A method and equipment for continuous preparation of high-purity rhenium granules from high-purity rhenium powder.
By employing a continuous closed-loop process and multi-temperature gradient heating sintering, the problems of complex processes, impurity introduction, and high energy consumption in the preparation of high-purity rhenium particles have been solved, achieving the preparation of high-purity and highly consistent rhenium particles to meet the needs of high-end applications.
Patent Information
- Application Number
- CN202611472260.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing high-purity rhenium granule preparation processes are complex, have long production cycles, high risks of impurity introduction, high energy consumption, fragmented equipment, and poor product consistency, making it difficult to meet the ultra-high purity requirements of high-end applications.
Employing a continuous, closed-loop process, the process seamlessly integrates injection molding, gradient sintering, and precision cutting. High-purity binders and multi-temperature gradient sintering are used to achieve integrated manufacturing of high-purity rhenium powder into high-purity rhenium granules, avoiding the introduction of impurities and inefficiency.
It has achieved efficient preparation of high-purity rhenium granules with a purity of over 99.999% and a total impurity element content of less than 10 ppm. The product has good consistency, the production cycle has been shortened by more than 40%, energy consumption and equipment investment have been reduced, and the requirements of high-end fields such as aerospace have been met.
Smart Images

Figure CN123103002A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of rhenium material preparation methods, and particularly to a method and equipment for the continuous preparation of high-purity rhenium granules from high-purity rhenium powder. Background Technology
[0002] Rhenium is a rare refractory metal with excellent high-temperature strength, creep resistance, and corrosion resistance, making it widely used in high-end fields such as aerospace, electronics, and petrochemicals. High-purity rhenium granules are crucial raw materials for the preparation of single-crystal superalloys and electronic devices; their purity and quality directly affect the performance of the final products. However, current processes for preparing high-purity rhenium granules are typically complex, have long production cycles, and are prone to introducing impurities during production, making it difficult to meet the ultra-high purity requirements of advanced applications.
[0003] For example, CN113681019A discloses a novel process for preparing high-purity 5N-grade rhenium particles. This process employs traditional powder metallurgy methods and includes steps such as crude ammonium perrhenate pretreatment, high-temperature hydrogen reduction, primary grinding and sieving of rhenium powder, vacuum distillation of rhenium powder, secondary grinding and sieving of rhenium powder, pressing and molding, and vacuum activation sintering. Although this method can produce high-purity rhenium particles with a purity greater than 5N, its process is complex, requiring multiple grinding, sieving, and sintering steps, resulting in a long production cycle and high energy consumption.
[0004] CN111872409A discloses a production process for high-purity aerospace-grade rhenium granules, which includes six steps: ammonium perrhenate pretreatment, high-temperature reduction, grinding and classification, pressing and molding, high-temperature sintering, and surface treatment. Although it compresses two high-temperature reductions into one reduction and two high-temperature sinterings into one sintering, shortening the process flow, it still requires multiple independent steps and is prone to introducing impurities during material transfer.
[0005] CN109794598A discloses a method for preparing ultra-high purity rhenium ingots. This method involves steps such as powder sieving, powder mixing and pressing of billets, pre-firing, and high-temperature sintering to prepare ultra-high purity rhenium ingots. While this method can produce rhenium ingots with a purity ≥99.995%, it employs a traditional pressing process and requires two independent steps: pre-firing and high-temperature sintering, making continuous production impossible.
[0006] In summary, it can be seen that the existing methods for preparing high-purity rhenium granules usually face the following problems: (1) Complex process flow and long production cycle: Existing technologies usually require multiple independent processes, such as pretreatment, reduction, grinding, sieving, pressing, sintering, etc. Each process requires separate equipment and operation, resulting in a long production cycle and low efficiency; (2) High risk of impurity introduction: During the material transfer process between multiple processes, rhenium powder or rhenium granules are exposed to the air and are prone to adsorbing moisture, oxygen and other impurities, or introducing metal impurities when in contact with equipment, affecting the purity of the final product; (3) High energy consumption: Existing processes usually require multiple high-temperature treatments, such as multiple sintering, vacuum distillation, etc., which consume a lot of energy and increase production costs; (4) Dispersed equipment and processes: Existing processes require a variety of independent equipment, occupy a large area, have high investment costs, and the coordination and control between various equipment are complex; (5) Poor product consistency: Due to the complexity of the process, it is difficult to control the parameters of each process, resulting in poor consistency between product batches and unstable quality. Summary of the Invention
[0007] In view of the shortcomings of the existing technology, the purpose of this invention is to propose a method and equipment for the continuous preparation of high-purity rhenium granules from high-purity rhenium powder. This method can seamlessly connect the process steps such as injection molding, gradient sintering for impurity removal and precision cutting through a continuous and closed process flow, so as to realize the integrated manufacturing from high-purity rhenium powder to high-purity rhenium granules, and avoid the problems of impurity introduction and low efficiency in the traditional step-by-step preparation process.
[0008] The technical solution of the present invention is as follows: A method for the continuous preparation of high-purity rhenium granules from high-purity rhenium powder, comprising the following steps in an integrated closed device: (1) Mix high-purity rhenium powder and high-purity binder at a mass ratio of (15-25):1 at 60-80℃ to obtain a uniform mixture; (2) The mixture is heated to 80-120°C and injection molded into a cylindrical rhenium rod under a pressure of 50-150 MPa; (3) The rhenium rod is sintered in a protective atmosphere or vacuum environment with a multi-temperature gradient heating of 300-2400℃, and then cooled to obtain the sintered rhenium rod; (4) The sintered rhenium rod is cut, cleaned and vacuum dried to obtain the high-purity rhenium particles; The high-purity binder is selected from high-purity paraffin and / or high-purity polyethylene.
[0009] In the above preparation method of the present invention, high-purity polyethylene refers to polyethylene with a high ethylene content (i.e., a low content of non-ethylene monomer impurities).
[0010] The high-purity rhenium powder and high-purity binder mixture obtained by the above preparation method of the present invention has excellent rheological properties. During the hot-press injection stage, it can be successfully formed into a green body with regular shape, high strength and bonding force under specific pressure and temperature. It can also ensure that the binder is completely and cleanly removed in the low-temperature zone during the subsequent heating sintering, without incomplete decomposition or side reaction with rhenium in the high-temperature zone.
[0011] In the preparation method of the present invention, the multi-temperature gradient heating sintering process exhibits good matching between the low-temperature zone and the binder's volatilization temperature. Simultaneously, it allows for the oxidation or nitriding of impurities, providing active sites for the reduction decomposition reaction in the medium-temperature zone and accelerating the reaction rate. The medium-temperature zone is an active area for reduction decomposition and impurity volatilization. Under a protective atmosphere or vacuum environment, it can efficiently remove low-melting-point volatile impurities while providing shrinkage space and growth contact surface for the growth and densification of sintered grains in the high-temperature zone, reducing the shrinkage resistance during high-temperature densification. Compared to traditional single high-temperature sintering, the multi-temperature gradient heating sintering method adopted in this invention is more efficient and thorough, avoiding the problem of impurities being trapped inside the dense rhenium matrix during sintering and difficult to remove.
[0012] The preparation method of the present invention can complete the morphological transformation from powder to rod in a closed environment, avoiding the pollution risks caused by powder exposure and multiple transfers in traditional processes.
[0013] According to some preferred embodiments of the present invention, the vacuum drying process is performed at a temperature of 150-200°C for a time of 1-2 hours.
[0014] According to some preferred embodiments of the present invention, the vacuum drying process is carried out in a vacuum dryer.
[0015] According to some preferred embodiments of the present invention, the mixing is carried out under an inert atmosphere and the mixing time is 1-3 hours.
[0016] According to some preferred embodiments of the present invention, the mixing is performed mechanically at a mixing speed of 50-100 rpm.
[0017] According to some preferred embodiments of the present invention, the injection temperature of the injection molding is 90-110°C; and / or, the injection pressure is 80-120 MPa; and / or, the holding pressure is 30-80 MPa; and / or, the holding time is 10-30 s.
[0018] According to some preferred embodiments of the present invention, the rhenium rod has a diameter of 8-25 mm, a length of 50-300 mm, and a density of 6.5-8.5 g / cm³. 3 .
[0019] According to some preferred embodiments of the present invention, the multi-temperature zone gradient heating sintering is a five-temperature zone gradient heating sintering, wherein the first temperature zone is 300-500℃ and the holding time is 0.8-2h; the second temperature zone is 800-1000℃ and the holding time is 1-2h; the third temperature zone is 1200-1500℃ and the holding time is 1-2h; the fourth temperature zone is 1800-2200℃ and the holding time is 1-2h; and the fifth temperature zone is 2200-2400℃ and the holding time is 1-2h.
[0020] The inventors unexpectedly discovered that, in the above preferred embodiments of the present invention, the treatment in the first temperature zone can effectively remove binders and adsorbed water, the treatment in the second temperature zone can effectively remove oxides, the treatment in the third temperature zone can achieve preliminary densification, the treatment in the fourth temperature zone can deeply remove low-melting-point metal impurities such as K, Na, Pb, Zn, Cd, Bi, etc., and carbon impurities, and the treatment in the fifth temperature zone can complete the final densification. Meanwhile, the first temperature zone (300-500℃) can oxidize or nitride impurities, providing active sites for the subsequent reduction and decomposition reaction in the medium temperature zone, thus accelerating the reaction rate. The second temperature zone (800-1000℃) is the reaction zone where oxides and nitrides undergo reduction and decomposition, generating elemental impurities in a protective atmosphere such as hydrogen or a vacuum environment. At the same time, the remaining interstitial structures provide volatilization pathways for the subsequent volatilization of metallic impurities. The third temperature zone (1200-1500℃) is the active volatilization zone for low-melting-point impurity metals, which can efficiently remove low-melting-point impurities and simultaneously begin structural shrinkage, reducing porosity. In the fourth temperature zone (1800-2200℃), low-melting-point impurity metals continue to volatilize, while providing shrinkage space and growth contact surfaces for grain growth and densification during the final high-temperature sintering, reducing the shrinkage resistance of high-temperature densification.
[0021] According to some preferred embodiments of the present invention, the heating rate of the multi-temperature zone gradient heating sintering is 20-100℃ / h.
[0022] More preferably, the heating rate of the multi-temperature zone gradient heating sintering is 50-80℃ / h.
[0023] According to some preferred embodiments of the present invention, the purity of the high-purity rhenium powder is not less than 99.995%.
[0024] More preferably, the high-purity rhenium powder has a purity of 99.995-99.999%, wherein the O content is <500 ppm and the N content is <100 ppm.
[0025] According to some preferred embodiments of the present invention, the particle size of the high-purity rhenium powder is 100-800 mesh.
[0026] According to some preferred embodiments of the present invention, the purity of the high-purity adhesive is not less than 99.99%.
[0027] According to some preferred embodiments of the present invention, the high-purity paraffin has a melting point of 50-60°C.
[0028] According to some preferred embodiments of the present invention, the high-purity polyethylene has a molecular weight of 50,000-100,000.
[0029] According to some preferred embodiments of the present invention, the injection molding uses a mold preheated to 50-80°C.
[0030] More preferably, the preheating temperature is 60-70℃.
[0031] According to some preferred embodiments of the present invention, in step (3), the protective atmosphere is a hydrogen atmosphere with a purity ≥99.999% and a flow rate of 1-5 L / min.
[0032] According to some preferred embodiments of the present invention, the vacuum degree of the vacuum environment is ≤10Pa.
[0033] According to some preferred embodiments of the present invention, the cutting is performed using a multi-wire cutting method, the cutting wire is a diamond-coated rhenium wire and / or a diamond-coated molybdenum wire with a diameter of 0.1-0.3 mm, the cutting speed is 0.5-2 mm / min, and high-purity deionized water is used as the coolant during the cutting process.
[0034] According to some preferred embodiments of the present invention, the cleaning is performed using ultrasonic cleaning with an organic solvent.
[0035] More preferably, the organic solvent is selected from high-purity ethanol and / or high-purity acetone.
[0036] According to some preferred embodiments of the present invention, the ultrasonic cleaning is performed using an industrial-grade high-frequency ultrasonic cleaning machine.
[0037] According to some preferred embodiments of the present invention, the high-purity rhenium particles have a diameter of 10-50 mm and a thickness of 5-15 mm.
[0038] This invention further provides a high-purity rhenium granule preparation device for implementing the above method, comprising: an injection molding unit, a zone sintering unit, a multi-wire cutting unit, a sealed transfer channel, and an integrated control system. The injection molding unit includes a barrel, a screw, a heating system, a mold, and a demolding device, used to mix high-purity rhenium powder with a binder and inject it into cylindrical rhenium rods. The zone sintering unit includes a multi-temperature zone sintering furnace, an atmosphere control system, a pushing device, and a temperature control system, used to perform multi-temperature zone gradient heating sintering on the rhenium rods. The multi-wire cutting unit includes a multi-wire cutter, a cooling system, a pushing device, and a collection system, used to cut the sintered rhenium rods into rhenium granules of a specified size. The sealed transfer channel is a sealed channel connecting the other units, ensuring that the material does not come into contact with the external environment during transfer and preventing the introduction of impurities. The integrated control system is used to control the working status of each unit to achieve continuous production.
[0039] The high-purity rhenium particles prepared by the above method or equipment according to the present invention can reach a purity of over 99.999%, with a total content of 27 impurity elements of less than 10 ppm, a gaseous element content of less than 50 ppm O, less than 10 ppm N, less than 30 ppm C, and less than 10 ppm H.
[0040] The present invention has the following beneficial effects: (1) The present invention can continuously complete the four process steps of injection molding, gradient sintering, precision cutting and surface treatment in the same closed system. The material does not come into contact with the external environment throughout the process, which fundamentally solves the problem of impurity introduction and ensures the high purity of the product. (2) Compared with the existing technology which requires 5-7 independent processes, the present invention can compress the process into 3 core steps, shortening the production cycle by more than 40%; (3) The present invention innovatively adopts a five-temperature zone gradient heating method, which can realize staged impurity removal and product control. Compared with the traditional single-temperature sintering method, the impurity removal efficiency is improved by more than 60%, and it has a particularly significant removal effect on interstitial impurities such as O and N. (4) The purity of the product obtained by this invention can reach 5N grade (99.999%) or higher, the total content of 27 impurity elements is less than 10 ppm, the content of gaseous element O is less than 50 ppm, the content of N is less than 10 ppm, the content of C is less than 30 ppm, and the content of H is less than 10 ppm, which fully meets the requirements of high-end fields such as aerospace. (5) The product size tolerance obtained by the present invention can be controlled within ±0.1 mm, the density fluctuation is less than ±0.05 g / cm³, and the batch consistency reaches more than 99%, which ensures the stability of each batch of products in terms of size, density, purity, etc., and meets the stringent requirements of high-end applications for product stability. (6) The present invention can be used for continuous production with integrated equipment, which simplifies the process flow, reduces equipment investment and labor costs, reduces energy and material consumption, reduces production costs, and at the same time improves product yield and quality stability and reduces scrap rate. Attached Figure Description
[0041] Figure 1 A photograph of the high-purity rhenium granules prepared in Example 1; Figure 2 This is a photograph of the sintered rhenium rod prepared in Example 1. Detailed Implementation
[0042] The technical solutions of the present invention will be further described below with reference to embodiments thereof. The embodiments described below are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort should fall within the scope of protection of the present invention.
[0043] The following embodiments are all completed using an integrated device, which includes: an injection molding unit, a zone sintering unit, a multi-wire cutting unit, a sealed transfer channel, and an integrated control system. The injection molding unit includes a barrel, screw, heating system, mold, and demolding device, used to mix high-purity rhenium powder with a binder and inject it into cylindrical rhenium rods. The zone sintering unit includes a multi-temperature zone sintering furnace, an atmosphere control system, a pushing device, and a temperature control system, used to perform multi-temperature zone gradient heating sintering on the rhenium rods. The multi-wire cutting unit includes a multi-wire cutter, a cooling system, a pushing device, and a collection system, used to cut the sintered rhenium rods into rhenium granules of a specified size. The sealed transfer channel is a sealed channel connecting the remaining units. The integrated control system is used to control the working status of each unit to achieve continuous production.
[0044] Example 1 High-purity rhenium granules are prepared continuously through the following process: (1) 9.5 kg of high-purity rhenium powder with a purity of 99.999% and a particle size of 200-400 mesh and 0.5 kg of high-purity paraffin with a purity of 99.99%, a particle size of 200-400 mesh, a melting point of 60℃ and a purity of ≥99.99% (mass ratio 19:1) are placed into the injection molding unit barrel and mixed by screw stirring for 2 hours to obtain a uniform mixture; (2) The mixture is automatically injected into the molding mold preheated to 60°C by the injection molding unit under a pressure of 100MPa, and then heated to 100°C to form a cylindrical rhenium rod with a diameter of 20mm and a length of 100mm. (3) The rhenium rod is fed into the zone sintering furnace via a pushing device and subjected to gradient heating sintering in a hydrogen atmosphere with a flow rate of 2 L / min in five temperature zones: the first temperature zone is 400℃ and held for 1 h; the second temperature zone is 900℃ and held for 1.5 h; the third temperature zone is 1300℃ and held for 1.5 h; the fourth temperature zone is 2000℃ and held for 2 h; and the fifth temperature zone is 2300℃ and held for 2 h. The total heating and holding time is approximately 20 h. The rod is then cooled to below 200℃ in the furnace to obtain the sintered rhenium rod, as shown in the attached figure. Figure 2 As shown; (4) The sintered rhenium rod is fed into the multi-wire cutting area and cut with 0.2mm diamond-coated rhenium wire at a cutting speed of 1mm / min. The coolant is high-purity deionized water. The rhenium rod is cut into rhenium particles with a diameter of 15mm and a thickness of 6mm. (5) The cut rhenium granules were ultrasonically cleaned in a high-frequency ultrasonic cleaner with high-purity ethanol for 10 minutes, and then transferred to a vacuum dryer for drying at 150°C for 2 hours, yielding 8.2 kg of high-purity rhenium granules, as shown in the attached figure. Figure 1 As shown.
[0045] The obtained high-purity rhenium particles were tested using the following method: Purity was tested using glow discharge mass spectrometry (GDMS) and the 27 impurity elements involved were detected in accordance with the non-ferrous metal industry standard YS / T 1018-2015 to obtain the purity of the main element Re. The C and O contents were determined by infrared absorption method and the H and N contents were determined by thermal conductivity method.
[0046] The test results showed that the purity of the obtained high-purity rhenium particles was >99.9995%, the total content of 27 impurity elements (including Al, Fe, Ni, K, Na, Pb, Zn, Cd, Bi, etc.) was <5ppm, the O content was 30ppm, the N content was 4ppm, the C content was 10ppm, and the H content was 3ppm.
[0047] Furthermore, density and size tests were conducted, and the results showed that the density of the obtained high-purity rhenium particles was 19.91-19.97 g / cm³. 3 The diameter is 14.98-15.04mm and the thickness is 5.98-6.3mm. The product has good dimensional consistency and a smooth surface.
[0048] Example 2 High-purity rhenium granules are prepared continuously through the following process: (1) 9.6 kg of high-purity rhenium powder with a purity of 99.995% and a particle size of 400-600 mesh and 0.4 kg of high-purity polyethylene with a purity of 99.99% (i.e., ethylene monomer purity of 99.99wt%) and a molecular weight of 100,000 (mass ratio 24:1) are placed into the injection molding unit barrel and mixed by screw stirring for 1.5 h to obtain a uniform mixture; (2) The mixture is automatically injected into the molding mold preheated to 70°C by the injection molding unit under a pressure of 120MPa, and then heated to 110°C to form a cylindrical rhenium rod with a diameter of 20mm and a length of 150mm. (3) The rhenium rod is fed into the zone sintering furnace through a pushing device and sintered in a vacuum environment (vacuum degree is 5Pa) with gradient heating in five temperature zones: the temperature of the first temperature zone is 450℃ and the holding time is 1.2h; the temperature of the second temperature zone is 950℃ and the holding time is 1.2h; the temperature of the third temperature zone is 1400℃ and the holding time is 1.2h; the temperature of the fourth temperature zone is 2100℃ and the holding time is 1.8h; the temperature of the fifth temperature zone is 2400℃ and the holding time is 1.8h. The total heating and holding time is about 21.2h. The rod is cooled to below 200℃ in the furnace to obtain the sintered rhenium rod. (4) The sintered rhenium rod is fed into the multi-wire cutting area and cut with a 0.25mm diamond-coated molybdenum wire at a cutting speed of 1.5mm / min. The coolant is high-purity deionized water. The rod is cut into rhenium particles with a diameter of 14.5mm and a thickness of 8mm. (5) After cutting the rhenium particles, place them in a high-frequency ultrasonic cleaner with high-purity acetone and ultrasonically clean them for 10 minutes. Then transfer them to a vacuum dryer for drying. The drying temperature is 150℃ and the time is 2 hours to obtain 8.3 kg of high-purity rhenium particles.
[0049] The obtained high-purity rhenium granules were subjected to the same testing as in Example 1. The results showed that its purity was >99.9992%, the total content of 27 impurity elements was <8 ppm, the O content was 48 ppm, the N content was 5 ppm, the C content was 20 ppm, and the H content was 3 ppm; the density was 19.94-19.98 g / cm³. 3 The diameter is 14.48-14.54mm and the thickness is 7.97-8.03mm. The product has good dimensional consistency and a smooth surface.
[0050] Example 3 High-purity rhenium granules are prepared continuously through the following process: (1) 9.6 kg of high-purity rhenium powder with a purity of 99.995% and a particle size of 600-800 mesh and 0.6 kg of high-purity paraffin with a purity of 99.999%, a particle size of 200-400 mesh, a melting point of 60℃ and a purity of ≥99.99% (mass ratio 16:1) are placed into the injection molding unit barrel and mixed by screw stirring for 2 hours to obtain a uniform mixture; (2) The mixture is automatically injected into the molding mold preheated to 50°C by the injection molding unit under a pressure of 80MPa, and then heated to 90°C to form a cylindrical rhenium rod with a diameter of 25mm and a length of 80mm. (3) The rhenium rod is fed into the zone sintering furnace through a pushing device and sintered in a hydrogen atmosphere with a flow rate of 3L / min in five temperature zones: the temperature of the first temperature zone is 350℃ and the holding time is 0.8h; the temperature of the second temperature zone is 850℃ and the holding time is 1h; the temperature of the third temperature zone is 1250℃ and the holding time is 1h; the temperature of the fourth temperature zone is 1900℃ and the holding time is 1.5h; the temperature of the fifth temperature zone is 2300℃ and the holding time is 1h. The total heating and holding time is about 18.8h. The rod is cooled to below 200℃ in the furnace to obtain the sintered rhenium rod. (4) The sintered rhenium rod is fed into the multi-wire cutting area and cut with 0.15mm diamond-coated rhenium wire at a cutting speed of 0.8mm / min. The coolant is high-purity deionized water. The rhenium rod is cut into rhenium particles with a diameter of 17.5mm and a thickness of 8mm. (5) After cutting the rhenium particles, place them in a high-frequency ultrasonic cleaner with high-purity ethanol for 10 minutes and then transfer them to a vacuum dryer for drying. The drying temperature is 150℃ and the time is 2 hours to obtain 8.5 kg of high-purity rhenium particles.
[0051] The obtained high-purity rhenium granules were subjected to the same testing as in Example 1. The results showed that its purity was >99.9993%, the total content of 27 impurity elements was <7 ppm, the O content was 55 ppm, the N content was 6 ppm, the C content was 15 ppm, and the H content was 3 ppm; the density was 19.81-19.86 g / cm³. 3 The diameter is 17.48-17.54mm and the thickness is 7.96-8.02mm. The product has good dimensional consistency and a smooth surface.
[0052] Comparative Example 1 High-purity rhenium granules were prepared using the same process as in Example 1, except that the mass ratio of high-purity rhenium powder to high-purity paraffin was adjusted to 30:1.
[0053] During the preparation process, it was found that the powder flowability deteriorated and the uniformity of filling the mold deteriorated, resulting in the cylindrical rhenium rods being prone to breakage and the powder bonding strength of the blank being low.
[0054] The obtained high-purity rhenium granules were subjected to the same testing as in Example 1. The results showed that the O and C contents were reduced to 20 ppm and 6 ppm, respectively, while the overall impurity content was slightly higher than that in Example 1. The density of the obtained rhenium granules was reduced to 18.95-19.35 g / cm³. 3 The diameter varies significantly, ranging from 14.75 to 15.17 mm; the product surface has a dull color.
[0055] Comparative Example 2 High-purity rhenium granules were prepared using the same process as in Example 1, except that the mass ratio of high-purity rhenium powder to high-purity paraffin was adjusted to 10:1.
[0056] During the preparation process, it was found that the obtained cylindrical rhenium rods exhibited large differences in local shrinkage after sintering, resulting in problems such as warping, twisting, or large dimensional fluctuations.
[0057] The obtained high-purity rhenium granules were subjected to the same tests as in Example 1. The test results showed that the O and C contents increased significantly, reaching 98 ppm and 54 ppm respectively. Simultaneously, the contents of some low-melting-point impurities exceeded the standard limits (see Table 1 for detailed test results). The density of the obtained rhenium granules fluctuated widely, ranging from 19.15 to 19.89 g / cm³. 3 After the product is cut, some surfaces show large air holes and irregular shapes.
[0058] Comparative Example 3 High-purity rhenium granules were prepared using the same process as in Example 2, except that the mass ratio of high-purity rhenium powder to high-purity polyethylene was adjusted to 15:1.
[0059] During the preparation process, it was found that the obtained cylindrical rhenium rods were broken, and the sintered green body showed large local shrinkage differences.
[0060] The obtained high-purity rhenium granules were subjected to the same tests as in Example 1. The test results showed that the O and C contents increased significantly, reaching 75 ppm and 45 ppm respectively, and the C content exceeded the standard limit (see Table 1 for test results). The density of the obtained high-purity rhenium granules fluctuated significantly, ranging from 19.18 to 19.74 g / cm³. 3 The diameter is 14.81-15.04mm; large pores and irregular shapes are occasionally seen on the product surface.
[0061] Comparative Example 4 High-purity rhenium particles were prepared using the same process as in Example 1, except that the injection pressure in step (2) was adjusted to 50 MPa.
[0062] During the preparation process, it was found that the powder did not fully bond and formed multiple small round rods after demolding, indicating that the powder could not be completely bonded together.
[0063] Comparative Example 5 High-purity rhenium granules were prepared using the same process as in Example 1, except that the sintering temperature in step (3) was adjusted to be 900°C for the first temperature zone and held for 1 hour; 900°C for the second temperature zone and held for 1.5 hours; 1300°C for the third temperature zone and held for 1.5 hours; 1300°C for the fourth temperature zone and held for 2 hours; and 2300°C for the fifth temperature zone and held for 2 hours. The total sintering temperature rise and holding time was about 20 hours. The sintered rhenium rods were obtained by cooling the furnace to below 200°C.
[0064] The obtained high-purity rhenium granules were subjected to the same testing as in Example 1. The results showed that its purity was >99.9949%, the total content of 27 impurity elements was <51ppm, and many low-melting-point impurity elements failed to volatilize effectively; the O content was 120ppm, the N content was 15ppm, the C content was 42ppm, and the H content was 10ppm, with some impurities exceeding the standard limits; the density was 19.61-19.67g / cm³. 3 The diameter is 15.05-15.08mm and the thickness is 9.98-10.3mm.
[0065] The results of the impurity element content detection of the products obtained in the above embodiments and comparative examples are shown in Table 1: Table 1. Results of Impurity Element Content Detection
[0066] It should be noted that the above descriptions are merely preferred embodiments of the present invention and should not limit the scope of protection of the technical solutions of the present invention. Any modifications made to the technical solutions described in the foregoing embodiments, or equivalent substitutions of technical features, by those skilled in the art within the spirit and principles of the present invention, should be included within the scope of protection of the present invention.
Claims
1. A method for the continuous preparation of high-purity rhenium granules from high-purity rhenium powder, characterized in that, It includes: in The following steps are performed in an integrated sealed device: (1) Mix high-purity rhenium powder and high-purity binder at a mass ratio of (15-25):1 at 60-80℃ to obtain a uniform mixture; (2) The mixture is heated to 80-120°C and injection molded into a cylindrical rhenium rod under a pressure of 50-150 MPa; (3) The rhenium rod is sintered in a protective atmosphere or vacuum environment with a multi-temperature gradient heating of 300-2400℃, and then cooled to obtain the sintered rhenium rod; (4) The sintered rhenium rod is cut, cleaned and vacuum dried to obtain the high-purity rhenium particles; The high-purity binder is selected from high-purity paraffin and / or high-purity polyethylene.
2. The method according to claim 1, characterized in that, The vacuum drying process is carried out at a temperature of 150-200℃ for 1-2 hours.
3. Among them, The multi-temperature zone gradient heating sintering is a five-temperature zone gradient heating sintering, wherein the first temperature zone is 300-500℃, and the holding time is 0.8-2h; the second temperature zone is 800-1000℃, and the holding time is 1-2h; the third temperature zone is 1200-1500℃, and the holding time is 1-2h; the fourth temperature zone is 1800-2200℃, and the holding time is 1-2h; the fifth temperature zone is 2200-2400℃, and the holding time is 1-2h; and / or, the heating rate of the multi-temperature zone gradient heating sintering is 20-100℃ / h.
4. The method according to claim 1, characterized in that, in, The purity of the high-purity rhenium powder is not less than 99.995%, and / or the particle size of the high-purity rhenium powder is 100-800 mesh; and / or the purity of the high-purity binder is not less than 99.99%; and / or the melting point of the high-purity paraffin is 50-60℃; and / or the molecular weight of the polyethylene is 50,000-100,000.
5. The method according to claim 1, characterized in that, The injection molding process uses a mold preheated to 50-80°C.
6. The method according to claim 1, characterized in that, In step (3), the protective atmosphere is a hydrogen atmosphere with a purity of ≥99.999% and a flow rate of 1-5 L / min; and / or, the vacuum degree of the vacuum environment is ≤10 Pa.
7. The method according to claim 1, characterized in that, in, The cleaning process employs ultrasonic cleaning with organic solvents; and / or, the cutting process employs multi-wire cutting, with the cutting wire being diamond-coated rhenium wire and / or diamond-coated molybdenum wire with a diameter of 0.1-0.3 mm, the cutting speed being 0.5-2 mm / min, and high-purity deionized water being used as the coolant during the cutting process.
8. The method according to claim 1, characterized in that, The cleaning process employs an industrial-grade high-frequency ultrasonic cleaner; the cleaning utilizes an organic solvent for ultrasonic cleaning; the organic solvent is selected from high-purity ethanol and / or high-purity acetone.
9. The method according to claim 1, characterized in that, The high-purity rhenium particles have a diameter of 10-50 mm and a thickness of 5-15 mm.
10. A high-purity rhenium granule preparation apparatus for implementing the method of any one of claims 1-9, characterized in that, It includes: The system comprises an injection molding unit, a zone sintering unit, a multi-wire cutting unit, a sealed transfer channel, and an integrated control system. The injection molding unit includes a barrel, screw, heating system, mold, and demolding device, used to mix high-purity rhenium powder with a binder and injection mold it into cylindrical rhenium rods. The zone sintering unit includes a multi-temperature zone sintering furnace, an atmosphere control system, a pushing device, and a temperature control system, used for multi-temperature zone gradient heating sintering of the rhenium rods. The multi-wire cutting unit includes a multi-wire cutter, a cooling system, a pushing device, and a collection system, used to cut the sintered rhenium rods into rhenium granules of a specified size. The sealed transfer channel connects the other units, ensuring that the material does not come into contact with the external environment during transfer and preventing the introduction of impurities. The integrated control system controls the operating status of each unit to achieve continuous production.
Citation Information
Patent Citations
Manufacturing method for ultrapure rhenium ingots
CN109794598A
Production process of high-purity aviation-grade rhenium particles
CN111872409A