A forging method for high-quality GH4169 alloy multi-step gyroscope-shaped forgings

By designing specific roughing and die forging processes, the problem of uneven deformation in GH4169 alloy multi-step gyroscope forgings was solved, achieving high-quality manufacturing of forgings and meeting the high standards required for aero-engines.

CN123102914APending Publication Date: 2026-11-17SHAANXI HONGYUAN AVIATION FORGING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611260517.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, GH4169 alloy multi-step gyroscope forgings have uneven deformation during the forging process, resulting in unqualified grain size and uneven microstructure, which cannot meet the high standards required for aero-engines.

Method used

A specific blank design is adopted, which is a "shield" shape with less material in the core and more material at the edge, which is the opposite of the characteristics of forgings. The blank is made by mold and combined with the die forging process to ensure that the metal material is accurately positioned in the mold, increase the amount of deformation, eliminate the deformation dead zone, and use solution and aging heat treatment to improve the uniformity of the structure.

Benefits of technology

The grain size of GH4169 alloy multi-step gyroscope forgings reached level 8 or above, with good microstructure uniformity, meeting the high standard requirements of aero-engines and improving the overall performance of the forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102914A_ABST
    Figure CN123102914A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of forging technology and relates to a forging method for a high-quality GH4169 alloy multi-step gyroscope-shaped forging. The method includes: designing a rough shape; using a die to prepare a "shield"-shaped rough shape with less material at the core and more at the edges, the characteristics of which are opposite to those of the forging; both the upper and lower end faces of the rough shape have recesses with a certain slope, and the lower end has a positioning slope that does not require machining; placing the rough shape into the lower mold cavity, so that the positioning slope of the rough shape fits against the mold slope, and the upper and lower recesses of the rough shape are aligned with the core cavity; during die forging, because the rough shape has less material at the core and more at the edges, as the pressure increases, some metal near the edges will be continuously squeezed back into the core cavity and the central step cavity, while the outward-flowing metal fills the edge cavity, ultimately forming the forging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of forging technology and relates to a forging method for a high-quality GH4169 alloy multi-step gyroscope forging. Background Technology

[0002] GH4169 nickel-based high-temperature alloy possesses excellent comprehensive mechanical properties and is used in key heat-resistant components for aerospace engines. A certain GH4169 high-pressure turbine disk forging is a crucial rotating component in an aero-engine, requiring a high-strength manufacturing process. During early trial production, it was discovered that the process route of directly die-forging using a bar mill with a positioning table resulted in uneven deformation across the forging, incomplete recrystallization, and problems such as inhomogeneous microstructure and coarse grains under low magnification, failing to meet the standard requirement of a grain size ≥8. Summary of the Invention

[0003] Purpose of the invention: A forging method for high-quality GH4169 alloy multi-step gyroscope-shaped forgings is provided, which deforms the disk center, middle steps and disk edge of the forging as a whole, increases the deformation amount of the ultra-high disk center, and obtains GH4169 alloy multi-step gyroscope-shaped disk forgings that meet the requirements of qualified grain size (≥8 grade) and uniform microstructure.

[0004] Technical solution: A forging method for a high-quality GH4169 alloy multi-step gyroscope-shaped forging, wherein the GH4169 alloy disc shaft sequentially comprises an ultra-high disc center, multiple intermediate steps of different heights, and a relatively thin disc rim, the method comprising: Step 1: Obtain a blank through the molding process. The upper part of the blank is cylindrical, and the lower part is a truncated cone with a larger upper part and a smaller lower part. Step 2: Use a punch to press the upper surface of the blank to form a pit on the upper surface, thus obtaining the blank shape. The blank shape is the opposite of the forging shape, and is a "shield" shape with less material in the core and more material at the edges. Step 3: Place the rough die into the lower mold cavity, so that the positioning slope of the rough die fits into the mold slope. At this time, the upper and lower recesses of the rough die are aligned with the core cavity. For rough die forging: Since there is less material in the core and more material at the edge of the rough die, as the pressure increases, the metal near the edge will be continuously squeezed back into the core cavity and the middle step cavity. At the same time, the outward flowing metal fills the edge cavity, and finally forms the forging.

[0005] Furthermore, the outer edge of the rough shape has a draft angle, and the upper end of the outer edge has a chamfer of R5.

[0006] Furthermore, the draft angle of the outer edge of the rough mold is 3°~5°.

[0007] Furthermore, the upper end face of the rough shape has a recess at the center with a radius less than or equal to the outer diameter of the upper end face of the forging, a depth of 15-20mm, and an angle of 40°~50°, and the edges inside and outside the recess are rounded (R5-R15).

[0008] Furthermore, the lower end face of the rough shape has a recess at the center of the axis with a radius less than or equal to the outer diameter of the lower end face, a depth of 5-15mm, and an angle of 40°~50°, and the edges inside and outside the recess are rounded (R5).

[0009] Furthermore, the outer side of the recess at the lower end of the rough shape has a slope with an angle of 35°~40° and a height of 20-25mm, and the edge of the slope is chamfered with R5.

[0010] Furthermore, in step 1: The bar stock is heated to 990℃~1010℃. A soft sleeve is used during heating, and insulation cotton is added to the upper and lower end faces.

[0011] Furthermore, in step 2, the mold forming process employs a flat anvil and a punch for upsetting.

[0012] Further, in step 3, forging includes: The blank is heated to 990℃~1010℃. During heating, it needs to be taken out of the furnace for soft wrapping before being put back into the furnace for reheating. During die forging, the positioning slope at the bottom of the blank is made to contact the die for positioning. A 100MN hydraulic press is used for die forging. The die preheating temperature is 250℃~350℃, the pressing speed is 3-7mm / s, and the pressure is held for 4-6s until the die is closed to ensure the final forging temperature is ≥930℃.

[0013] Furthermore, after step 3 (forging), the method further includes: The solution treatment and aging heat treatment are carried out. Solution treatment regime: ≤800℃ into the furnace, heat up to 815-835℃, hold for 55-65min, continue to heat up to 965-985℃, hold for 60-65min, and oil cool. Aging regime: ≤600℃ into the furnace, heat up to 590-610℃, hold for 55-65min, continue to heat up to 690-710℃, hold for 60-65min, then heat up to 710-730℃, hold for 480-495min, furnace cool at 40-60℃ / h to 610-630℃, hold for 480-495min, and air cool to obtain the final forging.

[0014] Beneficial effects: The invention first designs the rough shape, and uses a die to make a blank to obtain a "shield" shaped rough shape with less material in the core and more material at the edge, which is the opposite of the characteristics of forgings. This rough shape can be positioned in the mold without machining, saving materials.

[0015] During the die forging process, the metal at position 1 flows upward, forming the upper part of the center and the upper end of the middle step; the metal at position 2 flows outward, forming the edge of the disc; and the metal at position 3 flows downward, forming the lower part of the center and the lower slope area of ​​the middle step. The advantage of this design is that by moving the material outward, the amount of metal in the center is reduced, avoiding material accumulation in the excessively high center area during die forging, expanding the metal flow range, increasing the overall deformation of the forging, and eliminating the deformation dead zone. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. The drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is the final forging drawing.

[0018] Figure 2 Forging pattern of tire mold.

[0019] Figure 3 This is a wasteland-type map.

[0020] Figure 4 This is a diagram of a die forging material. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] The features and illustrative embodiments of various aspects of the present invention will now be described in detail. Numerous specific details are set forth in the following detailed description to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that the invention may be practiced without requiring some of these specific details. The following description of embodiments is merely intended to provide a better understanding of the invention by illustrating examples of the invention. The invention is by no means limited to any specific setups and methods set forth below, but covers any improvements, substitutions, and modifications to structures, methods, and devices without departing from the spirit of the invention. Well-known structures and techniques are not shown in the drawings and the following description to avoid unnecessarily obscuring the invention.

[0023] In the description of this invention, it should be noted that the directions or positional relationships indicated by terms such as "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer" are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing and simplifying the invention, and should not be construed as limiting the invention. Furthermore, the use of ordinal numbers (e.g., "first and second," etc.) is for distinguishing objects and is not limited to this order, and should not be construed as indicating or implying relative importance.

[0024] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly, encompassing both direct connection and indirect connection via an intermediate medium. Those skilled in the art can understand the specific meaning of these terms in this invention based on the specific circumstances.

[0025] It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other, and the various embodiments can be referenced and cited in each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0026] This invention provides a forging method for a GH4169 alloy multi-step gyroscope-shaped disk forging, such as... Figure 1 As shown, the GH4169 alloy disc shaft sequentially includes an ultra-high disc center, multiple central steps of varying heights, and a relatively thin disc rim, as... Figure 3 As shown, the designed rough die is a "shield" shape with less material in the core and more material at the edges, contrary to the characteristics of forgings, and has positioning bevels and upper and lower recesses; the die cavity includes a core chamber, a stepped chamber with large bevels, and a rim chamber; the method includes the following steps: Step 1: Cut the material and machine a beveled surface on one end of the GH4169 alloy bar for positioning, providing a positioning platform for the billet process and ensuring that the bar is placed in a suitable position on the mold; Step 2: Heat the bar stock to 990℃~1010℃. Use a soft sleeve during heating and place the bar stock in the mold (see...). Figure 2 Upsetting was performed using a 2500t high-speed forging mill. Insulation cotton was added to the upper and lower ends of the bar stock. During upsetting, a flat anvil was used first, followed by upsetting with a punch (see...). Figure 2 ), pressed into the designed rough shape (see Figure 3 ); Among them, the wild-shaped form has the following characteristics: 1. To avoid the formation of a dead zone in the core of the disc forging, the rough die is designed as a "shield" shape with less material in the core and more material at the edges, the opposite of the forging. 2. A draft angle (3°~5°) is formed between the outer edge of the rough mold and the die, and the upper end of the outer edge is chamfered with R5; 3. At the center of the upper end face, there is a recess with a radius of less than or equal to 30mm (corresponding to the outer diameter of the upper end face), a depth of 15-20mm, and an angle of 40°~50°. All edges inside and outside the recess are rounded (R5-R15). 4. A recess with a radius of less than or equal to 20 mm (corresponding to the outer diameter of the lower end face), a depth of 5-15 mm, and an angle of 40°~50° is provided at the center of the lower end face. All edges and corners of the recess are rounded (R5). The lower outer edge has a bevel with a height of 20-25mm (angle of 35°~40°) at a position 30-50mm from the axis (outside the recess), and the edge of the bevel has a chamfer of R5.

[0027] Step 3: Heat the rough die to 990℃~1010℃. During heating, it needs to be removed from the furnace for soft wrapping before being put back into the furnace for reheating. During die forging, the positioning bevel at the bottom of the rough die should contact the mold for positioning (see...). Figure 4 The process involves forging using a 100MN hydraulic press with a preheated die temperature of 250℃~350℃, a pressing speed of 3-7mm / s, pressing until the die closes, and holding the pressure for 4-6s to ensure a final forging temperature ≥930℃.

[0028] The results of simulation and actual die forging show that Figure 3 The metal at position 1 flows upwards, forming the upper part of the center and the upper part of the central step; the metal at position 2 flows outwards, forming the edge of the disc; the metal at position 3 flows downwards, forming the lower part of the center and the lower sloping area of ​​the central step. The advantage of this design is that by moving the material outwards, the amount of metal in the center is reduced, avoiding material accumulation in the excessively high center area during die forging, expanding the range of metal flow, increasing the overall deformation of the forging, and eliminating the deformation dead zone.

[0029] Step 4: After forging, the forging is subjected to solution treatment and aging heat treatment. Solution treatment regime: ≤800℃ into the furnace, heat to 815-835℃, hold for 55-65min, continue to heat to 965-985℃, hold for 60-65min, and oil cool. Aging regime: ≤600℃ into the furnace, heat to 590-610℃, hold for 55-65min, continue to heat to 690-710℃, hold for 60-65min, then heat to 710-730℃, hold for 480-495min, furnace cool at 40-60℃ / h to 610-630℃, hold for 480-495min, and air cool to obtain the final forging.

[0030] Example 1 The present invention discloses a GH4169 alloy multi-step gyroscope disk forging. The outer diameter of the disk is Φ252mm, the height is 153mm, and the weight is 90Kg. A reasonable rough shape is obtained by blanking with a die, which can be positioned without machining, thus expanding the flow range of the metal and increasing the overall deformation of the forging. The resulting forging structure and properties meet the standard requirements, and all indicators have sufficient margin.

[0031] The manufacturing process is detailed below: 1. Cutting: Sawing machine, cutting size Φ150×260mm; 2. Billet machining: The bar stock is chamfered to R10, and a bevel is machined on one end for positioning; 3. Billet Formation: Heat the bar stock to 1005℃, using a soft sleeve during heating. Place the bar stock in a die and upset it using a 2500t high-speed forging mill. See the attached diagram for a diagram showing the bar stock placement. Figure 2 Insulating cotton is added to the upper and lower ends of the bar stock. First, it is upset using a flat anvil. After upsetting to the appropriate height, the punch is changed to press it into the required rough shape. 4. Die forging: A 100MN hydraulic press is used for die forging. The die preheating temperature is 325℃, and the preheating time is 20 hours. The rough mold is heated to 1000℃ and held for 110 minutes. After being removed from the furnace, it is wrapped with 15mm thick insulation cotton. After wrapping, it is placed back into the furnace for another 30 minutes of holding. During die forging, the positioning bevel of the rough mold is placed in contact with the die for positioning. (See attached...) Figure 4 Place the billet, deform at a rate of 5 mm / s, press it into the mold and close it, and hold the pressure for 5 seconds to ensure the final forging temperature is ≥930℃.

[0032] 6. After forging, the forgings are subjected to heat treatment. The heat treatment regime is solution treatment and aging. Solution treatment regime: ≤800℃ into the furnace, heat up to 825℃, hold for 60min, continue to heat up to 975℃, hold for 60min, and oil cool. Aging regime: ≤600℃ into the furnace, heat up to 600℃, hold for 60min, continue to heat up to 700℃, hold for 60min, then heat up to 720℃, hold for 480min, furnace cool at 50℃ / h to 620℃, hold for 480min, and air cool to obtain the final forging.

[0033] The GH4169 alloy multi-step gyroscope disk forging obtained by this forging method was tested and found that: the grain size of each part of the forging is uniform and reaches level 10; all mechanical properties meet the standard requirements and have a certain margin.

[0034] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. A forging method for a high-quality GH4169 alloy multi-step gyroscope-shaped forging, wherein the GH4169 alloy disc shaft sequentially comprises an ultra-high disc center, multiple intermediate steps of different heights, and a relatively thin disc rim, characterized in that... The method includes: Step 1: Obtain a blank through the molding process. The upper part of the blank is cylindrical, and the lower part is a truncated cone with a larger upper part and a smaller lower part. Step 2: Use a punch to press the upper surface of the blank to form a pit on the upper surface, thus obtaining the blank shape. The blank shape is the opposite of the forging shape, and is a "shield" shape with less material in the core and more material at the edges. Step 3: Place the rough die into the lower mold cavity, so that the positioning slope of the rough die fits into the mold slope. At this time, the upper and lower recesses of the rough die are aligned with the core cavity. For rough die forging: Since there is less material in the core and more material at the edge of the rough die, as the pressure increases, the metal near the edge will be continuously squeezed back into the core cavity and the middle step cavity. At the same time, the outward flowing metal fills the edge cavity, and finally forms the forging.

2. The method according to claim 1, characterized in that, The outer edge of the rough shape has a draft angle, and the upper end of the outer edge has a chamfer of R5.

3. The method according to claim 1, characterized in that, The draft angle of the outer edge of the rough mold is 3°~5°.

4. The method according to claim 1, characterized in that, The upper end face of the rough shape has a recess at the center of the axis with a radius less than or equal to the outer diameter of the upper end face of the forging, a depth of 15-20mm, and a slope of 40°~50°. The edges and corners inside and outside the recess are rounded (R5-R15).

5. The method according to claim 1, characterized in that, The lower end face of the rough shape has a pit at the center of the axis with a radius less than or equal to the outer diameter of the lower end face, a depth of 5-15mm, and an angle of 40°~50°. The edges and corners inside and outside the pit are rounded (R5).

6. The method according to claim 1, characterized in that, The outer side of the recess at the lower end of the rough shape has a slope with an angle of 35°~40° and a height of 20-25mm, and the edge of the slope is chamfered with R5.

7. The method according to claim 1, characterized in that, In step 1: The bar stock is heated to 990℃~1010℃. A soft sleeve is used during heating, and insulation cotton is added to the upper and lower end faces.

8. The method according to claim 1, characterized in that, In step 2, the mold is formed by using a flat anvil and a punch for upsetting.

9. The method according to claim 1, characterized in that, Step 3, forging, includes: The blank is heated to 990℃~1010℃. During heating, it needs to be taken out of the furnace for soft wrapping before being put back into the furnace for reheating. During die forging, the positioning slope at the bottom of the blank is made to contact the die for positioning. A 100MN hydraulic press is used for die forging. The die preheating temperature is 250℃~350℃, the pressing speed is 3-7mm / s, and the pressure is held for 4-6s until the die is closed to ensure the final forging temperature is ≥930℃.

10. The method according to claim 1, characterized in that, After step 3, forging, the method further includes: The solution treatment and aging heat treatment are carried out. Solution treatment regime: ≤800℃ into the furnace, heat up to 815-835℃, hold for 55-65min, continue to heat up to 965-985℃, hold for 60-65min, and oil cool. Aging regime: ≤600℃ into the furnace, heat up to 590-610℃, hold for 55-65min, continue to heat up to 690-710℃, hold for 60-65min, then heat up to 710-730℃, hold for 480-495min, furnace cool at 40-60℃ / h to 610-630℃, hold for 480-495min, and air cool to obtain the final forging.