A casting and rolling method for preparing layered aluminum-aluminum composite materials of different aluminum alloys

By using aluminum strip surface treatment and fluoroaluminate activators, combined with local atmosphere protection and casting and rolling process optimization, the problems of oxide film removal and interface bonding in aluminum alloy solid-liquid composites have been solved, realizing the preparation of high-strength and clean aluminum-aluminum composite materials, which are suitable for automotive heat exchangers, battery cooling plates, electronic packaging, building decoration and aerospace components and other fields.

CN123102969APending Publication Date: 2026-11-17HENAN YONGTONG COMPOSITE NEW MATERIAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611203915.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the solid-liquid casting-rolling composite process of different aluminum alloys, how to stably break the oxide film on the surface of solid coated aluminum strip without relying on a fully enclosed, high-cost protective atmosphere, improve the wetting and spreading ability of aluminum liquid on coated aluminum strip, and avoid the formation of inclusion layers by fluoroaluminate activators, so as to obtain a continuous, clean, and high-strength metallurgical bonding interface.

Method used

After grinding, degreasing and cleaning the solid coated aluminum strip, a low amount of fluoroaluminate activator is applied. Combined with local inert atmosphere protection and continuous casting and rolling pressing to remove salt, the interlayer bonding between the coated aluminum strip and the base aluminum liquid is promoted. The contact time and pressing time are controlled to form a non-finished product salt removal edge to reduce the risk of inclusion retention.

Benefits of technology

A layered aluminum-aluminum composite material with stable interfacial bonding and low delamination during subsequent rolling was achieved in a shorter process, making it suitable for continuous industrial production and improving interfacial bonding strength and anti-delamination performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102969A_ABST
    Figure CN123102969A_ABST
Patent Text Reader

Abstract

This application relates to the field of composite aluminum alloy rolling technology, specifically a casting and rolling method for preparing layered aluminum-aluminum composite materials of different aluminum alloys. The method includes grinding, degreasing, cleaning, and drying a solid coated aluminum strip; applying a low-amount fluoroaluminate activator slurry to its surface and drying it to form an activator coating; melting and purifying the base aluminum ingot; distributing the molten aluminum onto the activator coating surface through a flow channel and casting nozzle; continuously casting and rolling the composite under a low dew point inert atmosphere; and forming non-finished salt removal edges on both sides of the composite slab; subsequently, cooling, cold rolling, annealing, and trimming are performed to obtain the layered aluminum-aluminum composite material. The fluoroaluminate activator in this application can promote the activation of the oxide film on the coated surface and improve the wetting of the molten aluminum; by controlling the low-amount coating, contact, and casting and rolling time of the activator, and by setting non-finished salt removal edges, the risk of residual activator and interfacial inclusions remaining in the effective area of ​​the finished product can be reduced, thereby improving the interlayer bonding strength and anti-delamination performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of composite aluminum alloy rolling technology, specifically to a casting and rolling method for preparing layered aluminum-aluminum composite materials of different aluminum alloys. Background Technology

[0002] Layered aluminum composite materials are sheet and strip materials made by combining aluminum alloys of different grades and functions in a layered manner. Through material combination design, the core layer can bear the functions of strength, stiffness, or thermal conductivity, while the cladding layer can bear the functions of brazing, corrosion resistance, wear resistance, decoration, or forming. Layered aluminum composite materials have been widely used in automotive heat exchangers, battery cooling plates, electronic packaging, architectural decoration, aerospace components, and lightweight structural parts.

[0003] The preparation technology of aluminum alloy layered composite materials has generally followed the development path of solid-state composite, liquid-solid composite, and short-process continuous composite. Early solid-state composite processes such as explosive composite, diffusion welding, and hot rolling composite were commonly used, with hot rolling composite being the most widely applied. However, this requires separate preparation of core material and cladding ingots or slabs, followed by surface treatment, assembly, heating, billet opening, multi-pass hot rolling, and annealing—a lengthy process with high energy consumption and slow production cycle. While brazing composite can introduce filler metal between layers to achieve connection, the filler metal layer is prone to component contamination, and the interface is susceptible to the formation of brittle phases or residual flux inclusions, making it unsuitable as a universal preparation method for high-load-bearing composite plates and strips. Casting-rolling composite technology combines the solidification and forming of molten aluminum with rolling composite, shortening the process flow and representing an important direction for the preparation of aluminum alloy composite plates and strips.

[0004] Chinese patent application CN115366502A discloses a heat-transfer composite aluminum plate with a self-fusion layered microstructure and its preparation method. It adopts a solid-liquid-solid composite casting and rolling process, which involves grinding the coating surface, cleaning with acetone, preheating in a protective atmosphere, and introducing argon gas during the casting and rolling process to form a self-fusion layer between the 3XXX aluminum alloy melt and the 4XXX aluminum alloy coating strip. This technology utilizes melting point differences and shallow fusion at the solid-liquid interface to improve composite efficiency. However, aluminum and aluminum alloys readily form a dense Al2O3 oxide film in air. Even after polishing, acetone cleaning, and argon protection, it is still difficult to completely avoid oxide film, moisture, oil, or wear debris residue during long-line continuous casting and rolling in industrial applications. Once these residues are trapped between the molten aluminum and the solid coated aluminum strip, even if local fusion occurs, they can easily form a discontinuous metallurgical interface, leading to reduced interfacial shear strength, increased thermal resistance at the thermally conductive interface, localized corrosion at inclusions, and delamination during subsequent cold rolling or bending. At the same time, maintaining a stable low-oxygen, low-moisture protective atmosphere over long distances requires high equipment sealing, gas consumption, and safety management costs, which limits its large-scale industrial application.

[0005] How to effectively remove the interfacial oxide film without using a large amount of protective gas is a technical problem that urgently needs to be solved in the solid-liquid casting and rolling of aluminum alloys. Chinese patent application document with publication number CN119635074A discloses a coated pre-formed brazing filler metal, which coats the outer periphery of the aluminum-silicon alloy brazing filler metal with fluoroaluminate flux to remove the oxide film on the surface of the brazing filler metal and the welding interface, thereby improving the welding yield. While the fluoroaluminate flux in this technology has an activating and film-breaking effect on aluminum oxide films, it is only used for removing oxide films in local welds. Brazing is a short-term, localized, and near-static connection process, where the flux can remain in the weld area and work with the filler metal to complete wetting and filling. However, continuous casting and rolling composites involve a large-area, continuous strip feeding, high-speed movement, and pressure solidification dynamic interface. This not only requires film breaking but also requires wetting and promotion in a very short time. It also requires consideration of interface cleanliness, continuous metallurgical bonding, and no cracking during subsequent cold rolling. This is very different from the welding conditions of fluoroaluminate flux. Applying fluoroaluminate flux to continuous casting and rolling composite scenarios will lead to new problems such as residual fluoride salts being drawn into the composite interface to form a continuous inclusion layer, fluoroaluminate powdering and contamination during strip transport, and difficulty in breaking the oxide film within a short reaction window.

[0006] Therefore, existing technologies still need to address the following technical issues: how to stably break the oxide film on the surface of solid coated aluminum strips without relying on a fully enclosed, high-cost protective atmosphere during the solid-liquid casting and rolling composite process of different aluminum alloys, thereby improving the wetting and spreading ability of the aluminum melt on the coated aluminum strips; at the same time, how to ensure that the introduced fluoroaluminate activator can be controlled to be discharged or dispersed discontinuously after exerting its film-breaking and activating effect, avoiding the formation of fluoride salt inclusions and new interface defects, so as to obtain a continuous, clean, and high-strength metallurgical bonding interface. Summary of the Invention

[0007] This application aims to overcome at least one of the deficiencies of the prior art by providing a casting and rolling preparation method for layered aluminum-aluminum composite materials of different aluminum alloys. Through surface pretreatment of the coated aluminum strip, coating with a low amount of fluoroaluminate activator, purification of the molten aluminum, protection with a local inert atmosphere, and continuous casting and rolling pressing to remove salt, the interlayer bonding between the solid coated aluminum strip and the substrate molten aluminum is promoted. This process is beneficial for activating the oxide film on the surface of the coated aluminum strip, improving the wetting and spreading performance of the molten aluminum, and reducing the risk of residual activator, oxide film fragments, and other interface inclusions remaining in the effective area of ​​the finished product, thereby improving the bonding strength and anti-delamination performance, and is suitable for continuous industrial production.

[0008] In a first aspect, embodiments of this application provide a method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling, which is achieved through the following technical solution: A method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling includes the following steps: S1. Select solid coated aluminum strip, grind, degrease, clean and dry it to obtain clean coated aluminum strip; S2. A fluoroaluminate activator slurry is coated onto the surface of the cleaned coated aluminum strip. After drying, the fluoroaluminate activator slurry forms an activator coating, resulting in an activated coated aluminum strip. The fluoroaluminate activator slurry comprises fluoroaluminate powder, a volatile solvent, and a film-forming binder. The coating amount of the activator coating, based on the fluoroaluminate powder, is 0.15–1.2 g / m². 2 ; S3. Select aluminum ingots as the base material and melt them to obtain molten aluminum; S4. The molten aluminum obtained in step S3 is distributed onto the surface of the activator coating of the activated coating aluminum strip obtained in step S2 through a flow channel and a casting nozzle, and then continuously cast and rolled to obtain a composite slab; wherein, during casting and rolling, non-finished salt removal edges are formed on both sides of the width direction of the composite slab; the contact wetting and activation time between the molten aluminum and the activated coating aluminum strip is 1.3 to 1.6 s, and the pressing and salt removal time is 5 to 7 s; S5. The composite slab is post-processed, and the non-finished salt-removing edges on both sides are removed to obtain a layered aluminum-aluminum composite material.

[0009] The casting and rolling preparation method of layered aluminum-aluminum composite materials of different aluminum alloys according to the embodiments of this application has at least the following beneficial effects: This application involves coating a low-aluminate fluoroaluminate activator onto the surface of a solid coated aluminum strip after grinding, degreasing, cleaning, and drying. This ensures the coated aluminum strip has good surface cleanliness and activation conditions before entering the casting-rolling composite zone. When the molten aluminum substrate comes into contact with the activator coating, the fluoroaluminate activator can activate or break down the oxide film on the surface of the coated aluminum strip, improving the wetting and spreading state of the molten aluminum on the solid coated aluminum strip surface, thereby reducing the adverse effects of the oxide film on the solid-liquid composite interface.

[0010] This application controls the contact wetting and activation time between molten aluminum and activated coated aluminum strip to 1.3–1.6 s, and controls the pressing and salt removal time to 5–7 s. This allows the activator to play an activating, film-breaking, and wetting-aiding role in the initial contact of molten aluminum. Subsequently, under the action of casting and rolling pressure, it provides process conditions for the transfer of residual activator, broken oxide film, and related inclusions to the edge non-finished area, reducing the risk of them remaining in the effective area of ​​the finished product and forming interface defects, which is beneficial to improving the stability of interlayer bonding.

[0011] This application creates non-finished salt removal edges on both sides of the composite slab width during casting and rolling, and removes them during post-processing. This arrangement is equivalent to reserving non-finished edge areas outside the effective width of the finished product, providing space for the edge transfer of residual activators, oxide film fragments, and related inclusions during casting, rolling, pressing, and slab widening. Subsequent edge trimming reduces the risk of these residues entering the effective area of ​​the finished product, thereby improving the interfacial bonding strength and anti-delamination properties of the layered aluminum-aluminum composite material.

[0012] This application involves post-processing the composite slab after continuous casting and rolling, and removing the non-finished salt removal edges on both sides. This can further improve the slab size and shape, release some residual stress during processing, and remove defect-rich areas on the edges.

[0013] Through the above-mentioned process combination, this application can achieve continuous composite bonding between different aluminum alloys in a shorter process, and obtain a layered aluminum-aluminum composite material with stable interface bonding and not easy to delaminate during subsequent rolling and forming processes, which is suitable for continuous industrial production.

[0014] In step S4 of this application, the contact wetting and activation time between the molten aluminum and the activated coating aluminum strip refers to the time between the first contact of the molten aluminum with the activator coating and the entry into the roll gap pressing zone, which can be calculated by dividing the path length by the casting and rolling speed; the pressing and salt removal time refers to the time for the strip to pass through the roll gap pressing zone and complete the interface pressing and lateral discharge of residues under the action of rolling force, which can be calculated by dividing the pressing contact arc length by the casting and rolling speed.

[0015] According to some embodiments of this application, the solid-coated aluminum strip in step S1 is selected from 4-series or 6-series aluminum alloy strips, the thickness of the solid-coated aluminum strip in step S1 is 0.4 to 1.8 mm, and the base aluminum ingot in step S3 is selected from 1-series, 3-series, 5-series or 8-series aluminum alloys.

[0016] The base aluminum ingots are selected from 1-series, 3-series, 5-series, or 8-series aluminum alloys, while the solid cladding aluminum strips are selected from 4-series or 6-series aluminum alloy strips. Material matching can be tailored to different application requirements such as thermal conductivity, corrosion resistance, brazing properties, strength, and forming capabilities, thus expanding the applicability of the casting-rolling composite process. Limiting the thickness of the solid cladding aluminum strip to 0.4–1.8 mm helps ensure the functional thickness of the cladding and the stability of the strip feeding process. This avoids damage and wrinkling caused by an excessively thin cladding, or insufficient heating and unstable interfacial bonding caused by an excessively thick cladding, thereby improving the forming quality and performance consistency of the composite strip.

[0017] According to some embodiments of this application, in step S1, after grinding, the surface roughness of the solid coated aluminum strip is Ra0.8–1.5 μm. Controlling the surface roughness of the solid coated aluminum strip after grinding to Ra0.8–1.5 μm can remove surface oxide film, oil stains, and attached impurities while forming a moderately rough morphology on the surface of the coated aluminum strip, improving the spreadability and adhesion stability of the fluoroaluminate activator slurry, and reducing local detachment during subsequent strip feeding; at the same time, it is beneficial to increase the effective contact area between the molten aluminum and the coated aluminum strip, promote wetting and pressing composite, and avoid insufficient wetting due to excessive surface gloss or inclusions, scratches, and interface defects caused by excessively rough surface.

[0018] According to some embodiments of this application, the mass ratio of the film-forming binder to the fluoroaluminate powder in step S2 is 0.3–2:100. Controlling the mass ratio of the film-forming binder to the fluoroaluminate powder to 0.3–2:100 ensures the adhesion stability of the fluoroaluminate powder while avoiding excessive binder usage that could lead to increased organic residue after drying. This ratio is beneficial for forming a thin and uniform activator coating, reducing powder shedding and coating detachment during strip conveying, and lowering the risk of gas release, carbon residue, and interface inclusions during casting-rolling composite, thereby improving the cleanliness and bonding stability of the composite interface.

[0019] According to some embodiments of this application, the fluoroaluminate powder in step S2 includes at least one of KAlF4, K2AlF5, K3AlF6, CsAlF4, Cs2AlF5, and Cs3AlF6. Using the above-mentioned potassium-based or cesium-based fluoroaluminate powder as an activator can effectively activate and break down the oxide film on the surface of the coated aluminum strip at the aluminum melt contact temperature, promoting the wetting and spreading of the aluminum melt. Simultaneously, it has good compatibility with the aluminum system, and the residue after the reaction is easily discharged towards the non-finished product salt discharge edge under rolling force, reducing the risk of inclusion residue in the finished product area.

[0020] According to some embodiments of this application, in step S2, the D50 particle size of the fluoroaluminate powder is 1-8 μm, and the D90 particle size is no greater than 15 μm. This particle size is beneficial for the activator slurry to form a uniform and stable thin coating, improving the dispersion and adhesion uniformity of the powder on the surface of the coated aluminum strip; at the same time, the finer particle size can increase the contact area between the activator and the oxide film, improve the film breaking activation efficiency, and reduce the adverse effects of large particle inclusions on the composite interface, thereby facilitating the acquisition of a stable and clean metallurgical bonding interface.

[0021] According to some embodiments of this application, in step S2, the volatile solvent includes at least one selected from water, ethanol, isopropanol, n-propanol, and propylene glycol methyl ether. These solvents can effectively disperse fluoroaluminate powder and adjust the workability of the slurry, facilitating the formation of a uniform, continuous, and controllable activator coating on the surface of the coated aluminum strip. Simultaneously, these solvents are easily evaporated and removed at lower temperatures, reducing residual volatiles after drying and lowering the risk of porosity, flue gas, and interface inclusions during casting and rolling composite processes.

[0022] According to some embodiments of this application, in step S2, the film-forming binder includes a self-crosslinking acrylic emulsion and / or a self-crosslinking polyurethane emulsion. This binder can form a uniform, continuous film with good adhesion after drying, improving the fixation of fluoroaluminate powder on the surface of the coated aluminum strip and the coating's resistance to conveying friction, reducing powder shedding and uneven coating during unwinding, guiding, and feeding processes; simultaneously, its dosage is low, and it leaves little residue after heating, which helps reduce interfacial gas and carbon residue, ensuring the cleanliness of the cast-rolled composite interface.

[0023] According to some embodiments of this application, the drying temperature in step S2 is 80–160°C, the drying time is 30 seconds–5 minutes, and the mass content of residual volatile solvent in the activator coating after drying is no more than 0.8%. This condition ensures sufficient solvent evaporation while preventing overheating cracking, powdering, or decreased adhesion of the coating, allowing the fluoroaluminate activator to form a uniform and stable thin coating on the surface of the coated aluminum strip. This reduces powder shedding during the strip feeding process and porosity, fumes, and interface inclusions caused by solvent residue during casting and rolling contact, thus improving the cleanliness and bonding stability of the composite interface.

[0024] According to some embodiments of this application, in step S2, the activator coating is an intermittent coating layer, which includes a plurality of V-shaped coating units arranged at intervals along the length direction of the activated coating aluminum strip, and a V-shaped discharge gap with a width of 0.1 to 1 mm is formed between adjacent V-shaped coating units; the V-shaped discharge gap includes two guide gap sections that extend obliquely from the middle region of the activated coating aluminum strip in the width direction to the two non-finished product salt discharge edges, respectively, and the angle between the guide gap sections and the length direction of the activated coating aluminum strip is 10° to 45°, and they are connected to the two non-finished product salt discharge edges; the area coverage of the activator coating is 70 to 95%.

[0025] The spacer coating layer employs V-shaped coating units spaced apart along the strip length. Adjacent coating units form V-shaped discharge gaps that diagonally connect from the central region of the strip width towards the non-finished salt discharge edges on both sides. This structure, while ensuring activation and wetting in the main composite areas, provides a channel for the transfer of interfacial gases, residual activators, broken oxide films, and their reaction products to the non-finished areas at the edges. This allows these residues to more easily leave the effective finished product area under rolling pressure and slab widening, reducing the risk of interfacial defects within the effective finished product area. This improves bonding stability and reduces the risk of blistering and delamination during subsequent rolling and forming processes.

[0026] According to some embodiments of this application, step S3, after melting, further includes refining and degassing, settling, composition adjustment, online degassing, ceramic filtration, and grain refinement treatment, while controlling the aluminum melt temperature at 680–725°C. The post-melting treatment effectively reduces the hydrogen content, inclusion content, and compositional fluctuations in the aluminum melt, improving its cleanliness and uniformity. Controlling the aluminum melt temperature in the holding furnace at 680–725°C ensures suitable fluidity and superheat, preventing insufficient spreading due to excessively low temperatures or accelerated oxidation and burn-off due to excessively high temperatures.

[0027] Furthermore, the refining and degassing process employs a refining agent, the amount of which is 0.1-0.3% of the aluminum melt mass. This dosage ensures effective dehydrogenation and slag removal while reducing inclusion residues and compositional fluctuations caused by excessive refining agent introduction, thereby improving the cleanliness and compositional stability of the aluminum melt. This provides a stable and clean base aluminum melt for subsequent casting and rolling composite processes, and reduces the adverse effects of defects such as porosity and inclusions on the bonding quality of the composite interface.

[0028] Furthermore, the settling time is 10–16 minutes. Settling allows bubbles introduced or generated during the refining process to rise and escape fully, and promotes further separation of inclusions and slag from the molten aluminum, reducing the hydrogen content and non-metallic inclusion content in the molten aluminum. This settling time ensures the purification effect of the molten aluminum while avoiding excessive temperature drop or secondary oxidation caused by excessive settling, thereby improving the cleanliness and bonding stability of the subsequent casting-rolling composite interface.

[0029] Furthermore, the online degassing uses argon or an argon-nitrogen mixture, with a gas flow rate of 0.3–0.6 m³ / s. 3 / h. This condition allows bubbles to fully disperse in the molten aluminum and carry away dissolved hydrogen and fine inclusions, reducing the gas content and inclusion level of the molten aluminum; at the same time, it avoids insufficient degassing due to too small a gas volume or turbulence, gas entrapment, and secondary oxidation of the molten aluminum due to too large a gas volume, thereby improving the cleanliness of the molten aluminum and the bonding stability of the casting-rolling composite interface.

[0030] Furthermore, the ceramic filter uses a 30–50 μm ceramic filter plate. Using a 30–50 μm ceramic filter plate to filter the molten aluminum can trap oxide inclusions, refining residues, and other non-metallic particles in the molten aluminum, reducing the probability of inclusions entering the solid-liquid composite interface. Simultaneously, this pore size range balances filtration accuracy and molten aluminum permeability, reducing flow resistance and temperature fluctuations in the molten aluminum, which is beneficial for maintaining the stability of the casting and rolling supply, reducing the risk of interface inclusion defects, and improving the consistency of slab quality.

[0031] Furthermore, the grain refinement treatment incorporates an aluminum-titanium-boron (ATiB) grain refiner, the amount of which is 0.15–0.5% of the aluminum melt mass. Adding 0.15–0.5% of the ATiB grain refiner by mass of the aluminum melt provides effective nucleation sites during aluminum solidification, refines the microstructure of the aluminum alloy substrate during casting and rolling, reduces grain size differences and solidification segregation, and mitigates the adverse effects of hot cracking, shrinkage cavities, and microstructure inhomogeneity on the composite interface. This, in turn, improves the forming stability, interfacial bonding reliability, and subsequent cold rolling performance of the composite slab.

[0032] According to some embodiments of this application, in step S4, the flow channel undergoes a preheating treatment at a temperature of 660–710°C. Preheating the flow channel to 660–710°C can reduce temperature drop and crust formation during the aluminum molten material transport process.

[0033] According to some embodiments of this application, in step S4, during continuous casting and rolling composite, a protective gas is introduced into the contact area between the molten aluminum and the activated coated aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature of the contact area between the molten aluminum and the activated coated aluminum strip at the casting and rolling inlet is ≤-20℃, and the oxygen volume fraction is ≤0.5%. This condition can reduce the degree of secondary oxidation of the molten aluminum before and after contact with the coated aluminum strip, reduce the formation of oxide inclusions and interface gas defects; at the same time, combined with low dew point atmosphere control, it is beneficial to suppress oxidation and hydrogen absorption caused by water vapor, improve the wetting stability of the molten aluminum and the bonding reliability of the casting and rolling composite interface.

[0034] Furthermore, the protective gas is argon or nitrogen.

[0035] According to some embodiments of this application, in step S4, the casting speed during continuous casting and rolling composite is 300–1200 mm / min, the roll surface temperature is 40–100°C, the rolling force is 1000–2200 tons, and the tension of the activated coating aluminum strip is 1–6 t. By controlling the casting speed at 300–1200 mm / min and the roll surface temperature at 40–100°C, the molten aluminum can maintain a suitable solidification and wetting state in the composite zone. Combined with a rolling force of 1000–2200 t and a coating aluminum strip tension of 1–6 t, the stability of the solid-liquid interface pressing can be improved, residual activator and oxide film fragments can be discharged to the edges, interface inclusions and wrinkles can be reduced, and the bonding strength and shape stability of the composite slab can be improved.

[0036] According to some embodiments of this application, in step S4, the width of the composite slab is 10-50 mm greater than the width of the finished product, so that the width of the non-finished product salt discharge edge is 5-25 mm.

[0037] By making the width of the composite slab wider than the width of the finished product, and reserving non-finished salt removal edges on both sides of the composite slab, space can be provided for the transfer of residual fluoroaluminate activator, broken oxide film and their reaction products to the edge under the action of casting and rolling, reducing the risk of them being retained in the effective width of the finished product and forming interface defects; the non-finished salt removal edges are removed during subsequent edge trimming, which is beneficial to improving the bonding strength and processing stability of the finished product.

[0038] According to some embodiments of this application, in step S5, the post-processing includes: shearing the composite slab to length and uniformly cooling it, followed by multi-pass cold rolling; intermediate annealing when the total cold rolling deformation reaches 40-60%, and then further cold rolling to the target thickness followed by full annealing. By shearing the composite slab to length and uniformly cooling it, the temperature and dimensional state of the slab can be stabilized, reducing plate deformation and interlayer thermal stress concentration caused by uneven cooling; the subsequent multi-pass cold rolling, with intermediate annealing when the total cold rolling deformation reaches 40-60%, can alleviate work hardening, restore material plasticity, and prevent edge cracking, interface cracking, or delamination during continued rolling; further cold rolling to the target thickness followed by full annealing can eliminate residual stress, improve plate shape and forming performance, and enhance the processing stability of the layered aluminum-aluminum composite material.

[0039] Furthermore, the cooling rate for uniform cooling is 5–15 °C / s. This method avoids excessively rapid cooling, which can cause interlayer thermal stress concentration, plate warping, or interfacial microcracks. It also prevents excessively slow cooling, which can lead to microstructure coarsening and excessive interfacial reaction. By controlling the cooling rate, the temperature distribution of the composite slab is made more uniform in both the thickness and width directions, which helps maintain interfacial bonding stability and improves the anti-delamination performance and plate shape quality during subsequent cold rolling processes.

[0040] Furthermore, the total deformation of the multi-pass cold rolling is 60-85%, and the deformation of each pass does not exceed 40%. Controlling the total deformation of the multi-pass cold rolling to 60-85% allows the composite slab to undergo sufficient plastic deformation in subsequent rolling processes, promoting further compaction of the composite interface and improving the stability of interlayer bonding. Controlling the deformation of each pass to no more than 40% avoids excessive reduction in a single pass, which could lead to shear stress concentration, edge cracking, or delamination at the interface, thereby improving the stability of the cold rolling process and the quality of the finished strip.

[0041] Furthermore, the intermediate annealing temperature is 330–390°C, and the holding time is 1–2 hours. This method can effectively eliminate work hardening and some residual stress after cold rolling deformation to 40–60%, restore the material's plasticity, and avoid cracking or interface delamination caused by excessive hardening during continued cold rolling. At the same time, this temperature range will not cause excessive interface diffusion or significant deterioration of coating performance, which is beneficial to maintaining the bonding stability of layered composite materials and subsequent rolling processing performance.

[0042] Furthermore, the complete annealing temperature is 320–380°C, and the holding time is 2–5 hours. This method can effectively eliminate cold rolling work hardening and residual stress while avoiding excessive diffusion, abnormal grain growth, or performance degradation between the coating and the substrate. It also improves the plasticity and shape stability of the composite strip, enhances its adaptability to subsequent stamping, bending, and other forming processes, and reduces the risk of cracking and delamination at the composite interface during use and processing.

[0043] Secondly, embodiments of this application provide layered aluminum-aluminum composite materials prepared by the casting and rolling method of the above-mentioned layered aluminum-aluminum composite materials using different aluminum alloys.

[0044] The layered aluminum-aluminum composite material according to the embodiments of this application has at least the following beneficial effects: The layered aluminum-aluminum composite material obtained by the above casting and rolling method exhibits high bonding strength and good processing stability between different aluminum alloy layers. The results of interfacial shear strength, 180° bending, peeling, cold rolling blistering, and thermal cycling tests show that this composite material is not prone to delamination, blistering, or interfacial cracking during subsequent cold rolling, annealing, and forming processes, demonstrating good anti-delamination performance and thermal cycling stability.

[0045] In this article, the numerical ranges mentioned all include the endpoint values ​​and cover any subranges within that range, such as the ranges obtained by arbitrarily combining the specifically listed numerical values. Attached Figure Description

[0046] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0047] Figure 1 This is a schematic diagram of the casting and rolling process for layered aluminum-aluminum composite materials of different aluminum alloys in this application; Figure 2 This is a schematic diagram of the structure of the spacer coating layer of the activated coating aluminum strip in this application; Figure 3 This is a comparison chart showing the data on the shear strength retention rate and finished product qualification rate of the layered aluminum-aluminum composite materials prepared in Examples 1-4 and Comparative Examples 1-3 of this application after thermal cycling. Figure 4 This is a comparison diagram of the interfacial shear strength of the layered aluminum-aluminum composite materials prepared in Examples 1-4 and Comparative Examples 1-3 of this application before and after thermal cycling. Detailed Implementation

[0048] To make the objectives, technical solutions, and advantages of this application clearer, a further detailed description will be provided below in conjunction with specific embodiments. The embodiments described herein are merely some examples of this application and should not be construed as limiting the scope of protection of this application. Unless otherwise specified, the raw materials used in the embodiments are all commercially available, and the equipment and testing methods used are conventional equipment and methods in the art.

[0049] Example 1 This embodiment prepares a 3003 / 4343 layered aluminum-aluminum composite material, wherein the substrate is 3003 aluminum alloy and the cladding is 4343 aluminum alloy. The preparation method is as follows: (1) Select 4343 aluminum alloy strip with a thickness of 1.0 mm and a width of 430 mm as solid coated aluminum strip. After leveling and trimming the 4343 aluminum alloy strip, use nylon abrasive belt to continuously grind the surface to be coated to remove the natural oxide film on the surface, so that the surface roughness after grinding is Ra1.1μm. Then, use alkaline degreasing solution to spray and clean, rinse with deionized water and dry with hot air to make the surface free of visible oil and water stains, and obtain clean coated aluminum strip; (2) Preparation of fluoroaluminate activator slurry: The fluoroaluminate powder is a mixture of KAlF4 and K2AlF5 in a mass ratio of 70:30, with a D50 particle size of 4.2 μm and a D90 particle size of 11.5 μm; the volatile solvent is a mixture of ethanol and water in a mass ratio of 80:20; the film-forming binder is a mixture of self-crosslinking acrylic emulsion and self-crosslinking polyurethane emulsion in a mass ratio of 4:1 based on solid content; the mass ratio of the film-forming binder to the fluoroaluminate powder in terms of solid content is 0.8:100; the fluoroaluminate activator slurry is prepared by gravure roller coating. Salt activator slurry is coated onto the clean, coated aluminum strip surface to be laminated, forming V-shaped coating units spaced apart along the length of the aluminum strip. V-shaped discharge gaps are formed between adjacent V-shaped coating units, with a width of 0.3 mm. Two guide gap sections of the V-shaped discharge gaps extend obliquely from the middle region of the aluminum strip width towards the two non-finished salt discharge edges, connecting with them. The angle between the guide gap sections and the length direction of the aluminum strip is 25°. The activator coating area coverage is 85%, and the coating amount of the activator coating, calculated as fluoroaluminate powder, is 0.45 g / m². 2 After coating, the aluminum strip is dried in a hot air oven at 120℃ for 90 seconds. After drying, the mass content of residual volatile solvent in the activator coating is 0.42%, thus obtaining the activated coating aluminum strip. (3) 3003 aluminum alloy ingots were selected as the base aluminum ingots and melted in a smelting furnace to obtain molten aluminum. A refining agent of 0.2% by mass of the molten aluminum was added for refining and degassing. After standing for 12 minutes, slag was removed, and samples were taken for direct-reading spectral analysis. Al-Mn and Al-Cu master alloys were used to adjust the composition to meet the requirements of 3003 aluminum alloy. Subsequently, online argon degassing was performed at an argon flow rate of 0.4 m³ / s. 3 / h, then filter through a 40μm ceramic filter plate, and after filtration, add Al-5Ti-1B grain refiner accounting for 0.3% of the mass of aluminum liquid, stir evenly, and stabilize the temperature of aluminum liquid at 700℃; (4) The treated aluminum liquid is transferred into the holding furnace, the temperature of which is controlled at 700°C. The flow channel connecting the holding furnace and the casting nozzle is preheated to 680°C. The composite area of ​​the casting and rolling mill is dehumidified by hot air and preheated to 60°C. Argon gas is introduced locally into the contact area between the aluminum liquid and the activated coating aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature in this area is -28°C and the oxygen volume fraction is 0.32%. (5) The activated coating aluminum strip is continuously fed into the casting and rolling mill with a tension of 3t. The aluminum liquid is evenly distributed on the surface of the activator coating through the preheating channel and the casting nozzle. The continuous casting and rolling composite is carried out. The nozzle outlet width is 430mm, the finished product design width is 400mm, and a non-finished salt removal edge with a width of 15mm is formed on both sides of the composite slab width direction. The contact wetting and activation time between the aluminum liquid and the activated coating aluminum strip is 1.45s, and the pressing and salt removal time is 6s. The casting and rolling speed is 760mm / min, the roll surface temperature is 80℃, and the rolling force is 1550 tons. A continuous composite slab with a thickness of 8.0mm is obtained. (6) The composite slab is cut to length and cooled uniformly with water mist at a rate of 10℃ / s. Then, it is cold rolled in multiple passes with a total deformation of 80% and a deformation of no more than 35% per pass. When the total deformation of the cold rolling reaches 50%, intermediate annealing is performed at a temperature of 360℃ for 1.5 hours and then air-cooled to room temperature. Then, cold rolling is continued to the target thickness of 1.6mm, and full annealing is performed at a temperature of 350℃ for 4 hours and then furnace-cooled to room temperature. Finally, 15mm of non-finished salt removal edges are removed from both sides to obtain 3003 / 4343 layered aluminum-aluminum composite material.

[0050] Example 2 This embodiment prepares an 8011 / 6061 layered aluminum-aluminum composite material, wherein the substrate is 8011 aluminum alloy and the cladding is 6061 aluminum alloy. The preparation method is as follows: (1) Select 6061 aluminum alloy strip with a thickness of 0.4 mm and a width of 510 mm as solid coated aluminum strip. After leveling and trimming the 6061 aluminum alloy strip, use a grinding belt to continuously grind the surface to be coated to remove the natural oxide film on the surface, so that the surface roughness after grinding is Ra0.8μm. Then, use alkaline degreasing solution to spray and clean it. After rinsing with deionized water, dry it with hot air so that there is no visible oil or water stains on the surface, and obtain a clean coated aluminum strip. (2) Preparation of fluoroaluminate activator slurry: The fluoroaluminate powder is a mixture of CsAlF4 and K3AlF6 in a mass ratio of 30:70, with a D50 particle size of 1.0 μm and a D90 particle size of 8.6 μm; the volatile solvent is a mixture of isopropanol and water in a mass ratio of 75:25; the film-forming binder is a self-crosslinking acrylic emulsion; the mass ratio of the film-forming binder to the fluoroaluminate powder, based on solid content, is 0.3:100; the fluoroaluminate activator slurry is coated onto a clean aluminum coating using a gravure roller coating method. The surface to be coated with aluminum strip is formed with V-shaped coating units spaced apart along the length of the aluminum strip. V-shaped discharge gaps are formed between adjacent V-shaped coating units, with a width of 0.1 mm. Two guide gap sections of the V-shaped discharge gaps extend obliquely from the middle region of the aluminum strip width towards the two non-finished product salt discharge edges, and connect with the two non-finished product salt discharge edges. The angle between the guide gap sections and the length direction of the aluminum strip is 45°. The activator coating area coverage is 95%, and the coating amount of the activator coating, calculated as fluoroaluminate powder, is 0.15 g / m². 2 After coating, the aluminum strip is dried in a hot air furnace at 160℃ for 30 seconds. After drying, the mass content of residual volatile solvent in the activator coating is 0.31%, thus obtaining the activated coating aluminum strip. (3) 8011 aluminum alloy ingots were selected as the base aluminum ingots and melted in a smelting furnace to obtain molten aluminum. A refining agent of 0.1% by mass of the molten aluminum was added for refining and degassing. After standing for 16 minutes, slag was removed, and samples were taken for direct-reading spectral analysis. Al-Si and Al-Fe master alloys were used to adjust the composition to meet the requirements of 8011 aluminum alloy. Subsequently, online argon degassing was performed at an argon flow rate of 0.6 m³ / s. 3 / h, then filter through a 30μm ceramic filter plate, and after filtration, add Al-5Ti-1B grain refiner accounting for 0.15% of the mass of aluminum liquid, stir evenly, and stabilize the temperature of aluminum liquid at 725℃; (4) The treated aluminum liquid is transferred to the holding furnace, the temperature of which is controlled at 725°C. The flow channel connecting the holding furnace and the casting nozzle is preheated to 710°C. The composite area of ​​the casting and rolling mill is dehumidified by hot air and preheated to 65°C. Nitrogen gas is introduced locally into the contact area between the aluminum liquid and the activated coating aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature in this area is -21°C and the oxygen volume fraction is 0.50%. (5) The activated coating aluminum strip is continuously fed into the casting and rolling mill with a tension of 1t. The aluminum liquid is evenly distributed on the surface of the activator coating through the preheating channel and the casting nozzle. The continuous casting and rolling composite is carried out. The nozzle outlet width is 510mm, the finished product design width is 500mm, and a non-finished salt removal edge with a width of 5mm is formed on both sides of the composite slab width direction. The contact wetting and activation time between the aluminum liquid and the activated coating aluminum strip is 1.3s, and the pressing and salt removal time is 7s. The casting and rolling speed is 1200mm / min, the roll surface temperature is 40℃, and the rolling force is 2200 tons. A continuous composite slab with a thickness of 5.5mm is obtained. (6) The composite slab is cut to length and cooled uniformly with water mist at a rate of 5℃ / s. Then, it is cold rolled in multiple passes with a total deformation of 60% and a deformation of no more than 40% per pass. When the total deformation of the cold rolling reaches 40%, intermediate annealing is performed at a temperature of 390℃ for 1 hour and then air-cooled to room temperature. Then, cold rolling is continued to the target thickness of 2.2mm, and full annealing is performed at a temperature of 320℃ for 5 hours and then furnace-cooled to room temperature. Finally, the non-finished salt-removing edges on both sides are removed to obtain 8011 / 6061 layered aluminum-aluminum composite material.

[0051] Example 3 This embodiment prepares a 5052 / 6082 layered aluminum-aluminum composite material, wherein the substrate is 5052 aluminum alloy and the cladding is 6082 aluminum alloy. The preparation method is as follows: (1) Select 6082 aluminum alloy strip with a thickness of 1.8 mm and a width of 650 mm as solid coated aluminum strip. After leveling and trimming the 6082 aluminum alloy strip, use a grinding belt to continuously grind the surface to be coated to remove the natural oxide film on the surface, so that the surface roughness after grinding is Ra1.5μm. Then, use alkaline degreasing solution to spray and clean it. After rinsing with deionized water, dry it with hot air to make the surface free of visible oil and water stains, and obtain a clean coated aluminum strip. (2) Preparation of fluoroaluminate activator slurry: The fluoroaluminate powder is a mixture of K2AlF5, Cs2AlF5 and Cs3AlF6 in a mass ratio of 50:30:20, with a D50 particle size of 8.0 μm and a D90 particle size of 15.0 μm; the volatile solvent is a mixture of ethanol, n-propanol and water in a mass ratio of 60:20:20; the film-forming binder is a self-crosslinking polyurethane emulsion; the mass ratio of the film-forming binder to the fluoroaluminate powder, based on solid content, is 2:100; the fluoroaluminate activator slurry is applied by gravure roller coating. The material is coated onto the clean, coated aluminum strip surface to be laminated, forming V-shaped coating units spaced apart along the length of the aluminum strip. V-shaped discharge gaps are formed between adjacent V-shaped coating units, with a width of 1.0 mm. Two guide gap sections of the V-shaped discharge gaps extend obliquely from the middle region of the aluminum strip width towards the two non-finished product salt discharge edges, connecting with these edges. The angle between the guide gap sections and the length direction of the aluminum strip is 10°. The activator coating area coverage is 70%, and the coating amount of the activator coating, calculated as fluoroaluminate powder, is 1.2 g / m². 2 After coating, the aluminum strip is dried in an 80°C hot air furnace for 5 minutes. After drying, the mass content of residual volatile solvent in the activator coating is 0.78%, thus obtaining the activated coating aluminum strip. (3) 5052 aluminum alloy ingots were selected as the base aluminum ingots and melted in a smelting furnace to obtain molten aluminum. A refining agent of 0.3% by mass of the molten aluminum was added for refining and degassing. After standing for 10 minutes, slag was removed, and samples were taken for direct-reading spectral analysis. Al-Mg and Al-Cr master alloys were used to adjust the composition to meet the requirements of 5052 aluminum alloy. Subsequently, online argon-nitrogen mixed gas degassing was performed at a flow rate of 0.3 m³ / s. 3 / h, then filter through a 50μm ceramic filter plate, and after filtration, add Al-5Ti-1B grain refiner accounting for 0.5% of the mass of aluminum liquid, stir evenly, and stabilize the temperature of aluminum liquid at 680℃. (4) The treated aluminum liquid is transferred to the holding furnace, the temperature of which is controlled at 680°C. The flow channel connecting the holding furnace and the casting nozzle is preheated to 660°C. The composite area of ​​the casting and rolling mill is dehumidified by hot air and preheated to 70°C. Argon gas is introduced locally into the contact area between the aluminum liquid and the activated coating aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature in this area is -35°C and the oxygen volume fraction is 0.18%. (5) The activated coating aluminum strip is continuously fed into the casting and rolling mill with a tension of 6t. The aluminum liquid is evenly distributed on the surface of the activator coating through the preheating channel and the casting nozzle. The continuous casting and rolling composite is carried out. The nozzle outlet width is 650mm, the finished product design width is 600mm, and a non-finished salt removal edge with a width of 25mm is formed on both sides of the composite slab width direction. The contact wetting and activation time between the aluminum liquid and the activated coating aluminum strip is 1.6s, and the pressing and salt removal time is 5s. The casting and rolling speed is 300mm / min, the roll surface temperature is 100℃, and the rolling force is 1000 tons to obtain a continuous composite slab with a thickness of 10.0mm. (6) The composite slab is cut to length and cooled uniformly with water mist at a rate of 15℃ / s. Then, it is cold rolled in multiple passes with a total deformation of 85% and a deformation of no more than 32% per pass. When the total deformation of the cold rolling reaches 60%, intermediate annealing is performed at a temperature of 330℃ for 2 hours and then air-cooled to room temperature. Then, cold rolling is continued to the target thickness of 1.5mm, and full annealing is performed at a temperature of 380℃ for 2 hours and then furnace-cooled to room temperature. Finally, the non-finished salt-removing edges on both sides are removed to obtain 5052 / 6082 layered aluminum-aluminum composite material.

[0052] Example 4 This embodiment prepares a 1060 / 4045 layered aluminum-aluminum composite material, wherein the substrate is 1060 aluminum alloy and the cladding is 4045 aluminum alloy. The preparation method is as follows: (1) Select 4045 aluminum alloy strip with a thickness of 1.3mm and a width of 540mm as solid coated aluminum strip. After leveling and trimming the 4045 aluminum alloy strip, use a grinding belt to continuously grind the surface to be coated to remove the natural oxide film on the surface, so that the surface roughness after grinding is Ra1.2μm. Then, use alkaline degreasing solution to spray and clean it. After rinsing with deionized water, dry it with hot air to make the surface free of visible oil and water stains, and obtain a clean coated aluminum strip. (2) Preparation of fluoroaluminate activator slurry: The fluoroaluminate powder is a mixture of KAlF4, K2AlF5, and CsAlF4 in a mass ratio of 60:25:15, with a D50 particle size of 5.6 μm and a D90 particle size of 12.8 μm; the volatile solvent is a mixture of ethanol, propylene glycol methyl ether, and water in a mass ratio of 65:15:20; the film-forming binder is a mixture of self-crosslinking acrylic emulsion and self-crosslinking polyurethane emulsion in a mass ratio of 3:2 based on solid content; the mass ratio of the film-forming binder to the fluoroaluminate powder in terms of solid content is 1.2:100; using a concave... The fluoroaluminate activator slurry is applied to the clean, coated aluminum strip surface to be laminated using a roller coating method, forming V-shaped coating units spaced apart along the length of the aluminum strip. V-shaped discharge gaps are formed between adjacent V-shaped coating units, with a width of 0.6 mm. Two guide gap sections of the V-shaped discharge gaps extend obliquely from the middle region of the aluminum strip width towards the two non-finished salt discharge edges, connecting with them. The angle between the guide gap sections and the length direction of the aluminum strip is 32°. The activator coating area coverage is 82%, and the coating amount of the activator coating, calculated as fluoroaluminate powder, is 0.72 g / m². 2 After coating, the aluminum strip is dried in a hot air furnace at 135℃ for 110s. After drying, the mass content of residual volatile solvent in the activator coating is 0.47%, thus obtaining the activated coating aluminum strip. (3) 1060 aluminum alloy ingots were selected as the base aluminum ingots and melted in a smelting furnace to obtain molten aluminum. A refining agent of 0.22% by mass of the molten aluminum was added for refining and degassing. After standing for 14 minutes, slag was removed, and samples were taken for direct-reading spectral analysis. An Al-Mn master alloy was used to adjust the composition to meet the requirements of 1060 aluminum alloy. Subsequently, online argon degassing was performed at an argon flow rate of 0.45 m³ / s. 3 / h, then filter through a 40μm ceramic filter plate, and after filtration, add Al-5Ti-1B grain refiner accounting for 0.28% of the mass of aluminum liquid, stir evenly, and stabilize the temperature of aluminum liquid at 708℃. (4) The treated aluminum liquid is transferred into the holding furnace, the temperature of which is controlled at 708°C. The flow channel connecting the holding furnace and the casting nozzle is preheated to 690°C. The composite area of ​​the casting and rolling mill is dehumidified by hot air and preheated to 60°C. Nitrogen gas is introduced locally into the contact area between the aluminum liquid and the activated coating aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature in this area is -26°C and the oxygen volume fraction is 0.36%. (5) The activated coating aluminum strip is continuously fed into the casting and rolling mill with a tension of 3.5t. The aluminum liquid is evenly distributed on the surface of the activator coating through the preheating channel and the casting nozzle. The continuous casting and rolling composite is carried out. The nozzle outlet width is 540mm, the finished product design width is 510mm, and a non-finished salt removal edge with a width of 15mm is formed on both sides of the composite slab width direction. The contact wetting and activation time between the aluminum liquid and the activated coating aluminum strip is 1.55s, and the pressing and salt removal time is 6.5s. The casting and rolling speed is 650mm / min, the roll surface temperature is 72℃, and the rolling force is 1680 tons. A continuous composite slab with a thickness of 7.5mm is obtained. (6) The composite slab is cut to length and cooled uniformly with water mist at a rate of 11℃ / s. Then, it is cold rolled in multiple passes with a total deformation of 76% and a deformation of no more than 34% per pass. When the total deformation of the cold rolling reaches 52%, intermediate annealing is performed at a temperature of 365℃ for 1.6 hours and then air-cooled to room temperature. Then, cold rolling is continued to the target thickness of 1.8mm, followed by full annealing at a temperature of 345℃ for 3.5 hours and then furnace-cooled to room temperature. Finally, the non-finished salt-removing edges on both sides are removed to obtain 1060 / 4045 layered aluminum-aluminum composite material.

[0053] Comparative Example 1 (The difference from Example 1 is that the 4343 aluminum alloy strip is not coated with fluoroaluminate activator slurry after grinding, degreasing, cleaning and drying, and is directly fed into the casting and rolling mill as a solid coated aluminum strip for continuous casting and rolling composite) This comparative example prepared a 3003 / 4343 layered aluminum-aluminum composite material, wherein the substrate was 3003 aluminum alloy and the cladding was 4343 aluminum alloy. The preparation method was as follows: (1) Select 4343 aluminum alloy strip with a thickness of 1.0 mm and a width of 430 mm as solid coated aluminum strip. After leveling and trimming the 4343 aluminum alloy strip, use nylon abrasive belt to continuously grind the surface to be coated to remove the natural oxide film on the surface, so that the surface roughness after grinding is Ra1.1μm. Then, use alkaline degreasing solution to spray and clean, rinse with deionized water and dry with hot air to make the surface free of visible oil and water stains, and obtain clean coated aluminum strip; (2) 3003 aluminum alloy ingots were selected as the base aluminum ingots and melted in a smelting furnace to obtain molten aluminum. A refining agent of 0.2% by mass of the molten aluminum was added for refining and degassing. After standing for 12 minutes, slag was removed, and samples were taken for direct-reading spectral analysis. Al-Mn and Al-Cu master alloys were used to adjust the composition to meet the requirements of 3003 aluminum alloy. Subsequently, online argon degassing was performed at an argon flow rate of 0.4 m³ / s. 3 / h, then filter through a 40μm ceramic filter plate, and after filtration, add Al-5Ti-1B grain refiner accounting for 0.3% of the mass of aluminum liquid, stir evenly, and stabilize the temperature of aluminum liquid at 700℃; (3) The treated aluminum liquid is transferred into the holding furnace, the temperature of which is controlled at 700℃. The flow channel connecting the holding furnace and the casting nozzle is preheated to 680℃. The composite area of ​​the casting and rolling mill is dehumidified by hot air and preheated to 60℃. Argon gas is introduced locally into the contact area between the aluminum liquid and the clean coated aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature in this area is -28℃ and the oxygen volume fraction is 0.32%. (4) The clean coated aluminum strip is continuously fed into the casting and rolling mill with a tension of 3t. The aluminum liquid is evenly distributed on the surface of the clean coated aluminum strip through the preheating channel and the casting nozzle. The continuous casting and rolling composite is carried out. The nozzle outlet width is 430mm, the finished product design width is 400mm, and a non-finished salt removal edge with a width of 15mm is formed on both sides of the composite slab width direction. The contact wetting and activation time between the aluminum liquid and the activated coated aluminum strip is 1.45s, and the pressing and salt removal time is 6s. The casting and rolling speed is 760mm / min, the roll surface temperature is 80℃, and the rolling force is 1550 tons. A continuous composite slab with a thickness of 8.0mm is obtained. (5) The composite slab is cut to length and cooled uniformly with water mist at a rate of 10℃ / s. Then, it is cold rolled in multiple passes with a total deformation of 80% and a deformation of no more than 35% per pass. When the total deformation of the cold rolling reaches 50%, intermediate annealing is performed at a temperature of 360℃ for 1.5 hours and then air-cooled to room temperature. Then, cold rolling is continued to the target thickness of 1.6mm, and full annealing is performed at a temperature of 350℃ for 4 hours and then furnace-cooled to room temperature. Finally, 15mm of non-finished salt removal edges are removed from both sides to obtain 3003 / 4343 layered aluminum-aluminum composite material.

[0054] Comparative Example 2 (different from Example 1 in that the coating amount of the activator, calculated as fluoroaluminate powder, is 2.5 g / m²) 2 Furthermore, the activator coating is a full, continuous coating, without forming a V-shaped discharge gap. This comparative example prepared a 3003 / 4343 layered aluminum-aluminum composite material, wherein the substrate was 3003 aluminum alloy and the cladding was 4343 aluminum alloy. The preparation method was as follows: (1) Select 4343 aluminum alloy strip with a thickness of 1.0 mm and a width of 430 mm as solid coated aluminum strip. After leveling and trimming the 4343 aluminum alloy strip, use nylon abrasive belt to continuously grind the surface to be coated to remove the natural oxide film on the surface, so that the surface roughness after grinding is Ra1.1μm. Then, use alkaline degreasing solution to spray and clean, rinse with deionized water and dry with hot air to make the surface free of visible oil and water stains, and obtain clean coated aluminum strip; (2) Preparation of fluoroaluminate activator slurry: The fluoroaluminate powder is a mixture of KAlF4 and K2AlF5 in a mass ratio of 70:30, with a D50 particle size of 4.2 μm and a D90 particle size of 11.5 μm; the volatile solvent is a mixture of ethanol and water in a mass ratio of 80:20; the film-forming binder is a mixture of self-crosslinking acrylic emulsion and self-crosslinking polyurethane emulsion in a mass ratio of 4:1 based on solid content; the mass ratio of the film-forming binder to the fluoroaluminate powder in terms of solid content is 0.8:100; the fluoroaluminate activator slurry is applied continuously and fully to the clean coated aluminum strip surface to be laminated using a gravure roller coating method, with an activator coating area coverage of 100% and an activator coating amount of 2.5 g / m² based on fluoroaluminate powder. 2 After coating, the aluminum strip is dried in a hot air oven at 120℃ for 90 seconds. After drying, the mass content of residual volatile solvent in the activator coating is 0.42%, thus obtaining the activated coating aluminum strip. (3) 3003 aluminum alloy ingots were selected as the base aluminum ingots and melted in a smelting furnace to obtain molten aluminum. A refining agent of 0.2% by mass of the molten aluminum was added for refining and degassing. After standing for 12 minutes, slag was removed, and samples were taken for direct-reading spectral analysis. Al-Mn and Al-Cu master alloys were used to adjust the composition to meet the requirements of 3003 aluminum alloy. Subsequently, online argon degassing was performed at an argon flow rate of 0.4 m³ / s. 3 / h, then filter through a 40μm ceramic filter plate, and after filtration, add Al-5Ti-1B grain refiner accounting for 0.3% of the mass of aluminum liquid, stir evenly, and stabilize the temperature of aluminum liquid at 700℃; (4) The treated aluminum liquid is transferred into the holding furnace, the temperature of which is controlled at 700°C. The flow channel connecting the holding furnace and the casting nozzle is preheated to 680°C. The composite area of ​​the casting and rolling mill is dehumidified by hot air and preheated to 60°C. Argon gas is introduced locally into the contact area between the aluminum liquid and the activated coating aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature in this area is -28°C and the oxygen volume fraction is 0.32%. (5) The activated coating aluminum strip is continuously fed into the casting and rolling mill with a tension of 3t. The aluminum liquid is evenly distributed on the surface of the activator coating through the preheating channel and the casting nozzle. The continuous casting and rolling composite is carried out. The nozzle outlet width is 430mm, the finished product design width is 400mm, and a non-finished salt removal edge with a width of 15mm is formed on both sides of the composite slab width direction. The contact wetting and activation time between the aluminum liquid and the activated coating aluminum strip is 1.45s, and the pressing and salt removal time is 6s. The casting and rolling speed is 760mm / min, the roll surface temperature is 80℃, and the rolling force is 1550 tons. A continuous composite slab with a thickness of 8.0mm is obtained. (6) The composite slab is cut to length and cooled uniformly with water mist at a rate of 10℃ / s. Then, it is cold rolled in multiple passes with a total deformation of 80% and a deformation of no more than 35% per pass. When the total deformation of the cold rolling reaches 50%, intermediate annealing is performed at a temperature of 360℃ for 1.5 hours and then air-cooled to room temperature. Then, cold rolling is continued to the target thickness of 1.6mm, and full annealing is performed at a temperature of 350℃ for 4 hours and then furnace-cooled to room temperature. Finally, 15mm of non-finished salt removal edges are removed from both sides to obtain 3003 / 4343 layered aluminum-aluminum composite material.

[0055] Comparative Example 3 (different from Example 1 in that the coating amount of the activator, calculated as fluoroaluminate powder, is 0.05 g / m²) 2 ) This comparative example prepared a 3003 / 4343 layered aluminum-aluminum composite material, wherein the substrate was 3003 aluminum alloy and the cladding was 4343 aluminum alloy. The preparation method was as follows: (1) Select 4343 aluminum alloy strip with a thickness of 1.0 mm and a width of 430 mm as solid coated aluminum strip. After leveling and trimming the 4343 aluminum alloy strip, use nylon abrasive belt to continuously grind the surface to be coated to remove the natural oxide film on the surface, so that the surface roughness after grinding is Ra1.1μm. Then, use alkaline degreasing solution to spray and clean, rinse with deionized water and dry with hot air to make the surface free of visible oil and water stains, and obtain clean coated aluminum strip; (2) Preparation of fluoroaluminate activator slurry: The fluoroaluminate powder is a mixture of KAlF4 and K2AlF5 in a mass ratio of 70:30, with a D50 particle size of 4.2 μm and a D90 particle size of 11.5 μm; the volatile solvent is a mixture of ethanol and water in a mass ratio of 80:20; the film-forming binder is a mixture of self-crosslinking acrylic emulsion and self-crosslinking polyurethane emulsion in a mass ratio of 4:1 based on solid content; the mass ratio of the film-forming binder to the fluoroaluminate powder in terms of solid content is 0.8:100; the fluoroaluminate activator slurry is prepared by gravure roller coating. A salt activator slurry is applied to the clean, coated aluminum strip surface to be laminated, forming V-shaped coating units spaced apart along the length of the aluminum strip. V-shaped discharge gaps are formed between adjacent V-shaped coating units, with a width of 0.3 mm. Two guide gap sections of the V-shaped discharge gaps extend obliquely from the middle region of the aluminum strip width towards the two non-finished salt discharge edges, connecting with them. The angle between the guide gap sections and the length direction of the aluminum strip is 25°. The activator coating area coverage is 85%, and the coating amount of the activator coating, calculated as fluoroaluminate powder, is 0.05 g / m². 2 After coating, the aluminum strip is dried in a hot air oven at 120℃ for 90 seconds. After drying, the mass content of residual volatile solvent in the activator coating is 0.42%, thus obtaining the activated coating aluminum strip. (3) 3003 aluminum alloy ingots were selected as the base aluminum ingots and melted in a smelting furnace to obtain molten aluminum. A refining agent of 0.2% by mass of the molten aluminum was added for refining and degassing. After standing for 12 minutes, slag was removed, and samples were taken for direct-reading spectral analysis. Al-Mn and Al-Cu master alloys were used to adjust the composition to meet the requirements of 3003 aluminum alloy. Subsequently, online argon degassing was performed at an argon flow rate of 0.4 m³ / s. 3 / h, then filter through a 40μm ceramic filter plate, and after filtration, add Al-5Ti-1B grain refiner accounting for 0.3% of the mass of aluminum liquid, stir evenly, and stabilize the temperature of aluminum liquid at 700℃; (4) The treated aluminum liquid is transferred into the holding furnace, the temperature of which is controlled at 700°C. The flow channel connecting the holding furnace and the casting nozzle is preheated to 680°C. The composite area of ​​the casting and rolling mill is dehumidified by hot air and preheated to 60°C. Argon gas is introduced locally into the contact area between the aluminum liquid and the activated coating aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature in this area is -28°C and the oxygen volume fraction is 0.32%. (5) The activated coating aluminum strip is continuously fed into the casting and rolling mill with a tension of 3t. The aluminum liquid is evenly distributed on the surface of the activator coating through the preheating channel and the casting nozzle. The continuous casting and rolling composite is carried out. The nozzle outlet width is 430mm, the finished product design width is 400mm, and a non-finished salt removal edge with a width of 15mm is formed on both sides of the composite slab width direction. The contact wetting and activation time between the aluminum liquid and the activated coating aluminum strip is 1.45s, and the pressing and salt removal time is 6s. The casting and rolling speed is 760mm / min, the roll surface temperature is 80℃, and the rolling force is 1550 tons. A continuous composite slab with a thickness of 8.0mm is obtained. (6) The composite slab is cut to length and cooled uniformly with water mist at a rate of 10℃ / s. Then, it is cold rolled in multiple passes with a total deformation of 80% and a deformation of no more than 35% per pass. When the total deformation of the cold rolling reaches 50%, intermediate annealing is performed at a temperature of 360℃ for 1.5 hours and then air-cooled to room temperature. Then, cold rolling is continued to the target thickness of 1.6mm, and full annealing is performed at a temperature of 350℃ for 4 hours and then furnace-cooled to room temperature. Finally, 15mm of non-finished salt removal edges are removed from both sides to obtain 3003 / 4343 layered aluminum-aluminum composite material.

[0056] Experimental Example The layered aluminum-aluminum composite materials prepared in Examples 1-4 and Comparative Examples 1-3 were tested for their main properties.

[0057] The testing items and methods are as follows: The interfacial shear strength was tested according to the shear test method in GB / T 6396-2008 and in combination with the size of the aluminum-aluminum composite material specimen.

[0058] The 180° bending test was conducted in accordance with GB / T 232-2024, and the length of the interface delamination was counted along the length of the specimen after bending.

[0059] The peel test used strip-shaped specimens with a width of 20 mm. After the coated aluminum strip was pre-opened with the substrate material, it was peeled 180°, and the peel force and failure mode were recorded.

[0060] The stability of cold rolling was evaluated by statistically analyzing the number of bubbles and the length of edge cracks within the effective width of the composite slab after it was cold rolled to the target thickness.

[0061] The thermal cycling test involves 100 cycles between -40℃ and 120℃, with each high and low temperature cycle lasting 30 minutes. After the test, the interfacial shear strength is tested again and the strength retention rate is calculated.

[0062] The finished product qualification rate is calculated based on the percentage of effective lengths without bubbling, delamination, or through-cracks in 100m strips produced continuously.

[0063] The test data is shown in Table 1 below: Table 1 Performance test results of layered aluminum-aluminum composite materials Reference Figure 2 , Figure 3 As shown in Table 1, Examples 1-4 all achieved high interfacial shear strength. No interfacial delamination occurred after 180° bending. In the peel test, the main manifestations were coating tearing or localized coating tearing, without continuous peeling along the composite interface. Simultaneously, the number of bubbles within the effective width after cold rolling to the target thickness was low, the interfacial shear strength retention rate was high after thermal cycling, and the finished product qualification rate was high during the continuous preparation process. The above performance test results indicate that this application, through the combination of solid-state coated aluminum strip surface pretreatment, low-aluminate fluoroaluminate activator coating, V-shaped discharge gap, contact and pressing time control, and the formation and removal of non-finished salt-removing edges, can improve the bonding stability between different aluminum alloy layers and enhance the anti-delamination performance during subsequent cold rolling, bending, and thermal cycling processes.

[0064] In Example 1, a 3003 / 4343 composite system was used. With optimal activator coating amount, contact time, rolling force, and post-treatment, the interfacial shear strength reached 98 MPa, the 180° bending delamination length was 0, no blistering was observed within the effective width after cold rolling, the interfacial shear strength retention rate after thermal cycling was 93.9%, and the finished product qualification rate reached 98.6%, demonstrating good overall performance. Examples 2-4 correspond to 8011 / 6061, 5052 / 6082, and 1060 / 4045 composite systems, respectively. Although the strength, plasticity, and thermal conductivity of different alloy systems differ, they all exhibited the characteristics of no bending delamination, no continuous interfacial delamination during peeling, a small number of cold-rolled blisters, and a high interfacial strength retention rate after thermal cycling. This indicates that the method of this application has good applicability to continuous casting-rolling composites between 1-series, 3-series, 5-series, and 8-series aluminum alloy substrates and 4-series and 6-series aluminum alloy claddings.

[0065] Compared to Example 1, Comparative Example 1 did not apply a fluoroaluminate activator to the surface of the coated aluminum strip; the composite process relied solely on grinding, degreasing, drying, and localized inert atmosphere protection. Its interfacial shear strength was only 61 MPa, the delamination length after 180° bending was 18 mm / 100 mm, the peel test showed interfacial delamination, the number of bubbles increased significantly after cold rolling, and the interfacial shear strength retention rate decreased to 72.1% after thermal cycling, resulting in a lower finished product yield. These results indicate that in the solid-liquid casting-rolling composite process of different aluminum alloys, conventional mechanical cleaning and atmosphere protection alone are insufficient to reliably eliminate the adverse effects of the oxide film on the interfacial bonding of the coated aluminum strip. A low amount of fluoroaluminate activator has a significant effect on improving aluminum melt wetting and enhancing interfacial bonding strength.

[0066] Compared with Example 1, the amount of activator coated in Comparative Example 2 was increased to 2.5 g / m². 2 Furthermore, a full, continuous coating was used, without forming a V-shaped discharge gap. Its interfacial shear strength decreased to 56 MPa, and after 180° bending, the delamination length reached 35 mm / 100 mm. Continuous interfacial delamination occurred in the peel test, and the number of bubbles increased significantly after cold rolling. After thermal cycling, the interfacial shear strength retention rate was only 64.3%, resulting in a low finished product yield. These results indicate that higher amounts of fluoroaluminate activator are not necessarily better. Excessive activator may increase the risk of interfacial residual defects during continuous casting and rolling, leading to increased bubbling or delamination during cold rolling, bending, and thermal cycling. Therefore, this application uses a low-volume coating and a V-shaped discharge gap, which can reduce the risk of residue retention while ensuring the activation effect of the coating.

[0067] Compared with Example 1, Comparative Example 3 also had a V-shaped discharge gap and a non-finished product salt discharge edge, but the amount of activator coating was reduced to 0.05 g / m. 2The content is below the limit specified in this application. Its interfacial shear strength is 70 MPa. After 180° bending, local delamination of 12 mm / 100 mm occurs. Peel tests show localized interfacial peeling, and a certain number of bubbles remain after cold rolling. These results indicate that when the activator dosage is too low, its effect on damaging and promoting wetting of the oxide film on the coated aluminum strip surface is insufficient, making it difficult to form a stable and continuous metallurgical bonding interface. Therefore, the activator coating amount is limited to 0.15–1.2 g / m². 2 It is necessary.

[0068] Based on the results of Examples 1-4 and Comparative Examples 1-3, it is evident that the technical effect of this application does not solely rely on the introduction of fluoroaluminate activator, but rather on the synergistic effect of low-volume activator coating, discharge gap, non-finished product salt discharge edge, contact and pressing time control, and post-processing edge trimming. Insufficient activator results in inadequate film breaking and wetting; excessive activator or lack of discharge channels easily leads to interface residual defects. The non-finished product salt discharge edge provides space for residual activator and related inclusions to transfer to the non-finished product area at the edge. Through the synergistic control of the above process parameters, this application can significantly improve the interfacial shear strength, bending anti-delamination performance, cold rolling stability, and thermal cycling reliability of layered aluminum-aluminum composite materials, making it suitable for the continuous industrial production of layered composite sheets and strips of different aluminum alloys.

[0069] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions or alterations can be made to these embodiments without departing from the principles and spirit of this application, and the technical solutions resulting from such changes, modifications, substitutions or alterations will all fall within the protection scope of this application.

Claims

1. A method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling, characterized in that, Includes the following steps: S1. Select solid coated aluminum strip, grind, degrease, clean and dry it to obtain clean coated aluminum strip; S2. A fluoroaluminate activator slurry is coated onto the surface of the cleaned coated aluminum strip. After drying, the fluoroaluminate activator slurry forms an activator coating, resulting in an activated coated aluminum strip. The fluoroaluminate activator slurry comprises fluoroaluminate powder, a volatile solvent, and a film-forming binder. The coating amount of the activator coating, based on the fluoroaluminate powder, is 0.15–1.2 g / m². 2 ; S3. Select aluminum ingots as the base material and melt them to obtain molten aluminum; S4. The molten aluminum obtained in step S3 is distributed onto the surface of the activator coating of the activated coating aluminum strip obtained in step S2 through a flow channel and a casting nozzle, and then continuously cast and rolled to obtain a composite slab; wherein, during casting and rolling, non-finished salt removal edges are formed on both sides of the width direction of the composite slab; the contact wetting and activation time between the molten aluminum and the activated coating aluminum strip is 1.3 to 1.6 s, and the pressing and salt removal time is 5 to 7 s; S5. The composite slab is post-processed, and the non-finished salt-removing edges on both sides are removed to obtain a layered aluminum-aluminum composite material.

2. The method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling according to claim 1, characterized in that, The solid-coated aluminum strip in step S1 is selected from 4-series or 6-series aluminum alloy strips, and the thickness of the solid-coated aluminum strip in step S1 is 0.4 to 1.8 mm. The base aluminum ingot in step S3 is selected from 1-series, 3-series, 5-series or 8-series aluminum alloys.

3. The method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling according to claim 1, characterized in that, The mass ratio of the film-forming binder to the fluoroaluminate powder in step S2 is 0.3 to 2:100; And / or, the D50 particle size of the fluoroaluminate powder in step S2 is 1-8 μm, and the D90 particle size is not greater than 15 μm; And / or, the fluoroaluminate powder in step S2 includes at least one of KAlF4, K2AlF5, K3AlF6, CsAlF4, Cs2AlF5, and Cs3AlF6; And / or, the drying temperature in step S2 is 80-160°C, the drying time is 30s-5min, and the mass content of residual volatile solvent in the activator coating after drying is not greater than 0.8%.

4. The casting and rolling preparation method of layered aluminum-aluminum composite materials of different aluminum alloys according to claim 1, characterized in that, In step S2, the activator coating is an intermittent coating layer, which includes multiple V-shaped coating units arranged at intervals along the length of the activated coating aluminum strip. A V-shaped discharge gap with a width of 0.1 to 1 mm is formed between adjacent coating units. The V-shaped discharge gap includes two guide gap sections that extend obliquely from the middle region of the activated coating aluminum strip in the width direction to the two non-finished product salt discharge edges. The angle between the guide gap sections and the length direction of the activated coating aluminum strip is 10° to 45°, and they are connected to the two non-finished product salt discharge edges. The area coverage of the activator coating is 70% to 95%.

5. The method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling according to claim 1, characterized in that, Step S3, after melting, also includes refining and degassing, settling, composition adjustment, online degassing, ceramic filtration, and grain refinement treatment, and controlling the temperature of the aluminum liquid at 680-725℃.

6. The method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling according to claim 1, characterized in that, In step S4, the flow channel undergoes a preheating treatment at a temperature of 660–710°C. And / or, in step S4, during continuous casting and rolling, a protective gas is introduced into the contact area between the molten aluminum and the activated coating aluminum strip at the casting and rolling inlet, so that the local atmosphere dew point temperature of the contact area between the molten aluminum and the activated coating aluminum strip at the casting and rolling inlet is ≤-20℃ and the oxygen volume fraction is ≤0.5%.

7. The casting and rolling preparation method of layered aluminum-aluminum composite materials of different aluminum alloys according to claim 1, characterized in that, In step S4, the casting speed during continuous casting and rolling composite is 300-1200 mm / min, the roll surface temperature is 40-100℃, the rolling force is 1000-2200 tons, the tension of the activated coating aluminum strip is 1-6t, the width of the composite slab is 10-50 mm greater than the finished product width, and the width of the non-finished product salt discharge edge is 5-25 mm.

8. The method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling according to claim 1, characterized in that, In step S5, the post-processing includes: cutting the composite slab to length and cooling it uniformly, followed by multiple cold rolling passes; when the total cold rolling deformation reaches 40-60%, intermediate annealing is performed, and cold rolling continues to the target thickness before full annealing.

9. The method for preparing layered aluminum-aluminum composite materials of different aluminum alloys by casting and rolling according to claim 8, characterized in that, In the post-processing, the cooling rate of the uniform cooling is 5-15℃ / s, the total deformation of the multi-pass cold rolling is 60-85%, the deformation of each pass does not exceed 40%, the intermediate annealing temperature is 330-390℃, the holding time is 1-2h, the full annealing temperature is 320-380℃, and the holding time is 2-5h.

10. A layered aluminum-aluminum composite material prepared by the casting and rolling method of a layered aluminum-aluminum composite material of different aluminum alloys as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Heat transfer composite aluminum plate with self-fusion layered microstructure and preparation method of heat transfer composite aluminum plate

    CN115366502A

  • Coating type preformed brazing filler metal and preparation method and application thereof

    CN119635074A