A copper alloy heat sink based on laser additive manufacturing and its preparation method

By using laser additive manufacturing technology to integrally form a copper alloy heat sink and designing a composite gradient liquid absorption core layer, the problems of complex manufacturing process and high contact thermal resistance in the existing technology are solved, achieving efficient thermal management and structural reliability, and meeting the heat dissipation requirements of high heat flux density.

CN123103012APending Publication Date: 2026-11-17SHAANXI SIRUI COPPER ALLOY INNOVATION CENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611138407.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing heat spreaders have complex manufacturing processes and high contact thermal resistance, making them difficult to meet the heat dissipation requirements of high heat flux density. Furthermore, the assembly process of multi-level structures can easily introduce additional interface layers, resulting in limited overall heat transfer efficiency and difficulty in improving long-term operational reliability.

Method used

Laser additive manufacturing technology is used to integrally form the upper cover plate, lower base plate, support columns, and three-dimensional capillary core structure. A composite gradient liquid absorption core layer is designed, including a microneedle rib array, a variable cross-section micropillar array, and a microporous mesh structure. Through a partitioned scanning strategy and sintering treatment, the porosity gradient and structural morphology are optimized to achieve efficient circulation and heat transfer of the working fluid.

Benefits of technology

It significantly improves the overall thermal conductivity and structural reliability of the heat spreader, solves the problem of local drying under high heat flux density, optimizes the flow path of the liquid working fluid, and maintains excellent temperature uniformity and operational stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103012A_ABST
    Figure CN123103012A_ABST
Patent Text Reader

Abstract

This application discloses a copper alloy vapor chamber and its preparation method, relating to the fields of additive manufacturing and electronic heat dissipation technology. The copper alloy vapor chamber includes an integrally formed upper cover plate, a lower base plate, support columns, and a three-dimensional capillary core structure. A sealed vacuum chamber is formed between the upper cover plate and the lower base plate. The three-dimensional capillary core structure includes a composite gradient liquid-absorbing core layer disposed on the inner wall of the lower base plate. The composite gradient liquid-absorbing core layer includes a micro-needle rib array, a variable cross-section micro-pillar array, and a microporous mesh structure arranged sequentially from bottom to top, with the porosity of the micro-needle rib array, the variable cross-section micro-pillar array, and the microporous mesh structure increasing sequentially. This application enables the integral molding of the vapor chamber, eliminates interfacial contact thermal resistance, and optimizes the working fluid circulation through the gradient capillary structure, thereby improving heat transfer efficiency and reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of additive manufacturing technology, and in particular to a copper alloy heat spreader based on laser additive manufacturing and its preparation method. Background Technology

[0002] With the rapid development of electronic information technology, electronic components are evolving towards higher power density, miniaturization, and integration, leading to a sharp increase in heat flux density per unit area. Efficient thermal management has become a key factor in ensuring stable equipment operation and extending its service life. Vacuum chamber heat exchangers, as highly efficient heat dissipation devices that utilize the phase change of the working fluid for heat transfer, are widely used in high-performance processors, power modules, and communication base stations due to their extremely high equivalent thermal conductivity and excellent temperature uniformity. Currently, these devices typically consist of a shell, internal support structure, and capillary wick. They achieve rapid heat transfer through the endothermic vaporization of the working fluid at the evaporation end and the exothermic liquefaction at the condensation end.

[0003] In traditional manufacturing processes, vapor chambers are typically manufactured in a modular fashion, with the upper and lower cover plates, support columns, and capillary cores prepared separately, and then assembled using processes such as diffusion welding, brazing, or sintering. This multi-step manufacturing approach requires precise control over the dimensional fit and interfacial bonding quality of each component. However, due to limitations in existing processing technologies, vapor chambers lack the freedom to form complex three-dimensional capillary structures, and the assembly process of multi-level structures can easily introduce additional interfacial layers. This leads to common technical bottlenecks in practical applications, such as limited overall heat transfer efficiency, difficulty in further improving long-term operational reliability, and inability to meet the demands of extremely high heat flux densities. Summary of the Invention

[0004] The main objective of this application is to provide a copper alloy vapor chamber based on laser additive manufacturing and its preparation method, aiming to solve the technical problems of complex manufacturing process and high contact thermal resistance of vapor chambers in the prior art.

[0005] To achieve the above objectives, this application provides a copper alloy heat spreader based on laser additive manufacturing, comprising an integrally formed upper cover plate, a lower base plate, a support column, and a three-dimensional capillary core structure. A sealed vacuum chamber is formed between the upper cover plate and the lower base plate, and the support columns are arranged in an array within the vacuum chamber; The three-dimensional capillary core structure includes a composite gradient liquid-absorbing core layer disposed on the inner wall of the lower base plate. The composite gradient liquid-absorbing core layer includes a microneedle rib array, a variable cross-section microcolumn array, and a microporous mesh structure arranged sequentially from bottom to top, and the porosity of the microneedle rib array, the variable cross-section microcolumn array, and the microporous mesh structure increases sequentially.

[0006] Optionally, the porosity of the microneedle rib array is 20%-30%, the porosity of the variable cross-section micropillar array is 40%-50%, and the porosity of the microporous mesh structure is 55%-65%.

[0007] Optionally, the cross-section of the microneedle ribs in the microneedle rib array is triangular or trapezoidal, with a height of 0.2mm-0.5mm and a base width of 30μm-50μm.

[0008] Optionally, the bottom diameter of the variable cross-section micropillars in the variable cross-section micropillar array is 100μm-150μm, and the top diameter is 40μm-60μm, exhibiting an inverted conical or stepped contraction.

[0009] Optionally, the copper alloy component in the copper alloy heat sink includes, by mass percentage: Cr: 0.2%-0.8%, Ni: 0.5%-2.0%, with the balance being Cu and impurities.

[0010] Furthermore, to achieve the above objectives, this application also provides a method for preparing the aforementioned copper alloy heat sink based on laser additive manufacturing, comprising the following steps: A three-dimensional model of the copper alloy heat exchanger is constructed. The three-dimensional model includes an upper cover plate, a lower base plate, support columns, and a three-dimensional capillary core structure. The three-dimensional capillary core structure includes a composite gradient liquid absorption core layer. Set the printing parameters of the laser additive manufacturing equipment, and use a partitioned scanning strategy to print to obtain a homogeneous slab blank; The heat-soaking plate blank is removed from the substrate of the laser additive manufacturing equipment, and then the removed heat-soaking plate blank is subjected to powder removal treatment. The heat-soaked slab blank after powder removal is then subjected to sintering treatment; A working fluid is injected into the vacuum chamber, and a vacuum is drawn and sealed to obtain the copper alloy heat exchange plate.

[0011] Optionally, the partitioned scanning strategy includes: for the dense area of ​​the bottom plate, scanning is performed using a first scanning parameter, which includes: power 600W-700W and speed 1000mm / s. For the composite gradient liquid absorption core layer, the second scanning parameters are used for scanning, and for the variable cross-section micropillar region, a spiral gradient filling scanning strategy is adopted. The second scanning parameters include: power 500W-600W, speed 1200mm / s-1500mm / s.

[0012] Optionally, the preparation method further includes: generating a slicing path with optimized self-supporting angle for the variable cross-section micropillar region of the three-dimensional model.

[0013] Optionally, the sintering process is as follows: the heat-soaked slab blank after powder removal is placed in a reducing atmosphere furnace and held at 850℃-950℃ for 1 hour to 3 hours.

[0014] Optionally, the powder removal process involves removing unmelted residual powder from the three-dimensional capillary core structure inside the heat-soaked slab blank by mechanical vibration or an air gun.

[0015] Compared with the prior art, this application has the following beneficial effects: This application employs laser additive manufacturing technology to integrally form the upper cover plate, lower base plate, support columns, and three-dimensional capillary core structure, eliminating the interfacial contact thermal resistance caused by welding or bonding in traditional assembly processes, significantly improving the overall thermal conductivity and structural reliability of the heat spreader. Due to the structural gradient of the composite gradient wicking core layer, from the microneedle rib array at the bottom to the microporous mesh structure at the top, optimal matching of capillary driving force and permeability is achieved. The high-density microneedle ribs at the bottom enhance the working fluid supply in the evaporation section, while the mesh structure at the top reduces reflux resistance, effectively solving the problem of localized drying that easily occurs under high heat flux density. Furthermore, the composite gradient wicking core layer has a porosity gradient that increases along the height direction, further optimizing the flow path of the liquid working fluid. Utilizing Darcy's law, the viscous resistance during reflux is reduced, improving the working fluid circulation efficiency. The synergistic effect of the structural gradient and porosity gradient allows the heat spreader to maintain excellent temperature uniformity and operational stability even under high-power heat loads. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the structure of the copper alloy heat sink based on laser additive manufacturing in the embodiments of this application; Figure 2 This is a flowchart illustrating the preparation method of a copper alloy heat sink based on laser additive manufacturing in this application embodiment; Figure 3 The images shown are scanning electron microscope (SEM) images of the gradient pore capillary core structure and its porosity distribution in the embodiments of this application. Figure 1 ; Figure 4 The images shown are scanning electron microscope (SEM) images of the gradient pore capillary core structure and its porosity distribution in the embodiments of this application. Figure 2 ; Figure 5 This is a physical image of the copper alloy heat spreader prepared in the embodiments of this application.

[0017] The attached figures are labeled as follows: 1-Upper cover plate; 2-Lower base plate; 3-Support column; 4-Three-dimensional capillary core structure; 5-Vacuum chamber; 6-Composite gradient liquid absorption core layer; 7-Microneedle rib array; 8-Variable cross-section micro-pillar array; 9-Microporous mesh structure. Detailed Implementation

[0018] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0019] like Figure 1 As shown, this application provides a copper alloy heat exchanger based on laser additive manufacturing. The heat exchanger includes: an upper cover plate 1, a lower base plate 2, support columns 3, and a three-dimensional capillary core structure 4. A sealed vacuum chamber 5 is formed between the upper cover plate 1 and the lower base plate 2, and the support columns 3 are arrayed within the vacuum chamber 5. The three-dimensional capillary core structure 4 includes a composite gradient liquid-absorbing core layer 6 disposed on the inner wall of the lower base plate 2. The composite gradient liquid-absorbing core layer 6 includes, from bottom to top, a microneedle rib array 7, a variable cross-section micropillar array 8, and a microporous mesh structure 9, with the porosity of the microneedle rib array 7, the variable cross-section micropillar array 8, and the microporous mesh structure 9 increasing sequentially.

[0020] Specifically, the upper cover plate 1 and the lower base plate 2 serve as the outer shell of the heat spreader, integrally formed using laser additive manufacturing. Together, they enclose an internally sealed vacuum chamber 5, providing the necessary pressure environment for the phase change heat transfer of the working fluid. An array of support columns 3 is distributed within the vacuum chamber 5, with their ends connected to the upper cover plate 1 and the lower base plate 2 respectively. These columns bear external loads and prevent shell deformation caused by pressure differences between the inside and outside of the chamber, ensuring the structural stability of the heat spreader under high pressure differential conditions. The arrangement density and cross-sectional shape of the support columns 3 can be optimized according to actual strength and fluid resistance requirements; for example, they can be cylindrical, prismatic, or grid-shaped.

[0021] The three-dimensional capillary core structure 4 is a non-TPMS structure, including a composite gradient liquid-absorbing core layer 6 disposed on the inner wall of the lower base plate 2. The composite gradient liquid-absorbing core layer 6 has dual characteristics of structural morphology gradient and porosity gradient. In this embodiment, the three-dimensional capillary core structure 4 adopts a non-TPMS (Triply Periodic Minimal Surface) structural design. Compared with the traditional TPMS structure, this structural form has unique advantages in terms of manufacturing process complexity and control of capillary transport capability in a specific direction. The composite gradient liquid-absorbing core layer 6, as the core functional unit of the three-dimensional capillary core structure 4, is directly disposed on the inner wall of the lower base plate 2. Its main function is to use capillary force to transport the condensed liquid working fluid from the condensation section (usually located near the upper cover plate 1) back to the evaporation section (usually located near the lower base plate 2). This structure, through the dual gradient design of structural morphology and porosity, solves the contradiction between capillary pressure and liquid permeability that is difficult to balance in a single porosity capillary core, and achieves efficient transport of the working fluid in the vertical direction.

[0022] The structural gradient extends along the height from the bottom plate 2 into the vacuum chamber 5, transitioning from a microneedle rib array 7 to a variable cross-section micropillar array 8, and then from the variable cross-section micropillar array 8 to a microporous mesh structure 9. Specifically, from bottom to top along the height direction, the composite gradient liquid-absorbing core layer 6 is divided into three continuous regions with different topological characteristics. The bottom layer is the microneedle rib array 7, which adheres closely to the inner wall of the bottom plate 2. Its main function is to maximize the contact area with the heat source and provide extremely high capillary pressure, ensuring rapid replenishment of the working fluid in the evaporation section to prevent drying. The microneedle rib array 7 has a small feature size and a high specific surface area, which can significantly reduce the evaporation thermal resistance. The middle layer is the variable cross-section micropillar array 8, which acts as a transport channel connecting the upper and lower layers. The cross-sectional dimensions of the variable cross-section micropillar array 8 gradually change along the height direction, using the Laplace pressure difference principle to drive the liquid upward flow.

[0023] The cross-sectional dimensions of the variable cross-section micropillar array 8 can be designed to gradually decrease from bottom to top, according to the Laplace equation:

[0024] in, P c For capillary pressure, The surface tension of the liquid, Contact angle, Let be the effective capillary radius. From this formula, we can see that as the capillary pressure increases with the effective capillary radius, a continuous pressure gradient is formed in the vertical direction, continuously propelling the liquid upwards against gravity.

[0025] The top layer is a microporous mesh structure 9, located near the center of the vacuum chamber 5. This layer has high porosity and interconnected pores, primarily serving to provide low-resistance liquid diffusion channels, facilitating rapid condensate recirculation and uniform distribution, while also providing space for vapor escape and reducing flow resistance at the gas-liquid interface. The porosity gradient increases gradually along the height from the bottom plate 2 towards the interior of the vacuum chamber 5. In this design, the porosity variation is synchronized with the evolution of the structural morphology. From the inner wall of the bottom plate 2 towards the interior of the vacuum chamber 5, the porosity of the composite gradient liquid-absorbing core layer 6 gradually increases. The bottom layer of microneedle rib array 7 has low porosity to ensure high capillary suction and structural strength; the variable cross-section micropillar array 8 has moderate porosity, balancing transmission resistance and driving force; and the top layer of microporous mesh structure 9 has high porosity to minimize the viscous resistance of liquid recirculation.

[0026] The working process and principle of this application are as follows: when the bottom plate 2 of the heat spreader is heated by the heat source, the working fluid in the vacuum chamber 5 absorbs heat and vaporizes in the evaporation section to form steam. The steam diffuses rapidly to the inner wall of the upper cover plate 1 under the action of a small pressure difference and condenses and releases heat. The condensed liquid working fluid adheres to the inner wall of the upper cover plate 1 and flows back downward under the drive of gravity and the capillary force of the three-dimensional capillary core structure 4. During the backflow process, the liquid working fluid first enters the microporous mesh structure 9 of the top layer, which quickly gathers and permeates downward by utilizing its high porosity characteristics. Then it enters the variable cross-section micro-pillar array 8 of the middle layer, which accelerates the downward transmission by utilizing the continuous capillary pressure gradient generated by the variable cross-section structure. Finally, it enters the micro-needle rib array 7 of the bottom layer, which provides strong capillary suction to tightly adsorb the working fluid and transport it to the heat source center of the inner wall of the bottom plate 2, completing the cyclic phase change heat transfer process of the working fluid.

[0027] In another embodiment, the porosity of the microneedle rib array 7 is 20%-30%, the porosity of the variable cross-section micropillar array 8 is 40%-50%, and the porosity of the microporous mesh structure 9 is 55%-65%.

[0028] The aforementioned parameter ranges are specific numerical intervals set for the three different levels of the composite gradient wicking core layer 6 along the height direction from the lower base plate 2 to the interior of the vacuum chamber 5. In the microneedle rib array 7 region near the lower base plate 2, the lower porosity ensures a large solid contact area between the three-dimensional capillary core structure 4 and the lower base plate 2, thereby reducing contact thermal resistance, ensuring efficient heat conduction in the evaporation region, and providing higher capillary pressure to overcome liquid flow resistance. In the variable cross-section micropillar array 8 region, the moderate increase in porosity effectively reduces the frictional resistance of liquid flow while maintaining structural support strength, playing a crucial role in the transmission process. In the region corresponding to the microporous mesh structure 9, the higher porosity greatly optimizes the connectivity of the vapor channel, facilitating rapid vapor diffusion to the condensation end and smooth return of the condensate.

[0029] This layered porosity specification, unlike the traditional three-dimensional capillary core structure with single porosity or random distribution, creates a continuous and reasonable capillary pressure gradient field by precisely controlling the porosity parameters of each layer. This enables efficient circulation of the working fluid throughout the evaporation, transport, and condensation processes, significantly improving the heat transfer performance and operational stability of the heat spreader.

[0030] In another embodiment, the cross-section of the rib array 7 in the microneedle rib array can be triangular or trapezoidal, with a height of 0.2mm-0.5mm and a base width of 30μm-50μm. Unlike conventional designs, this application innovatively limits the cross-section of the microneedle ribs to triangular or trapezoidal, rather than the traditional rectangular or circular cross-section. The triangular or trapezoidal cross-section provides a smaller effective capillary radius, thereby generating greater capillary pressure to drive the working fluid flow. The 0.2mm-0.5mm height design ensures that the microneedle ribs have a sufficient aspect ratio, providing a larger specific surface area to enhance evaporative heat transfer while avoiding the risk of structural instability due to excessive height. Simultaneously, the small size of 30μm-50μm base width greatly increases the rib density per unit area while ensuring structural strength, thereby improving the overall capillary pumping capability.

[0031] Through the above technical solution, this application achieves precise control of the geometric parameters of the microneedle ribs. By adopting triangular or trapezoidal cross-sections with specific height and width ranges, the design limitations of traditional microneedle rib structures in terms of capillary driving force and structural strength are overcome. This enables the composite gradient liquid-absorbing core layer to possess excellent working fluid wetting performance and rapid start-up capability in the bottom region, effectively solving the technical problem of easy drying at the evaporation end of the heat spreader under high heat flux density, thereby significantly improving the heat transfer limit and operational stability of the heat spreader.

[0032] In another embodiment, the bottom diameter of the variable cross-section micropillars in the variable cross-section micropillar array 8 is 100μm-150μm, and the top diameter is 40μm-60μm, exhibiting an inverted conical or stepped contraction.

[0033] The variable cross-section micropillar adopts a structural design with a larger bottom diameter and a smaller top diameter. The larger bottom diameter provides sufficient structural support strength to ensure that the heat spreader does not deform or collapse under the atmospheric pressure difference inside the vacuum chamber 4, thereby maintaining the geometric stability of the vacuum chamber 4; the smaller top diameter can significantly increase the curvature of the liquid-gas interface, thereby generating greater capillary pressure and driving the condensed liquid to flow back to the evaporation zone quickly.

[0034] This variable cross-section design, with a large base and a small top, differs from conventional constant cross-section microcolumn structures. This application innovatively utilizes geometrical variations along the height direction to construct a continuous Laplace pressure gradient. This design overcomes the performance trade-offs between capillary actuation and mechanical support inherent in traditional single-aperture structures, offering unique advantages in achieving efficient working fluid circulation and structural reliability under high heat flux density conditions.

[0035] In terms of specific form, the inverted conical contraction provides a smooth fluid transition and reduces liquid flow resistance; the stepped contraction, on the other hand, can generate a sudden pressure jump through its stepped structure, making it suitable for scenarios requiring stronger driving force. This application does not limit the specific contraction form of the variable cross-section micropillar, and the form can be selected according to actual fluid dynamics requirements.

[0036] Through the above technical solution, this application achieves synergistic optimization of the variable cross-section micropillars in terms of structural support and capillary drive function. The bottom diameter design of 100μm-150μm ensures the compressive strength of the micropillar array, effectively overcoming the external pressure load problem caused by the vacuum environment inside the heat spreader; the top diameter design of 40μm-60μm maximizes the capillary pumping capability, promoting the rapid reflux of condensate. The inverted conical or stepped contraction geometry not only constructs a pressure gradient conducive to the upward transport of liquid, but also avoids the forming difficulty of complex curved surface structures in the laser additive manufacturing process through the flexibility of the non-TPMS structure, thereby significantly improving the overall heat transfer performance and manufacturing feasibility of the heat spreader.

[0037] In another optional embodiment, this application also provides a copper alloy composition. The copper alloy composition in the copper alloy heat sink comprises, by mass percentage: Cr: 0.2%-0.8%, Ni: 0.5-2.0%, with the balance being Cu and impurities.

[0038] In this compositional design, the main role of Cr (chromium) is to improve the absorption rate of laser energy by the copper alloy matrix, reduce the forming difficulty caused by high reflectivity, and refine the grain size, thereby improving the mechanical properties of the material. The addition of Ni (nickel) helps to improve the fluidity of the molten pool, reduce spheroidization defects and crack sensitivity during laser additive manufacturing, thus improving the density and surface quality of the printed parts. The remaining Cu (copper) serves as the matrix material, ensuring that the vapor chamber itself possesses excellent thermal conductivity. Through the above technical solution, this application achieves the adaptation of material composition to the laser additive manufacturing process, solving the technical problems of high reflectivity and low forming density of pure copper in laser additive manufacturing, thus obtaining an integrated vapor chamber structure with high thermal conductivity, high density, and high structural strength.

[0039] In another alternative embodiment, such as Figure 2The diagram shown is a flowchart of a method for preparing a copper alloy heat sink based on laser additive manufacturing, according to an embodiment of this application. The method includes the following steps: Step S1: Construct a three-dimensional model of the copper alloy heat exchanger. The three-dimensional model includes an upper cover plate 1, a lower base plate 2, a support column 3, and a three-dimensional capillary core structure 4. The three-dimensional capillary core structure 4 includes a composite gradient liquid absorption core layer 6.

[0040] Using computer-aided design (CAD) software, a digital geometric model of the vapor chamber was established based on the structural parameters defined in the aforementioned embodiments. This model fully encompasses the functional components of the vapor chamber, specifically including an upper cover plate 1 and a lower base plate 2 serving as the outer shell, a support 3 for maintaining the cavity height, and a three-dimensional capillary core structure 4, the core heat transfer component. The three-dimensional capillary core structure 4 is modeled as a solid feature with specific morphological and porosity gradients, and its geometric dimensions strictly correspond to the distribution requirements of the microneedle rib array 4, the variable cross-section micropillar array 8, and the microporous mesh structure 9. After modeling, the three-dimensional model was converted to a standard data exchange format (such as stereolithography, STL format) and imported into the slicing processing system of the laser additive manufacturing equipment to generate the layer data and scanning path planning basis required for subsequent processing.

[0041] Step S2: Set the printing parameters of the laser additive manufacturing equipment, and use the partitioned scanning strategy to print to obtain a homogenized plate blank.

[0042] Based on the layer data generated from the slicing process, the process parameters of the laser additive manufacturing equipment (such as a selective laser melting (SLM) machine) are configured. A zoned scanning strategy is implemented to address the functional requirements of different areas of the vapor chamber, i.e., different energy input parameters are set for the dense shell area and the porous capillary core area. For areas requiring high density and high mechanical strength, such as the upper cover plate 1 and the lower base plate 2, a higher laser power and an appropriate scanning speed are set to ensure sufficient fusion of the metal powder. For the composite gradient liquid-absorbing core layer area, the laser energy density is adjusted to a lower level to avoid pore blockage due to excessive remelting, thereby preserving the preset porosity to maintain capillary performance. During the printing process, the laser beam melts the metal powder layer by layer according to the planned path, stacking and forming the vapor chamber blank containing complex internal flow channels and fine capillary structures on the substrate.

[0043] Step S3: Remove the heat-soaking plate blank from the substrate of the laser additive manufacturing equipment, and then perform powder removal treatment on the removed heat-soaking plate blank.

[0044] After molding, the heat-soaking plate blank is separated from the molding substrate by mechanical processing methods such as wire cutting, electrical discharge machining, or milling. This process requires strict control of the cutting position to avoid damaging the bottom structure of the blank. Subsequently, a powder removal process is performed on the complex three-dimensional capillary core structure 4 inside the blank. Because the capillary core contains numerous micropores, unmelted metal powder easily remains. Therefore, a combination of mechanical vibration and high-pressure airflow is used to purge the residual powder particles through the capillary channels. For areas with particularly complex structures or many blind holes, ultrasonic cleaning or chemical cleaning processes can be used to thoroughly remove internal residues, ensuring the unobstructed flow of capillary channels and surface cleanliness, preventing powder blockage that could affect subsequent working fluid flow and heat transfer efficiency.

[0045] Step S4: Sinter the homogenized slab blank after powder removal.

[0046] The cleaned, homogenized slab is then placed in a high-temperature furnace for sintering heat treatment to eliminate residual internal stress accumulated during additive manufacturing and optimize the material's microstructure. The sintering process is carried out in a reducing atmosphere (such as hydrogen or decomposed ammonia) to prevent oxidation of the copper alloy surface. The heating temperature is controlled within a specific range below the solidus line of the copper alloy and maintained for a certain duration to promote atomic diffusion and metallurgical bonding between particles. This treatment not only enhances the connection strength between the micro-needles, variable cross-section micropillars, and microporous mesh structure, improving the overall structure's resistance to liquid erosion, but also prevents the collapse of the porous structure. Thus, while ensuring mechanical stability, it maintains the excellent capillary absorption performance of the composite gradient liquid-absorbing core layer.

[0047] Step S5: Inject working fluid into vacuum chamber 5 and perform vacuuming and sealing to obtain a copper alloy heat exchange plate.

[0048] The sintered and strengthened vapor chamber blank possesses the final geometric shape and structural strength, and then enters the encapsulation and activation stage. Based on the target operating temperature range of the vapor chamber, deionized water, methanol, or ammonia is selected as the heat transfer medium. A precisely calculated amount of the medium is injected into the vacuum chamber 5 inside the blank, ensuring that the medium fully wets the capillary wick while leaving sufficient vapor space. After injection, the vacuum chamber 5 is immediately evacuated using a vacuum pump to remove non-condensable gases such as air, reducing the internal pressure to the level corresponding to the saturated vapor pressure of the medium, thereby lowering the evaporation initiation temperature of the medium. Once the vacuum level reaches the predetermined target, the injection port is permanently sealed using methods such as cold pressure welding, argon arc welding, or laser welding. Thus, a copper alloy vapor chamber filled with the medium and in a sealed vacuum state is prepared, possessing complete phase change heat transfer capabilities.

[0049] Through the above steps, the preparation method provided in this application realizes a complete manufacturing process from digital model to high-performance vapor chamber. The three-dimensional model construction ensures the geometric accuracy of the non-TPMS three-dimensional capillary core structure; the zoned scanning strategy allocates energy differently according to the density and porosity requirements of different regions, balancing the molding quality of the shell strength and the function of the capillary core; powder removal and sintering processes ensure the cleanliness of the internal channels and the reliability of the structure; and the final liquid injection and sealing endows the vapor chamber with thermal circulation functionality. Each step is closely integrated, working together to solve the technical problems of cumbersome procedures, high contact thermal resistance, and structural limitations in traditional manufacturing processes.

[0050] In another optional embodiment, the method further includes: scanning the dense area of ​​the lower base plate 2 using first scanning parameters, the first scanning parameters including: power 600W-700W, speed 1000mm / s; scanning the composite gradient liquid absorption core layer 6 using second scanning parameters, and for the variable cross-section micropillar region, using a spiral gradient filling scanning strategy, the second scanning parameters including: power 500W-600W, speed 1200mm / s-1500mm / s.

[0051] The first scanning parameter, serving as the process specification for constructing the dense substrate of the vapor chamber, corresponds to a high energy density. This high energy density input aims to ensure complete melting of the metal powder within the dense area of ​​the lower base plate and achieve sufficient metallurgical bonding, thereby eliminating porosity and crack defects and guaranteeing extremely high airtightness and thermal conductivity in this area. In specific implementation, the laser power can be set to 600W-700W, and the scanning speed can be set to 1000mm / s. For example, when the laser power is set to 650W and the scanning speed is set to 1000mm / s, the laser energy input can form a molten pool with a suitable aspect ratio, resulting in a dense microstructure between the remelted layer and the solidified layer, thus meeting the vapor chamber's requirements for substrate strength.

[0052] The second scanning parameter is used to construct the porous structure of the composite gradient liquid-absorbing core layer 6. Its design must balance the shape preservation of the capillary core structure with the maintenance of porosity. Compared to the first scanning parameter, the second scanning parameter corresponds to a lower energy density to avoid the collapse or loss of connectivity of the microstructure due to excessive melting. Specifically, the laser power is set to 500W-600W, and the scanning speed is set to 1200mm / s-1500mm / s. For example, the laser power can be set to 550W, and the scanning speed can be set to 1300mm / s. With this relatively low linear energy density input, the powder particles mainly form sintered neck connections or partial melting bonds, thereby accurately preserving the geometry of the microneedle rib array 7, the variable cross-section micropillar array 8, and the microporous network structure 9, ensuring the effective realization of the porosity gradient characteristics.

[0053] To address the specific geometric feature of the variable cross-section micropillar region, a spiral gradient filling scanning strategy is employed for path planning. The diameter of the variable cross-section micropillar region varies along its height (e.g., bottom diameter 100μm-150μm, top diameter 40μm-60μm). Using conventional parallel grating scanning, uneven heat accumulation at the variable cross-section easily leads to step effects or structural deformation. The spiral gradient filling scanning strategy is configured to start from the bottom base region of the micropillar and extend upwards layer by layer along a continuous spiral path. During this strategy, the scanning path naturally contracts towards the center as the micropillar diameter shrinks. By dynamically adjusting the laser focus point, the laser energy is ensured to always act on the geometric center or solid part of the variable cross-section. This scanning method can homogenize the heat input at the variable cross-section and reduce thermal stress concentration caused by sudden changes in scanning direction, thereby ensuring that the inverted conical or stepped-concave micropillar structure has precise dimensional accuracy and good perpendicularity.

[0054] The aforementioned partitioned scanning strategy treats the dense region of the lower base plate 2 and the composite gradient liquid-absorbing core layer 6 differently, utilizing differentiated configurations of the first and second scanning parameters to achieve high mechanical properties in the dense region and structural fidelity in the porous region within the same printing process. Simultaneously, by introducing a spiral gradient filling scanning strategy into the variable cross-section micropillar region, the forming difficulty of complex gradient structures in additive manufacturing is overcome. This results in a final homogenized plate blank that possesses both the sealed vacuum chamber 5 and a complete three-dimensional capillary core structure 4, providing a high-quality blank foundation for subsequent powder removal and sintering processes.

[0055] In an alternative implementation, the method further includes generating a self-supporting angle-optimized slicing path for the variable cross-section micropillar region of the three-dimensional model.

[0056] In laser additive manufacturing, variable cross-section micropillar arrays typically exhibit an inverted conical or stepped shrinkage shape with a large bottom diameter and a small top diameter. As the printing height increases, its cantilever characteristics become significantly enhanced, easily leading to powder collapse or insufficient interlayer adhesion, resulting in structural deformation or molding failure. Therefore, a slicing path optimization mechanism is introduced in the data processing stage to plan the layered paths of the variable cross-section micropillar region. This process, based on the geometric features of the 3D model and the process constraints of laser printing, calculates the relationship between the overhang angle of each printed layer and the critical forming angle, adjusting the filling order, direction, and start and end points of the scanning vectors to generate optimized slicing paths.

[0057] A slicing algorithm is used to identify the suspended profile of the variable cross-section micropillar, and the scanning path is designed as a spiral or concentric circle path that gradually changes inward along the edge of the profile. This path planning utilizes the solidified preceding layer as the physical support for the subsequent cladding layer, constructing a self-supporting structure similar to an arch bridge effect. The generated self-supporting angle-optimized slicing path serves as a specific process instruction file, containing the scanning trajectory coordinates, laser switch control points, and scanning speed vector for each layer. This path aims to ensure that the variable cross-section micropillar maintains morphological stability by relying on its own accumulated solidified molten pool layer in the absence of an external support structure.

[0058] Furthermore, the horizontal cross-section of the variable cross-section micropillars is divided into several sectors, and an alternating scanning strategy is adopted to allow heat accumulation between adjacent scan lines, forming tiny temporary support steps. This self-supporting angle-optimized slicing path provides precise data input for the subsequent partitioned scanning strategy, enabling the laser beam to clad layers according to a predetermined trajectory, effectively avoiding printing defects caused by excessive overhang angles. Through this slicing path optimization, the integrity of the variable cross-section micropillar array structure can be maintained while eliminating the introduction of internal support structures, reducing post-processing steps, and improving the surface quality and pore connectivity of the composite gradient liquid-absorbing core layer.

[0059] In another embodiment, the sintering process specifically involves placing the heat-soaked slab blank after powder removal in a reducing atmosphere furnace and holding it at 850℃-950℃ for 1-3 hours.

[0060] After descaling, the homogenized slab blank is placed in a reducing atmosphere furnace for heat treatment. The reducing atmosphere furnace can provide an oxygen-free or low-oxygen environment during the heating process. By introducing reducing gases such as hydrogen, ammonia decomposition gas, or carbon monoxide into the furnace, the oxidation reaction of copper alloy materials at high temperatures is effectively suppressed, thereby ensuring the surface quality and material properties of the workpiece.

[0061] The sintering temperature is controlled between 850℃ and 950℃. This temperature range is set based on the recrystallization temperature of the copper alloy and the activation energy of atomic diffusion between powder particles. If the temperature is below 850℃, the atomic diffusion capacity is insufficient, making it difficult to form an effective metallurgical bond, resulting in low strength of the green body. If the temperature is above 950℃, it may cause overheating or coarse grains, thereby weakening the mechanical properties. In practice, the sintering temperature can be specifically set to 880℃, 900℃, or 920℃, etc., to ensure that the material achieves densification in the solid state.

[0062] The holding time is set to 1 to 3 hours. During this period, the internal temperature of the billet tends to be uniform and maintained for a sufficient time to complete the physical metallurgical process. For example, the holding time can be selected as 1.5 hours, 2 hours, or 2.5 hours. The holding process not only releases the residual internal stress generated by rapid heating and cooling in laser additive manufacturing, reducing the risk of workpiece deformation or cracking, but also promotes necking and growth between powder particles through solid-state sintering. This process increases the bonding area between particles, improves the overall strength and mechanical stability of the three-dimensional capillary core structure, and maintains the connectivity of the pore structure, ensuring that the heat spreader has excellent capillary performance in the subsequent liquid injection and operation stages.

[0063] In another optional embodiment, the powder removal process specifically involves removing unmelted residual powder from the three-dimensional capillary core structure 4 inside the homogenized slab blank by mechanical vibration or an air gun.

[0064] In the vapor chamber preform formed by laser additive manufacturing, the composite gradient liquid-absorbing core layer has a complex three-dimensional microstructure, particularly with numerous micropores between the microneedle rib array and the variable cross-section micropillar array. During the printing process, some unmelted or semi-melted metal powder inevitably remains inside these structures or adheres to their surfaces. If not effectively removed, this residual powder will block capillary channels, disrupt the capillary flow path of the working fluid, and ultimately lead to heat transfer failure of the vapor chamber. Therefore, it is necessary to remove the residual powder trapped inside the complex structure using physical means to restore the designed pore connectivity.

[0065] The specific cleaning process employs mechanical vibration, air gun purging, or a combination thereof. In mechanical vibration treatment, the heated slab blank is fixed on an ultrasonic vibration table or mechanical vibration device. By controlling the vibration frequency and amplitude, the blank generates high-frequency micro-amplitude vibrations. The vibration energy is transferred to the interior of the three-dimensional capillary core structure 4, disrupting the surface adhesion and friction between the unmelted residual powder and the solidified structure, causing the powder particles to loosen and detach from the structure surface. Subsequently, under the action of gravity, they flow out from the bottom opening or the reserved powder cleaning holes.

[0066] In the air gun purging process, high-pressure compressed air is directed through a precision nozzle onto the internal chamber 5 and the composite gradient liquid-absorbing core layer 6 of the homogenized slab. The high-speed airflow creates turbulence and shear force within the pore channels of the three-dimensional capillary core structure 4, lifting and carrying away small powder particles with low adhesion to the outside of the slab. In actual operation, the high-pressure air gun is first inserted into the vacuum chamber to purge the variable cross-section micro-pillar array 8 and the microporous mesh structure 9, using a large flow of air to disperse deep-seated powder. Subsequently, mechanical vibration is used to shake off and discharge the more difficult-to-remove powder from the bottom micro-needle rib array 7. Through the synergistic effect of the mechanical vibration and air gun purging, the three-dimensional capillary core structure 4 inside the homogenized slab maintains its designed porosity and connectivity, providing a smooth physical channel for subsequent working fluid circulation.

[0067] Example 1 This embodiment provides a method for preparing a copper alloy heat sink based on laser additive manufacturing, including the following steps: (1) Gas-atomized Cu-Cr-Ni copper alloy powder was selected, with a powder particle size range of 15μm-45μm; the alloy composition by mass percentage was: Cr 0.5%, Ni 1.2%, Cu 98.3%. In this ratio, Cr improves the laser absorption rate and refines the grains, making it suitable for SLM laser additive manufacturing and avoiding the defects of high reflection and easy spheroidization cracking of pure copper.

[0068] (2) Establish a three-dimensional model of the heat exchanger, which includes an upper cover plate 1, a lower bottom plate 2, array support columns 3, and a composite gradient liquid absorption core layer 6 (including a microneedle rib array 7, a variable cross-section microcolumn array 8, and a microporous mesh structure 9). For the variable cross-section microcolumn region, generate a self-supporting angle-optimized slicing path and adopt a concentric spiral gradient filling trajectory to eliminate heat accumulation defects in the suspended layer and ensure the geometric accuracy of the inverted cone shape at the bottom (100μm-150μm) and top (40μm-60μm) of the microcolumns.

[0069] (3) A 500W fiber selective laser melting device was selected, with a spot diameter of 80μm, a printing layer thickness of 60μm, and a scanning interval of 0.12mm. Printing was carried out according to the following printing strategy to obtain a homogenized slab blank: 1) Dense area of ​​the bottom plate (first scanning parameters): laser power 650W, scanning speed 900mm / s, high energy density to achieve full fusion, ensuring the airtightness of the vacuum chamber, the actual shell density is 99.5%.

[0070] 2) Composite gradient liquid absorption core layer (second scanning parameters): laser power 550W, scanning speed 1200mm / s; the variable cross-section micropillar region uses a separate spiral gradient filling scanning strategy, which shrinks the scanning trajectory synchronously with the shrinkage of the cross-section micropillar diameter to homogenize heat input and avoid step deformation.

[0071] (4) The heat-soaked slab blank is cut off from the substrate by wire cutting. First, the vacuum chamber 5 is directionally purged with a high-pressure air gun, and then ultrasonic mechanical vibration is used to remove the powder. The unmelted powder inside the micro-needle ribs and variable cross-section micro-pillars is completely removed to ensure that the capillary channels are fully connected.

[0072] (5) The hot plate blank after cleaning is placed in a hydrogen protective atmosphere furnace and kept at 900℃ for 2 hours to eliminate the residual stress of rapid SLM melting and strengthen the metallurgical bond of the microstructure without destroying the gradient pore structure.

[0073] (6) After sintering, inject a measured amount of deionized water working fluid into vacuum chamber 5 and evacuate to 10°C. -3Pa, cold-press welding seals the injection port, resulting in a finished copper alloy heat spreader (such as...). Figure 5 (As shown).

[0074] The finished copper alloy heat sink prepared in this embodiment was subjected to electron microscopy scanning and performance testing. The results are as follows: (1) such as Figure 3 As shown, the microneedle rib array 7 in the gradient pore capillary core structure 6 has a trapezoidal cross-section, a height of 0.3 mm, a bottom width of 40 μm, and a measured porosity of 26%. The surface of the ribs is continuously porous, with a large specific surface area, resulting in a significant enhancement effect on evaporative heat transfer. (2) such as Figure 4 As shown, in the gradient pore capillary core structure 6, the microcolumn array 8 with variable cross-section has a bottom diameter of 120 μm and a top diameter of 50 μm, exhibiting a smooth inverted conical shrinkage, with a measured porosity of 44%; the column does not collapse or have powder adhesion, and the continuous capillary pressure gradient is fully formed. (3) The measured porosity of the microporous mesh structure 9 is 61%, and the three-dimensional interconnected pores provide a low-resistance channel for vapor diffusion and condensate reflux.

[0075] (4) The finished copper alloy heat spreader is integrally formed without interfacial contact thermal resistance, and the measured shell density is 99.5%. Under the condition of heat flux density of 120W / cm², there is no local drying, and the temperature difference on the plate surface is ≤2.1℃; the cavity is stable under pressure, and the vacuum sealing meets the requirements for long-term electronic heat dissipation.

[0076] Example 2 This embodiment provides a method for preparing a copper alloy heat sink based on laser additive manufacturing, including the following steps: (1) Gas atomized Cu-Cr-Ni copper alloy powder with a particle size of 15-45μm; alloy composition by mass percentage: Cr 0.3%, Ni 0.8%, Cu 98.9%. Reducing the amount of Cr and Ni increases the proportion of copper in the matrix and slightly improves the basic thermal conductivity.

[0077] (2) The overall structure dimensions of the heat spreader and the geometric parameters of the gradient capillary core are the same as those in Example 1; only the thickness of the printed slice layer is adjusted to 40μm; the self-supporting optimized slice + spiral gradient filling scanning path is used for the variable cross-section micro-pillar area to ensure the accuracy of the micro-structure dimensions.

[0078] (3) The printing equipment used is the same as in Example 1, with the spot diameter set to 80 μm, the scanning spacing set to 0.12 mm, and the layer thickness set to 40 μm. Printing is performed according to the following printing strategy to obtain a homogeneous heat-generating plate blank: 1) Dense area of ​​the bottom plate: The laser power is 650W and the scanning speed is 1000mm / s; thin-layer printing further improves the shell density, and the measured shell density is 99.7%.

[0079] 2) Composite gradient liquid absorption core layer: laser power is 550W, scanning speed is 1300mm / s; variable cross-section micropillars adopt the spiral gradient filling scanning strategy, and thin-layer molding reduces the risk of thermal deformation of microstructures.

[0080] (4) The powder removal and sintering process parameters are the same as in Example 1, and the finished copper alloy heat exchange plate is obtained.

[0081] The finished copper alloy heat sink prepared in this embodiment was subjected to electron microscopy scanning and performance testing. The results are as follows: 1) The porosity of the microneedle rib array 7 was measured to be 24%, and the trapezoidal cross-section needle ribs were formed regularly without interlayer misalignment.

[0082] 2) The measured porosity of the cross-sectional micro-pillar array 8 is 42%. The surface of the inverted conical column is smooth and there is no powder agglomeration blocking the pores.

[0083] The measured porosity of the top microporous mesh structure is 59%, and the gradient pore distribution is continuous and uniform.

[0084] 3) The measured shell density is 99.5%. Under the same high heat flux of 120W / cm², the plate surface temperature difference is ≤2.3℃, and the heat transfer performance is basically the same as that of Example 1.

[0085] The above are merely preferred embodiments of this application and do not limit the patent scope of this application. Any equivalent structural or procedural transformations made using the content of this application's specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of this application.

Claims

1. A copper alloy heat spreader based on laser additive manufacturing, characterized in that, It includes an integrated upper cover plate, lower base plate, support columns, and a three-dimensional capillary core structure; A sealed vacuum chamber is formed between the upper cover plate and the lower base plate, and the support columns are arranged in an array within the vacuum chamber; The three-dimensional capillary core structure includes a composite gradient liquid-absorbing core layer disposed on the inner wall of the lower base plate. The composite gradient liquid-absorbing core layer includes a microneedle rib array, a variable cross-section microcolumn array, and a microporous mesh structure arranged sequentially from bottom to top, and the porosity of the microneedle rib array, the variable cross-section microcolumn array, and the microporous mesh structure increases sequentially.

2. The copper alloy heat spreader based on laser additive manufacturing according to claim 1, characterized in that, The porosity of the microneedle rib array is 20%-30%, the porosity of the variable cross-section micropillar array is 40%-50%, and the porosity of the microporous mesh structure is 55%-65%.

3. The copper alloy heat spreader based on laser additive manufacturing according to claim 1, characterized in that, The microneedle ribs in the microneedle rib array have triangular or trapezoidal cross sections with a height of 0.2mm-0.5mm and a base width of 30μm-50μm.

4. The copper alloy heat spreader based on laser additive manufacturing according to claim 1, characterized in that, The variable cross-section micropillar array has a bottom diameter of 100μm-150μm and a top diameter of 40μm-60μm, exhibiting an inverted conical or stepped contraction.

5. The copper alloy heat spreader based on laser additive manufacturing according to claim 1, characterized in that, The copper alloy components in the copper alloy heat sink, by mass percentage, include: Cr: 0.2%-0.8%, Ni: 0.5%-2.0%, with the balance being Cu and impurities.

6. A method for preparing a copper alloy heat sink based on laser additive manufacturing as described in any one of claims 1-5, characterized in that, Includes the following steps: A three-dimensional model of the copper alloy heat exchanger is constructed. The three-dimensional model includes an upper cover plate, a lower base plate, support columns, and a three-dimensional capillary core structure. The three-dimensional capillary core structure includes a composite gradient liquid absorption core layer. Set the printing parameters of the laser additive manufacturing equipment, and use a partitioned scanning strategy to print to obtain a homogeneous slab blank; The heat-soaking plate blank is removed from the substrate of the laser additive manufacturing equipment, and then the removed heat-soaking plate blank is subjected to powder removal treatment. The heat-soaked slab blank after powder removal is then subjected to sintering treatment; A working fluid is injected into the vacuum chamber, and a vacuum is drawn and sealed to obtain the copper alloy heat exchange plate.

7. The preparation method according to claim 6, characterized in that, The partitioned scanning strategy includes: for the dense area of ​​the bottom plate, scanning is performed using a first scanning parameter, which includes: power 600W-700W and speed 1000mm / s. For the composite gradient liquid absorption core layer, the second scanning parameters are used for scanning, and for the variable cross-section micropillar region, a spiral gradient filling scanning strategy is adopted. The second scanning parameters include: power 500W-600W, speed 1200mm / s-1500mm / s.

8. The preparation method according to claim 7, characterized in that, Also includes: For the variable cross-section microcolumn region of the three-dimensional model, a self-supporting angle-optimized slicing path is generated.

9. The preparation method according to claim 6, characterized in that, The sintering process is as follows: the heat-soaked slab blank after powder removal is placed in a reducing atmosphere furnace and held at 850℃-950℃ for 1 hour to 3 hours.

10. The preparation method according to claim 6, characterized in that, The powder removal process involves removing unmelted residual powder from the three-dimensional capillary core structure inside the heat-soaked slab blank using mechanical vibration or an air gun.