Forging process of a crescent-shaped 5A06 aluminum alloy forging for aviation use
The process for forging crescent-shaped 5A06 aluminum alloy for aerospace applications by precisely designing billet dimensions and optimizing forging parameters has solved the problems of raw material waste and high mold costs, achieving high-efficiency production and making it suitable for mass production of crescent-shaped 5A06 aluminum alloy forgings for aerospace applications.
Patent Information
- Application Number
- CN202611301568.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
The current production of crescent-shaped 5A06 aluminum alloy forgings for aviation applications suffers from problems such as high raw material loss, high mold costs, and low production efficiency.
By employing precise design of billet dimensions and optimization of forging parameters, and through the processes of open forging and split forging, the billet is formed directly by die forging without the need for bending dies. Combined with heat treatment processes, this improves material utilization and production efficiency.
It significantly improves material utilization to 11%, saves mold costs, reduces forging cycles, enhances production efficiency, and produces high-quality forming parts. It is suitable for mass production of crescent-shaped 5A06 aluminum alloy forgings for aerospace applications.
Smart Images

Figure CN123102899A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy forging technology, specifically to a forging process for a crescent-shaped 5A06 aluminum alloy forging for aerospace applications. Background Technology
[0002] 5A06 aluminum alloy belongs to the Al-Mg series of rust-resistant aluminum alloys. It has high strength and good corrosion stability, and is widely used in the manufacture of important load-bearing components in the aerospace field. The shapes of aerospace structural components are usually quite complex, with crescent-shaped products being particularly difficult to form.
[0003] Currently, the production of crescent-shaped 5A06 aluminum alloy forgings for aerospace applications mainly faces the following problems: First, crescent-shaped aluminum alloy forgings are traditionally produced using free forging. While free forging equipment is highly versatile, it consumes a great deal of raw materials, with material utilization typically not exceeding 10%, resulting in serious material waste.
[0004] Secondly, if die forging is used for production, due to the special shape of the crescent-shaped forging, the forging blank obtained by free forging needs to be made by adding bending dies. This not only increases the cost of dies, but also increases the number of forging passes, which significantly increases the production cost.
[0005] Third, the existing processes are inefficient and cannot meet the aviation industry's demand for mass production of complex structural components.
[0006] Therefore, it is necessary to develop a forging process for crescent-shaped 5A06 aluminum alloy forgings for aviation applications that can improve material utilization, reduce mold investment and forging cycles, and increase production efficiency. Summary of the Invention
[0007] This invention addresses the technical problems of high raw material loss and high cost caused by the need for bending dies in the existing forging process of crescent-shaped 5A06 aluminum alloy forgings for aviation applications, and provides a forging process for crescent-shaped 5A06 aluminum alloy forgings for aviation applications.
[0008] The present invention aims to solve the following technical problems: (1) reduce raw material loss and improve material utilization; (2) avoid the use of bending dies in die forging production and reduce die costs; (3) reduce the number of forging passes and improve production efficiency.
[0009] To achieve the above-mentioned objectives, this invention provides a forging process for a crescent-shaped 5A06 aluminum alloy forging for aerospace applications, comprising the following steps: Step 1, Forging the billet The 5A06 aluminum alloy raw material bar is heated and then upset forged. The heating temperature is controlled at 430-450℃, and the holding time is 1.5-1.6 mm / min × H.heat (H) heat (This refers to the maximum effective thickness of the billet). The deformation per forging pass is controlled at 20-30%, with the hammer pressing down at a uniform speed of 20-30 mm / s to obtain the billet. Preferably, the billet forging process involves one forging pass.
[0010] Step 2, Billet Preparation: Based on the finished dimensions of the crescent-shaped forging, calculate the billet dimensions using the following formula: Total length of billet L1 = L × L X L X This is an empirical coefficient for length, with a value ranging from 0.95 to 0.97, where L is the length of the forged part after forming. Total height of billet H1 = H × H X H X This is a high-empirical coefficient, with a value range of 0.88 to 0.90, where H is the height of the forging after forming. The length of the billet at the middle is L3 = 2 × (R² - (R + h - H / 2)²). 1 / 2 R is the radius of the arc groove in the middle of the formed forging, and h is the distance from the bottom of the arc groove to the bottom of the formed forging. The included angle in the middle of the billet is Deg = 135°; The height of the billet at the middle is h1 = H1 / 2; billet width W1 = W × W X W X W is an empirical coefficient for width, with a value ranging from 0.73 to 0.75 mm, where W is the width of the forged part after forming. For concave fillets, r1 = 60-70 mm; for convex fillets, r2 = 5-8 mm. The blank dimensions calculated using the above formula can be directly used for subsequent die forging without the need for additional bending and blank preparation.
[0011] Step 3, Die Forging Die forging is performed in two heats: First heating: Heat the billet to 430-450℃ and hold for 1.5-1.6 mm / min × H1. Position the billet in the mold, clean the cavity with compressed air to remove dirt, and evenly spray mold lubricant onto the mold cavity surface using a spray gun. Place the billet in the mold cavity along its outer shape, lightly tap it with the first hammer to position it, and then set the striking force to 40-50 MN for the second hammer blow. After air cooling, polish to remove damage.
[0012] Second heat: Heat the billet after the first heat to 430-450℃ and hold for 120-240 minutes. Similarly, place the billet in the mold, use compressed air to blow away the dirt in the cavity, spray the mold lubricant evenly on the surface of the mold cavity with a spray gun, place the billet in the mold cavity along the shape of the cavity, and strike with a hammer with a force of 50MN-60MN.
[0013] Step 4, heat treatment The forgings are placed in a warm charging furnace and held at 370–390°C for 430–440 minutes, then air-cooled. Beneficial effects
[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) Significantly improves material utilization. The material utilization rate of crescent-shaped 5A06 aluminum alloy forgings produced by the traditional free forging process is only 7%, while the material utilization rate of the process of this invention can be increased to 11%, effectively reducing the consumption of raw materials.
[0015] (2) Save on mold costs. Compared with the traditional die forging process, which requires an additional bending mold for blank preparation, the present invention, through precise design and calculation of the blank size, allows the blank after blank preparation to be directly used for die forging, saving a bending mold.
[0016] (3) Reduce the number of forging passes. Since there is no need for bending and billet preparation, the present invention reduces one forging pass compared with the traditional die forging process, thereby improving production efficiency and reducing energy consumption.
[0017] (4) Good forming quality. Ten complex 5A06 aluminum alloy crescent-shaped structural parts for aviation were trial-produced using the process of this invention. The forming effect was good and no scrap occurred. Attached Figure Description
[0018] Figure 1 This is a drawing of the crescent-shaped 5A06 aluminum alloy forging for aviation applications according to the present invention; Figure 2 for Figure 1 A cross-sectional view of BB; Figure 3 For the billet drawing; Figure 4 for Figure 3 AA sectional view. Detailed Implementation
[0019] The present invention will be further described below with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and should not be used to limit the scope of protection of the present invention.
[0020] Example 1: A crescent-shaped 5A06 aluminum alloy forging for aerospace applications was developed using the process of this invention, such as... Figure 1 and 2 As shown, the specific steps are as follows:
[0021] Step 1, Forging the billet Heat the 5A06 aluminum alloy raw material bar to 440℃, and hold it at that temperature for 1.55mm / min × H. heat Calculation (H) heat (This refers to the maximum effective thickness of the billet). Upsetting forging is performed, with the deformation controlled at 25% per pass. The hammer is pressed down at a uniform speed of 25 mm / s, and one pass is performed.
[0022] Step 2, blank preparation Based on the finished dimensions of the crescent-shaped forging, such as Figure 3 and 4 Calculate the blank size using the following parameters: Length empirical coefficient L X Take 0.96, and use the highly empirical coefficient H. X Take 0.89, the empirical coefficient for width, W X Take 0.74; The included angle in the middle of the billet is Deg = 135°; The concave fillet has a radius of r1 = 60 mm, and the convex fillet has a radius of r2 = 8 mm. The total length L1, total height H1, intermediate length L3, intermediate height h1, and width W1 of the billet are calculated using the formula.
[0023] Step 3, Die Forging First heat: Heat the billet to 440℃ and hold for 1.55mm / min × W1. Position the billet in the mold, use compressed air to blow away any dirt from the cavity, and evenly spray mold lubricant onto the mold cavity surface using a spray gun. Place the billet in the mold cavity along its outer shape, lightly tap it with the first hammer to position it, and then set the second hammer blow to a striking force of 45MN. After air cooling, polish to remove any damage.
[0024] Second heat: Heat the billet to 440℃ and hold for 180 minutes. Place the billet in the mold, use compressed air to blow away the dirt in the cavity, spray the mold lubricant evenly on the surface of the mold cavity with a spray gun, place the billet in the mold cavity along the shape of the cavity, and strike with a hammer force of 55MN.
[0025] Step 4, heat treatment The forgings are placed in a preheated furnace and held at 380℃ for 435 minutes, then air-cooled.
[0026] Using the process described in this embodiment, a total of 10 complex crescent-shaped 5A06 aluminum alloy structural parts for aerospace applications were trial-produced. The forming effect was good, and no scrap occurred. According to statistics, the raw material utilization rate increased from 7% in the traditional free forging process to 11%, and a bending die and one forging cycle were saved.
[0027] Example 2: The difference between this example and Example 1 is that the process parameters are different.
[0028] In step one, the heating temperature is 430℃, the deformation per firing is controlled at 20%, and the pressing speed is 20mm / s.
[0029] In step two, the empirical coefficient L for length X Take 0.95, and use the empirical coefficient H. X Take 0.88, width empirical coefficient W X Take 0.73; for the concave fillet, r1 = 65mm, and for the convex fillet, r2 = 5mm.
[0030] In step three, the first heating temperature is 430℃ and the impact force is 40MN; the second heating temperature is 430℃, the holding time is 120min, and the impact force is 50MN.
[0031] In step four, the heat treatment temperature is 370℃ and the holding time is 430min.
[0032] This embodiment can also produce crescent-shaped 5A06 aluminum alloy forgings with good forming quality.
[0033] Example 3: The difference between this example and Example 1 is that the process parameters are different.
[0034] In step one, the heating temperature is 450℃, the deformation per firing is controlled at 30%, and the pressing speed is 30mm / s.
[0035] In step two, the empirical coefficient L for length X Take 0.97, and use the highly empirical coefficient H. X Take 0.90, width empirical coefficient W X Take 0.75; for the concave fillet, r1 = 70 mm, and for the convex fillet, r2 = 7 mm.
[0036] In step three, the first heating temperature is 450℃ and the impact force is 50MN; the second heating temperature is 450℃, the holding time is 240min, and the impact force is 60MN.
[0037] In step four, the heat treatment temperature is 390℃ and the holding time is 440min.
[0038] This embodiment can also produce crescent-shaped 5A06 aluminum alloy forgings with good forming quality.
[0039] The forging process for crescent-shaped 5A06 aluminum alloy forgings for aerospace applications provided by this invention achieves direct die forging without bending dies through precise design of billet dimensions and optimization of forging parameters. This significantly improves material utilization, reduces the number of forging passes, and lowers production costs. The process is simple to operate, produces stable and reliable forming quality, and is suitable for the mass production of crescent-shaped 5A06 aluminum alloy forgings for aerospace applications, showing broad prospects for industrial application.
[0040] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A forging process for a crescent-shaped 5A06 aluminum alloy forging for aviation applications, characterized in that, Includes the following steps: Step 1, Forging: Heat the 5A06 aluminum alloy raw material bar to 430-450℃ and hold for 1.5-1.6 mm / min × H. heat H heat The maximum effective thickness of the billet is determined, and then upsetting forging is carried out. The deformation amount per forging is controlled at 20-30%. The hammer is pressed down at a uniform speed of 20-30 mm / s to obtain the billet. Step 2, Billet Preparation: Based on the finished dimensions of the crescent-shaped forging, calculate the billet dimensions using the following formula: Total length of billet L1 = L × L X L X This is an empirical coefficient for length, with a value ranging from 0.95 to 0.97, where L is the length of the forged part after forming. Total height of billet H1 = H × H X H X This is a high-empirical coefficient, with a value range of 0.88 to 0.90, where H is the height of the forging after forming. The length of the billet at the middle is L3 = 2 × (R² - (R + h - H / 2)²). 1 / 2 R is the radius of the arc groove in the middle of the formed forging, and h is the distance from the bottom of the arc groove to the bottom of the formed forging. The included angle in the middle of the billet is Deg = 135°; The middle height of the billet is h1 = H1 / 2; billet width W1 = W × W X W X W is an empirical coefficient for width, with a value range of 0.73 to 0.75, where W is the width of the forged part after forming. For concave fillets, r1 = 60-70 mm; for convex fillets, r2 = 5-8 mm. Step 3, Die forging: Forging is carried out in two stages. First heat: Heat the billet to 430-450℃ and hold it for 1.5-1.6 mm / min × H1. Place the billet in the mold cavity along the outer shape of the cavity. Use the first hammer to lightly strike and position it. Set the second hammer to a striking force of 40MN-50MN. After air cooling, polish to remove damage. Second heat: Heat the billet after the first heat to 430-450℃ and hold it for 120-240 minutes. Place the billet in the mold cavity and strike it with a hammer with a force of 50MN-60MN. Step 4, heat treatment: Place the forged part in a preheated furnace and hold it at 370-390℃ for 430-440 minutes, then air cool.
2. The forging process of the crescent-shaped 5A06 aluminum alloy forging for aviation use according to claim 1, characterized in that, In step one, the billet forging process involves one forging pass.
3. The forging process of the crescent-shaped 5A06 aluminum alloy forging for aviation use according to claim 1, characterized in that, In step three, before the first and second forging, compressed air is used to blow away the dirt inside the mold cavity, and mold lubricant is evenly sprayed onto the surface of the mold cavity using a spray gun.