A laser composite additive remanufacturing process for valve production
By employing a stepwise laser additive manufacturing process involving interface conditioning and structural restoration of additive materials, the problem of interface exposure affecting defect areas in valve laser additive remanufacturing was solved, thus improving the quality and stability of the repaired area.
Patent Information
- Application Number
- CN202611635569.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing valve laser additive remanufacturing process, the state of the exposed interface after the defect area is removed affects the subsequent structural restoration of the additive area, which can easily cause internal defects in the repair area and reduce the reliability of valve remanufacturing.
The defect area is subjected to a first laser additive treatment using an interface conditioning additive material to form an interface conditioning additive layer. A portion is removed along the direction away from the valve substrate, while the metallurgical bonding portion near the substrate is retained. Subsequently, a second laser additive treatment is performed using a structural restoration additive material. The interface conditioning material and the structural restoration material have different chemical compositions.
By using a step-by-step process of interface conditioning and structural restoration additive materials, the adverse effects of exposed interface conditions on the repaired area are reduced, the quality and stability of the repaired area are improved, and the functional distinction between interface condition improvement and structural restoration is achieved.
Smart Images

Figure CN123103018A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser additive remanufacturing technology, and specifically to a laser composite additive remanufacturing process for valve production. Background Technology
[0002] As a crucial component of fluid control equipment, valves may develop defects such as cracks, shrinkage cavities, porosity, or inclusions during the casting process. During service, they may also suffer localized damage from pressure, erosion, corrosion, and mechanical forces. To address these defects, existing technologies typically employ laser additive manufacturing to repair these areas. This involves using a laser to melt metal powder or wire and deposit it onto the area to be repaired, restoring the valve's structural dimensions. Some existing technologies further enhance the performance of the repaired area by adding different material layers or using functional additive materials, such as transition layers, functional layers, or wear-resistant layers, to improve the repaired area's service life.
[0003] However, in current valve laser additive remanufacturing processes, after removing obvious defects, structural restoration additive materials are typically used directly to repair the exposed interface. Even after defect removal, the exposed interface may still contain residual oxides, inclusions, or contaminated areas at the defect edges. This interface condition affects the subsequent additive repair area, easily causing internal defects and reducing the reliability of the remanufactured valve. Therefore, how to effectively condition the defect-exposed interface before structural restoration additive processing to improve the quality of the subsequent additive repair area is a problem that needs to be solved in current valve laser composite additive remanufacturing processes. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a laser composite additive remanufacturing process for valve production. This method solves the problem that in existing valve laser additive remanufacturing processes, the exposed interface state after the removal of defective areas affects the subsequent structural restoration additive area, making the structural restoration additive area prone to defects.
[0005] To achieve the above objectives, the present invention provides the following technical solution: A laser composite additive remanufacturing process for valve production includes the following steps: S1. Perform defect detection on the valve to be repaired, determine the defect area, and remove the defective material in the defect area to form a repair area with an exposed interface; S2. The repair area is subjected to a first laser additive treatment using an interface conditioning additive material to form an interface conditioning additive layer, wherein the interface conditioning additive layer forms a metallurgical bond with the exposed interface. S3. Remove the portion of the interface conditioning additive layer away from the valve substrate along a direction away from the valve substrate, and retain the remaining portion close to the valve substrate that forms a metallurgical bond with the valve substrate to form an interface conditioning area for subsequent additive repair. S4. A second laser additive process is performed on the interface conditioning region using a structural restoration additive material to form a structural restoration additive region. The interface conditioning additive material has a different chemical composition from the structural restoration additive material. S5. The additive manufacturing area of the structure is machined to restore the target size of the valve.
[0006] Furthermore, the interface conditioning additive material is an iron-based alloy powder material, including Fe, Cr, Ni, Mn, Si and B elements.
[0007] Further, the interface conditioning additive material comprises, by weight percentage: Cr: 16-22 wt% Ni: 8-14 wt% Mo: 0.5–3 wt% Mn: 0.8–3 wt% Si: 0.8–2.5 wt% B: 0.1–0.8 wt% Ti: 0.05~0.5wt%; The balance consists of Fe and unavoidable impurities.
[0008] Furthermore, the heat input of the first laser additive processing is lower than that of the second laser additive processing.
[0009] Furthermore, the thickness of the interface conditioning additive layer is 0.5–2.0 mm.
[0010] Furthermore, the thickness of the removed interface conditioning additive layer accounts for 30% to 70% of the total thickness of the interface conditioning additive layer.
[0011] Furthermore, the interface-conditioning additive material is conveyed to the laser-acting area of the first laser additive processing via a coaxial powder feeding method, and the powder particle size of the interface-conditioning additive material is 15-80 μm.
[0012] Furthermore, the structural restoration additive material is an iron-based alloy material, including Fe, Cr, Ni and Mo elements.
[0013] Further, the structural restoration additive material comprises, by weight percentage: Cr: 18–24 wt% Ni: 9–16 wt% Mo: 1-4 wt% Nb: 0.2–1 wt%; W: 0.5–2 wt%; The balance consists of Fe and unavoidable impurities.
[0014] Furthermore, the defective area includes areas with cracks, shrinkage cavities, looseness, or inclusions, and the valve includes a stainless steel valve or an alloy steel valve.
[0015] This invention provides a laser composite additive remanufacturing process for valve production. It offers the following advantages: 1. This invention uses interface conditioning additive materials to perform a first laser additive processing on the repair area after defect removal to form an interface conditioning additive layer. The portion of the interface conditioning additive layer away from the valve substrate is removed along the direction away from the valve substrate, and the remaining portion close to the valve substrate and forming a metallurgical bond with the valve substrate is retained as the interface conditioning area. This allows the subsequent structural restoration additive processing to be based on the interface conditioning area, reducing the adverse effects of the exposed interface state on the structural restoration additive area and improving the quality of the repair area.
[0016] 2. This invention sets up interface conditioning additive materials and structural restoration additive materials, so that the interface conditioning additive materials are used to improve the interface state of the repair area, and the structural restoration additive materials are used to restore the valve structural dimensions, thereby realizing the functional distinction between the interface conditioning process and the structural restoration process.
[0017] 3. By controlling the heat input of the first laser additive manufacturing process to be lower than that of the second laser additive manufacturing process, the first and second laser additive manufacturing processes can meet the interface conditioning and structural restoration requirements respectively, which is beneficial to improving the remanufacturing stability of valve defect areas. Attached Figure Description
[0018] Figure 1 This is a flowchart of a laser composite additive remanufacturing process for valve production according to the present invention; Figure 2 This is a schematic diagram of the interface conditioning additive layer processing relationship of the present invention; Figure 3 This is a comparison chart of the test results of the repaired area defects in Embodiment 1 and Comparative Example 1 of the present invention; Figure 4 This is a comparison chart of the interface bonding defect test results of Embodiment 1 and Comparative Example 2 of the present invention. Detailed Implementation
[0019] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0020] As critical pressure-bearing components in industrial equipment, valves may contain defects such as cracks, shrinkage cavities, porosity, or inclusions during the manufacturing process. During long-term service, they may also be subject to erosion, corrosion, and mechanical damage. Existing laser additive remanufacturing methods typically use repair materials to directly additive process the repaired area after defect removal to restore the valve's structural dimensions. However, because the formation of internal defects in valve castings may be accompanied by oxides, inclusions, and contaminated defect interfaces, residual defects may still exist at the exposed interface after removing obvious defects, affecting the quality of subsequent additive bonding. This can easily lead to defect accumulation in the repaired area during direct structural restoration additive processing, reducing remanufacturing reliability. Current valve laser repair technologies mostly focus on improving the performance of the repaired area by optimizing laser cladding materials or adding functional layers, such as using transition layers to improve bonding performance or using wear-resistant materials to form a surface repair layer. However, these methods primarily address the performance improvement of the repair layer and do not address the condition conditioning of the exposed interface after defect removal.
[0021] Based on the above problems, the inventors have studied the laser composite additive remanufacturing process for valve defect areas. They discovered that if, before the structural restoration additive processing, an interface conditioning additive material with interface conditioning properties is first applied to the repair area using a first laser additive processing method, the resulting interface conditioning additive layer forms a metallurgical bond with the exposed interface. This first laser additive processing method alters the interface state of the repair area. Then, the portion of the interface conditioning additive layer away from the valve substrate is removed along the direction away from the valve substrate, retaining the remaining portion close to the valve substrate and forming a metallurgical bond with it as the interface conditioning area. Based on this, a second laser additive processing method using a structural restoration additive material is then applied to restore the missing valve structure. For example... Figure 1 As shown, the present invention is a laser composite additive remanufacturing process method for valve production based on the above-mentioned technical concept.
[0022] In this invention, the interface conditioning additive material and the structural restoration additive material play different roles. The interface conditioning additive material is used to form an interface conditioning additive layer to adjust the interface state of the repair area; the structural restoration additive material is used to form a structural restoration additive area to restore the valve's structural dimensions. Through this two-stage laser additive processing method, the interface conditioning process and the structural restoration process of the valve defect area are distinguished, avoiding the direct use of structural restoration additive material to additively repair exposed defect interfaces.
[0023] The experimental materials used in the following examples are all commercially available analytical grade or industrial grade materials. Unless otherwise specified, the experimental materials have not undergone any further processing.
[0024] In this embodiment of the invention, the interface conditioning additive material and the structure restoration additive material are prepared using metal alloy powder materials, and the main experimental raw materials used include: Iron powder, Fe, CAS No.: 7439-89-6; Chromium powder, Cr, CAS No.: 7440-47-3; Nickel powder, Ni, CAS No.: 7440-02-0; Molybdenum powder, Mo, CAS No.: 7439-98-7; Manganese powder, Mn, CAS No.: 7439-96-5; Silicon powder, Si, CAS No.: 7440-21-3; Boron powder, B, CAS No.: 7440-42-8; Titanium powder, Ti, CAS No.: 7440-32-6; Niobium powder, Nb, CAS No.: 7440-03-1; Tungsten powder, W, CAS No.: 7440-33-7.
[0025] The above-mentioned metal raw materials were weighed according to the mass percentage specified in the example, and formed into an alloy melt by vacuum induction melting. Then, inert gas was used to atomize and sieve the powder to prepare interface conditioning additive materials and structure restoration additive materials respectively. Both interface conditioning additive materials and structure restoration additive materials use pre-alloyed powders, and do not use direct mechanical mixing of powders of each element as additive materials.
[0026] In this invention, the thermal input of the first laser additive processing and the second laser additive processing is characterized by the thermal input per unit scan length, Q=P / v, where P is the laser power and v is the scanning speed. Under the condition that the laser spot and equipment conditions are the same, the thermal input of the first laser additive processing and the second laser additive processing are compared by the Q value.
[0027] The second laser additive processing adopts a layer-by-layer deposition method. Based on the remaining depth of the repair area after the formation of the interface conditioning area, the structural restoration additive material deposition is repeated until a structural restoration additive area that meets the requirements of subsequent machining is formed.
[0028] Example 1 This embodiment provides a laser composite additive remanufacturing process for valve production, specifically for repairing defective areas in stainless steel valve castings. First, the valve to be repaired undergoes defect detection to identify crack, shrinkage, porosity, or inclusion defect areas on the valve surface. The defective material in these areas is then removed using machining, creating a repair area with an exposed interface. In this embodiment, the valve to be repaired is a CF8M stainless steel valve, and the defective area is a shrinkage defect formed during the casting process. Testing determined the maximum defect depth to be 3.2 mm. Milling is then used to remove the material from the defective area, creating a repair area with a depth of 3.8 mm.
[0029] like Figure 2 As shown, after the repair area is prepared, the repair area is subjected to a first laser additive treatment using an interface conditioning additive material to form an interface conditioning additive layer. In this embodiment, the interface conditioning additive material is an iron-based alloy powder material, which, by mass percentage, includes Cr 16wt%, Ni 8wt%, Mo 0.5wt%, Mn 0.8wt%, Si 0.8wt%, B 0.1wt%, Ti 0.05wt%, with the balance being Fe and unavoidable impurities. The interface conditioning additive material is delivered to the laser action area via a coaxial powder feeding method, and the powder particle size ranges from 15μm to 80μm. The first laser additive treatment uses process parameters of 800W laser power, 18mm / s scanning speed, and 3g / min powder feeding rate to melt the interface conditioning additive material and form a metallurgical bond with the exposed interface, forming an interface conditioning additive layer with a thickness of 0.5mm.
[0030] After the interface conditioning additive layer is formed, a portion of the interface conditioning additive layer with a thickness of 0.15 mm away from the valve substrate is removed along the direction away from the valve substrate. The thickness of the removed portion accounts for 30% of the total thickness of the interface conditioning additive layer. The remaining portion that is close to the valve substrate and forms a metallurgical bond with the valve substrate is retained as the interface conditioning area.
[0031] After the interface conditioning region is prepared, a second laser additive manufacturing process is performed using a structural restoration additive material. In this embodiment, the structural restoration additive material is an iron-based alloy material, comprising, by mass percentage: Cr 18wt%, Ni 9wt%, Mo 1wt%, Nb 0.2wt%, W 0.5wt%, with the balance being Fe and unavoidable impurities. The second laser additive manufacturing process uses process parameters of 2200W laser power, 10mm / s scanning speed, and 8g / min powder feed rate to deposit the structural restoration additive material on the surface of the interface conditioning region, forming the structural restoration additive region and restoring the missing valve structure.
[0032] After completing the second laser additive processing, the structural restoration additive area is machined to restore the repaired area to the target size of the valve, and the surface quality and dimensions of the processed valve are inspected.
[0033] Example 2 This embodiment provides a laser composite additive remanufacturing process for valve production. Unlike Embodiment 1, this embodiment is used for repairing crack defects in alloy steel valves. First, the valve to be repaired undergoes defect detection to identify the crack defect area. Then, the material in the crack area is removed by machining, creating an exposed interface in the repair area. In this embodiment, the repair area depth is 8 mm.
[0034] An interface-conditioned additive manufacturing process is performed using an interface-conditioned additive material to form an interface-conditioned additive layer. The interface-conditioned additive material, by weight percentage, comprises 22wt% Cr, 14wt% Ni, 3wt% Mo, 3wt% Mn, 2.5wt% Si, 0.8wt% B, and 0.5wt% Ti, with the balance being Fe and unavoidable impurities. The first laser additive manufacturing process uses a laser power of 1600W, a scanning speed of 8mm / s, and a powder feed rate of 8g / min to melt the interface-conditioned additive material and form the interface-conditioned additive layer. In this embodiment, the thickness of the formed interface-conditioned additive layer is 2.0mm.
[0035] After the interface conditioning additive layer is formed, a portion of the interface conditioning additive layer with a thickness of 1.4 mm away from the valve substrate is removed along the direction away from the valve substrate. The thickness of the removed portion accounts for 70% of the total thickness of the interface conditioning additive layer. The remaining portion that is close to the valve substrate and forms a metallurgical bond with the valve substrate is retained as the interface conditioning area.
[0036] Subsequently, a second laser additive manufacturing process was performed using a structural restoration additive material. In this embodiment, the structural restoration additive material, by mass percentage, comprises 24wt% Cr, 16wt% Ni, 4wt% Mo, 1wt% Nb, and 2wt% W, with the balance being Fe and unavoidable impurities. The second laser additive manufacturing process uses a laser power of 3500W, a scanning speed of 6mm / s, and a powder feeding rate of 12g / min to form a structural restoration additive region. This region is then mechanically machined to restore the target dimensions of the valve.
[0037] Example 3 This embodiment provides a laser composite additive remanufacturing process for valve production. Unlike Embodiment 1, this embodiment is used for repairing inclusion defects in stainless steel valves. In this embodiment, the valve to be repaired is first inspected to identify the inclusion defect areas, and then these areas are removed to form the repair area.
[0038] The first laser additive manufacturing process was performed using an interface-modified additive material. This material contained Fe, Cr, Ni, Mn, Si, and B elements, with the following content: Cr 19 wt%, Ni 11 wt%, Mo 2 wt%, Mn 1.5 wt%, Si 1.5 wt%, B 0.4 wt%, Ti 0.2 wt%, and the balance being Fe and unavoidable impurities. The first laser additive manufacturing process used a laser power of 1200 W, a scanning speed of 12 mm / s, and a powder feed rate of 5 g / min, resulting in an interface-modified additive material layer with a thickness of 1.2 mm.
[0039] After the interface conditioning additive layer is formed, the portion of the interface conditioning additive layer away from the valve substrate with a thickness of 0.6 mm is removed along the direction away from the valve substrate. The thickness of the removed portion accounts for 50% of the total thickness of the interface conditioning additive layer, and the remaining portion with a thickness of 0.6 mm is retained as the interface conditioning area.
[0040] A second laser additive manufacturing process is performed on the interface conditioning region using a structural restoration additive material. The structural restoration additive material comprises 21wt% Cr, 12wt% Ni, 2.5wt% Mo, 0.5wt% Nb, and 1wt% W, with the balance being Fe and unavoidable impurities. In this embodiment, the second laser additive manufacturing process uses process parameters of 2200W laser power, 10mm / s scanning speed, and 8g / min powder feed rate. A layer-by-layer deposition method is used to deposit the structural restoration additive material onto the surface of the interface conditioning region, forming the structural restoration additive region. After the second laser additive manufacturing process is completed, the structural restoration additive region is machined to restore the target dimensions of the valve.
[0041] Example 4 This embodiment provides a laser composite additive remanufacturing process for valve production. This embodiment is used to repair porous defect areas in stainless steel valves. Except for the heat input parameters of the first and second laser additive treatments and the thickness of the interface conditioning additive layer, the other process conditions are the same as in Embodiment 1. Specifically, the first laser additive treatment uses a laser power of 1000W and a scanning speed of 15mm / s to form an interface conditioning additive layer; the second laser additive treatment uses a laser power of 3000W and a scanning speed of 8mm / s to form a structural restoration additive region. The heat input of the first laser additive treatment is lower than that of the second laser additive treatment.
[0042] In this embodiment, the thickness of the interface conditioning additive layer is 1.5 mm. A portion of the interface conditioning additive layer with a thickness of 0.75 mm away from the valve substrate is removed along the direction away from the valve substrate. The thickness removed accounts for 50% of the total thickness of the interface conditioning additive layer. The remaining portion that is close to the valve substrate and forms a metallurgical bond with the valve substrate is retained as the interface conditioning area, and a second laser additive processing is performed on the interface conditioning area.
[0043] Comparative Example 1 This comparative example provides a laser additive remanufacturing process for valve production. The difference from Example 1 is that no interface conditioning additive layer is set up to form an interface conditioning additive material. Instead, structural restoration additive material is directly used to perform laser additive processing on the repair area.
[0044] Specifically, the valve to be repaired undergoes defect detection to identify the defective area, and the defective material in the defective area is removed to form a repair area with an exposed interface. Subsequently, a structural restoration additive material is used to perform laser additive processing on the repair area, allowing the structural restoration additive material to be directly deposited on the exposed interface to form a structural restoration additive area. After the additive processing is completed, the structural restoration additive area is machined to restore the valve to its target dimensions.
[0045] In this comparative example, the structural restoration additive material is an iron-based alloy material, including Fe, Cr, Ni and Mo elements, and the same structural restoration additive material and second laser additive processing parameters as in Example 1 are used.
[0046] Comparative Example 2 This comparative example provides a laser composite additive remanufacturing process for valve production. The difference from Example 1 is that after forming the interface conditioning additive layer, the interface conditioning additive layer is not partially removed. Instead, a second laser additive treatment is performed directly on the surface of the complete interface conditioning additive layer.
[0047] Specifically, the valve to be repaired undergoes defect detection to identify the defective area, and the defective material in the defective area is removed to form a repair area. The same interface conditioning additive material as in Example 1 is used for the first laser additive processing to form an interface conditioning additive layer with a thickness of 0.5 mm.
[0048] Subsequently, without partially removing the interface conditioning additive layer, a second laser additive process is performed on the surface of the complete interface conditioning additive layer using structural restoration additive material to form a structural restoration additive area, and the target dimensions of the valve are restored through machining.
[0049] Comparative Example 3 This comparative example provides a laser composite additive remanufacturing process for valve production. The difference from Example 1 is that commercially available 316L stainless steel pre-alloy powder is used as the first additive material to replace the interface conditioning additive material. The particle size of the 316L stainless steel pre-alloy powder is the same as that of the interface conditioning additive material in Example 1. Except for the different type of the first additive material, the first laser additive processing parameters, the structure restoration additive material, the second laser additive processing parameters, and the machining conditions are all the same as those in Example 1.
[0050] Specifically, the valve to be repaired undergoes defect detection to identify the defective area, and the defective material in the defective area is removed to form the repair area. Then, 316L stainless steel pre-alloyed powder is used to perform a first laser additive manufacturing process on the repair area, forming a first additive layer with a thickness of 0.5 mm. A 0.15 mm portion of the first additive layer away from the valve substrate is removed, retaining the remaining portion near the valve substrate. Subsequently, a second laser additive manufacturing process is performed using the same structure restoration additive material as in Example 1, forming a structure restoration additive region. After completing the second laser additive manufacturing process, the structure restoration additive region is machined to restore the valve to its target dimensions.
[0051] Comparative Example 4 This comparative example provides a laser composite additive remanufacturing process for valve production, differing from Example 4 only in the heat input of the first laser additive treatment. The first laser additive treatment uses a laser power of 3000W and a scanning speed of 8mm / s, while the second laser additive treatment also uses a laser power of 3000W and a scanning speed of 8mm / s, ensuring the same heat input per unit scan length for both processes; all other process conditions are the same as in Example 4. Specifically, after defect detection and formation of the repair area in the valve to be repaired, the first laser additive treatment is performed using the same interface conditioning additive material as in Example 4 to form an interface conditioning additive layer; the portion of the interface conditioning additive layer away from the valve substrate is removed along the direction away from the valve substrate, and the second laser additive treatment is performed using the same structure recovery additive material as in Example 4.
[0052] Test Example 1: Impact of Interface Conditioning Additive Layer on Defects in the Repaired Area This test case is used to verify the effect of using interface conditioning additive materials to form an interface conditioning additive layer, and then using structural restoration additive materials to form a structural restoration additive region, on the defects in the repaired area.
[0053] Repair samples prepared in Example 1 and Comparative Example 1 were selected for testing. In Example 1, an interface conditioning additive material was used to perform a first laser additive treatment on the repair area to form an interface conditioning additive layer. The portion of the interface conditioning additive layer away from the valve substrate was then removed along the direction away from the valve substrate to form an interface conditioning area. After that, a second laser additive treatment was performed using a structural restoration additive material. In Comparative Example 1, no interface conditioning additive layer was formed, and a structural restoration additive material was directly used to perform laser additive treatment on the repair area with exposed interfaces.
[0054] The repaired areas after machining were inspected under the same ultrasonic non-destructive testing conditions. The number of defects was counted within the same inspection area, and the percentage of defect area in the repaired area was calculated. The same defect judgment criteria were used for each group of samples. The percentage of defect area in the repaired area was calculated as the ratio of the sum of the equivalent areas of all defects determined by ultrasonic non-destructive testing to the corresponding inspection area. The test results are as follows:
[0055] Depend on Figure 3 The test results show that, compared with directly using structural restoration additive materials for additive processing, in Example 1, an interface conditioning additive layer was first formed, and the portion of the interface conditioning additive layer away from the valve substrate was removed along the direction away from the valve substrate before forming the structural restoration additive area. This resulted in a reduction in the number of defects per unit inspection area and the proportion of defect area in the repaired area. This indicates that the interface conditioning additive layer and its partial removal process have an effect on defect control in the subsequent structural restoration additive area.
[0056] Test Example 2: Impact of Interface Conditioning Additive Layer Removal Process on Testing This test case is used to verify the necessity of removing the portion of the interface conditioning additive layer away from the valve substrate along the direction away from the valve substrate, while retaining the remaining portion close to the valve substrate and forming a metallurgical bond with the valve substrate to form the interface conditioning region.
[0057] Repair samples prepared in Example 1 and Comparative Example 2 were selected for testing. In Example 1, after forming an interface conditioning additive layer with a thickness of 0.5 mm, a portion of the interface conditioning additive layer with a thickness of 0.15 mm away from the valve substrate was removed, with the removed thickness accounting for 30% of the total thickness of the interface conditioning additive layer. In Comparative Example 2, after forming an interface conditioning additive layer of the same thickness, no partial removal was performed, and the structural restoration additive material was directly used for the second laser additive processing, with the remaining corresponding process conditions remaining consistent with those in Example 1.
[0058] Using the same ultrasonic nondestructive testing conditions as in Test Example 1, the number of interface bonding defects at corresponding locations between the interface conditioning additive layer and the structural restoration additive region was counted, and the area ratio of interface bonding defects was calculated. The area ratio of interface bonding defects was calculated as the ratio of the sum of the equivalent areas of interface bonding defects determined by ultrasonic nondestructive testing to the corresponding detected interface area. The test results are as follows:
[0059] Depend on Figure 4 The test results show that after removing the portion of the interface conditioning additive layer away from the valve substrate and retaining the remaining portion that is close to the valve substrate and forms a metallurgical bond with the valve substrate to form the interface conditioning area, the number of interface bonding defects and the proportion of interface bonding defect area are both lower than those of the control group 2 without partial removal. This indicates that the partial removal step of the interface conditioning additive layer is beneficial to reducing interface bonding defects after the subsequent second laser additive processing.
[0060] Test Example 3: Impact of Interface Conditioning Additive Materials on Defects in the Repaired Area This test case is used to verify the effects of interface conditioning additive materials and 316L stainless steel pre-alloyed powder on defects in the repaired area when used in the first laser additive process.
[0061] Repair samples prepared in Example 1 and Comparative Example 3 were selected for testing. In Example 1, an interface-conditioning additive material was used for the first laser additive treatment; in Comparative Example 3, 316L stainless steel pre-alloyed powder was used as the first additive material instead of the interface-conditioning additive material. Except for the difference in the first additive material, the parameters of the first laser additive treatment, the structural restoration additive material, the parameters of the second laser additive treatment, and the machining conditions were kept consistent.
[0062] Using the same ultrasonic non-destructive testing conditions as in Test Example 1, the repaired area after machining was inspected, and the number of defects per unit inspected area was counted. The test results are as follows:
[0063] The test results show that, under the condition that the partial removal process, structural restoration additive material, second laser additive processing parameters and machining conditions are kept consistent, the number of defects in the repaired area obtained by using interface conditioning additive material for the first laser additive processing is lower than that obtained by using 316L stainless steel pre-alloyed powder. This indicates that interface conditioning additive material is beneficial to reducing defects in the repaired area.
[0064] Test Example 4: Test of the thermal input relationship between the first and second laser additive processing. This test case is used to verify the effect of the lower heat input of the first laser additive process compared to the second laser additive process on the defects in the repaired area.
[0065] Repair samples prepared in Example 4 and Comparative Example 4 were selected for testing. In Example 4, the first laser additive processing used a laser power of 1000W and a scanning speed of 15mm / s, while the second laser additive processing used a laser power of 3000W and a scanning speed of 8mm / s. Based on the heat input per unit scanning length Q=P / v, the heat input of the first laser additive processing was lower than that of the second laser additive processing. In Comparative Example 4, the first and second laser additive processing used the same heat input per unit scanning length, while keeping the other process conditions consistent.
[0066] The repaired area was inspected using the same ultrasonic non-destructive testing conditions as in Test Example 1. The number of defects per unit area was counted, and the test results are as follows:
[0067] The test results show that when the heat input of the first laser additive process is lower than that of the second laser additive process, the number of defects in the repaired area is lower than when the same heat input is used for both laser additive processes. This indicates that using different heat inputs at different stages is compatible with the process requirements of interface conditioning additive and structural restoration additive.
[0068] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A laser composite additive remanufacturing process for valve production, characterized in that, Includes the following steps: S1. Perform defect detection on the valve to be repaired, determine the defect area, and remove the defective material in the defect area to form a repair area with an exposed interface; S2. The repair area is subjected to a first laser additive treatment using an interface conditioning additive material to form an interface conditioning additive layer, wherein the interface conditioning additive layer forms a metallurgical bond with the exposed interface. S3. Remove the portion of the interface conditioning additive layer away from the valve substrate along a direction away from the valve substrate, and retain the remaining portion close to the valve substrate that forms a metallurgical bond with the valve substrate to form an interface conditioning area for subsequent additive repair. S4. A second laser additive process is performed on the interface conditioning region using a structural restoration additive material to form a structural restoration additive region. The interface conditioning additive material has a different chemical composition from the structural restoration additive material. S5. Machining is performed on the additive manufacturing area of the structure to restore the target size of the valve; The interface conditioning additive material is an iron-based alloy powder material, including Fe, Cr, Ni, Mn, Si and B elements; The structural restoration additive material is an iron-based alloy material, including Fe, Cr, Ni and Mo elements.
2. The laser composite additive remanufacturing process for valve production according to claim 1, characterized in that: The interface-conditioning additive material comprises, by weight percentage: Cr: 16-22 wt% Ni: 8-14 wt% Mo: 0.5–3 wt% Mn: 0.8–3 wt% Si: 0.8–2.5 wt% B: 0.1–0.8 wt% Ti: 0.05~0.5wt%; The balance consists of Fe and unavoidable impurities.
3. The laser composite additive remanufacturing process for valve production according to claim 1, characterized in that: The heat input of the first laser additive process is lower than that of the second laser additive process.
4. The laser composite additive remanufacturing process for valve production according to claim 1, characterized in that: The thickness of the interface conditioning additive layer is 0.5–2.0 mm.
5. The laser composite additive remanufacturing process for valve production according to claim 1, characterized in that: The thickness of the removed interface conditioning additive layer accounts for 30% to 70% of the total thickness of the interface conditioning additive layer.
6. The laser composite additive remanufacturing process for valve production according to claim 1, characterized in that: The interface-conditioning additive material is delivered to the laser-acting area of the first laser additive processing via a coaxial powder feeding method, and the powder particle size of the interface-conditioning additive material is 15-80 μm.
7. The laser composite additive remanufacturing process for valve production according to claim 1, characterized in that: The structural restoration additive material comprises, by weight percentage: Cr: 18–24 wt% Ni: 9–16 wt% Mo: 1-4 wt% Nb: 0.2–1 wt%; W: 0.5–2 wt%; The balance consists of Fe and unavoidable impurities.
8. The laser composite additive remanufacturing process for valve production according to claim 1, characterized in that: The defective areas include cracks, shrinkage cavities, looseness, or inclusion defects, and the valves include stainless steel valves or alloy steel valves.