rounded corner radius, thereby actively adjusting the stress distribution state of the arc-shaped flange region 200 and the adjacent planar region 100, and can more effectively control the springback instability of the planar region 100.
[0105] After confirming that the cause of springback instability originates from the curved flange area, a primary target back-press radius smaller than the product's fillet radius can be determined based on the severity of the collapse as characterized by the initial springback collapse value and the final fillet state defined by the product's fillet radius. Subsequently, a primary back-press forming scheme can be generated based on the primary target back-press radius, allowing the semi-finished sheet material to first form a fillet with the primary target back-press radius, and then back-pressing this fillet into a fillet with the product's fillet radius. This alters the residual stress distribution in the curved flange area after forming and suppresses localized depressions in the connected planar area.
[0106] In some implementations, the method for determining the target backpressure radius includes, but is not limited to, steps S310 to S350: S310. Determine the target back pressure amount based on the initial rebound collapse value and the material characteristics of the semi-finished sheet material; S320. Determine the initial back pressure radius based on the target back pressure amount and the product fillet radius; wherein, the initial back pressure radius is smaller than the product fillet radius, and the target back pressure amount represents the radial distance between the fillet vertex of the initial back pressure radius and the fillet vertex of the product fillet radius; S330. Generate the corresponding initial primary forming back pressure scheme based on the initial back pressure radius; S340. Based on the initial one-time molding back pressure scheme, perform formability simulation verification on the part to be molded. S350. If the initial back pressure radius passes the molding simulation verification, the initial back pressure radius is determined as the target back pressure radius.
[0107] In step S310, the target back pressure amount is determined based on the initial springback collapse value and the material characteristics of the semi-finished sheet.
[0108] The initial springback collapse value characterizes the severity of localized indentation or springback instability in a planar region under the initial forming scheme. The material characteristics of the semi-finished sheet metal characterize its plastic deformation capacity, springback sensitivity, and failure risk during stamping. These material characteristics may include material grade, yield strength, tensile strength, elongation, work hardening index, anisotropy coefficient, elastic modulus, sheet thickness, and material forming limit curve. Different materials produce different stress redistribution effects and formability risks under the same back pressure. For example, materials with higher strength or higher springback sensitivity may require larger back pressure to achieve sufficient springback improvement; while materials with lower elongation or smaller forming margins need to limit excessive back pressure to avoid cracking or excessive thinning.
[0109] The target backpressure amount is a parameter used to characterize the degree of geometric backpressure in a single-stage backpressure forming process. Specifically, the target backpressure amount can represent the radial distance between the initial backpressure radius or the radius corresponding to the target backpressure radius and the radius corresponding to the product fillet radius; that is, the amount of geometric adjustment experienced by the small radius fillet when it is backpressured to the product fillet radius. A larger target backpressure amount usually means that the semi-finished sheet material undergoes more thorough reverse adjustment in the fillet area, and the change in residual stress distribution is more significant. However, if the target backpressure amount is too large, the initial backpressure radius will decrease accordingly, and the formability risk will increase.
[0110] In one alternative implementation, the weight of the initial backpressure amount can be determined based on the material characteristics of the semi-finished sheet material, and this weight can be matched with the absolute value of the initial springback collapse value to obtain the target initial backpressure amount. For example, the target initial backpressure amount can be set to be positively correlated with the absolute value of the initial springback collapse value. In another implementation, the target initial backpressure amount can also be determined through candidate backpressure amount simulation. For example, multiple candidate target initial backpressure amounts can be set based on the initial springback collapse value, and corresponding initial backpressure radii can be generated for each. Candidate values that can both improve springback instability and have good formability can be selected through formability simulation verification and springback simulation results.
[0111] In step S320, after determining the target back pressure amount, the initial back pressure radius is determined based on the target back pressure amount and the product fillet radius. The initial back pressure radius is smaller than the product fillet radius, and the target back pressure amount represents the radial distance between the fillet vertex of the initial back pressure radius and the fillet vertex of the product fillet radius.
[0112] The initial backpressure radius is a candidate radius initially calculated or selected based on the target backpressure amount, used to form the initial backpressure forming scheme. Since the initial backpressure radius has not yet been verified by formability simulation, whether it can be used as the final target backpressure radius requires further verification.
[0113] Here, the fillet vertex can be understood as the characteristic vertex of the corresponding rounded arc surface in the cross-sectional profile or the geometric reference point for the rounded arc transition. In stamping simulation or mold design, within the same cross-section, using the fillet vertex of the arc surface corresponding to the product's fillet radius as a reference, the radial distance between the fillet vertex of the arc surface corresponding to the initial back pressure radius and this vertex can be compared to obtain the target back pressure amount. Since there may be differences in springback compensation or surface compensation between the actual product fillet and the mold fillet, the aforementioned radial distance can be determined based on either the theoretical fillet cross-section of the product or the cross-section of the mold used for forming, as long as the comparison is performed under the same evaluation criterion.
[0114] When determining the initial backpressure radius, an arc-shaped surface corresponding to the initial backpressure radius can be constructed in the fillet section based on the product's fillet radius and the target backpressure amount. Generally, the larger the target backpressure amount, the smaller the initial backpressure radius; conversely, the smaller the target backpressure amount, the closer the initial backpressure radius is to the product's fillet radius. For complex cross-sections or non-standard arc transition structures, a fitted circle method can also be used to determine the initial backpressure radius. This involves fitting the local arc-shaped surface to an arc and using the radius of this fitted arc as the initial backpressure radius.
[0115] In step S330, after determining the initial back-press radius, a corresponding initial one-time forming back-press scheme is generated based on the initial back-press radius. The initial one-time forming back-press scheme is a candidate process scheme constructed using the initial back-press radius as an intermediate fillet radius. This scheme is used to first form the semi-finished sheet material into fillets with the initial back-press radius, and then back-press the fillets with the initial back-press radius into fillets with the product fillet radius. In other words, the initial one-time forming back-press scheme is a candidate scheme for the one-time back-press forming scheme when the radius parameters have not yet been finalized.
[0116] In steps S340 and S350, after generating the initial one-time molding back pressure scheme, the formability simulation verification of the part to be molded is performed based on the initial one-time molding back pressure scheme. If the formability simulation verification passes, the initial back pressure radius is determined as the target back pressure radius.
[0117] Formability simulation verification refers to determining whether a part can be safely formed during the initial one-step forming back pressure scheme through stamping forming simulation. This verification focuses on the material strain, thinning rate, wrinkling tendency, cracking risk, and local material accumulation in the curved flange area and the connected planar area during the forming process. Because the initial back pressure radius is smaller than the product's fillet radius, the semi-finished sheet metal may experience more severe bending and plastic deformation at this fillet location. Therefore, formability simulation verification is needed to confirm that it will not cause unacceptable forming defects. In practice, formability simulation verification can include forming limit diagram checks, thinning rate checks, principal and secondary strain checks, material failure index checks, wrinkling tendency checks, and local contour quality checks. If the formability simulation results show cracking, excessive thinning, or significant wrinkling in the curved flange area, it indicates that the initial back pressure radius is too small or the initial one-step forming back pressure scheme is unsuitable for direct use. If the formability simulation results do not show the above unacceptable defects, then the initial back pressure radius can be considered a potential target back pressure radius.
[0118] The initial backpressure radius passing the formability simulation verification means that when the part to be formed is formed according to the initial one-time forming backpressure scheme, there are no unacceptable cracks, excessive thinning, wrinkles, or other formability defects in the arc-shaped flange area and related areas. This indicates that the initial backpressure radius determined based on the target backpressure amount and the product's fillet radius is feasible in terms of forming safety. Therefore, it can be used as the target backpressure radius to generate a one-time backpressure forming scheme and further conduct one-time backpressure springback simulation.
[0119] It should be noted that determining the initial backpressure radius as the target backpressure radius does not necessarily mean that this target backpressure radius will ensure that the first rebound collapse value meets the maximum collapse tolerance. If the first rebound collapse value obtained from the backpressure-rebound simulation meets the maximum collapse tolerance, then the first backpressure forming scheme can be determined as the target forming scheme; if the first rebound collapse value does not meet the maximum collapse tolerance, and the target backpressure radius has reached the forming limit, then the process of determining the second backpressure forming scheme can proceed. Specifically, if the first rebound collapse value does not meet the maximum collapse tolerance, and the target backpressure radius has not reached the forming limit, it is also possible to appropriately increase the first target backpressure amount. However, in normal circumstances, the target backpressure amount is the maximum acceptable backpressure value obtained based on material characteristics and experience, so this scenario is relatively rare.
[0120] In some embodiments, after performing formability simulation verification on the part to be molded based on the initial one-time molding back pressure scheme in step S340, further steps including but not limited to S360 to S390 may be performed: S360. If the initial back pressure radius fails the formability simulation verification, the initial back pressure radius is increased sequentially according to the preset first adjustment step to obtain a candidate back pressure radius. S370. Generate a corresponding candidate primary molding back pressure scheme based on the primary candidate back pressure radius; S380. Based on the candidate one-time molding back pressure scheme, perform formability simulation verification on the part to be molded. S390. The smallest candidate back pressure radius that passes the first formability check is determined as the target back pressure radius.
[0121] In step S360, if the initial back pressure radius fails the molding simulation verification, the initial back pressure radius is increased sequentially according to the preset first adjustment step size to obtain a candidate back pressure radius.
[0122] If the initial back pressure radius fails the formability simulation verification, it usually indicates that the radius is too small, leading to excessive local plastic deformation or unstable material flow in the curved flange area during forming. To reduce the risk of cracking, excessive thinning, or wrinkling, the radius can be gradually increased based on the initial back pressure radius to make the rounded corner forming smoother, thereby improving formability.
[0123] The first adjustment step size refers to the radius adjustment amount used each time the initial back pressure radius is increased. The first adjustment step size can be set based on the product's fillet radius, sheet thickness, simulation accuracy requirements, and process design experience. For example, for parts with smaller sheet thickness, smaller fillet radii, or those that are more sensitive to radius changes during springback, a smaller first adjustment step size can be used; for parts with larger fillet radii or larger forming margins, a larger first adjustment step size can be used to improve simulation iteration efficiency. The first adjustment step size can be a fixed value or an adaptive value that changes with the number of iterations.
[0124] The primary candidate backpressure radius refers to the candidate radius obtained by increasing the initial backpressure radius after the initial backpressure radius fails the formability simulation verification. The primary candidate backpressure radius is still smaller than the product's fillet radius and is used to form a new candidate primary molding backpressure scheme. Generally, the closer the primary candidate backpressure radius is to the product's fillet radius, the easier it is to improve formability. However, a decrease in the primary backpressure amount between it and the product's fillet radius may reduce its ability to improve springback instability. Therefore, a balance needs to be struck between formability and springback control during the adjustment process.
[0125] In step S370, after obtaining the first-stage candidate backpressure radius, a corresponding candidate one-stage forming backpressure scheme is generated based on the first-stage candidate backpressure radius. The candidate one-stage forming backpressure scheme is a process scheme constructed using the first-stage candidate backpressure radius as an intermediate fillet radius. It is used to first form a fillet with the first-stage candidate backpressure radius on the semi-finished sheet material, and then backpressure the fillet with the first-stage candidate backpressure radius into a fillet with the product fillet radius. Compared with the initial one-stage forming backpressure scheme, the intermediate fillet radius in the candidate one-stage forming backpressure scheme is larger, and the fillet area forming is smoother, thus generally exhibiting better formability. When generating the candidate one-stage forming backpressure scheme, other process parameters besides the first-stage candidate backpressure radius can be kept as unchanged as possible, such as maintaining the same pressing conditions, mold movement path, flanging direction, and evaluation criteria, so as to accurately determine the impact of radius adjustment itself on formability. Of course, in some embodiments, while adjusting the first-stage candidate backpressure radius, the local pressing force, lubrication conditions, or transition fillet connection method can also be appropriately optimized to improve the feasibility of the scheme.
[0126] In step S380, after generating candidate one-time molding back-press schemes, a formability simulation verification is performed on the part to be molded based on the candidate one-time molding back-press schemes. This formability simulation verification can use the same verification rules and evaluation criteria as the initial one-time molding back-press scheme, such as checking for problems like cracking, excessive thinning, or wrinkling in the curved flange area. To ensure consistent judgment results, simulations are preferably performed under the same material model, mesh conditions, friction coefficient, and process boundary conditions.
[0127] If the current candidate backpressure radius still fails the formability simulation verification, the candidate backpressure radius can be increased by the first adjustment step size, and a new candidate first-stage forming backpressure scheme can be generated for simulation verification. This process can be repeated until a candidate backpressure radius that passes the formability simulation verification is obtained.
[0128] In step S390, the smallest candidate backpressure radius verified through formability simulation is determined as the target backpressure radius. This is chosen to retain as large a backpressure effect as possible while ensuring acceptable formability. A smaller candidate backpressure radius typically has a greater geometric difference from the product's fillet radius, resulting in a stronger stress distribution adjustment effect when backpressured to the fillet radius. Conversely, a larger candidate backpressure radius, while reducing formability risk, weakens the backpressure effect, potentially making it difficult to meet the maximum collapse tolerance for the subsequent first rebound collapse value. Therefore, selecting the smallest candidate backpressure radius verified through formability simulation is beneficial for balancing rebound instability control and forming safety.
[0129] In some embodiments, when the first springback collapse value does not meet the maximum collapse tolerance and the primary target backpressure radius reaches the forming limit, a secondary target backpressure radius greater than the product fillet radius can be further determined based on the initial springback collapse value, the primary target backpressure radius, and the product fillet radius. By introducing the secondary target backpressure radius, the backpressure adjustment effect in the fillet region can be increased without further reducing the primary target backpressure radius. This allows the semi-finished sheet material to sequentially pass through the fillet states corresponding to the primary target backpressure radius, the secondary target backpressure radius, and the product fillet radius, thereby further adjusting the residual stress distribution in the arc-shaped flange region and its adjacent planar regions.
[0130] In this process, the secondary target backpressure radius is greater than the product fillet radius, and the product fillet radius is greater than the primary target backpressure radius. That is, if the primary target backpressure radius, product fillet radius, and secondary target backpressure radius are denoted as R1, R, and R2 respectively, then they satisfy the following order: R2 > R > R1. The secondary target backpressure radius does not represent the fillet radius of the final product state of the part to be formed, but rather the intermediate fillet radius in the secondary backpressure forming scheme. The final part to be formed still retains the product fillet radius.
[0131] In some embodiments, the method for determining the secondary target backpressure radius includes, but is not limited to, steps S710 to S750: S710. Determine the secondary target back pressure amount based on the initial rebound collapse value and the material characteristics of the semi-finished sheet material; S720. Determine the secondary initial back pressure radius based on the secondary target back pressure amount and the first target back pressure radius; wherein, the secondary initial back pressure radius is greater than the product fillet radius, and the secondary target back pressure amount represents the radial distance between the fillet vertex of the secondary initial back pressure radius and the fillet vertex of the first target back pressure radius; S730. Generate the initial secondary back pressure forming scheme based on the secondary initial back pressure radius; S740. Based on the initial secondary back pressure molding scheme, perform secondary back pressure springback simulation on the part to be molded to obtain the initial second springback collapse value. S750. If the initial secondary rebound collapse value meets the maximum collapse tolerance, the secondary initial backpressure radius is determined as the secondary target backpressure radius.
[0132] In step S710, the secondary target back pressure amount is determined based on the initial rebound collapse value and the material characteristics of the semi-finished sheet.
[0133] The initial springback collapse value is used to characterize the severity of springback instability in the planar region under the initial forming scheme. Although the first springback collapse value has been obtained before entering the secondary backpressure forming scheme, the secondary target backpressure amount is still mainly based on the initial springback collapse value.
[0134] The material characteristics of the semi-finished sheet metal are used to define the degree of deformation and springback response characteristics that the material can withstand during the secondary back-pressing process. These material characteristics may include material grade, yield strength, tensile strength, elongation, modulus of elasticity, work hardening index, anisotropy coefficient, sheet thickness, and forming limit curve. For sheets with high strength and high springback sensitivity, a larger secondary target back-pressing amount may be required to sufficiently change the residual stress distribution in the curved flange area; for sheets with low elongation or prone to wrinkling, it is necessary to control the secondary target back-pressing amount to avoid material accumulation, wrinkling, or localized crushing during the transition from the primary target back-pressing radius to the secondary target back-pressing radius.
[0135] The secondary target backpressure amount is a parameter used to characterize the degree of geometric backpressure adjustment from the fillet corresponding to the primary target backpressure radius to the fillet corresponding to the secondary target backpressure radius in a secondary backpressure forming scheme. Specifically, the secondary target backpressure amount characterizes the radial distance between the fillet vertex of the secondary target backpressure radius and the fillet vertex of the primary target backpressure radius. The larger this radial distance, the more sufficient the geometric adjustment occurs when the semi-finished sheet transitions from the primary target backpressure radius to the secondary target backpressure radius, and the more significant the redistribution of stress state in the curved flange area is usually.
[0136] In some implementations, the secondary backpressure weight can be obtained based on the material characteristics of the semi-finished sheet metal, and the secondary target backpressure amount can be determined based on the secondary backpressure weight and the initial springback collapse value. The secondary backpressure weight is used to characterize the degree of influence of material characteristics on the selection of the secondary target backpressure amount, and it can be determined based on historical simulation data, trial mold data, or process experience of similar materials. For example, for conventional automotive cold-stamped steel sheets, the secondary backpressure weight can be set to an empirical value, such as a correspondence of approximately 1.2 times between the absolute value of the secondary target backpressure amount and the initial springback collapse value. This empirical value is only used to illustrate an optional value method and does not constitute a fixed limitation; in practical applications, the secondary backpressure weight can be adjusted according to the material strength grade, sheet thickness, product fillet radius, flange height, length of the arc flange area, and simulation results.
[0137] In step S720, after determining the secondary target backpressure amount, the secondary initial backpressure radius is determined based on the secondary target backpressure amount and the first target backpressure radius. The secondary initial backpressure radius is greater than the product fillet radius, and the secondary target backpressure amount represents the radial distance between the fillet vertex of the secondary initial backpressure radius and the fillet vertex of the primary target backpressure radius. The process of determining the secondary initial backpressure radius based on the secondary target backpressure amount and the first target backpressure radius can be referenced in the above embodiment, which describes the process of determining the primary initial backpressure radius based on the primary target backpressure amount and the product fillet radius.
[0138] In step S730, after determining the secondary initial back pressure radius, an initial secondary back pressure molding scheme is generated based on the secondary initial back pressure radius.
[0139] The initial secondary back-pressing forming scheme is a candidate secondary back-pressing process scheme constructed using the secondary initial back-pressing radius as the intermediate fillet radius. This scheme is used to sequentially form fillets with the primary target back-pressing radius, fillets with the secondary initial back-pressing radius, and fillets with the final product fillet radius from the semi-finished sheet material. The fillet forming path can be summarized as: semi-finished sheet material → R1 → R2′ → R, where R1 represents the primary target back-pressing radius, R2′ represents the secondary initial back-pressing radius, and R represents the final product fillet radius.
[0140] The initial secondary back-pressing forming scheme can include a local mold surface for forming the primary target back-pressing radius, a back-pressing or shaping surface for forming the secondary initial back-pressing radius, a product surface for finally forming the product's fillet radius, and process elements such as flanging inserts, shaping inserts, pressure plates, support plates, and motion paths that cooperate with the above surfaces. Depending on the actual process layout, the initial secondary back-pressing forming scheme can be implemented through two or more existing processes, as long as the semi-finished sheet material can sequentially undergo the fillet states corresponding to the primary target back-pressing radius, the secondary initial back-pressing radius, and the product's fillet radius.
[0141] In step S740, based on the initial secondary back pressure molding scheme, a secondary back pressure springback simulation is performed on the part to be molded to obtain the initial second springback collapse value.
[0142] The initial second springback collapse value refers to the springback collapse value generated in the planar region when the part to be formed leaves the mold after adopting the initial secondary backpressure molding scheme. It is used to evaluate whether the secondary initial backpressure radius can meet the requirements for springback instability control in the planar region. To ensure the comparability of the evaluation results, the secondary backpressure springback simulation preferably uses the same or comparable material model, mesh generation, friction conditions, blanking conditions, and springback evaluation benchmark as the initial backpressure springback simulation and the primary backpressure springback simulation.
[0143] In the simulation of secondary backpressure and springback, it is necessary to fully simulate the process of forming a rounded corner with a primary target backpressure radius, a secondary initial backpressure radius, and a final product rounded corner radius from a semi-finished sheet material. If the simulation results show that the local depressions in the planar area are significantly reduced, and the initial second springback collapse value meets the maximum collapse tolerance, it indicates that the initial secondary backpressure forming scheme corresponding to the secondary initial backpressure radius can effectively control springback instability.
[0144] In some implementations, the formability of the part to be formed can be verified through simulation based on the initial secondary back-pressing molding scheme. This formability simulation verification is used to determine whether there are formability problems such as cracking, excessive thinning, wrinkling, or local crushing in the semi-finished sheet material during the transition from the primary target back-pressing radius to the secondary initial back-pressing radius, and then back-pressing to the product fillet radius. Generally, because the change range of the secondary target back-pressing amount relative to the product fillet radius is small, and the secondary initial back-pressing radius is larger than the product fillet radius, the sheet material usually does not easily reach the forming limit before reaching the expected secondary target back-pressing amount; however, for parts to be formed that are thin, have a narrow planar area, or have restricted material flow, this formability simulation verification can still be added to improve process safety. If the formability simulation verification fails, the current initial secondary back-pressing molding scheme can be considered unusable, and if necessary, the secondary initial back-pressing radius (reducing the secondary initial back-pressing radius), the mold transition surface, or process constraints can be adjusted; if it still fails, it can be determined that the control of the arc-shaped flange springback instability has failed or other process schemes need to be adopted.
[0145] In step S750, if the initial secondary rebound collapse value meets the maximum collapse tolerance, the secondary initial backpressure radius is determined as the secondary target backpressure radius. Meeting the maximum collapse tolerance means that after adopting the initial secondary backpressure molding scheme, the maximum amount of indentation or the degree of local collapse in the planar area is within a preset allowable range. This indicates that the intermediate rounded corner path formed based on the secondary initial backpressure radius can provide sufficient stress redistribution, therefore the secondary initial backpressure radius can be determined as the secondary target backpressure radius.
[0146] In some embodiments, after performing secondary backpressure springback simulation on the part to be molded based on the initial secondary backpressure molding scheme and obtaining the initial second springback collapse value, if the initial secondary springback collapse value does not meet the maximum collapse tolerance, it indicates that the backpressure adjustment effect provided by the secondary initial backpressure radius is still insufficient. In this case, the secondary initial backpressure radius can be sequentially increased according to a preset second adjustment step size to obtain secondary candidate backpressure radii, and secondary backpressure springback simulation and formability simulation verification can be performed on the candidate secondary molding backpressure schemes corresponding to the secondary candidate backpressure radii.
[0147] Therefore, in some embodiments, in step S740, based on the initial secondary backpressure molding scheme, a secondary backpressure springback simulation is performed on the part to be molded to obtain the initial second springback collapse value. Further steps including but not limited to S760 to S790 may also be included. S760. If the initial secondary rebound collapse value does not meet the maximum collapse tolerance, the secondary initial backpressure radius is increased sequentially according to the preset second adjustment step size to obtain the secondary candidate backpressure radius. S770, Generate corresponding candidate secondary forming back pressure schemes according to the secondary candidate back pressure radius in sequence; S780: Based on the candidate secondary forming back pressure scheme, perform secondary back pressure springback simulation and formability simulation verification on the part to be formed to obtain the candidate second springback collapse value. S790. When the candidate second rebound collapse value meets the maximum collapse tolerance and the result of the shapeability simulation verification is passed, the current secondary candidate backpressure radius is determined as the secondary target backpressure radius.
[0148] In step S760, if the initial secondary rebound collapse value does not meet the maximum collapse tolerance, the secondary initial backpressure radius is increased sequentially according to the preset second adjustment step size to obtain the secondary candidate backpressure radius.
[0149] If the initial secondary rebound collapse value does not meet the maximum collapse tolerance, it usually indicates that the geometric adjustment from the primary target backpressure radius to the secondary initial backpressure radius is insufficient, and the residual stress distribution in the curved flange area and adjacent planar areas has not been sufficiently altered. Therefore, the geometric adjustment during the secondary backpressure process can be increased by increasing the secondary initial backpressure radius. This allows the semi-finished sheet material to transition from the primary target backpressure radius to a larger intermediate fillet radius before backpressure to the final product fillet radius, thereby enhancing the rebound instability control effect.
[0150] The second adjustment step size refers to the radius adjustment amount used each time the initial secondary backpressure radius is increased. The second adjustment step size can be determined based on the fillet radius of the part to be formed, the initial springback collapse value, the sheet thickness, material characteristics, and simulation efficiency requirements. The secondary candidate backpressure radius refers to the candidate radius obtained by increasing the initial secondary backpressure radius according to the second adjustment step size. The secondary candidate backpressure radius is still larger than the fillet radius of the part and is used to generate candidate secondary forming backpressure schemes. As the secondary candidate backpressure radius gradually increases, the adjustment effect of the secondary backpressure process on the residual stress distribution is usually enhanced, but it may also increase the risk of material buildup, wrinkling, or local morphological instability. Therefore, it is necessary to combine it with formability simulation verification for judgment.
[0151] In step S770, after obtaining the secondary candidate backpressure radius, corresponding candidate secondary forming backpressure schemes are generated sequentially based on the secondary candidate backpressure radius. This scheme is used to sequentially form the semi-finished sheet material into fillets with a primary target backpressure radius, fillets with secondary candidate backpressure radii, and fillets with the product fillet radius. Compared to the initial secondary backpressure forming scheme, the intermediate fillet radius in the candidate secondary forming backpressure scheme is larger, providing a stronger backpressure adjustment effect. When generating candidate secondary forming backpressure schemes, it is preferable to keep other process parameters unchanged except for the secondary candidate backpressure radius, such as keeping the primary target backpressure radius, product fillet radius, pressing conditions, mold movement path, friction conditions, and evaluation criteria consistent, in order to accurately compare the influence of different secondary candidate backpressure radii on springback collapse value and formability.
[0152] In step S780, after generating candidate secondary forming back pressure schemes, secondary back pressure springback simulation and formability simulation verification are performed on the part to be formed based on the candidate secondary forming back pressure schemes to obtain candidate second springback collapse values.
[0153] The candidate second springback collapse value refers to the springback collapse value generated in the planar area when the part to be formed leaves the mold after adopting the candidate secondary forming backpressure scheme. This value is used to evaluate whether the candidate secondary forming backpressure scheme corresponding to the current secondary candidate backpressure radius can meet the maximum collapse tolerance. Secondary backpressure springback simulation is used to determine the improvement effect of the candidate secondary forming backpressure scheme on springback instability in the planar area; formability simulation verification is used to determine whether there are unacceptable cracking, excessive thinning, wrinkling, local material accumulation, or local crushing problems during the forming process of the candidate secondary forming backpressure scheme. Since the larger the secondary candidate backpressure radius, the greater the geometric adjustment amount when the semi-finished sheet changes from the primary target backpressure radius to the secondary candidate backpressure radius, although the springback improvement effect may be enhanced, the risk of wrinkling or material accumulation may also increase. Therefore, the candidate second springback collapse value and the formability simulation verification result need to be used together as the basis for whether the secondary candidate backpressure radius is usable.
[0154] In one implementation, the current candidate secondary forming backpressure scheme can be first verified by formability simulation. If the formability simulation verification fails, there is no need to continue confirming the springback effect of the scheme, or it can be marked as an unusable scheme. Alternatively, secondary backpressure springback simulation can be performed first to obtain the candidate second springback collapse value, and then the formability simulation verification result can be used for comprehensive judgment.
[0155] In step S790, when the candidate second rebound collapse value meets the maximum collapse tolerance and the result of the shapeability simulation verification is passed, the current secondary candidate backpressure radius is determined as the secondary target backpressure radius.
[0156] The candidate second rebound collapse value meets the maximum collapse tolerance, indicating that the candidate secondary forming backpressure scheme corresponding to the current secondary candidate backpressure radius can control the local collapse in the planar area within the allowable range. The result of the formability simulation verification is passed, indicating that the candidate secondary forming backpressure scheme did not exhibit unacceptable cracking, excessive thinning, wrinkling, or other formability defects during the forming process. Only when both of the above conditions are met simultaneously can the current secondary candidate backpressure radius be suitable as the secondary target backpressure radius.
[0157] In one implementation, the secondary candidate backpressure radius that first satisfies the condition of "the candidate second springback collapse value meets the maximum collapse tolerance and the formability simulation verification passes" during the second adjustment step increment process can be determined as the secondary target backpressure radius. This can meet the springback control requirements while avoiding excessively large secondary candidate backpressure radii that could increase formability risks or mold design complexity. In another implementation, if multiple secondary candidate backpressure radii meet the requirements, one can be selected as the secondary target backpressure radius based on springback control margin, formability safety margin, mold processing convenience, and production stability. For example, when there are large batch fluctuations in material during production, a secondary candidate backpressure radius with a larger springback control margin can be selected; when the wrinkling risk is more sensitive, a secondary candidate backpressure radius with a relatively small radius that just meets the maximum collapse tolerance can be selected.
[0158] Understandably, if the formability simulation fails during the process of sequentially increasing the secondary initial backpressure radius, and the candidate second springback collapse value still does not meet the maximum collapse tolerance, it indicates that further increasing the secondary candidate backpressure radius is already limited by formability, and the current secondary backpressure path still cannot control the springback instability in the planar region within the allowable range. In this case, it can be determined that the control of springback instability in the arc-shaped flange has failed, or other supplementary process measures are needed, such as adjusting the pressing conditions, changing the local supplementary surface, optimizing the flange sequence, adding local shaping methods, or re-evaluating the product structure.
[0159] Through steps S760 to S790, when the secondary initial springback collapse value does not meet the maximum collapse tolerance, the secondary initial backpressure radius is gradually increased according to the second adjustment step size. Secondary candidate backpressure radii are then screened through secondary backpressure springback simulation and formability simulation verification. This allows for obtaining a secondary target backpressure radius that effectively controls springback instability in planar areas while ensuring the safety of semi-finished sheet metal forming. This ensures that the secondary backpressure forming scheme has sufficient stress redistribution without causing wrinkling or other forming defects due to excessive backpressure.
[0160] Understandably, formability simulation verification can be used to determine whether the arc-shaped flange area can be stably formed when the part to be formed is formed according to the forming back pressure scheme corresponding to the first initial back pressure radius, the first candidate back pressure radius, the second candidate back pressure radius, or other back pressure radii.
[0161] In some embodiments, the molding simulation verification may include, but is not limited to, steps S351 to S353: S351. Obtain the molding simulation results of the part to be molded; S352. Based on the molding simulation results, perform a morphological inspection on the arc-shaped flange area; S353. If at least one of the following is found in the arc-shaped flange area: cracking, excessive thinning, and wrinkling, the molding simulation verification is deemed unsuccessful.
[0162] In step S351, the forming simulation result refers to the result data obtained after performing stamping forming simulation on the part to be formed or the semi-finished sheet metal based on the corresponding forming back pressure scheme. This forming back pressure scheme can be an initial first-stage forming back pressure scheme, a candidate first-stage forming back pressure scheme, an initial second-stage forming back pressure scheme, a candidate second-stage forming back pressure scheme, or other forming schemes used to form the back pressure radius. The forming simulation result can include the geometry, strain distribution, stress distribution, thickness distribution, thinning rate distribution, forming limit diagram results, wrinkling risk area, failure index, and local material flow state of the part to be formed at each forming stage. When obtaining the forming simulation result, stamping forming simulation software can be used to simulate the process of the semi-finished sheet metal from entering the current process to the end of forming. To ensure that the formability simulation verification is consistent with the actual process conditions, the simulation can use material models, sheet metal thickness, friction coefficient, blank holder force, die movement path, die fillet radius, flanging insert structure, and process boundary conditions that match actual production. For single-stage backpressure related formability simulation verification, the simulation results should reflect the process of the semi-finished sheet material first forming a fillet smaller than the product's fillet radius and then backpressured to the product's fillet radius. For double-stage backpressure related formability simulation verification, the simulation results should reflect the process of the semi-finished sheet material sequentially passing through the first target backpressure radius, the second target backpressure radius or the second candidate backpressure radius, and the product's fillet radius. Forming simulation results can be output in the form of numerical data, contour maps, cross-sectional views, or animation results. For example, forming limit maps can be used to determine whether the material strain state is close to or exceeds the cracking limit; thickness distribution contour maps can be used to determine whether there is excessive thinning; wrinkling risk contour maps or local morphological results can be used to determine whether wrinkling or material accumulation exists.
[0163] In step S352, after obtaining the molding simulation results, a morphological inspection of the arc-shaped flange area is performed based on the molding simulation results. The arc-shaped flange area is a key area for adjusting the fillet back pressure in this application. It includes the final fillet area with the product fillet radius, and may also include intermediate fillet areas with an initial back pressure radius, a candidate back pressure radius, a target back pressure radius, a secondary initial back pressure radius, a secondary candidate back pressure radius, or a secondary target back pressure radius during the molding process. Since adjusting the back pressure radius directly changes the curvature, material flow path, and local strain state of this area, a focused morphological inspection of the arc-shaped flange area is necessary.
[0164] Morphological inspection can include a comprehensive check of the geometry, material condition, and local defect risks of the curved flange area. Specifically, it can check whether the curved flange area remains continuous and smooth during and after forming, and whether there are obvious sharp bends, local material accumulation, or abnormal waves in the rounded corner transition; it can check whether the strain state of the curved flange area exceeds the material forming limit; it can check whether the thickness of the curved flange area is lower than the allowable thickness; and it can also check whether there are local out-of-plane fluctuations or wrinkles in the curved flange area.
[0165] In step S353, after performing a morphological check on the curved flange area, if the curved flange area exhibits at least one of the following: cracking, excessive thinning, and wrinkling, the formability simulation verification is deemed unsuccessful. Cracking refers to a situation where the local strain in the curved flange area exceeds the material forming limit during the forming process, leading to material fracture or an unacceptable risk of fracture. Excessive thinning refers to a local reduction in plate thickness in the curved flange area exceeding a preset allowable threshold. Wrinkling refers to out-of-plane waves, wrinkles, or local instability in the curved flange area caused by local compressive stress, material accumulation, or insufficient constraint.
[0166] In some embodiments, if the curved flange area is free from cracking, excessive thinning, and wrinkling, the formability simulation verification is considered passed. Alternatively, under more stringent process requirements, the curved flange area may be further inspected for issues such as localized pressure marks, material buildup, uneven fillets, excessive contour deviation, or residual creases after back pressing; if these issues are not unacceptable, the formability simulation verification is considered passed. In other words, the cracking, excessive thinning, and wrinkling listed in the claims are typical scenarios for failing the formability simulation verification, and the addition of other formability assessment items based on actual product requirements is not excluded.
[0167] In some embodiments, determining the target backpressure amount based on the initial rebound collapse value and the material characteristics of the semi-finished sheet material may include: obtaining the corresponding backpressure amount weight based on the material characteristics of the semi-finished sheet material; and calculating the product of the backpressure amount weight and the initial rebound collapse value as the target backpressure amount. This method, by correlating the initial rebound instability with the material rebound characteristics, makes the determination of the target backpressure amount more targeted.
[0168] Since the initial rebound collapse value may be negative or positive under different simulation coordinate systems, in order to make the primary target backpressure amount represent the degree of geometric backpressure, the absolute value of the initial rebound collapse value can be used in the calculation in actual practice. That is to say, the primary target backpressure amount is used to represent the distance or geometric adjustment amount, and it is usually a non-negative value.
[0169] In one implementation, the target backpressure amount can be denoted as... L 1. Let the initial rebound collapse value be denoted as 'a', and let the weight of the first backpressure amount be denoted as 'a'. K 1. The target backpressure amount can be determined based on the following relationship: L 1= K 1·∣a∣.
[0170] The weight of the initial backpressure amount can be determined based on the material characteristics of the semi-finished sheet metal. These material characteristics may include material grade, yield strength, tensile strength, elongation, elastic modulus, work hardening index, sheet thickness, and forming limit curve. For materials with high springback sensitivity, the initial backpressure amount weight can be appropriately increased to provide a stronger stress redistribution effect; for materials with low forming margin and high cracking risk, the initial backpressure amount weight can be appropriately decreased and corrected through subsequent formability simulation verification. For common automotive cold stamping sheet metal, the initial backpressure amount weight can be selected based on simulation data and trial molding experience of similar parts, such as a value of 1.2.
[0171] In some implementations, the weight of the first-stage backpressure can also be determined through a material database or an empirical mapping table. For example, a correspondence between material grades and the weight of the first-stage backpressure can be established in advance; multiple value ranges can also be divided according to the material strength grade, sheet thickness range, and product fillet radius range. For new materials or special structural parts, empirical values can be used for simulation first, and then the weight of the first-stage backpressure can be corrected based on the first springback collapse value and the formability simulation verification results.
[0172] Understandably, in some embodiments, the secondary target backpressure amount can also be determined based on the initial rebound collapse value and the material characteristics of the semi-finished sheet. Specifically, the corresponding secondary backpressure amount weight can be obtained based on the material characteristics of the semi-finished sheet, and the secondary target backpressure amount can be determined based on the absolute value of the secondary backpressure amount weight and the initial rebound collapse value. The comparison will not be elaborated further.
[0173] Understandably, in the various embodiments of this application, initial springback simulation, first-stage springback simulation, second-stage springback simulation, and formability simulation verification can all be implemented based on sheet metal stamping finite element simulation. "Simulation" is used to predict the material flow, stress-strain state, springback morphology, and formability risk of the part to be formed under different forming schemes before actual mold making or mold repair, thereby providing a basis for determining the primary target springback radius, secondary target springback radius, and target forming scheme. Simulation can be performed using stamping simulation software, such as AutoForm, PAM-STAMP, Dynaform, LS-DYNA, Abaqus, or other finite element software capable of sheet metal forming analysis and springback analysis.
[0174] Understandably, different types of simulations can be obtained by modifying the same basic simulation model. Specifically, initial springback simulation can be based on an initial forming scheme, allowing the semi-finished sheet to be formed into the product state according to the initial forming scheme, and releasing the mold constraints after forming to calculate the springback result. First-stage springback simulation can modify the local rounded corner forming path of the arc-shaped flange area based on the initial forming scheme, first forming a rounded corner with a first-stage target springback radius, and then pressing the rounded corner with the first-stage target springback radius back into a rounded corner with the product's rounded corner radius. Second-stage springback simulation can further introduce a second-stage target springback radius based on the first-stage springback forming path, allowing the semi-finished sheet to sequentially form rounded corners with the first-stage target springback radius, rounded corners with the second-stage target springback radius, and rounded corners with the product's rounded corner radius.
[0175] The embodiments of this application have been described in detail above with reference to the accompanying drawings. However, this application is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of this application. Furthermore, unless otherwise specified, the embodiments and features described in the embodiments of this application can be combined with each other.
Claims
1. A method for controlling the springback instability of an arc-shaped flange, characterized in that, An application to the processing of parts to be formed, the parts having an arc-shaped flanged area and a planar area connected to the arc-shaped flanged area, the arc-shaped flanged area having a product fillet radius, the method comprising: Obtain the initial molding scheme and maximum collapse tolerance of the part to be molded; Based on the initial molding scheme, an initial springback simulation is performed on the part to be molded to obtain the initial springback collapse value. Based on the initial springback collapse value and the product fillet radius, a primary target backpressure radius smaller than the product fillet radius is determined, and a primary backpressure forming scheme is generated based on the primary target backpressure radius. The primary backpressure forming scheme is used to first form the semi-finished sheet material into a fillet with the primary target backpressure radius, and then backpressure the fillet with the primary target backpressure radius into a fillet with the product fillet radius. Based on the aforementioned one-stage back-pressure forming scheme, a one-stage back-pressure springback simulation is performed on the part to be formed to obtain the first springback collapse value. If the first rebound collapse value meets the maximum collapse tolerance, the single-stage backpressure forming scheme is determined as the target forming scheme; Based on the target forming scheme, the semi-finished sheet material is subjected to arc-shaped flanging to obtain the part to be formed.
2. The method for controlling the springback instability of an arc-shaped flange according to claim 1, characterized in that, Based on the aforementioned single-stage back-pressure forming scheme, a single-stage back-pressure springback simulation is performed on the part to be formed to obtain a first springback collapse value. The process then further includes: If the first springback collapse value does not meet the maximum collapse tolerance and the primary target backpressure radius reaches the forming limit, a secondary target backpressure radius greater than the product fillet radius is determined based on the initial springback collapse value, the primary target backpressure radius, and the product fillet radius. A secondary backpressure forming scheme is then generated based on the secondary target backpressure radius. The secondary backpressure forming scheme is used to sequentially form the semi-finished sheet material into fillets with the primary target backpressure radius, fillets with the secondary target backpressure radius, and fillets with the product fillet radius. Based on the aforementioned secondary back-pressure forming scheme, a secondary back-pressure springback simulation is performed on the part to be formed to obtain the second springback collapse value. If the second rebound collapse value meets the maximum collapse tolerance, the secondary backpressure forming scheme is determined as the target forming scheme.
3. The method for controlling the springback instability of an arc-shaped flange according to claim 1, characterized in that, The initial springback simulation of the part to be formed, based on the initial forming scheme, is performed to obtain the initial springback collapse value, including: Based on the initial molding scheme, an initial springback simulation is performed on the part to be molded to obtain the initial molding form of the part after it leaves the mold. Based on the initial forming shape, the initial springback displacement distribution of the planar region is obtained; Based on the initial rebound displacement distribution, the initial rebound instability region of the planar region is obtained; The maximum indentation in the initial rebound instability region is extracted as the initial rebound collapse value.
4. The method for controlling the springback instability of an arc-shaped flange according to claim 3, characterized in that, The planar area includes a planar design area; Based on the initial molding scheme, the initial springback simulation of the part to be molded is performed to obtain the initial springback collapse value, and then the process further includes: A first stress release simulation was performed on the arc-shaped flange area in the initial forming shape to obtain the first release springback displacement distribution of the planar area; A second stress release simulation is performed on the planar shaping area of the initial forming shape to obtain the second release springback displacement distribution of the planar area; Based on the first release rebound displacement distribution, the first release rebound instability region and the first release rebound collapse value are extracted; Based on the second release rebound displacement distribution, extract the second release rebound instability region and the second release rebound collapse value; Based on the first release rebound instability area and the second release rebound instability area, and / or the first release rebound collapse value and the second release rebound collapse value, determine whether the rebound instability of the initial rebound instability area originates from the arc-shaped flange area; If it is determined that the cause of the rebound instability originates from the arc-shaped flange area, the step of determining a primary target back pressure radius smaller than the product fillet radius is performed based on the initial rebound collapse value and the product fillet radius.
5. The method for controlling the springback instability of an arc-shaped flange according to claim 1, characterized in that, The step of determining a primary target backpressure radius smaller than the product corner radius based on the initial rebound collapse value and the product corner radius includes: Based on the initial rebound collapse value and the material characteristics of the semi-finished sheet, determine the target back pressure amount for one operation; Based on the target back pressure amount and the product fillet radius, an initial back pressure radius is determined; wherein, the initial back pressure radius is smaller than the product fillet radius, and the target back pressure amount represents the radial distance between the fillet vertex of the initial back pressure radius and the fillet vertex of the product fillet radius; Based on the initial back pressure radius, a corresponding initial primary forming back pressure scheme is generated; Based on the initial one-time molding back pressure scheme, the formability simulation verification of the part to be molded is performed. If the initial backpressure radius passes the molding simulation verification, the initial backpressure radius is determined as the target backpressure radius.
6. The method for controlling the springback instability of an arc-shaped flange according to claim 5, characterized in that, After performing formability simulation verification on the part to be molded based on the initial one-time molding back pressure scheme, the method further includes: If the initial back pressure radius fails the molding simulation verification, the initial back pressure radius is increased sequentially according to the preset first adjustment step size to obtain a candidate back pressure radius. Based on the first candidate back pressure radius, a corresponding candidate first-stage forming back pressure scheme is generated; Based on the candidate one-time molding back pressure scheme, the formability simulation verification of the part to be molded is performed. The candidate back pressure radius that passes the molding simulation and is the smallest is determined as the target back pressure radius.
7. The method for controlling the springback instability of an arc-shaped flange according to claim 2, characterized in that, The step of determining a secondary target backpressure radius greater than the product corner radius based on the initial rebound collapse value, the primary target backpressure radius, and the product corner radius includes: The secondary target back pressure amount is determined based on the initial rebound collapse value and the material characteristics of the semi-finished sheet material; The secondary initial back pressure radius is determined based on the secondary target back pressure amount and the primary target back pressure radius; wherein, the secondary initial back pressure radius is greater than the product fillet radius, and the secondary target back pressure amount represents the radial distance between the fillet vertex of the secondary initial back pressure radius and the fillet vertex of the primary target back pressure radius; An initial secondary back pressure forming scheme is generated based on the aforementioned secondary initial back pressure radius; Based on the initial secondary back pressure molding scheme, a secondary back pressure springback simulation is performed on the part to be molded to obtain the initial second springback collapse value. If the initial secondary rebound collapse value satisfies the maximum collapse tolerance, the secondary initial backpressure radius is determined as the secondary target backpressure radius.
8. The method for controlling the springback instability of an arc-shaped flange according to claim 7, characterized in that, Based on the initial secondary backpressure molding scheme, a secondary backpressure springback simulation is performed on the part to be molded to obtain the initial second springback collapse value. The process then further includes: If the initial secondary rebound collapse value does not meet the maximum collapse tolerance, the secondary initial backpressure radius is increased sequentially according to the preset second adjustment step size to obtain the secondary candidate backpressure radius; Candidate secondary forming back pressure schemes are generated sequentially based on the secondary candidate back pressure radii. Based on the candidate secondary forming back pressure scheme, the part to be formed is subjected to secondary back pressure springback simulation and formability simulation verification to obtain the candidate second springback collapse value. When the candidate second rebound collapse value meets the maximum collapse tolerance and the result of the shapeability simulation verification is passed, the current secondary candidate backpressure radius is determined as the secondary target backpressure radius.
9. The method for controlling the springback instability of an arc-shaped flange according to claim 5, 6, or 8, characterized in that, The moldability simulation verification includes: Obtain the molding simulation results of the part to be molded; Based on the molding simulation results, the morphology of the arc-shaped flange area is checked; If at least one of the following conditions exists in the arc-shaped flange area: cracking, excessive thinning, and wrinkling, the molding simulation verification is deemed to have failed.
10. The method for controlling the springback instability of an arc-shaped flange according to claim 5, characterized in that, The step of determining the target backpressure amount based on the initial rebound collapse value and the material characteristics of the semi-finished sheet material includes: Based on the material characteristics of the semi-finished sheet material, the corresponding weight of the first back pressure amount is obtained; The product of the backpressure weight and the initial rebound collapse value is calculated as the target backpressure.