A composition for metal injection molded gears, a gear, and a method for preparing the gear.

By combining ultrafine near-spherical iron-nickel-based metal powder with a high proportion of polyoxymethylene binder, the problem of insufficient tooth tip filling in metal injection molded gears is solved, achieving high precision, smoothness, and high density of the gears, meeting the requirements of precision transmission devices.

CN123102984APending Publication Date: 2026-11-17SHENZHEN MIM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611283796.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing metal injection molding technology, insufficient filling of complex tooth profiles and tooth tips leads to low gear accuracy, making it difficult to meet the requirements of precision transmission devices.

Method used

By employing the synergistic combination of ultrafine near-spherical iron-nickel-based metal powder and a high-proportion polyoxymethylene binder system, the filling capacity of the feed melt in complex tooth-shaped mold cavities and the green blank shape retention capacity are improved. By optimizing the particle size distribution and binder ratio, combined with carburizing or carbonitriding heat treatment, the precision, surface finish and sintering density of the gears are enhanced.

Benefits of technology

It achieves high precision (grade 8), high surface finish (Ra≤0.6μm) and high sintering density (≥7.65g/cm³) for gears, meeting the service requirements of heavy-duty and wear-resistant transmission conditions. The tooth profile accuracy is improved by 1 to 2 grades, and the surface hardness reaches HRC 45 to 55.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102984A_ABST
    Figure CN123102984A_ABST
Patent Text Reader

Abstract

This invention discloses a composition for metal injection molded gears, a gear, and a method for preparing the gear. The composition comprises metal powder and a binder system, with the binder system comprising 44% by volume. The metal powder is an iron-nickel-based alloy powder, with a content of [missing information] and a balance of [missing information]. The particle size distribution of the metal powder is [missing information] and its morphology is nearly spherical. The composition exhibits good flowability, full filling of the gear teeth without underfilling, and the resulting gear achieves a precision grade of 8 (GB / T10095.1-2022). The tooth surface roughness is [missing information], the sintering density is [missing information], and the surface hardness after carburizing or carbonitriding heat treatment is HRC45-55. The preparation method includes material preparation, heating and premixing, melt mixing, granulation, injection molding, debinding, and sintering steps. This invention overcomes the technical bottleneck of conventional MIM gear precision grades of 9-12 and is suitable for the large-scale stable manufacturing of precision transmission gears.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of powder metallurgy and metal injection molding technology, and specifically relates to a composition for metal injection molding of gears, a gear made from the composition, and a method for preparing the gear. Background Technology

[0002] Metal injection molding (MIM) technology is widely used in gear manufacturing due to its advantages such as high material utilization, near-net-shape forming of complex tooth profiles, and suitability for mass production. However, for parts with complex tooth structures, such as micro-module gears, helical gears, and spiral gears, the elongated mold cavity at the tooth tip and the complex melt flow path make it prone to molding defects such as incomplete filling and short shots during the feeding process. These defects directly affect the tooth profile accuracy and surface consistency of the final gear. Furthermore, due to limitations in the matching relationship between feed flowability, powder loading, and green blank shape retention, the manufactured MIM gears still struggle to meet the requirements of precision transmission devices in terms of tooth profile accuracy and surface quality.

[0003] Therefore, how to solve the problem of low gear accuracy caused by insufficient filling of complex tooth profiles and tooth tips in MIM process is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0004] In order to overcome the shortcomings and deficiencies of the existing technology, the present invention aims to provide a composition, a gear, and a method for preparing a metal injection molded gear. By synergistically combining ultrafine near-spherical iron-nickel-based metal powder with a high proportion of polyoxymethylene binder system, the filling capacity of the feed melt in the complex tooth cavity and the green blank shape retention capacity are improved, thereby simultaneously improving the tooth profile accuracy, tooth surface finish and sintering density of the gear.

[0005] This invention is achieved through the following technical solution:

[0006] In a first aspect, this application provides a composition for metal injection molded gears, comprising metal powder and a binder system, wherein the binder system comprises 42% to 46% by volume in the composition; the metal powder is an iron-nickel-based metal powder, wherein the content of Ni is 3.5 to 4.5 wt%, and the balance is Fe; the particle size distribution of the metal powder is D90 ≤ 8 μm, and the particle morphology is nearly spherical.

[0007] In the above technical solution, with a binder system of 42%–46% by volume, the corresponding volume loading of metal powder is 54%–58%. This loading range allows the feed melt to maintain a low injection viscosity while possessing sufficient powder solid content, which is beneficial for the complete filling of complex tooth cavities, especially the narrow and elongated tooth tips. Ultrafine near-spherical iron-nickel-based metal powder has the characteristics of high bulk density and good flowability. A particle size of D90≤8μm significantly reduces the microscopic undulations of the tooth surface after sintering, and the near-spherical morphology reduces mechanical interlocking and flow resistance between particles. Both factors together ensure full filling of the tooth tips without underfilling. Ni element is dissolved in the iron matrix in the range of 3.5–4.5wt%, improving the strength, toughness, and hardenability of the sintered gear, providing a basis for subsequent carburizing or carbonitriding surface strengthening.

[0008] Preferably, the binder system comprises 44% by volume in the composition. This loading amount corresponds to a metal powder volume loading of 56%, which, within the scope of this application, achieves optimal overall performance in terms of melt flowability, green shape retention, tooth tip filling effect, and gear dimensional stability.

[0009] Preferably, the binder system comprises the following components in parts by weight: 80-85 parts polyoxymethylene, 4-7 parts high-density polyethylene, 3-6 parts polypropylene, 3-5 parts polyamide internal lubricant, 1-3 parts zinc stearate, 1-2 parts ammonium sulfate, and 0.5-1.0 parts silane coupling agent. In the above technical solution, polyoxymethylene serves as the main binder, providing green strength and injection molding properties; high-density polyethylene serves as the skeleton component, maintaining the shape of the green body during catalytic degreasing; polypropylene regulates melt flow and improves green toughness; the polyamide internal lubricant synergistically combines with zinc stearate to provide dynamic lubrication during melt mixing and injection filling, improving demolding performance and reducing injection internal stress; ammonium sulfate decomposes at high temperatures, reducing coking and carbonization of polymer materials and mitigating the adverse effects of residual carbon on the metal matrix; and the silane coupling agent improves the interfacial bonding between the metal powder and the binder, enhancing mixing uniformity.

[0010] Preferably, the polyoxymethylene (POM) content is 82-85 parts by weight. Increasing the POM content to 80-85 parts (based on the total weight of the binder system) is higher than the 55-65 parts POM level in conventional MIM feedstocks, significantly enhancing the bending strength and dimensional stability of the green body, and making it less prone to deformation during transport and placement before degreasing and sintering. Preferably, the polyamide internal lubricant is a copolymer polyamide with a melting point of 140-180°C, and its content is 4 parts by weight; this melting point range matches the processing temperature of POM, allowing it to disperse uniformly and migrate to the feed surface during melt mixing, forming a synergistic lubrication system with zinc stearate.

[0011] Preferably, the particle size distribution of the metal powder is: D10 of 2.2–2.8 μm, D50 of 5.0–6.0 μm, and D90 ≤ 8 μm; the near-spherical shape refers to a particle sphericity ≥ 0.90, or a particle aspect ratio not greater than 1.5. The above particle size distribution takes into account both the sintering activity of fine powder and the particle size distribution and packing density. The quantitative definition of the near-spherical morphology ensures that the powder flowability index is repeatable and detectable.

[0012] Secondly, this application provides a metal injection-molded gear, which is made of iron-nickel-based metal powder with a Ni content of 3.5–4.5 wt% and the balance being Fe; the gear has a sintered density ≥7.65 g / cm³, a tooth surface roughness Ra ≤0.6 μm, and a gear precision grade not lower than grade 8 (GB / T 10095.1—2022); the gear has a surface hardness of HRC 45–55 after carburizing or carbonitriding heat treatment; the gear is made from a composition of metal powder and binder system through injection molding, debinding, and sintering. This gear, characterized by its measurable density, roughness, precision, and hardness performance, possesses comprehensive properties of high density, high surface finish, high precision, and heat-treatable strengthening, meeting the service requirements of heavy-duty and wear-resistant transmission conditions.

[0013] Thirdly, this application provides a method for preparing the aforementioned metal injection molded gear, including material preparation, heating and premixing, melt mixing, granulation, injection molding, degreasing, and sintering steps. In the above technical solution, the metal powder is first heated to above the melting point of the binder before adding the binder components for premixing, so that the binder forms a preliminary coating layer on the surface of the powder particles, and then uniform dispersion at the microscale is achieved through melt mixing; the process is compact, the process window is wide, and it is suitable for large-scale stable production.

[0014] Compared with related technologies, this application has the following advantages: First, the synergistic effect of ultrafine near-spherical metal powder (D90≤8μm) and a binder system of 42%–46% by volume ensures that the feed melt fully fills the complex tooth cavity, with no underfill at the tooth tip. Second, the ultrafine particle size significantly reduces the micro-undulations of the tooth surface after sintering, achieving a surface roughness of Ra≤0.6μm, which is superior to the Ra level of conventional MIM gears (Ra 0.8–1.6μm). Third, the high activity and bulk density of the fine powder promote sintering densification, resulting in a gear sintering density of over 7.65g / cm³, higher than the 6.8–7.2g / cm³ level of conventional MIM gears. Fourth, the Ni content of 3.5–4.5wt%, combined with subsequent carburizing or carbonitriding heat treatment, achieves a gear surface hardness of HRC 45–55, higher than the HRC of conventional MIM gears. Fifth, the unidirectional linear shrinkage rate of the composition is controlled at 20.5% to 23.5%, and the shrinkage behavior is isotropic and highly consistent, providing a stable design basis for mold shrinkage compensation. Taking all these effects into account, the precision grade of the manufactured gears is improved from the conventional MIM gear grade 9-12 to grade 8 (GB / T 10095.1—2022). Attached Figure Description

[0015] The present invention will be further described with reference to the accompanying drawings, but the embodiments in the drawings do not constitute any limitation on the present invention. For those skilled in the art, other drawings can be obtained based on the following drawings without creative effort.

[0016] Figure 1 This is a process flow diagram of a gear manufacturing method according to an embodiment of the present invention; Figure 2 Precision grade diagram for gears manufactured for commercially available general-purpose feeders; Figure 3 This is a diagram showing the precision grade of a gear made from the composition in one embodiment of the present invention; Figure 4 This is a comparison diagram of the surface roughness of the composition in one embodiment of the present invention and the gear made from a commercially available general feedstock; Figure 5 This is a micrograph of the injection-molded gear tooth tip filling state according to an embodiment of the present invention. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0018] In this embodiment, the composition for metal injection molded gears includes metal powder and a binder system. The binder system comprises 42% to 46% by volume in the composition, i.e., the volume loading of the metal powder is 54% to 58%. Within this volume percentage range, the feed melt has both a low injection viscosity, which is beneficial for the complete filling of complex tooth tips such as micro-module gears and helical gears, and sufficient powder solid content, making the sintering shrinkage rate stable and controllable. In this embodiment, the volume percentage of the binder system is preferably 44%, corresponding to a metal powder volume loading of 56%.

[0019] The metal powder is an iron-nickel-based metal powder, wherein the Ni content is 3.5–4.5 wt%, and the balance is Fe. The iron-nickel-based metal powder can be a pre-alloyed powder (i.e., an alloy powder obtained by atomizing an iron-nickel alloy melt) or a mixed powder made by mixing iron powder and nickel powder in a specific ratio; both powder forms can achieve the technical solution of this application. The role of Ni is to improve the strength, toughness, and hardenability of the gear, enabling it to undergo heat treatment for strengthening. When the Ni content is below 3.5 wt%, the hardenability improvement is insufficient, and the hardness after heat treatment is difficult to reach HRC 45 or higher; when the Ni content is above 4.5 wt%, the raw material cost increases while the performance gain tends to saturate.

[0020] The metal powder has a particle size distribution of D90 ≤ 8 μm and a near-spherical morphology; preferably, the particle size distribution is D10 of 2.2–2.8 μm, D50 of 5.0–6.0 μm, and D90 ≤ 8 μm. In the above technical solution, the ultrafine particle size significantly reduces the microscopic undulations of the tooth surface after sintering, making the tooth surface roughness Ra ≤ 0.6 μm; the near-spherical particles have a high packing density and good flowability, reducing mechanical interlocking and flow resistance between particles, which is beneficial to the complete filling of complex tooth shapes; the fine powder has a large specific surface area and high sintering activity, promoting sintering densification, making the gear sintering density reach 7.65 g / cm³ or higher. In this embodiment, "near-spherical" is defined in a quantifiable way: the sphericity of the particles measured by dynamic image analysis is ≥ 0.90, or the aspect ratio of the particles is not greater than 1.5.

[0021] The adhesive system comprises the following components in parts by weight: 80-85 parts polyoxymethylene (POM), 4-7 parts high-density polyethylene (HDPE), 3-6 parts polypropylene (PP), 3-5 parts polyamide internal lubricant, 1-3 parts zinc stearate, 1-2 parts ammonium sulfate, and 0.5-1.0 parts silane coupling agent. Wherein: Polyoxymethylene (POM) serves as the primary binder, providing green strength and injection molding properties. The POM content is 80-85 parts by weight, higher than the typical 55-65 parts by weight in conventional MIM feedstocks. In this technical solution, POM exhibits high strength and high crystallinity; the increased content significantly enhances the flexural strength and dimensional stability of the green body, making it less prone to deformation during transport and placement before debinding and sintering, thus ensuring the high precision of the final gear. In a preferred embodiment, the POM content is 82-85 parts by weight.

[0022] High-density polyethylene (HDPE) acts as a skeletal agent, partially retained during catalytic degreasing to maintain the shape of the green body and improve dimensional stability. Polypropylene (PP) is used to adjust the melt flowability of the composition and improve the toughness of the green body.

[0023] A polyamide internal lubricant is synergistically compounded with zinc stearate as a lubrication and release system. In this embodiment, the polyamide internal lubricant is a copolyamide with a melting point between 140 and 180°C (commercially available product codes include, but are not limited to, low-to-medium melting point copolyamides such as PA42), which can melt and disperse uniformly at the polyoxymethylene (POM) processing temperature. The polyamide internal lubricant improves the melt flowability of the composition, while zinc stearate has surface activity, auxiliary lubrication, and release properties. The synergistic effect of the two results in a composition with superior dynamic lubrication and release performance during injection molding, reducing internal stress and release deformation during injection. In a preferred embodiment, the polyamide internal lubricant is 4 parts by weight. In practice, any copolyamide product that meets the above melting point range and can be uniformly dispersed in the POM matrix can be used.

[0024] Ammonium sulfate decomposes at high temperatures to generate sulfur-containing gases and ammonia, reducing coking and carbonization of polymer materials and mitigating the adverse effects of residual carbon on the mechanical properties of the metal matrix. Silane coupling agents improve the interfacial bonding between metal powder and binder systems, enhancing mixing uniformity.

[0025] (II) Gear Manufacturing Methods In this embodiment, the method for manufacturing metal injection molded gears includes the following steps: (1) Material preparation: Weigh the iron-nickel based metal powder (Ni content 3.5-4.5wt%, balance Fe, particle size distribution D90≤8μm, particle morphology nearly spherical) and each component of the binder system according to the formula, and set aside. When using mixed powder, weigh the iron powder and nickel powder separately according to the formula and mix them evenly in advance; when using pre-alloyed powder, directly weigh the iron-nickel pre-alloyed powder of the corresponding composition.

[0026] (2) Heating and premixing: The metal powder is added to a high-speed mixer or internal mixer preheated to 160-200℃ and preheated to dry it to remove the moisture and gas adsorbed on the powder surface; then the components of the binder system are added, and solid preliminary mixing is carried out when the powder temperature reaches above the melting point of the binder, so that the binder initially coats the surface of the metal powder particles. The premixing time is 10-30 min, and the rotation speed is 10-20 r / min to obtain the premixed material.

[0027] (3) Melt mixing: The premixed materials are mixed in a molten state at 160-200℃ for 1-4 hours at a rotation speed of 20-40 r / min. During the melt mixing process, the binder system completely melts and uniformly coats the metal powder particles. The shearing action fully disperses the powder agglomerates, and each component achieves uniform dispersion at the microscale. In the above technical solution, the degree of mixing uniformity directly affects the rheological consistency and sintering shrinkage uniformity of the composition, and is one of the key processes that determine the final gear precision.

[0028] (4) Granulation: After the mixing is completed, the uniform paste mixture is discharged while hot. After being cooled by air or water, it is crushed and granulated by an extrusion granulator or a crusher to obtain a granular composition with a particle diameter of 2-5 mm, which is convenient for feeding and plasticizing of the injection molding machine.

[0029] (5) Injection Molding: The granular composition is injection molded at an injection temperature of 180–200°C and an injection pressure of 80–100 MPa to obtain a green body. In one embodiment, a twin-screw electric injection molding machine is used for injection molding. The twin-screw electric injection molding machine has high metering accuracy and fast response speed, which is compatible with the rheological properties of the composition of this application. Combined with the good flowability brought by the 42%–46% binder volume percentage, it can achieve stable filling of complex tooth-shaped mold cavities, and the tooth tips are fully filled without underfilling. It should be noted that the injection molding equipment is not limited to a twin-screw electric injection molding machine. Other injection molding equipment that can stably control the injection temperature and injection pressure can also achieve the technical solution of this application.

[0030] (6) Degreasing: The green body is degreased using nitric acid with a mass concentration of ≥95% at a degreasing temperature of 100-115℃ for 3.5-4.5 hours. Polyoxymethylene rapidly depolymerizes into formaldehyde gas in a nitric acid catalytic atmosphere, resulting in high degreasing efficiency and reducing the likelihood of cracking of the green body.

[0031] (7) Sintering: The degreased blank is sintered under argon protection at a temperature of 1280-1320℃ and a holding time of 3.5-4.5h to obtain metal injection molded gear.

[0032] (8) Heat treatment: In one embodiment, the sintered gear is subjected to carburizing heat treatment at a temperature of 880°C for 2 hours, followed by oil quenching and tempering at 180°C. After heat treatment, the surface hardness of the gear reaches HRC 45-55. In another embodiment, carbonitriding heat treatment is used to strengthen the surface of the gear. The carbonitriding temperature is 820-860°C for 2-4 hours, followed by oil quenching and tempering at 160-200°C.

[0033] In the above technical solution, ultrafine near-spherical metal powder forms a low-viscosity, high-filling solid-liquid mixture system in a molten binder. During the injection filling stage, the near-spherical particles exhibit low rolling friction and good fluidity. Combined with the matrix strength provided by the high proportion of polyoxymethylene binder, the melt can smoothly fill narrow mold cavities such as tooth tips, avoiding spraying and short shots. During the debinding stage, the high-content polyoxymethylene rapidly depolymerizes under nitric acid catalysis, while the high-density polyethylene skeleton is retained and supports the preform, reducing collapse and deformation. During the sintering stage, the ultrafine powder has a large specific surface area and high sintering activity, achieving densification at relatively low temperatures. The uniform distribution of Ni element in the iron matrix improves hardenability, enabling the gear to obtain a uniform hardened layer during subsequent carburizing or carbonitriding. These steps work together to simultaneously improve the gear's tooth profile accuracy, tooth surface finish, density, and surface hardness.

[0034] (III) Examples The present application will be further illustrated below through specific embodiments and comparative examples. Embodiment 1 is a preferred embodiment, while Embodiments 2 and 3 respectively cover values ​​near the endpoints of the binder volume percentage and process parameter ranges; Comparative Examples 1 to 4 each change a key variable to illustrate the correspondence between each technical feature and its technical effect.

[0035] Example 1 Metal powder: Iron-nickel based pre-alloyed powder, with Fe balance (96wt%) and Ni 4.0wt%; powder particle size distribution is D10=2.5μm, D50=5.5μm, D90=7.5μm; particle morphology is nearly spherical, with sphericity of 0.95 and aspect ratio of 1.2.

[0036] The binder system composition is as follows: 82 parts by weight of polyoxymethylene, 5 parts by weight of high-density polyethylene, 4 parts by weight of polypropylene, 4 parts by weight of copolyamide (melting point about 150℃, trade code PA42), 2 parts by weight of zinc stearate, 1.5 parts by weight of ammonium sulfate, and 0.5 parts by weight of silane coupling agent.

[0037] The metal powder and binder system were fed at a volume ratio of 56%:44% (corresponding to a weight ratio of approximately 88%:12%). The metal powder was added to a mixer preheated to 180°C and dried. Then, the binder system components were added and premixed for 20 minutes at a speed of 15 r / min. The mixture was then melt-mixed at 180°C and 30 r / min for 1 hour. After cooling, the mixture was extruded and granulated to obtain a granular composition with a particle diameter of 2–5 mm.

[0038] The granular composition was injection molded on a twin-screw electric injection molding machine at a nozzle temperature of 185℃ and an injection pressure of 90MPa to obtain a green body. It was degreased by catalytic degreasing with nitric acid of ≥95% mass concentration at a temperature of 100℃ for 4 hours. It was then sintered at 1300℃ under argon protection for 4 hours. It underwent carburizing heat treatment at 880℃ for 2 hours, followed by oil quenching and tempering at 180℃.

[0039] Performance test results: The actual gear has an accuracy grade of 8 (GB / T 10095.1—2022); the tooth surface roughness Ra is 0.55μm; the sintering density is 7.68g / cm³; the unidirectional linear shrinkage rate is 22.0%; the tooth tip is fully filled without any missing filling; and the surface hardness after heat treatment is HRC 52.

[0040] Example 2 Metal powder: Iron-nickel based pre-alloyed powder, with Fe balance (96.2 wt%) and Ni 3.8 wt%; the powder particle size distribution is D10=2.8 μm, D50=6.0 μm, and D90=7.8 μm; the particle morphology is nearly spherical with a sphericity of 0.92 and an aspect ratio of 1.4.

[0041] The binder system composition is as follows: 80 parts by weight of polyoxymethylene, 6 parts by weight of high-density polyethylene, 5 parts by weight of polypropylene, 3 parts by weight of copolyamide (melting point about 150℃, trade code PA42), 2.5 parts by weight of zinc stearate, 2 parts by weight of ammonium sulfate, and 0.5 parts by weight of silane coupling agent.

[0042] The metal powder and binder system were fed at a volume ratio of 58%:42%. The metal powder was added to a mixer preheated to 170°C and dried. Then, the components of the binder system were added and premixed for 25 minutes at a speed of 15 r / min. The mixture was then melt-mixed at 185°C and 25 r / min for 1.5 hours. After cooling, the mixture was extruded and granulated to obtain a granular composition.

[0043] The granular composition was injection molded on a twin-screw electric injection molding machine at a nozzle temperature of 190°C and an injection pressure of 85 MPa. Degreasing was carried out using nitric acid with a mass concentration of ≥95% at a temperature of 110°C for 3.5 hours. Sintering was performed at 1280°C under argon protection for 4.5 hours. Carburizing heat treatment was carried out at 880°C for 2 hours, followed by oil quenching and tempering at 180°C.

[0044] Performance test results: The actual gear has an accuracy grade of 8 (GB / T 10095.1—2022); the tooth surface roughness Ra is 0.58μm; the sintering density is 7.65g / cm³; the unidirectional linear shrinkage rate is 21.8%; the tooth tip is fully filled without any missing filling; and the surface hardness after heat treatment is HRC 48.

[0045] Example 3 Metal powder: a mixture of iron and nickel powder, with Fe balance (95.5wt%) and Ni 4.5wt%; the particle size distribution of the mixed powder is D10=2.2μm, D50=5.0μm, and D90=7.2μm; the particle morphology is nearly spherical, with a sphericity of 0.96 and an aspect ratio of 1.1.

[0046] The binder system composition is as follows: 85 parts by weight of polyoxymethylene, 4 parts by weight of high-density polyethylene, 3 parts by weight of polypropylene, 5 parts by weight of copolyamide (melting point about 150℃, trade code PA42), 1 part by weight of zinc stearate, 1 part by weight of ammonium sulfate, and 1.0 part by weight of silane coupling agent.

[0047] The metal powder and binder system were fed at a volume ratio of 54%:46% (corresponding to a weight ratio of approximately 87%:13%). Iron and nickel powders were first mixed in a V-type mixer for 30 minutes to obtain an iron-nickel-based mixed powder. This powder was then added to a Banbury mixer preheated to 190°C. After preheating and drying, the binder system components were added and premixed for 15 minutes at a speed of 20 r / min. The mixture was then melt-mixed at 190°C and 35 r / min for 2.5 hours. After cooling, the mixture was extruded and granulated to obtain a granular composition.

[0048] The granular composition was injection molded on a twin-screw electric injection molding machine at a nozzle temperature of 195℃ and an injection pressure of 95MPa. Degreasing was carried out using nitric acid with a mass concentration of ≥95% at a temperature of 115℃ for 4.5 hours. Sintering was performed at 1320℃ under argon protection for 3.5 hours. Carburizing heat treatment was carried out at 880℃ for 2 hours, followed by oil quenching and tempering at 180℃.

[0049] Performance test results: The actual gear has an accuracy grade of 8 (GB / T 10095.1—2022); the tooth surface roughness Ra is 0.50μm; the sintering density is 7.70g / cm³; the unidirectional linear shrinkage rate is 22.3%; the tooth tip is fully filled without any missing filling; and the surface hardness after heat treatment is HRC 54.

[0050] Comparative Example 1 The difference from Example 1 is that the metal powder used is a conventional iron-nickel-based pre-alloyed powder with a particle size of D90=15μm and D50=11μm, while the other components, proportions and process parameters are the same as in Example 1.

[0051] Performance test results: The actual gear has a precision grade of 10; the tooth surface roughness Ra is 1.15μm; the sintering density is 7.42g / cm³; slight under-filling occurs at the tooth tip; the surface hardness after heat treatment is HRC 47. The results indicate that ultrafine powder with D90≤8μm is the key factor in obtaining low tooth surface roughness and high sintering density.

[0052] Comparative Example 2 The difference from Example 1 is that the polyoxymethylene content in the adhesive system is changed to 60 parts by weight, and the high-density polyethylene is adjusted to 15 parts by weight accordingly. The remaining components, proportions and process parameters are the same as in Example 1.

[0053] Performance test results: The actual gear has a precision grade of 10; the tooth surface roughness Ra is 0.85μm; the sintering density is 7.55g / cm³; slight deformation occurred during the transport of the green body, and the tooth profile and direction deviation increased; the surface hardness after heat treatment is HRC 50. The results indicate that a high content of 80-85 parts of polyoxymethylene has a significant effect on the green body strength and the final gear precision.

[0054] Comparative Example 3 The difference from Example 1 is that the metal powder used is a water-atomized irregular morphology iron powder and nickel powder mixed powder (sphericity about 0.75, aspect ratio about 2.0), and the particle size distribution is adjusted to D90=7.5μm, D50=5.5μm (close to the particle size distribution of Example 1). The remaining components, proportions and process parameters are the same as those in Example 1.

[0055] Performance test results: The actual gear has a precision grade of 9; a tooth surface roughness Ra of 0.78 μm; a sintering density of 7.60 g / cm³; an injection pressure of over 110 MPa is required to fill the tooth tip cavity, and localized sticking occurs during green body demolding; the surface hardness after heat treatment is HRC 51. The results indicate that, under similar particle size conditions, near-spherical morphology significantly improves melt flowability, filling capacity, and demolding performance.

[0056] Comparative Example 4 The difference from Example 1 is that the Ni content in the metal powder is changed to 2.0 wt%, with the balance being Fe, while the remaining components, proportions, and process parameters are the same as in Example 1.

[0057] Performance test results: The gear precision and tooth surface roughness were similar to those of Example 1 (grade 8, Ra 0.58 μm), and the sintering density was 7.66 g / cm³; however, the surface hardness after carburizing heat treatment was only HRC 38, the depth of the hardened layer in the tooth was insufficient, and the hardenability and hardenability were significantly reduced. The results indicate that a Ni content of 3.5–4.5 wt% is a necessary condition for obtaining a surface hardness of HRC 45–55 for gears.

[0058] The performance test results of Examples 1-3 and Comparative Examples 1-4 are shown in the table below:

[0059] As can be seen from the table above, the gears manufactured using the composition and preparation method of this application are significantly superior to the comparative examples in terms of tooth profile accuracy, tooth surface roughness, sintering density, and surface hardness after heat treatment. The gears of Examples 1 to 3 all achieve an accuracy grade of 8 (GB / T 10095.1—2022), which is 1 to 2 grades higher than the 10 grades of Comparative Examples 1 and 2 and the 9 grades of Comparative Example 3; the tooth surface roughness Ra is 0.50 to 0.58 μm, which is significantly better than the 0.8 to 1.6 μm level of each comparative example and conventional MIM gears; the sintering density reaches 7.65 to 7.70 g / cm³, which is higher than the 6.8 to 7.2 g / cm³ level of conventional MIM gears; and the surface hardness after heat treatment reaches HRC 48 to 54, which is higher than the HRC 20 to 35 level of conventional MIM gears. Comparative Examples 1-4, which each changed only one variable, showed a performance decline, demonstrating that the four technical features—ultrafine particle size, high polyoxymethylene content, near-spherical morphology, and specific Ni content—each play an irreplaceable role in the technical solution of this application, jointly supporting the comprehensive technical effect of 8-level precision.

[0060] The above description is merely a preferred embodiment of this application and is not intended to limit the scope of this application. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the protection scope of this application. Therefore, the protection scope of this application should be determined by the scope of the claims. The content of this specification should not be construed as a limitation of this application.

Claims

1. A composition for metal injection molded gears, characterized in that, The composition includes a metal powder and a binder system, wherein the binder system comprises 42% to 46% by volume in the composition; the metal powder is an iron-nickel-based metal powder, wherein the Ni content is 3.5 to 4.5 wt% and the balance is Fe; the particle size distribution of the metal powder is D90 ≤ 8 μm, and the particle morphology of the metal powder is nearly spherical.

2. The composition for metal injection molded gears according to claim 1, characterized in that, The binder system comprises 44% by volume in the composition.

3. The composition for metal injection molded gears according to claim 1, characterized in that, The adhesive system comprises the following components in parts by weight: 80-85 parts polyoxymethylene, 4-7 parts high-density polyethylene, 3-6 parts polypropylene, 3-5 parts polyamide internal lubricant, 1-3 parts zinc stearate, 1-2 parts ammonium sulfate, and 0.5-1.0 parts silane coupling agent.

4. The composition for metal injection molded gears according to claim 3, characterized in that, The polyoxymethylene is in the form of 82-85 parts by weight; the polyamide internal lubricant is a copolymer polyamide with a melting point of 140-180℃, and the polyamide internal lubricant is in the form of 4 parts by weight.

5. The composition for metal injection molded gears according to claim 1, characterized in that, The particle size distribution of the metal powder is as follows: D10 is 2.2-2.8 μm, D50 is 5.0-6.0 μm, and D90 is ≤8 μm; the near-spherical shape refers to a particle sphericity ≥0.90 or a particle aspect ratio not greater than 1.

5.

6. A metal injection-molded gear, characterized in that, The gear is made of iron-nickel-based metal powder with a Ni content of 3.5–4.5 wt% and the balance being Fe. The sintered density of the gear is ≥7.65 g / cm³, the surface roughness of the tooth surface Ra is ≤0.6 μm, and the gear accuracy grade is not lower than grade 8 (GB / T 10095.1—2022). The surface hardness of the gear after carburizing or carbonitriding heat treatment is HRC 45–55. The gear is made by injection molding, debinding, and sintering of a composition of metal powder and binder system.

7. A method for manufacturing a metal injection molded gear, characterized in that, Includes the following steps: (1) Weigh the iron-nickel-based metal powder and each component of the binder system according to the ratio and set aside; the content of Ni in the iron-nickel-based metal powder is 3.5 to 4.5 wt%, and the balance is Fe. The particle size distribution of the metal powder is D90≤8μm and the particle morphology is nearly spherical. (2) Heat the metal powder to 160-200°C, add each component of the binder system and premix, so that the binder system initially coats the surface of the metal powder particles to obtain a premixed material; (3) The premixed material is melt-mixed at 160-200°C; (4) After cooling, granulation is performed to obtain a granular composition; (5) The granular composition is injection molded to obtain a green body; (6) Degrease the green body; (7) The degreased blank is sintered to obtain the metal injection molded gear.

8. The preparation method according to claim 6, characterized in that, In step (2), the premixing time is 10-30 min and the rotation speed is 10-20 r / min; in step (3), the melt mixing time is 1-4 h and the rotation speed is 20-40 r / min.

9. The preparation method according to claim 7, characterized in that, In step (4), the particle diameter of the granular composition is 2-5 mm; in step (5), the injection temperature is 180-200℃ and the injection pressure is 80-100 MPa.

10. The preparation method according to claim 7, characterized in that, In step (6), the degreasing is carried out using nitric acid with a mass concentration of ≥95% as a catalyst, the degreasing temperature is 100-115℃, and the degreasing time is 3.5-4.5h; in step (7), the sintering is carried out under argon protection, the sintering temperature is 1280-1320℃, and the holding time is 3.5-4.5h; after sintering, the gear is subjected to carburizing heat treatment or carbonitriding heat treatment, the carburizing temperature of the carburizing heat treatment is 880℃, the holding time is 2h, oil quenching is performed, and tempering is performed at 180℃.