A method and system for controlling the microstructure of alloys under low-temperature electromagnetic solidification
By acquiring the temperature curve without a magnetic field and monitoring the solidification state in real time, and dynamically controlling the electromagnetic field and cooling medium, the problems of eddy currents and induced temperature rise during the solidification process of aluminum alloys were solved, and the uniformity of the solidification structure and the stability of the low-temperature boundary of the aluminum alloy were achieved.
Patent Information
- Application Number
- CN202611515102.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, during the solidification process of aluminum alloys, the eddy currents and induced temperature rise caused by electromagnetic stirring affect the mold temperature, making it difficult to distinguish between normal heat transfer and thermal deviation caused by electromagnetic induction. Furthermore, the risk of low-temperature heat transfer medium entering the mold cavity is difficult to control, resulting in uneven casting.
By acquiring the non-magnetic temperature curve of the casting mold, the solidification state and temperature information are monitored in real time, and the electromagnetic generator and heat exchanger are dynamically controlled. The electromagnetic field and cooling medium are adjusted in stages to achieve real-time compensation and recovery of thermal deviation.
It achieves uniform control of the solidification structure of aluminum alloy, reduces the impact of sensor noise and the risk of cryogenic medium ingress, and ensures the stability of the cryogenic boundary and casting quality.
Smart Images

Figure CN123102973A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of alloy casting and solidification structure control technology, and in particular to a method and system for controlling the low-temperature electromagnetic solidification structure of alloys. Background Technology
[0002] The solidification structure of aluminum alloys is influenced by factors such as temperature gradient, cooling rate, melt flow, solute redistribution, crystal nucleation, and the nucleation and growth of second phases. Enhancing mold heat exchange can improve the melt heat extraction rate, but excessively strong or uneven local cooling may lead to premature formation of local solidified shells, restricting subsequent mold filling and melt flow.
[0003] Electromagnetic stirring can drive the flow of conductive melt without mechanical contact with it, and influence heat and solute transport during solidification. However, as the solidification process progresses and the solid fraction increases, the apparent flow resistance of the melt increases. If a fixed magnetic induction intensity, frequency, and duty cycle are used continuously throughout the solidification process, problems such as insufficient driving force in the liquid stage, decreased energy utilization in the pasty stage, or excessive local disturbances can easily occur.
[0004] Graphite molds and composite molds including graphite heat exchange layers have high thermal conductivity, making them suitable for establishing enhanced heat transfer boundaries. However, graphite is a conductive material, and under the influence of alternating, rotating, or pulsed electromagnetic fields, it generates eddy currents and induced temperature rise. This induced temperature rise alters the actual temperature history of the mold, partially offsetting the preset low-temperature heat transfer effect. Simply setting an absolute upper limit for the mold temperature makes it difficult to distinguish between mold rise caused by normal heat transfer from the molten aluminum alloy and additional thermal deviation caused by electromagnetic induction; merely reducing electromagnetic power when the temperature exceeds the limit also cannot guarantee the timely recovery of the low-temperature heat transfer boundary.
[0005] In addition, when using a heat transfer medium at a temperature significantly lower than ambient temperature for aluminum alloy casting molds, it is also necessary to prevent the low-temperature heat transfer medium or condensate from entering the mold cavity and gating channel, while taking into account the medium level, electrical insulation, purging gas conditions, and thermal management of the electromagnetic generator components.
[0006] Therefore, there is a need for a unified closed-loop control scheme for the solidification structure of aluminum alloys that integrates electromagnetic field-free reference temperature curves, solidification state identification, staged electromagnetic control, induced thermal deviation identification of graphite molds, graded compensation, and backlash recovery. Summary of the Invention
[0007] In view of this, it is necessary to provide a method and system for controlling the microstructure of alloys under low-temperature electromagnetic solidification in order to solve the above problems.
[0008] In a first aspect, embodiments of the present invention provide a method for controlling the microstructure of alloys under low-temperature electromagnetic solidification, applicable to casting molds equipped with a heat exchange device and an electromagnetic generator, comprising the following steps: Obtain the non-magnetic temperature curve of the casting mold, wherein the non-magnetic temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic environment. After the heat exchange device is turned on and the alloy melt is poured into the casting mold, the solidification state of the alloy and the temperature information of the casting mold are obtained in real time. The electromagnetic generator is controlled to operate based on the solidification state of the alloy. Simultaneously, the thermal deviation parameter at the corresponding moment is calculated based on the temperature information of the casting mold and the temperature curve without magnetic field. The electromagnetic generator and / or the heat exchange device are controlled to operate based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold.
[0009] Furthermore, obtaining the non-magnetic temperature profile of the casting mold includes: For the same alloy composition, melt quality, mold structure, billet size, pre-cooling temperature and medium flow rate, at least three mold temperature curves are repeatedly collected without applying an electromagnetic field, and the average value, median value or statistical value after removing outliers is taken at each time step to form the magnetic field-free temperature curve.
[0010] Furthermore, the solidification state of the alloy includes a first solidification stage, a second solidification stage, and a third solidification stage. In the first solidification stage, the alloy melt is in a liquid state or is mainly liquid. In the second solidification stage, the alloy melt exhibits an increased solid content and a significant increase in apparent flow resistance. In the third solidification stage, the alloy melt is mainly solid.
[0011] Furthermore, controlling the operation of the electromagnetic generator based on the solidification state of the alloy includes: When the alloy is in the first solidification stage, the electromagnetic generating device applies a first electromagnetic field to cause the melt to form a controlled circumferential, axial or combined flow. When the alloy is in the second solidification stage, the electromagnetic generating device applies a second electromagnetic field, wherein the second electromagnetic field is achieved by changing the first electromagnetic field through the following means: reducing the magnetic induction intensity or duty cycle, changing the frequency, or switching to intermittent or pulsed action. When the alloy is in the third solidification stage, the electromagnetic generator reduces or stops applying the electromagnetic field.
[0012] Furthermore, the calculation of the thermal deviation parameter at the corresponding time based on the temperature information of the casting mold and the non-magnetic field temperature curve includes: Based on the temperature information of the casting mold, the measured mold temperature curve during the electromagnetic field is obtained. The measured mold temperature curve during the electromagnetic field is aligned with the temperature curve without magnetic field in time to determine the thermal deviation parameter of the casting mold. The thermal deviation parameter includes the thermal deviation amount and / or the mold thermal deviation change rate.
[0013] Further, the step of controlling the operation of the electromagnetic generator and / or the heat exchanger based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold includes: When the thermal deviation of the casting mold reaches a first thermal deviation threshold and continues for a first preset time, or when the thermal deviation change rate of the casting mold reaches a first change rate threshold and continues for the first preset time, a first-level compensation strategy is executed, wherein the first-level compensation strategy includes at least one of reducing the magnetic induction intensity of the electromagnetic field, reducing the frequency, reducing the duty cycle, and pausing the application of the electromagnetic field. Within a second preset time after the execution of the first-level compensation strategy, if the thermal deviation of the casting mold does not decrease to below the first recovery threshold, or if the thermal deviation change rate of the casting mold is still higher than the recovery change rate threshold, a second-level compensation strategy is executed. The second-level compensation strategy includes at least one of increasing the circulation flow rate of the non-aqueous low-temperature heat transfer medium, increasing the cooling power, reducing the set temperature of the non-aqueous low-temperature heat transfer medium, and extending the electromagnetic pause time. When the thermal deviation of the mold decreases to below the second recovery threshold and continues for a third preset time, the electromagnetic parameters allowed in the current solidification stage are restored according to a preset slope. When the alloy melt reaches the preset solidification termination state, the applied electromagnetic field is reduced or stopped, and heat exchange with the casting mold continues through the cooling medium until a solidified alloy billet is obtained.
[0014] In a second aspect, embodiments of the present invention provide an alloy low-temperature electromagnetic solidification microstructure control device, comprising: First parameter acquisition module: used to acquire the non-magnetic temperature curve of the casting mold, wherein the non-magnetic temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic environment. The second parameter acquisition module is used to acquire the solidification state of the alloy and the temperature information of the casting mold in real time after the heat exchange device is turned on and the alloy melt is poured into the casting mold. Control and compensation module: used to control the operation of the electromagnetic generator based on the solidification state of the alloy; at the same time, based on the temperature information of the casting mold and the temperature curve without magnetic field, calculate the thermal deviation parameter at the corresponding time, and control the operation of the electromagnetic generator and / or the heat exchange device based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold.
[0015] In a third aspect, embodiments of the present invention provide an electronic device, comprising: processor; The memory stores computer instructions that cause the processor to perform the methods described above.
[0016] In a fourth aspect, embodiments of the present invention provide a computer-readable storage medium storing computer instructions for implementing the method described above.
[0017] In a fifth aspect, embodiments of the present invention provide an alloy low-temperature electromagnetic solidification microstructure control system, applicable to the alloy low-temperature electromagnetic solidification microstructure control method as described above, comprising a heat exchange device, a casting mold, an electromagnetic generator, a state acquisition component, and a controller. The heat exchange device has a heat exchange cavity for circulating cooling medium. The casting mold is installed within the heat exchange cavity. The electromagnetic generator is installed within the heat exchange cavity and surrounds the casting mold, used to generate an electromagnetic field acting on the casting mold. A melt temperature detection element is installed on the casting mold, and the detection end of the melt temperature detection element extends into the mold cavity of the casting mold. A mold temperature detection element is installed on the casting mold, and the detection end of the mold temperature detection element is used to measure the temperature of the casting mold. A medium temperature detection element is installed within the heat exchange cavity, and the detection end of the medium temperature detection element is used to measure the temperature of the cooling medium within the heat exchange cavity. The controller is electrically connected to the electromagnetic generator and the state acquisition component, used to control the operation of the electromagnetic generator and / or the heat exchange device according to the solidification state of the alloy and the thermal deviation parameters of the casting mold.
[0018] Compared with existing technologies: 1. By using a non-magnetic temperature curve that matches the actual working conditions, the normal solidification heat transfer background can be distinguished from the additional heat deviation caused by electromagnetic effects, thereby improving the targeting of heat compensation triggering. 2. Control should be performed in the order of first-stage electromagnetic load reduction, second-stage heat exchange compensation, and recovery with hysteresis to avoid directly and significantly changing the cooling conditions when there is a slight thermal deviation, and also to avoid the target low temperature boundary still not being able to recover after simply reducing the electromagnetic input. 3. Reduce the electromagnetic input according to the solidification state to match the electromagnetic effect with the changes in liquid phase ratio and flow resistance; 4. By acquiring temperature at multiple points, filtering, determining duration, and recovering hysteresis, the sensor noise and frequent switching caused by transient fluctuations are reduced; 5. By implementing liquid isolation, drying, gas purging, and safety interlocks, the risk of cryogenic media or condensate entering the mold cavity is reduced; 6. This scheme can be used for iron-containing aluminum alloys or recycled aluminum melts, providing repeatable thermal-fluid boundary control conditions for the regulation of grain size, iron-rich phase and solidification structure uniformity. Attached Figure Description
[0019] Figure 1 A flowchart illustrating a method for controlling the microstructure of an alloy under low-temperature electromagnetic solidification according to an embodiment of the present disclosure is shown schematically. Figure 2 A flowchart illustrating a method for calculating deviation parameters according to an embodiment of the present disclosure is shown schematically. Figure 3 A flowchart illustrating a primary compensation and secondary compensation strategy according to an embodiment of the present disclosure is shown schematically. Figure 4 A flowchart illustrating a hysteresis recovery and safety interlocking strategy according to an embodiment of the present disclosure is shown schematically. Figure 5 A schematic diagram of an alloy low-temperature electromagnetic solidification microstructure control device according to an embodiment of the present disclosure is shown. Figure 6 A schematic diagram of an electronic device according to an embodiment of the present disclosure is shown; Figure 7 A schematic diagram of an alloy low-temperature electromagnetic solidification microstructure control system according to an embodiment of the present disclosure is shown.
[0020] Postscript: Heat exchange device 710, temperature control tank 711, heat exchange tube 712, cold source 713, circulating pump 714, liquid level detection element 715; Casting mold 720, mold cavity 721, casting channel 722, pouring gate 723, liquid-stopping structure 724; Electromagnetic generator 730, electromagnetic temperature detection element 731; Melt temperature sensing element 740; Mold temperature sensing element 750; Medium temperature sensing element 760; Controller 770, storage unit 771, arithmetic unit 772, control unit 773; 780 sweeping and blowing assembly. Detailed Implementation
[0021] The technical solutions of this specification will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this specification, not all of them. Based on the embodiments in this specification, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this specification. Furthermore, the technical features involved in the different embodiments of this specification described below can be combined with each other as long as they do not conflict with each other.
[0022] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit this disclosure. The terms “comprising,” “including,” etc., as used herein indicate the presence of features, steps, operations, and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, or components.
[0023] All terms used herein (including technical and scientific terms) have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein are to be interpreted in a manner consistent with the context of this specification, and not in an idealized or overly rigid way.
[0024] When using expressions such as "at least one of A, B and C", they should generally be interpreted in accordance with the meaning that is commonly understood by those skilled in the art (e.g., "a system having at least one of A, B and C" should include, but is not limited to, a system having A alone, a system having B alone, a system having C alone, a system having A and B, a system having A and C, a system having B and C, and / or a system having A, B and C, etc.).
[0025] In existing technologies, magnetic stirring can drive the flow of conductive melt without mechanical contact with the melt and influence heat and solute transport during solidification. However, as the solidification process progresses and the solid fraction increases, the apparent flow resistance of the melt increases. If a fixed magnetic induction intensity, frequency, and duty cycle are used continuously throughout the solidification stage, problems such as insufficient driving force in the liquid stage, decreased energy utilization in the pasty region stage, or excessive local disturbances can easily occur.
[0026] Graphite molds and composite molds including graphite heat exchange layers have high thermal conductivity, making them suitable for establishing enhanced heat transfer boundaries. However, graphite is a conductive material, and under the influence of alternating, rotating, or pulsed electromagnetic fields, it generates eddy currents and induced temperature rise. This induced temperature rise alters the actual temperature history of the mold, partially offsetting the preset low-temperature heat transfer effect. Simply setting an absolute upper limit for the mold temperature makes it difficult to distinguish between mold rise caused by normal heat transfer from the molten aluminum alloy and additional thermal deviation caused by electromagnetic induction; merely reducing electromagnetic power when the temperature exceeds the limit also cannot guarantee the timely recovery of the low-temperature heat transfer boundary.
[0027] In addition, when using a heat transfer medium at a temperature significantly lower than ambient temperature for aluminum alloy casting molds, it is also necessary to prevent the low-temperature heat transfer medium or condensate from entering the mold cavity and gating channel, while taking into account the medium level, electrical insulation, purging gas conditions, and thermal management of the electromagnetic generator components.
[0028] Based on the deficiencies of the aforementioned related technologies, this disclosure provides a method for controlling the microstructure of alloys through low-temperature electromagnetic solidification, which is applied to the field of alloy casting and solidification microstructure control technology, aiming to achieve uniform solidification in all parts of the alloy.
[0029] In one possible embodiment, this disclosure provides a method for controlling the microstructure of an alloy under low-temperature electromagnetic solidification. This method is applicable to aluminum alloys, thereby achieving control over the solidification microstructure of aluminum alloys. Furthermore, this method can also be applied to other types of alloys.
[0030] Taking aluminum alloy as an example, the processor can acquire the non-magnetic field temperature curve of the casting mold, wherein the non-magnetic field temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic field environment; after the heat exchange device is turned on and the alloy melt is poured into the casting mold, the solidification state of the alloy and the temperature information of the casting mold are acquired in real time; the electromagnetic generator is controlled to operate based on the solidification state of the alloy; at the same time, the thermal deviation parameter at the corresponding time is calculated based on the temperature information of the casting mold and the non-magnetic field temperature curve, and the electromagnetic generator and / or the heat exchange device are controlled to operate based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold.
[0031] As can be seen from the above, in the embodiments of this disclosure: 1. By using a non-magnetic temperature curve that matches the actual working conditions, the normal solidification heat transfer background can be distinguished from the additional heat deviation caused by electromagnetic effects, thereby improving the targeting of heat compensation triggering. 2. Control should be performed in the order of first-stage electromagnetic load reduction, second-stage heat exchange compensation, and recovery with hysteresis to avoid directly and significantly changing the cooling conditions when there is a slight thermal deviation, and also to avoid the target low temperature boundary still not being able to recover after simply reducing the electromagnetic input. 3. Reduce the electromagnetic input according to the solidification state to match the electromagnetic effect with the changes in liquid phase ratio and flow resistance; 4. By acquiring temperature at multiple points, filtering, determining duration, and recovering hysteresis, the sensor noise and frequent switching caused by transient fluctuations are reduced; 5. By implementing liquid isolation, drying, gas purging, and safety interlocks, the risk of cryogenic media or condensate entering the mold cavity is reduced; 6. This scheme can be used for iron-containing aluminum alloys or recycled aluminum melts, providing repeatable thermal-fluid boundary control conditions for the regulation of grain size, iron-rich phase and solidification structure uniformity.
[0032] This disclosure provides a method for controlling the microstructure of alloys under low-temperature electromagnetic solidification, which is described below in conjunction with... Figure 1 This invention describes an alloy low-temperature electromagnetic solidification microstructure control method 100 according to an exemplary embodiment of the present disclosure, applicable to casting molds equipped with a heat exchange device and an electromagnetic generator, including steps S110-S130.
[0033] Step S110: Obtain the non-magnetic temperature curve of the casting mold, wherein the non-magnetic temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic environment. Step S120: After turning on the heat exchange device and pouring the alloy melt into the casting mold, the solidification state of the alloy and the temperature information of the casting mold are obtained in real time. Step S130: The electromagnetic generator is controlled to operate based on the solidification state of the alloy; at the same time, the thermal deviation parameter at the corresponding moment is calculated based on the temperature information of the casting mold and the temperature curve without magnetic field, and the electromagnetic generator and / or heat exchanger are controlled to operate based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than the threshold.
[0034] First, it should be noted that the "casting mold" mentioned in this application refers to a graphite mold, a graphite-based composite mold, or a composite mold including a graphite heat exchange layer. Graphite is a conductive material that generates eddy currents and induced temperature rise under the action of alternating, rotating, or pulsed electromagnetic fields. The heat exchange device is used to circulate and deliver cooling medium to the outer wall of the casting mold to achieve the heat exchange function of the casting mold. An electromagnetic generator is installed outside the casting mold to apply an electromagnetic field to the casting mold, thereby accelerating the flow of the alloy melt inside the casting mold.
[0035] The casting mold is installed in the heat exchange chamber of the heat exchange device, so that at least part of the heat exchange surface of the casting mold is in direct contact with the non-aqueous low-temperature heat transfer medium (i.e., the aforementioned cooling medium) or thermally coupled through the heat-conducting component, and the mold cavity and pouring channel of the casting mold are isolated from the non-aqueous low-temperature heat transfer medium; before the aluminum alloy melt is poured, the heat exchange device pre-cools at least part of the heat exchange surface of the casting mold to a preset mold temperature lower than the ambient temperature.
[0036] For example, before the alloy melt is poured, at least a portion of the heat exchange surface of the casting mold is precooled to [temperature missing]. 80℃~0℃, preferably 40℃~ 10℃. The preset mold temperature is the pre-pouring temperature of at least a portion of the heat exchange surfaces of the casting mold, without requiring all inner surfaces of the casting mold cavity to reach the same temperature.
[0037] It is important to note that the pouring gate of the casting mold should be at least 10 mm above the maximum permissible liquid level of the non-aqueous cryogenic heat transfer medium, and a liquid-barrier area should be provided between the mold cavity and pouring channel of the casting mold and the cryogenic heat exchange chamber; the mold cavity and pouring channel of the casting mold should be dried before pouring, and a dew point not exceeding [a certain value] should be used. Dry gas or inert gas at 20°C is used to purge the area above the mold cavity.
[0038] When an abnormal low-temperature heat transfer medium level is detected, the casting mold temperature signal fails, the electromagnetic generator temperature is abnormal, the purging gas flow rate is lower than the preset value, or the controller communication is abnormal, at least one of the following safety interlock measures is executed: prohibiting casting, suspending the application of the electromagnetic field, increasing the heat exchange capacity, shutting off the heating source, and issuing an alarm.
[0039] In this embodiment, the alloy is an aluminum alloy. Specifically, the aluminum alloy melt is an iron-containing aluminum alloy melt or an aluminum alloy melt prepared from recycled aluminum raw materials, with an iron content of 0.2–5.0 wt.%. Corresponding liquidus lines, solidus lines, cooling curve characteristics, and temperature-solid fraction calibration relationships are established for different alloy compositions. It is understood that parameters such as the alloy composition, melt mass, mold structure, billet size, pre-cooling temperature, and low-temperature heat transfer medium flow rate of the aluminum alloy can all be adjusted.
[0040] The implementation process of each step is illustrated below as an example.
[0041] Step S110: Obtain the non-magnetic temperature curve of the casting mold, wherein the non-magnetic temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic environment.
[0042] Since the casting mold contains graphite, in order to distinguish the normal solidification heat transfer background of the casting mold from the additional heat deviation caused by electromagnetic effects, it is first necessary to obtain the temperature curve of the casting mold under the influence of no magnetic field. The temperature curve without magnetic field is the curve of the temperature of the casting mold changing with the solidification time of the alloy. The solidification time of the alloy is taken as the zero point when the casting is completed or the filling is completed, and the time when the alloy is completely solidified is taken as the end point.
[0043] In some embodiments, obtaining the non-magnetic temperature profile of the casting mold includes: For the same alloy composition, melt quality, mold structure, billet size, pre-cooling temperature and medium flow rate, at least three mold temperature curves are repeatedly collected without applying an electromagnetic field. The average value, median value or statistical value after removing outliers is taken at each moment to form a magnetic field-free temperature curve.
[0044] For example, given a defined alloy composition, melt mass, mold structure, billet size, pre-cooling temperature, medium set temperature, and medium flow rate, the electromagnetic generator is first turned off, and at least three benchmark pours are performed under the same or comparable process conditions. The mold temperature at a preset distance from the mold cavity wall is continuously collected, with the completion time of filling defined as t=0.
[0045] Align the time axes of each benchmark test, remove obvious abnormal curves, and take the average or median value of each moment to form a non-magnetic field temperature curve. When there are small fluctuations in casting quality, initial melt temperature, or initial mold temperature, corrections can be made by time shifting, initial temperature offset correction, or segmented normalization, but the correction method and allowable range should be determined in advance in the control formula.
[0046] The non-magnetic field temperature profile is preferably saved in conjunction with alloy composition, melt quality, mold number, medium set temperature, and medium flow rate. When any major process condition exceeds the calibrated range, the controller does not directly recall the original non-magnetic field temperature profile, but instead prompts for recalibration or switching to a safety degradation mode.
[0047] Step S120: After turning on the heat exchange device and pouring the alloy melt into the casting mold, the solidification state of the alloy and the temperature information of the casting mold are obtained in real time.
[0048] In some embodiments, after casting is completed, at least two temperature parameters in the alloy melt, casting mold and low-temperature heat transfer medium are collected at 1 to 50 Hz; the cooling rate is determined by the first-order difference of temperature versus time, and the solidification characteristic points are determined by the cooling curve plateau, inflection point, peak of temperature change rate or characteristic interval matching the thermal analysis model.
[0049] For example, temperature parameters are collected at a sampling frequency of 1 to 50 Hz; at least one mold temperature detection point is located 2 to 10 mm away from the mold cavity wall and at a position of 0.3 to 0.7 times the height of the mold cavity.
[0050] In this embodiment, the solidification state of the alloy includes a first solidification stage, a second solidification stage, and a third solidification stage. The alloy melt in the first solidification stage is liquid or mainly liquid; the second solidification stage corresponds to a state where the solid fraction increases and the apparent flow resistance increases significantly; the alloy melt in the third solidification stage is mainly solid.
[0051] For example, taking A356 type aluminum-silicon alloy as an example, the range of solids fraction below approximately 0.18 to 0.20 can be used as the first solidification stage, the range of solids fraction between approximately 0.18 and 0.30 can be used as the switching window for the second solidification stage, and the range of solids fraction reaching 0.35 to 0.55 can be used as the switching window for the third solidification stage. The above solids fraction windows are only used to illustrate the control logic; the specific temperature and time thresholds should be determined through thermal analysis, thermodynamic calculations, and cooling curves of the actual alloy.
[0052] It is understood that the temperature information of the casting mold includes at least one of the mold temperature, melt temperature, and low-temperature heat transfer medium temperature.
[0053] Step S130: The electromagnetic generator is controlled to operate based on the solidification state of the alloy; at the same time, the thermal deviation parameter at the corresponding moment is calculated based on the temperature information of the casting mold and the temperature curve without magnetic field, and the electromagnetic generator and / or heat exchanger are controlled to operate based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than the threshold.
[0054] In some embodiments, controlling the operation of the electromagnetic generator based on the solidification state of the alloy includes: When the alloy is in the first solidification stage, the electromagnetic generator applies the first electromagnetic field to make the melt form a controlled circumferential, axial or combined flow. When the alloy is in the second solidification stage, the electromagnetic generator applies a second electromagnetic field. The second electromagnetic field can be achieved by changing the first electromagnetic field through the following means: reducing the magnetic induction intensity or duty cycle, changing the frequency, or switching to intermittent or pulsed action. When the alloy is in the third solidification stage, the electromagnetic field applied by the electromagnetic generator is reduced or stopped from being applied based on the second electromagnetic field.
[0055] For example, when the calibrated solid fraction is below 0.18 to 0.20, the first electromagnetic field is applied; when the calibrated solid fraction enters the range of 0.18 to 0.30, the process switches to the second solidification stage and applies the second electromagnetic field; when the calibrated solid fraction reaches the range of 0.35 to 0.55, the process switches to the third solidification stage and reduces or stops applying the electromagnetic field.
[0056] The electromagnetic field is a rotating electromagnetic field, an alternating electromagnetic field, a traveling wave electromagnetic field, or a pulsed electromagnetic field; the magnetic induction intensity in the effective working area of the mold cavity is 2-100 mT and the frequency is 1-250 Hz; the first solidification stage preferably uses 6-30 mT and 10-80 Hz, and the magnetic induction intensity in the second solidification stage is 30%-70% of that in the first solidification stage, with a duty cycle of 20%-60%.
[0057] Figure 2An exemplary method 200 for calculating thermal deviation parameters is disclosed. In some embodiments, the thermal deviation parameters at a corresponding time are calculated based on the temperature information of the casting mold and the temperature curve without a magnetic field, including: Based on the temperature information of the casting mold, the measured mold temperature curve Tm(t) during the electromagnetic field is obtained. The measured mold temperature curve Tm(t) during the electromagnetic field is aligned with the temperature curve Tref(t) without magnetic field to determine the thermal deviation parameter of the casting mold. The thermal deviation parameter includes the thermal deviation amount ΔTm(t) = Tm(t). Tref(t) and / or mold thermal deviation rate.
[0058] Specifically, the thermal deviation and the rate of change of thermal deviation are determined by applying a moving average of 0.5 to 2 s, low-pass filtering, or median filtering to Tm(t) and ΔTm(t).
[0059] Figure 3 Exemplary disclosures include primary and secondary compensation strategies 300. In some embodiments, the operation of the electromagnetic generator and / or heat exchanger is controlled based on thermal deviation parameters to reduce the thermal deviation parameters until they are no greater than a threshold, including: When the thermal deviation of the casting mold reaches the first thermal deviation threshold and continues for a first preset time, or when the thermal deviation change rate of the casting mold reaches the first change rate threshold and continues for a first preset time, a first-level compensation strategy is executed. The first-level compensation strategy includes at least one of reducing the magnetic induction intensity of the electromagnetic field, reducing the frequency, reducing the duty cycle, and pausing the application of the electromagnetic field. Within a second preset time after the execution of the first-level compensation strategy, if the thermal deviation of the casting mold does not decrease to below the first recovery threshold, or if the thermal deviation change rate of the casting mold is still higher than the recovery change rate threshold, the second-level compensation strategy is executed. The second-level compensation strategy includes at least one of increasing the circulation flow rate of the non-aqueous low-temperature heat transfer medium, increasing the cooling power, reducing the set temperature of the non-aqueous low-temperature heat transfer medium, and extending the electromagnetic pause time. When the thermal deviation of the mold decreases below the second recovery threshold and continues for a third preset time, the electromagnetic parameters allowed in the current solidification stage are restored according to the preset slope. When the alloy melt reaches the preset solidification termination state, the applied electromagnetic field is reduced or stopped, and heat exchange continues between the cooling medium and the casting mold until a solidified alloy billet is obtained.
[0060] In this embodiment, the first thermal deviation threshold is 3 to 10°C, the first rate of change threshold is 0.2 to 1.0°C / s, and the first preset time is 1 to 3 s; the first-level compensation strategy includes reducing the magnetic induction intensity by 15% to 30% and / or reducing the duty cycle by 10 to 30 percentage points.
[0061] In this embodiment, the second preset time is 2 to 5 seconds; when the thermal deviation does not decrease to below 1 to 3°C within the second preset time, the circulation flow rate of the non-aqueous low-temperature heat transfer medium is increased by 30% to 50%, the medium setting temperature is reduced by 2 to 5°C, and / or the electromagnetic field is paused for 2 to 5 seconds; the second recovery threshold is 1 to 3°C, the third preset time is 2 to 5 seconds, and a ramp recovery rate of 5% to 20% / s is used when restoring the electromagnetic parameters.
[0062] For example, the controller aligns the measured mold temperature curve Tm(t) during the actual solidification process with the non-magnetic field temperature curve Tref(t) at t=0, and calculates ΔTm(t)=Tm(t). Tref(t). A 0.5–2 s moving average, low-pass filter, or median filter is applied to Tm(t) and ΔTm(t) to suppress temperature measurement noise and transient disturbances.
[0063] A preferred control method is as follows: 1. When ΔTm reaches 5℃ or the thermal deviation rate reaches 0.5℃ / s and lasts for 2 s, the first-level compensation is triggered; 2. First-level compensation reduces magnetic flux density by 20% and duty cycle by 20 percentage points; 3. After the first-level compensation is executed, continue monitoring for 2 seconds; if ΔTm is still higher than 3℃ or the thermal deviation change rate is still higher than 0.2℃ / s, then trigger the second-level compensation; 4. Secondary compensation pauses the electromagnetic field for 2-5 seconds, while increasing the medium circulation flow rate by 30%-50% and reducing the medium set temperature by 2-5℃. 5. When ΔTm decreases to below 2℃ and the rate of change of thermal deviation is not higher than 0.1℃ / s, and this condition persists for 3 s, the electromagnetic parameters are restored to the allowable level for the current solidification stage at a ramp rate of 10% / s. 6. If the situation cannot be restored after two consecutive secondary compensations, or if the condition of the mold, electromagnetic generator, or medium exceeds the safety threshold, the electromagnetic field will be stopped and the system will enter a safe heat exchange state.
[0064] By employing duration determination and recovery hysteresis, frequent switching of the electromagnetic field and circulation pump can be avoided due to fluctuations in ΔTm near the threshold.
[0065] Figure 4 An exemplary hysteresis recovery and safety interlock strategy 400 is disclosed. In some embodiments, the hysteresis recovery strategy includes the following steps: Receive compensation status: Obtain the thermal deviation status after first-level compensation or second-level compensation; Continuous monitoring of recovery parameters: collecting thermal deviation, thermal deviation change rate, current solidification stage, electromagnetic parameters, and cooling medium status; Determine if the thermal deviation is below the second recovery threshold and persists for a third preset time. If not, maintain the current compensation state and continue monitoring the recovery parameters; if yes, proceed to the next step. Determine whether the thermal deviation rate of change has entered the recovery rate of change range and whether there is a new upward trend in thermal deviation. If not, maintain the current compensation status and extend the monitoring time; if yes, proceed to the next step. Initiate recovery with hysteresis: Recover the electromagnetic parameters allowed for the current solidification stage according to the preset slope (5%~20% slope recovery or graded incremental recovery). During the recovery process, does the thermal deviation amount reach the first thermal deviation threshold again or does the thermal deviation defense rate exceed the limit again? If yes, the recovery is stopped, and the process re-enters Level 1 compensation or, if necessary, Level 2 compensation; otherwise, proceed to the next step. Continue restoring to the target electromagnetic parameters for the current solidification stage, and determine whether restoration is complete and whether electromagnetic action can continue during the solidification stage. If yes, output the restoration completion status and return to normal phased electromagnetic control and continuous monitoring; otherwise, repeat this step.
[0066] In some embodiments, the security interlock strategy includes the following steps: Continuously monitor the safety status and determine if any installation abnormalities exist. If no abnormalities are found, recovery control or normal control is permitted; otherwise, proceed to the next step. The monitored parameters include liquid level, mold temperature signal, electromagnetic temperature, purging gas status, and controller communication status. Identify anomaly types: Anomaly types include: A. Abnormal liquid level of low-temperature heat transfer medium; B. Failure of mold temperature signal; C. Abnormal temperature of electromagnetic generator; D. Sweeping gas flow rate is lower than preset value or dew point is abnormal; E. Controller communication anomaly.
[0067] Triggering a safety interlock: Prohibits pouring or suspends the current process; The system executes interlock actions and determines whether the abnormality has been resolved and whether the signal has stabilized. If yes, the interlock conditions are released; otherwise, proceed to the next step. Interlock actions include pausing the application of the electromagnetic field, increasing heat exchange capacity and / or maintaining safe heat exchange, shutting down the heating source if necessary, and issuing an alarm signal. Releasing the interlock conditions includes confirming that the system is allowed to exit the interlock after a preset confirmation time and returning to recovery or normal control.
[0068] Maintain the interlock status, prohibit the restoration of electromagnetic action, and continue alarm and monitoring until there are no safety anomalies, then allow the execution of restoration control or normal control.
[0069] Figure 5 A schematic diagram of an alloy low-temperature electromagnetic solidification microstructure control device according to another embodiment of the present disclosure is shown. Figure 5 As shown, the alloy low-temperature electromagnetic solidification microstructure control device 500 includes: First parameter acquisition module 510: used to acquire the non-magnetic temperature curve of the casting mold, wherein the non-magnetic temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic environment. Second parameter acquisition module 520: used to acquire the solidification state of the alloy and the temperature information of the casting mold in real time after the heat exchange device is turned on and the alloy melt is poured into the casting mold. Control and compensation module 530: used to control the operation of the electromagnetic generator based on the solidification state of the alloy; at the same time, it calculates the thermal deviation parameter at the corresponding moment based on the temperature information of the casting mold and the temperature curve without magnetic field, and controls the operation of the electromagnetic generator and / or heat exchange device based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than the threshold.
[0070] In some embodiments, obtaining the non-magnetic temperature profile of the casting mold includes: For the same alloy composition, melt quality, mold structure, billet size, pre-cooling temperature and medium flow rate, at least three mold temperature curves are repeatedly collected without applying an electromagnetic field. The average value, median value or statistical value after removing outliers is taken at each moment to form a magnetic field-free temperature curve.
[0071] In some embodiments, the solidification state of the alloy includes a first solidification stage, a second solidification stage, and a third solidification stage. The alloy melt in the first solidification stage is liquid or mainly liquid phase. The alloy melt in the second solidification stage exhibits an increased solid phase content and a significant increase in apparent flow resistance. The alloy melt in the third solidification stage is mainly solid phase.
[0072] In some embodiments, controlling the operation of the electromagnetic generator based on the solidification state of the alloy includes: When the alloy is in the first solidification stage, the electromagnetic generator applies the first electromagnetic field to make the melt form a controlled circumferential, axial or combined flow. When the alloy is in the second solidification stage, the electromagnetic generator applies a second electromagnetic field. The second electromagnetic field is achieved by changing the first electromagnetic field through the following means: reducing the magnetic induction intensity or duty cycle, changing the frequency, or switching to intermittent or pulsed action. When the alloy is in the third solidification stage, the electromagnetic generator reduces or stops applying the electromagnetic field.
[0073] In some embodiments, the thermal deviation parameter at a corresponding time is calculated based on the temperature information of the casting mold and the temperature curve without a magnetic field, including: Based on the temperature information of the casting mold, the measured mold temperature curve during the electromagnetic field is obtained. The measured mold temperature curve during the electromagnetic field is aligned with the temperature curve without magnetic field to determine the thermal deviation parameters of the casting mold. The thermal deviation parameters include the thermal deviation amount and / or the mold thermal deviation change rate.
[0074] In some embodiments, controlling the operation of the electromagnetic generator and / or heat exchanger based on a thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold includes: When the thermal deviation of the casting mold reaches the first thermal deviation threshold and continues for a first preset time, or when the thermal deviation change rate of the casting mold reaches the first change rate threshold and continues for a first preset time, a first-level compensation strategy is executed. The first-level compensation strategy includes at least one of reducing the magnetic induction intensity of the electromagnetic field, reducing the frequency, reducing the duty cycle, and pausing the application of the electromagnetic field. Within a second preset time after the execution of the first-level compensation strategy, if the thermal deviation of the casting mold does not decrease to below the first recovery threshold, or if the thermal deviation change rate of the casting mold is still higher than the recovery change rate threshold, the second-level compensation strategy is executed. The second-level compensation strategy includes at least one of increasing the circulation flow rate of the non-aqueous low-temperature heat transfer medium, increasing the cooling power, reducing the set temperature of the non-aqueous low-temperature heat transfer medium, and extending the electromagnetic pause time. When the thermal deviation of the mold decreases below the second recovery threshold and continues for a third preset time, the electromagnetic parameters allowed in the current solidification stage are restored according to the preset slope. When the alloy melt reaches the preset solidification termination state, the applied electromagnetic field is reduced or stopped, and heat exchange continues between the cooling medium and the casting mold until a solidified alloy billet is obtained.
[0075] Figure 6 A schematic diagram of an electronic device according to an embodiment of the present disclosure is shown below, in conjunction with... Figure 6 This specification describes some embodiments of electronic devices.
[0076] Reference Figure 6 The electronic device 600 may include one or more of the following components: processing component 602, memory 604, power supply component 606, multimedia component 608, audio component 610, input / output (I / O) interface 612, sensor component 616, and communication component 618.
[0077] Processing component 602 typically controls the overall operation of electronic device 600, such as operations associated with display, telephone calls, data communication, camera operation, and recording operations. Processing component 602 may include one or more processors 620 to execute instructions. Furthermore, processing component 602 may include one or more modules to facilitate interaction between processing component 602 and other components. For example, processing component 602 may include a multimedia module to facilitate interaction between multimedia component 608 and processing component 602. As another example, processing component 602 may read executable instructions from memory to implement relevant functions of the electronic device.
[0078] Memory 604 is configured to store various types of data to support the operation of electronic device 600. Examples of such data include instructions for any application or method operating on electronic device 600, contact data, phonebook data, messages, pictures, videos, etc. Memory 604 can be implemented by any type of volatile or non-volatile storage device or a combination thereof, such as static random access memory (SRAM), electrically erasable programmable read-only memory (EEPROM), erasable programmable read-only memory (EPROM), programmable read-only memory (PROM), read-only memory (ROM), magnetic storage, flash memory, magnetic disk, or optical disk.
[0079] Power supply component 606 provides power to various components of electronic device 600. Power supply component 606 may include a power management system, one or more power supplies, and other components associated with generating, managing, and distributing power to electronic device 600.
[0080] Multimedia component 608 includes a display screen that provides an output interface between electronic device 600 and user. In some embodiments, multimedia component 608 includes a front-facing camera and / or a rear-facing camera. When electronic device 600 is in an operating mode, such as shooting mode or video mode, the front-facing camera and / or rear-facing camera can receive external multimedia data. Each front-facing camera and rear-facing camera can be a fixed optical lens system or have focal length and optical zoom capabilities.
[0081] Audio component 610 is configured to output and / or input audio signals. For example, audio component 610 includes a microphone (MIC) configured to receive external audio signals when electronic device 600 is in an operating mode, such as call mode, recording mode, and voice recognition mode. The received audio signals may be further stored in memory 604 or transmitted via communication component 618. In some embodiments, audio component 610 also includes a speaker for outputting audio signals.
[0082] I / O interface 612 provides an interface between processing component 602 and peripheral interface modules, such as keyboards, click wheels, buttons, etc. These buttons may include, but are not limited to, home buttons, volume buttons, start buttons, and lock buttons.
[0083] Sensor assembly 616 includes one or more sensors for providing state assessments of various aspects of electronic device 600. For example, sensor assembly 616 can detect the on / off state of electronic device 600, the relative positioning of components such as the display and keypad of electronic device 600, changes in position of electronic device 600 or one of its components, the presence or absence of user contact with electronic device 600, orientation or acceleration / deceleration of electronic device 600, and temperature changes of electronic device 600. Sensor assembly 616 may include a proximity sensor configured to detect the presence of nearby objects without any physical contact. Sensor assembly 616 may also include a light sensor, such as a CMOS or CCD image sensor, for use in imaging applications. In some embodiments, sensor assembly 616 may also include an accelerometer, gyroscope, magnetometer, pressure sensor, or temperature sensor.
[0084] Communication component 618 is configured to facilitate wired or wireless communication between electronic device 600 and other devices. Electronic device 600 can access wireless networks based on communication standards, such as Wi-Fi, 2G, 3G, 4G, 5G, or 6G, or combinations thereof. In one exemplary embodiment, communication component 618 receives broadcast signals or broadcast-related information from an external broadcast management system via a broadcast channel. In one exemplary embodiment, communication component 618 also includes a short-range communication (NFC) module to facilitate short-range communication. For example, the NFC module may be implemented based on radio frequency identification (RFID) technology, Infrared Data Association (IrDA) technology, ultra-wideband (UWB) technology, Bluetooth (BT) technology, and other technologies.
[0085] In an exemplary embodiment, the electronic device 600 may be implemented by one or more application-specific integrated circuits (ASICs), digital signal processors (DSPs), digital signal processing devices (DSPDs), programmable logic devices (PLDs), field-programmable gate arrays (FPGAs), controllers, microcontrollers, microprocessors, or other electronic components.
[0086] In an exemplary embodiment, a non-transitory computer-readable storage medium, such as a memory for instructions, is also provided, which, when executed by a processor of an electronic device, enables the electronic device to perform the alloy low-temperature electromagnetic solidification microstructure control method of any embodiment of the present disclosure.
[0087] Non-transitory computer-readable storage media can be ROM, random access memory (RAM), CD-ROM, magnetic tape, floppy disk, and optical data storage devices, etc.
[0088] This disclosure provides an alloy low-temperature electromagnetic solidification microstructure control system, which is described below in conjunction with... Figure 7 The following describes an alloy low-temperature electromagnetic solidification microstructure control system 700 according to an exemplary embodiment of the present disclosure, including a heat exchange device 710, a casting mold 720, an electromagnetic generator 730, a status acquisition component, and a controller 770; the heat exchange device 710 has a heat exchange chamber for circulating cooling medium; the casting mold 720 is installed in the heat exchange chamber; the electromagnetic generator 730 is installed in the heat exchange chamber and arranged around the casting mold 720 for generating an electromagnetic field acting on the casting mold 720; the status acquisition component has a detection end for detecting the melt temperature, the temperature of the casting mold 720, and / or the temperature of the cooling medium; the controller 770 is electrically connected to the electromagnetic generator 730 and the status acquisition component, and is used to control the operation of the electromagnetic generator 730 and / or the heat exchange device 710 according to the solidification state of the alloy and the thermal deviation parameters of the casting mold 720.
[0089] The heat exchange device 710 in this embodiment includes a temperature control tank 711, a heat exchange tube 712, a cold source 713, a circulation pump 714, and a liquid level detection element 715. The temperature control tank 711 forms a heat exchange cavity and contains a cooling medium. Both ends of the heat exchange tube 712 are connected to the temperature control tank 711. The cold source 713 can be a refrigerator or similar structure. The cold source 713 and the circulation pump 714 are both installed on the heat exchange tube 712 to control the cooling circulation flow through the cold source 713 and the temperature control tank 711, thereby controlling the temperature of the cooling medium in the temperature control tank 711. The liquid level detection element 715 is installed in the temperature control tank 711 to detect the liquid level height in the temperature control tank 711. At the same time, the liquid level detection element 715 and the cold source 713 are both electrically connected to the controller 770, which facilitates the control of the liquid level height in the temperature control tank 711 and the temperature of the cooling medium.
[0090] The temperature control tank 711 and the heat exchange tube 712 are both made of non-magnetic, low-conductivity materials and are equipped with a heat insulation layer. The cooling medium is a non-water low-temperature heat transfer medium. Specifically, the non-water low-temperature heat transfer medium is a low-temperature siloxane heat transfer liquid, a perfluoropolyether heat transfer liquid, or other dielectric heat transfer medium that is pumpable at the target working temperature and compatible with the mold material.
[0091] In this embodiment, the casting mold 720 has an internal cavity 721, with an opening at the top forming a casting channel 722. The top of the casting channel 722 forms a conical casting port. A liquid-separating structure 724 is also included to separate the casting mold 720 from the cooling medium. The casting port 723 should be higher than the maximum permissible liquid level of the non-aqueous low-temperature heat transfer medium.
[0092] In this embodiment, the electromagnetic generator 730 is disposed around the casting mold 720 and is used to generate an adjustable electromagnetic field in the area where the mold cavity 721 is located.
[0093] In one embodiment, the electromagnetic generating component includes a multiphase coil group arranged circumferentially along the mold cavity 721, the effective height of the coil covering more than 60% of the height of the mold cavity 721, and an electrical insulation and thermal isolation gap of 10 to 50 mm is provided between the inner edge of the coil and the outer wall of the graphite casting mold; the spatial uniformity deviation of the magnetic induction intensity in the effective working area of the mold cavity 721 is no greater than ±20%.
[0094] The status acquisition component in this embodiment includes at least one of the following: melt temperature detection element 740, mold temperature detection element 750, and medium temperature detection element 760.
[0095] In one embodiment, a melt temperature sensing element 740 is mounted on a casting mold 720, and the sensing end of the melt temperature sensing element 740 extends into the mold cavity 721 of the casting mold 720; a mold temperature sensing element 750 is mounted on the casting mold 720, and the sensing end of the mold temperature sensing element 750 is used to measure the temperature of the casting mold 720; a medium temperature sensing element 760 is mounted in a heat exchange cavity, and the sensing end of the medium temperature sensing element 760 is used to measure the temperature of the cooling medium in the heat exchange cavity.
[0096] The casting mold 720 is provided with sensor mounting holes to facilitate the installation of melt temperature detection element 740 and mold temperature detection element 750. The temperature measuring ends of the temperature detection element and the mold temperature detection element 750 are 2 to 10 mm away from the wall of the mold cavity 721.
[0097] This embodiment also includes an electromagnetic temperature detection element 731 installed in the heat exchange cavity. The electromagnetic temperature detection element 731 is used to detect the temperature of the electromagnetic generator 730 and is electrically connected to the controller 770.
[0098] The controller 770 in this embodiment includes a storage unit 771, a calculation unit 772, and a control unit 773. The storage unit 771 is used to store the temperature curve without magnetic field, the calculation unit 772 is used to calculate the thermal deviation of the mold and the rate of change of thermal deviation, and the control unit 773 is used to execute the first-level compensation strategy, the second-level compensation strategy, and the recovery strategy with hysteresis.
[0099] This embodiment also includes a sweeping and blowing assembly 780, which is disposed directly above the casting mold 720. The sweeping and blowing assembly 780 has a sweeping and blowing end facing the pouring port 723. The sweeping and blowing assembly is used to deliver dry gas or inert gas to the upper area of the mold cavity 721.
[0100] Example 1: The graphite casting mold uses isostatically pressed graphite, with a room temperature thermal conductivity preferably of 80–150 W / (m·K) and a resistivity preferably of 8–20 μΩ·m. The mold cavity is a cylindrical cavity with a diameter of 50 mm and a height of 100 mm; the mold outer diameter is 80 mm, the total height is 140 mm, the minimum radial wall thickness is 15 mm, and the bottom thickness is 20 mm; the mass of a single aluminum alloy melt is 0.45 ± 0.05 kg.
[0101] The melt temperature sensing element is positioned 3 mm from the mold cavity sidewall and at the midpoint of the mold cavity height, while the mold temperature sensing element is positioned 3–5 mm from the external heat exchange surface. The temperature sampling frequency is 10 Hz.
[0102] Non-aqueous low-temperature heat transfer media are used in A low-temperature siloxane or perfluoropolyether heat transfer fluid that remains pumpable around 40°C, is compatible with graphite and sealing materials, and has a sufficient flash point or inertness. The effective volume of the medium is 15–20 L, and the medium temperature is set before casting. 30±2℃, circulation flow rate is 10~15 L / min, cold source is The effective cooling capacity at 30℃ is 3-5 kW. The temperature of the mold heat exchange surface will reach... Pouring is permitted after the temperature has stabilized at 25±3℃ for at least 3 minutes.
[0103] The electromagnetic generation assembly employs a three-phase rotating magnetic field coil group, evenly distributed along the circumference of the mold cavity, with the effective height of the coils covering more than 80% of the mold cavity height; the equivalent radial gap between the inner edge of the coils and the outer wall of the mold is 10–25 mm. The measured magnetic induction intensity at the center of the mold cavity and at a position 0.7 times the center radius is used as calibration values to ensure that the uniformity deviation of the magnetic induction intensity within the effective operating area is no greater than ±15%. The designed operating point for the first solidification stage is 11±2 mT, 50 Hz.
[0104] Before casting, dry the mold cavity and gating channel at 100–150°C for 1–2 hours; then introduce an air stream with a dew point not exceeding [a certain value]. Dry nitrogen at 40°C is used for pre-purging for at least 5 minutes at a flow rate of 8–12 L / min; a protective flow rate of 5–10 L / min is maintained during pre-cooling and pouring. The lowest edge of the pouring nozzle is 30–50 mm above the maximum permissible liquid level of the low-temperature heat transfer medium.
[0105] Example 2: To differentiate the contributions of low-temperature heat transfer, electromagnetic effects, and staged thermal compensation, the following four operating conditions are preferred: Group A: Room temperature molds, no electromagnetic field, used to obtain conventional solidification references; Group B: Low-temperature mold, no electromagnetic field, used to evaluate the effect of low-temperature heat exchange alone; Group C: Room temperature mold, fixed parameters or staged electromagnetic field, used to evaluate individual electromagnetic effects and induced temperature rise of graphite mold; Group D: Cryogenic mold, staged electromagnetic field, first-stage electromagnetic unloading, second-stage heat exchange compensation and recovery with hysteresis, used to evaluate the complete closed-loop scheme.
[0106] Each group should be repeated at least three times, and the melt temperature, mold temperature, medium inlet and outlet temperatures, medium flow rate, electromagnetic parameters, stage switching time, peak thermal deviation, compensation trigger time, recovery time, and solidification time should be recorded. Microstructure characterization should include at least two of the following: average grain size, secondary dendrite spacing, average length or equivalent diameter of the iron-rich phase, aspect ratio of the iron-rich phase, and area fraction. Performance characterization may include at least one of the following: hardness, tensile strength, yield strength, elongation, electrical conductivity, and porosity.
[0107] When group D exhibits a smaller thermal deviation peak, a shorter thermal boundary recovery time, and a more uniform solidification structure compared to groups B and C, it can be used to demonstrate that graded compensation closed loop is not a simple parallel of low-temperature heat exchange and electromagnetic stirring.
[0108] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method of alloy cryo-electromagnetic solidification microstructure control, comprising: Applicable to casting molds equipped with heat exchangers and electromagnetic generators, including the following steps: Obtain the non-magnetic temperature curve of the casting mold, wherein the non-magnetic temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic environment. After the heat exchange device is turned on and the alloy melt is poured into the casting mold, the solidification state of the alloy and the temperature information of the casting mold are obtained in real time. The electromagnetic generator is controlled to operate based on the solidification state of the alloy. Simultaneously, the thermal deviation parameter at the corresponding moment is calculated based on the temperature information of the casting mold and the temperature curve without magnetic field. The electromagnetic generator and / or the heat exchange device are controlled to operate based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold.
2. The alloy cryogenic electromagnetic solidification microstructure management method of claim 1 wherein, The process of obtaining the non-magnetic temperature curve of the casting mold includes: For the same alloy composition, melt quality, mold structure, billet size, pre-cooling temperature and medium flow rate, at least three mold temperature curves are repeatedly collected without applying an electromagnetic field, and the average value, median value or statistical value after removing outliers is taken at each time step to form the magnetic field-free temperature curve.
3. The alloy cryo-electromagnetic solidification microstructure manipulation method of claim 1 wherein, The solidification state of the alloy includes a first solidification stage, a second solidification stage, and a third solidification stage. In the first solidification stage, the alloy melt is in a liquid state or is mainly liquid. In the second solidification stage, the alloy melt exhibits an increased solid content and a significant increase in apparent flow resistance. In the third solidification stage, the alloy melt is mainly solid.
4. The method for controlling the microstructure of alloys under low-temperature electromagnetic solidification according to claim 3, characterized in that, The control of the electromagnetic generator based on the solidification state of the alloy includes: When the alloy is in the first solidification stage, the electromagnetic generating device applies a first electromagnetic field to cause the melt to form a controlled circumferential, axial or combined flow. When the alloy is in the second solidification stage, the electromagnetic generating device applies a second electromagnetic field, wherein the second electromagnetic field is achieved by changing the first electromagnetic field through the following means: reducing the magnetic induction intensity or duty cycle, changing the frequency, or switching to intermittent or pulsed action. When the alloy is in the third solidification stage, the electromagnetic generator reduces or stops applying the electromagnetic field.
5. The method for controlling the microstructure of alloys under low-temperature electromagnetic solidification according to claim 1, characterized in that, The thermal deviation parameters calculated based on the temperature information of the casting mold and the non-magnetic field temperature curve at the corresponding time include: Based on the temperature information of the casting mold, the measured mold temperature curve during the electromagnetic field is obtained. The measured mold temperature curve during the electromagnetic field is aligned with the temperature curve without magnetic field in time to determine the thermal deviation parameter of the casting mold. The thermal deviation parameter includes the thermal deviation amount and / or the mold thermal deviation change rate.
6. The method for controlling the microstructure of alloys under low-temperature electromagnetic solidification according to claim 5, characterized in that, The step of controlling the operation of the electromagnetic generator and / or the heat exchanger based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold includes: When the thermal deviation of the casting mold reaches a first thermal deviation threshold and continues for a first preset time, or when the thermal deviation change rate of the casting mold reaches a first change rate threshold and continues for the first preset time, a first-level compensation strategy is executed, wherein the first-level compensation strategy includes at least one of reducing the magnetic induction intensity of the electromagnetic field, reducing the frequency, reducing the duty cycle, and pausing the application of the electromagnetic field. Within a second preset time after the execution of the first-level compensation strategy, if the thermal deviation of the casting mold does not decrease to below the first recovery threshold, or if the thermal deviation change rate of the casting mold is still higher than the recovery change rate threshold, a second-level compensation strategy is executed. The second-level compensation strategy includes at least one of increasing the circulation flow rate of the non-aqueous low-temperature heat transfer medium, increasing the cooling power, reducing the set temperature of the non-aqueous low-temperature heat transfer medium, and extending the electromagnetic pause time. When the thermal deviation of the mold decreases to below the second recovery threshold and continues for a third preset time, the electromagnetic parameters allowed in the current solidification stage are restored according to a preset slope. When the alloy melt reaches the preset solidification termination state, the applied electromagnetic field is reduced or stopped, and heat exchange with the casting mold continues through the cooling medium until a solidified alloy billet is obtained.
7. A device for controlling the microstructure of low-temperature electromagnetic solidification of alloys, characterized in that, include; First parameter acquisition module: used to acquire the non-magnetic temperature curve of the casting mold, wherein the non-magnetic temperature curve is the temperature change curve of the casting mold under the influence of the internal alloy temperature change and the cooling effect of the external heat exchange device in a non-magnetic environment. The second parameter acquisition module is used to acquire the solidification state of the alloy and the temperature information of the casting mold in real time after the heat exchange device is turned on and the alloy melt is poured into the casting mold. Control and compensation module: used to control the operation of the electromagnetic generator based on the solidification state of the alloy; at the same time, based on the temperature information of the casting mold and the temperature curve without magnetic field, calculate the thermal deviation parameter at the corresponding time, and control the operation of the electromagnetic generator and / or the heat exchange device based on the thermal deviation parameter to reduce the thermal deviation parameter until it is no greater than a threshold.
8. An electronic device, characterized in that, include: processor; A memory storing computer instructions for causing a processor to perform the method according to any one of claims 1 to 6.
9. A computer-readable storage medium, characterized in that, The device stores computer instructions for implementing the method according to any one of claims 1 to 6.
10. A system for controlling the microstructure of an alloy under low-temperature electromagnetic solidification, characterized in that, The method for controlling the microstructure of alloys under low-temperature electromagnetic solidification as described in any one of claims 1-6 includes: A heat exchange device having a heat exchange chamber for circulating cooling medium; A casting mold, wherein the casting mold is installed inside the heat exchange cavity; An electromagnetic generator is installed inside the heat exchange cavity and arranged around the casting mold, and is used to generate an electromagnetic field that acts on the casting mold. A status acquisition component, the status acquisition component having a detection end for detecting the melt temperature, the casting mold temperature and / or the cooling medium temperature; The controller is electrically connected to the electromagnetic generator and the state acquisition component, and is used to control the operation of the electromagnetic generator and / or the heat exchange device according to the solidification state of the alloy and the thermal deviation parameters of the casting mold.