A flash welding process for railway turnouts
By confirming the pre-welding condition of railway turnout rails, clamping the mobile welding and normalizing machine, and collecting welding parameters, combined with upsetting, weld bead removal, medium-frequency induction normalizing, and air jet cooling, the problem of discontinuous condition during the welding process of turnout rails was solved, and the stability of the welded joint quality was improved.
Patent Information
- Application Number
- CN202611588321.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-17
AI Technical Summary
During the on-site flash welding of railway turnout rails, the pre-weld preparation, clamping and welding, upsetting, and post-weld heat treatment processes are difficult to control continuously, leading to fluctuations in the quality of the welded joints.
The process involves confirming the pre-welding condition of the rails to be welded, including grinding the conductive contact areas of the rail ends and webs, and checking the straightness, to create a ready-to-weld state. A mobile welding and straightening integrated machine is used for centering and clamping, and welding parameters are collected for condition assessment. After welding, upsetting, weld bead removal, medium-frequency induction normalizing, and air cooling are performed to form a continuous welding and heat treatment process.
It improves the stability of rail clamping and alignment at the turnout welding site and reduces the quality fluctuation of welded joints caused by inconsistencies in contact state, clamping state, welding process state and post-weld heat treatment state.
Smart Images

Figure CN123103145A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rail welding technology, and more specifically, to a flash welding process for railway turnouts. Background Technology
[0002] Railway turnouts are crucial structures in railway tracks used for train switching, diversion, and track connection. They typically consist of switch rails, stock rails, connecting rails, frogs, guard rails, and related connecting components. During the manufacturing, laying, and maintenance of turnout components, rail joints are formed. Common connection methods include mechanical connection, aluminothermic welding, gas pressure welding, and flash welding. Flash welding utilizes the resistance heat generated by localized contact between the welded surfaces, and applies upsetting pressure after melting to form a welded joint. This method has been applied to the welding of rails and turnout components.
[0003] For example, CN101474713A discloses a flash butt welding method for high-manganese steel frogs and rails. This method uses stainless steel as the connecting medium. After the connecting medium is processed into the shape of a rail, it is first flash-butt welded to the rail. Then, a certain length of the connecting medium is retained and subjected to low-temperature annealing. Subsequently, the end of the connecting medium is flash-welded to the high-manganese steel frog. This cited document mainly addresses the transition connection between dissimilar materials when connecting high-manganese steel frogs and rails. For on-site welding operations of railway turnout rails, the electrical conductivity of the weld end face and rail web, the straightness of the rail, the clamping condition, the treatment of weld beads after upsetting, and the heat treatment of the weld joint all affect the quality of the weld joint. However, the aforementioned cited document does not provide complete limitations on the continuous process connection between pre-weld condition confirmation, clamping welding, upsetting and weld bead removal, and post-weld heat treatment during on-site flash welding of turnout rails. Therefore, the technical problem that still needs to be solved is: how to make the pre-weld preparation, clamping and welding, upsetting and pushing and post-weld heat treatment a continuous and controlled process connection during the on-site flash welding of railway turnout rails, so as to reduce the quality fluctuation of the welded joint caused by the inconsistency between the initial state and the post-weld thermal state of the joint.
[0004] Therefore, it is necessary to design a flash welding process for railway turnouts to solve the problems existing in the current technology. Summary of the Invention
[0005] In view of this, the present invention proposes a flash welding process for railway turnouts, aiming to solve the problem that the pre-weld contact state, rail straightness state, clamping and upsetting state, and post-weld heat treatment state are difficult to continuously control during the on-site flash welding of railway turnout rails, resulting in fluctuations in the quality of the welded joint.
[0006] This invention proposes a flash welding process for railway turnouts, comprising: Before welding, the rails of the railway turnout are confirmed to be in a state of readiness. The conductive contact area of the rail ends and rail webs is ground, with the grinding range not less than 670mm from the rail end face. The straightness of the rails is also checked. When the conductive contact area shows a metallic luster and the sagitta of the rails is less than 0.5mm, the rails are ready to be welded. In the weldable preparation state, the welding head of the mobile welding machine is moved to the turnout welding station, the rail to be welded is centered and clamped, and a clamping force of 1600kN to 2000kN is used to form the clamping position. In the clamped position state, continuous flash welding or pulsed flash welding is started according to the rail type and end face condition of the rail to be welded, and the welding current, welding voltage, moving clamp displacement and system oil pressure are collected; when the welding current, welding voltage, moving clamp displacement and system oil pressure are all within the set welding process range of the corresponding welding stage, a welding continuation state is formed; when at least one of the welding current, welding voltage, moving clamp displacement or system oil pressure exceeds the set welding process range of the corresponding welding stage and continues to reach the abnormal confirmation time, a welding abnormal state is formed. After the welding continuation state is formed and the welding procedure is completed, upsetting is performed with an upsetting force of 700kN to 800kN, and weld beads at the weld are removed to form a post-weld heat treatment state. In the post-weld heat treatment state, the normalizing assembly is moved to the weld and the normalizing coil is closed to perform medium-frequency induction normalizing on the weld. The normalizing is terminated when the rail top temperature reaches 850℃~920℃. After normalizing, the weld is cooled by air spraying to lower the rail top temperature to below 300°C, thus completing the flash welding joint of the railway turnout.
[0007] Furthermore, the flash welding process for railway turnouts employs a mobile integrated welding machine to perform the welding operation. The mobile integrated welding machine is integrated into a container and installed on a dual-purpose road-rail vehicle. The mobile integrated welding machine includes a welding head, a hanger assembly, a hydraulic pump station, a generator set, a chiller unit, an air compressor, an air tank, and an electrical control cabinet.
[0008] Furthermore, the welding head includes a pressure clamping cylinder, a push-button cylinder, a short-side clamp, a long-side clamp, an upsetting cylinder, a push-button cutter, and a normalizing assembly; when the clamping position is reached, the welding head is moved to the turnout welding station by the hanger assembly, and after the welding head is aligned with the rail to be welded, the short-side clamp and the long-side clamp are driven by the pressure clamping cylinder to clamp the rail to be welded.
[0009] Furthermore, the pre-welding status confirmation includes: grinding the protruding marks or text on the web of the rail to be welded until they are flush with the web surface, and not entering the weldable preparation state if the conductive contact area does not show a metallic luster or the sag of the rail to be welded is not less than 0.5mm.
[0010] Furthermore, after starting continuous flash welding or pulsed flash welding, welding control is executed through a dual-CPU control system. The main CPU collects and stores welding current, welding voltage, moving clamp displacement and system oil pressure, executes welding timing control from the CPU, and regulates the moving clamp feed speed through a proportional directional valve.
[0011] Furthermore, when the aforementioned welding abnormal state is formed, it includes: when at least one of the welding current, welding voltage, moving clamp displacement, or system hydraulic pressure exceeds the set welding process range, and the abnormal state continues to exceed the abnormal confirmation time, the current welded joint is determined to be unqualified, an alarm record is generated, and the welding program is re-entered after the unqualified weld is removed.
[0012] Furthermore, the upsetting distance is 12mm to 16mm; after upsetting is completed, the upsetting cylinder drives the upsetting knife to move along the weld seam to remove the weld beads formed after upsetting.
[0013] Furthermore, the normalizing assembly includes a normalizing transformer, a busbar, a first normalizing coil, and a second normalizing coil; when the normalizing assembly is moved to the weld and the normalizing coil is closed, the first normalizing coil is first rotated to the closed position around its own horizontal center line, and then the second normalizing coil is rotated to the closed position around its own vertical center line, so that the weld is closed and wrapped by the first normalizing coil and the second normalizing coil.
[0014] Furthermore, when performing medium-frequency induction normalizing on the weld, the normalizing is terminated when the rail top temperature reaches 850℃~920℃; when performing air-blast cooling on the weld, compressed air is sprayed onto the weld after the normalizing is completed to cool the rail top temperature to below 300℃.
[0015] Furthermore, the aforementioned flash welding process for railway turnouts is applicable to 50kg / m, 60kg / m, or 75kg / m rails; when changing the rail type to be welded, the welding machine electrode, limit block, and centering shim that match the rail type to be welded should be replaced.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: By grinding the conductive contact area of the rail end and rail web of the rail to be welded, and combining it with the rail straightness inspection to form a weldable preparation state, the situation of poor conductive contact and rail end condition not meeting the requirements can be eliminated before welding; by moving and centering the welding head in the weldable preparation state, and forming a clamping position with a clamping force of 1600kN to 2000kN, the stability of rail clamping and centering at the turnout welding site can be improved; by collecting welding current, welding voltage, moving clamp displacement and system oil pressure during flash welding, and distinguishing between welding continuation state and welding abnormal state, the welding process can be judged in a state-based manner; by performing upsetting, weld bead removal, medium frequency induction normalizing and air cooling in sequence after the welding procedure is completed, the welding, post-weld heat treatment and cooling processes can be continuously connected, thereby reducing the quality fluctuation of railway turnout rail welded joints caused by inconsistencies in the pre-weld contact state, clamping state, welding process state and post-weld heat treatment state. Attached Figure Description
[0017] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 A process flow diagram of the flash welding process for railway turnouts provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of the mobile welding and straightening integrated machine provided in an embodiment of the present invention; Figure 3 A schematic diagram of the front structure of the welding head provided in an embodiment of the present invention; Figure 4 This is a schematic diagram of the structure of the normalizing assembly provided in an embodiment of the present invention; Figure 5 A schematic diagram of the electrical principle of a welding circuit provided in an embodiment of the present invention; Figure 6 This is a logic block diagram of a welding quality monitoring system provided in an embodiment of the present invention.
[0018] The components include: 1. Welding head; 2. Hanger assembly; 3. Hydraulic pump station; 4. Generator set; 5. Chiller unit; 6. Air compressor; 7. Air tank; 8. Electrical control cabinet; 9. Container; 10. Road-rail dual-purpose vehicle; 11. Pressure clamping cylinder; 12. Pushing cylinder; 13. Short side clamp; 14. Long side clamp; 15. Upsetting cylinder; 16. Pushing knife; 17. Normalizing assembly; 18. Normalizing transformer; 19. Busbar; 20. First normalizing coil; 21. Second normalizing coil. Detailed Implementation
[0019] Exemplary embodiments of the present disclosure will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the present disclosure are shown in the drawings, it should be understood that the present disclosure may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the disclosure to those skilled in the art. It should be noted that, unless otherwise specified, embodiments and features in the embodiments of the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0020] In some embodiments of this application, see Figure 1-6 As shown, this application proposes a flash welding process for railway turnouts, comprising: S100: Confirm the pre-welding condition of the rails to be welded on railway turnouts, grind the conductive contact area of the rail ends and rail webs of the rails to be welded, with the grinding range not less than 670mm from the rail end face, and check the straightness of the rails to be welded. When the conductive contact area shows a metallic luster and the sagitta of the rails to be welded is less than 0.5mm, a weldable preparation state is formed. S200: In the welding preparation state, the welding head of the mobile welding and straightening machine is moved to the turnout welding station, the rail to be welded is centered and clamped, and the clamping position is formed with a clamping force of 1600kN to 2000kN. S300: When the rail is clamped in place, continuous flash welding or pulsed flash welding is started according to the rail type and end face condition of the rail to be welded. Welding current, welding voltage, moving clamp displacement and system oil pressure are collected. When the welding current, welding voltage, moving clamp displacement and system oil pressure are all within the set welding process range of the corresponding welding stage, a welding continuation state is formed. When at least one of the welding current, welding voltage, moving clamp displacement or system oil pressure exceeds the set welding process range of the corresponding welding stage and continues to reach the abnormal confirmation time, a welding abnormal state is formed. S400: After the welding continuity state is formed and the welding procedure is completed, upsetting is performed with an upsetting force of 700kN to 800kN, and the weld beads at the weld are removed to form a post-weld heat treatment state. S500: In the post-weld heat treatment state, the normalizing assembly is moved to the weld and the normalizing coil is closed to perform medium-frequency induction normalizing on the weld. The normalizing is terminated when the rail top temperature reaches 850℃~920℃. S600: After normalizing, the weld is cooled by air spraying to cool the rail top temperature to below 300℃, thus completing the flash welding joint of the railway turnout.
[0021] Specifically, in some embodiments, the flash welding process for railway turnouts of the present invention is applicable to the on-site welding construction of railway turnout rail joints. The rails to be welded can be 50kg / m, 60kg / m, or 75kg / m rails. The welding method can be continuous flash welding or pulsed flash welding, the post-weld heat treatment method can be medium-frequency induction normalizing, and the cooling method can be compressed air jet cooling. This embodiment continuously connects the pre-weld conductive contact state confirmation, rail straightness confirmation, welding head centering and clamping, flash welding process state judgment, upsetting and pushing back the weld bead, post-weld normalizing, and jet cooling for on-site welding processing of railway turnout rail joints.
[0022] Before welding operations, a welding process card matching the rail type to be welded is established. The welding process card records the grinding range, allowable straightness value, clamping force range, selection conditions for continuous flash welding or pulsed flash welding, welding current range, welding voltage range, moving clamp displacement range, system hydraulic pressure range, anomaly confirmation time, upsetting force range, upsetting distance range, normalizing temperature range, normalizing heating time, and air cooling time. The welding process card can be generated through process qualification of a sample rail of the same type. During process qualification, a sample rail with the same rail type, material, and web shape as the rail to be welded on site is selected, and trial welding is performed according to candidate grinding length, candidate clamping force, candidate welding mode, candidate upsetting force, candidate normalizing temperature, and candidate cooling time. After the trial welding is completed, the weld joint is visually inspected, the weld bead removal status is checked, non-destructive testing is performed, and the post-weld condition is checked. The parameter range that can stably complete clamping, flash welding, upsetting, weld bead removal, normalizing, and cooling, and whose trial weld joint passes inspection, is written into the welding process card as the set welding process range for formal welding. For rail types for which construction process documents or welding machine matching process cards have already been formed, the parameter range confirmed by the process evaluation can be directly called.
[0023] The mobile welding and straightening integrated machine is integrated into container 9 and installed on a dual-purpose road-rail vehicle 10. The mobile welding and straightening integrated machine includes a welding head 1, a lifting assembly 2, a hydraulic pump station 3, a generator set 4, a chiller unit 5, an air compressor 6, an air tank 7, and an electrical control cabinet 8. The dual-purpose road-rail vehicle 10 is used to transport the mobile welding and straightening integrated machine to the railway turnout welding site; container 9 is used to centrally arrange welding, power supply, hydraulic, cooling, air supply, and electrical control components; the lifting assembly 2 is used to lift the welding head 1 above the rail to be welded and to adjust the position of the welding head 1. The welding head 1 includes a pressure clamping cylinder 11, a push-button cylinder 12, a short-side clamp 13, a long-side clamp 14, an upsetting cylinder 15, a push-button cutter 16, and a normalizing assembly 17. The pressure clamping cylinder 11 is used to drive the short side clamp 13 and the long side clamp 14 to clamp the rail to be welded; the upsetting cylinder 15 is used to apply upsetting force after the welding process is completed; the spore-removing cylinder 12 is used to drive the spore-removing knife 16 to remove the weld spore at the weld; the normalizing assembly 17 is used to perform post-weld normalizing treatment on the weld area.
[0024] Before formal welding, the condition of the rail to be welded is confirmed. This confirmation includes grinding the conductive contact area and checking the rail straightness. During grinding, the conductive contact areas at the rail ends and webs are ground, with the grinding range at least 670mm from the rail end face. The grinding range is determined based on the effective contact length of the welding machine electrodes along the rail length, the on-site centering adjustment allowance of the welding head 1, and the allowance for cleaning rust, scale, and contaminants from the rail end. Specifically, the actual contact coverage of the electrodes of the short-side clamp 13 and long-side clamp 14 along the rail length is measured first. Then, the adjustment allowance of the welding head 1 at the turnout site is considered, along with the cleaning allowance near the rail end face. The sum of these lengths is rounded up to obtain the pre-weld grinding length. In this embodiment, the pre-weld grinding length is taken as at least 670mm from the rail end face.
[0025] After grinding, the conductive contact area of the rail to be welded will show a metallic luster. If there are raised marks or text on the rail web, grind them until they are flush with the rail web surface to reduce local suspension, excessively deep indentations, or discontinuous conductive contact during electrode clamping. If rust, scale, oil, or areas without a metallic luster still exist in the conductive contact area, continue grinding; if the conductive contact requirements are still not met, do not proceed to the next welding procedure.
[0026] The straightness of the rail is checked using a one-meter straightedge and a feeler gauge. During the inspection, the one-meter straightedge is placed against the rail top surface or rail web reference surface near the end to be welded along the longitudinal direction of the rail. The maximum gap between the one-meter straightedge and the rail surface is measured with a feeler gauge, and this maximum gap is taken as the sag of the rail to be welded, i.e., the straightness deviation within a 1-meter length. The allowable straightness value is determined through clamping tests and trial welding evaluations of the same type of rail sample. Specifically, a rail sample of the same type is selected, and rail sections with different sag states are made. Each rail section is then clamped by welding head 1, aligned at the end face, and trial welded in sequence. The end face misalignment, electrode contact status, displacement stability during welding, and post-weld inspection results are recorded. The maximum sag that meets the requirements of end face alignment, clamping stability, and post-weld inspection qualification is selected as the allowable straightness value. In this embodiment, when the sag of the rail to be welded is less than 0.5 mm, a welding preparation state is formed; when the sag of the rail to be welded is not less than 0.5 mm, the welding preparation state is not entered, and the state of the rail to be welded is readjusted.
[0027] After reaching a weldable state, the welding head 1 is moved to the turnout welding station via the hanger assembly 2. During alignment, the welding head 1 is first lowered above the rail to be welded, and then the lateral and height positions of the welding head 1 are adjusted. The contact positions of the short-side clamp 13, the long-side clamp 14, and the conductive contact areas on both sides of the rail to be welded are observed. When the electrodes of the short-side clamp 13 and the long-side clamp 14 are located in the conductive contact areas on both sides of the rail to be welded, the end face to be welded is within the allowable alignment range of the welding head 1, and the rail to be welded does not show significant deviation when the clamps are closed, the welding head 1 is considered to have completed alignment with the rail to be welded.
[0028] After alignment, the pressure-boosting clamping cylinder 11 is activated, clamping the rail to be welded between the electrodes using the short-side clamp 13 and the long-side clamp 14. The clamping force range is determined through a clamping stability test. Specifically, the clamping force is adjusted step by step on a sample rail of the same type, and the changes in electrode indentation, clamping slippage, end face misalignment, and displacement during the upsetting process are recorded. When the clamping force is too small, relative slippage of the rail or changes in the end face position are likely to occur during welding. When the clamping force is too large, the risk of electrode indentation, hydraulic system load, and rail surface damage increases. The clamping force range is determined by considering both clamping stability and surface damage. In this embodiment, the clamping force is controlled between 1600kN and 2000kN; when the clamping force enters the above range and the clamping state is stable, the clamping position is achieved.
[0029] Hydraulic pump station 3 uses a high-low pressure switching two-position valve to provide hydraulic power to welding head 1. The high-pressure oil circuit of hydraulic pump station 3 is controlled at 22MPa±1MPa, and the low-pressure oil circuit is controlled at 5MPa±0.5MPa. The working pressure of the clamping cylinder is controlled at 16MPa~18MPa, and the working pressure of the upsetting cylinder 15 is controlled at 20MPa±1MPa. The system oil pressure is collected by hydraulic pump station 3 or pressure detection elements in the hydraulic circuit to reflect the execution status of hydraulic actions such as clamping, feeding, upsetting, and pushing. When the system oil pressure is lower than the lower limit of the current action stage, it indicates insufficient hydraulic execution; when the system oil pressure is higher than the upper limit of the current action stage, it indicates abnormal hydraulic load or obstruction of the actuator. Therefore, the system oil pressure is involved in the judgment of welding continuity and abnormal welding status.
[0030] With the rail in the clamped position, continuous flash welding or pulsed flash welding is initiated based on the rail type and end face condition. Continuous flash welding can be used when the end face of the rail has good flatness after grinding and the end face contact is stable; pulsed flash welding can be used when the end face contact fluctuates significantly, or when periodic feeding is needed to improve the flash welding stability. The welding mode is selected in the welding process card according to the rail type, end face condition, and process qualification results. During welding, welding control is executed through a dual-CPU control system. The main CPU is used for human-machine interaction, welding parameter setting, welding current acquisition, welding voltage acquisition, moving clamp displacement acquisition, system hydraulic pressure acquisition, welding data storage, and weld joint quality evaluation; the slave CPU is used for welding timing control and constant welding current control, and regulates the moving clamp feed speed through a proportional directional valve.
[0031] The welding continuation state and welding abnormal state are determined jointly based on welding current, welding voltage, moving clamp displacement, and system hydraulic pressure. Specifically: During the process qualification stage, the welding current curve, welding voltage curve, moving clamp displacement curve, and system hydraulic pressure curve of the qualified weld joint are recorded, and these curves are divided into the initiation stage, flash stage, melting stage, and pre-upsetting stage according to the welding sequence. Upper and lower limits and allowable fluctuation times are determined for the qualified curves of each welding stage, forming the set welding process range for each welding stage. During formal welding, the dual-CPU control system collects the current welding current, welding voltage, moving clamp displacement, and system hydraulic pressure according to the sampling cycle and compares them with the set welding process range for the current welding stage. When the welding current, welding voltage, moving clamp displacement, and system hydraulic pressure are all within the set welding process range for the corresponding welding stage, a welding continuation state is formed, and the welding program continues to execute; when at least one of the welding current, welding voltage, moving clamp displacement, or system hydraulic pressure exceeds the set welding process range for the corresponding welding stage, and the excess state continues until the abnormal confirmation time, a welding abnormal state is formed.
[0032] The anomaly confirmation time is determined by the welding data sampling cycle and short-term fluctuations during qualified welding processes. Specifically, the duration of short-term fluctuations in welding current, welding voltage, moving clamp displacement, and system hydraulic pressure during qualified trial welding of the same type is first statistically analyzed. Then, the duration exceeding the normal short-term fluctuation duration is selected as the anomaly confirmation time. Alternatively, it can be determined based on the number of consecutive abnormal samplings. For example, if several consecutive sampling cycles exceed the set welding process range for the corresponding welding stage, the welding anomaly status is then confirmed. This secondary confirmation through the anomaly confirmation time reduces the likelihood of a single sampling interference directly triggering an abnormal shutdown.
[0033] When an abnormal welding condition occurs, the current weld joint is deemed unqualified, and the dual-CPU control system generates an alarm record. The alarm record includes the type of abnormal parameter, the stage of the abnormality, the time of the abnormality, and the duration of the abnormality. For unqualified welds, the current welding process is stopped, and the unqualified weld is removed by a welding machine disc shear located between the moving end electrode and the fixed end electrode. After removal, the end face to be welded is re-grinded, its straightness is checked, and it is centered and clamped. Once the requirements for conductive contact area, straightness, and clamping status are met again, the welding program is restarted.
[0034] After the welding process is completed and the welding continuity is achieved, the upsetting cylinder 15 is activated for upsetting. The upsetting force range is determined through upsetting forming tests. Specifically, trial welding is performed on a template rail with different upsetting forces, and the upsetting distance, weld bead formation state, end-face metal extrusion state, and post-weld inspection results are recorded. When the upsetting force is too small, the end-face oxides and molten metal are not fully discharged; when the upsetting force is too large, the deformation of the weld area and the weld bead size increase. The upsetting force range that can stably achieve an upsetting distance of 12mm to 16mm and pass post-weld inspection is taken as the formal upsetting force range. In this embodiment, the upsetting force is controlled at 700kN to 800kN, and the upsetting distance is controlled at 12mm to 16mm.
[0035] After upsetting, the weld bead remover 16 is driven by the weld bead remover cylinder 12 to move along the weld seam and remove the weld bead formed after upsetting. The weld bead removal action is performed after upsetting. The weld bead remover 16 passes along the outer periphery of the weld seam at the weld bead position, removing the excess weld bead from the weld seam. After the weld bead removal, the appearance of the weld seam is inspected. There should be no protruding weld bead at the weld seam that would affect the closure of the normalizing coil. After upsetting and weld bead removal are completed, the welded joint enters the post-weld heat treatment state.
[0036] The normalizing assembly 17 includes a normalizing transformer 18, a busbar 19, a first normalizing coil 20, and a second normalizing coil 21. In the post-weld heat treatment state, the normalizing assembly 17 is moved to the weld and its position is adjusted so that the heating centers of the first and second normalizing coils 20 and 21 are located in the center region of the weld. When closing the normalizing coils, the first normalizing coil 20 is first rotated to the closed position around its horizontal centerline, and then the second normalizing coil 21 is rotated to the closed position around its vertical centerline, so that the first and second normalizing coils 20 and 21 close and wrap around the weld. This closing action is suitable for post-weld normalizing operations in turnout areas where the surrounding space is limited.
[0037] When performing medium-frequency induction normalizing on the weld, the rail top temperature is collected using an infrared thermometer or a contact thermometer, and normalizing is terminated when the rail top temperature reaches 850℃~920℃. The normalizing temperature range is determined through post-weld heat treatment process evaluation. Specifically, medium-frequency induction heating is performed on trial welds of the same rail type at different rail top temperatures, and the hardness, metallographic structure, and non-destructive testing results of the weld and heat-affected zone are recorded; the temperature range that can improve the post-weld structure without overheating is taken as the normalizing temperature range. In this embodiment, the rail top temperature is controlled at 850℃~920℃. The normalizing heating time is determined according to the medium-frequency induction heating power, rail type, and rail top temperature rise curve; during the process evaluation stage, the time required for the rail top temperature to rise from the initial temperature to the target temperature range is recorded, and the heating time to stably enter the 850℃~920℃ temperature range is used as the heating control basis. If the target temperature range is not reached after 300 seconds of heating, heating is stopped and the position of the normalizing coil, power supply status, and temperature measurement status are checked.
[0038] After normalizing, the air spray system is activated, with air compressor 6 and air tank 7 supplying compressed air to the system. This compressed air is then sprayed onto the weld area for cooling, reducing the rail top temperature to below 300°C. The cooling time is determined using a post-weld cooling curve. Specifically, during the process evaluation phase, the temperature decrease curve of the weld area over time after normalizing is recorded, and the weld appearance, hardness, and non-destructive testing results are checked after cooling. The cooling time that allows for stable post-weld cooling and meets the quality requirements of the welded joint is selected as the air spray cooling time. In this embodiment, the rail top temperature is cooled to below 300°C. After cooling, the short-side clamp 13 and long-side clamp 14 are released, the welding head 1 is removed, and weld slag and spatter are cleaned, completing the flash welded joint of the railway turnout.
[0039] When changing the rail type to be welded, replace the welding machine electrodes, limit blocks, and centering shims according to the new rail type. After replacement, perform a no-load operation check and pre-welding status confirmation. The no-load operation check includes clamping action, upsetting action, stub pushing action, normalizing coil closing action, and air cooling action. The chiller unit 5 is used to provide circulating cooling for the transformer, electrodes, conductive shaft, and hydraulic system return oil in the welding head 1; the hydraulic pump station 3 is used to provide hydraulic power to the pressure clamping cylinder 11, stub pushing cylinder 12, and upsetting cylinder 15; the electrical control cabinet 8 is used to house the dual-CPU control system and welding control electrical components. Before each day's welding begins, molybdenum disulfide lithium-based grease can also be added to each lubrication point of the welding machine.
[0040] For example, when welding 60kg / m steel rail turnout joints on-site, the conductive contact areas of the rail ends and rail webs to be welded are ground. The grinding range is no less than 670mm from the rail end face. After grinding, the conductive contact areas are exposed with a metallic luster, and the raised marks on the rail webs are ground until they are flush with the rail web surface. The straightness of the rail to be welded is checked using a one-meter straightedge and feeler gauge. After the sagging is less than 0.5mm, it is ready for welding. The welding head 1 is moved to the turnout welding station through the hanger assembly 2. After alignment, the clamping cylinder drives the short side clamp 13 and long side clamp 14 to clamp the rail to be welded with a working pressure of 18MPa. The clamping force is approximately 1800kN. The flash welding program is initiated based on the rail profile and end face condition of the 60kg / m rail. The dual-CPU control system collects welding current, welding voltage, moving clamp displacement, and system hydraulic pressure. The welding program continues as long as the collected results are within the set welding process range for the corresponding welding stage. If any collected result exceeds the set welding process range for the corresponding welding stage and continues to exceed the abnormal confirmation time, the current weld joint is deemed unqualified. After the welding program completes normally, the upsetting cylinder 15 operates at a working pressure of 20MPa, with an upsetting force of approximately 750kN and an upsetting distance of approximately 10.5mm. Subsequently, the upsetting cylinder 12 drives the upsetting knife 16 to remove the weld bead. After upsetting, the normalizing assembly 17 is moved to the weld, the first normalizing coil 20 and the second normalizing coil 21 are closed, and the medium-frequency induction normalizing system is activated, controlling the rail top temperature to approximately 900℃ for a normalizing heating time of approximately 250 seconds. After normalizing, the weld is cooled by spraying compressed air at 0.6MPa for approximately 350 seconds. After cooling, loosen the clamps, remove the welding head 1, clean up the slag and spatter, and perform non-destructive testing on the weld.
[0041] In summary, by grinding the conductive contact areas of the rail ends and webs of the rail to be welded, and combining this with a rail straightness check to create a weldable preparation state, it is possible to eliminate situations where poor conductive contact and unsatisfactory rail end conditions exist before welding. By transferring and centering the welding head in this weldable preparation state, and using a clamping force of 1600kN to 2000kN to achieve proper clamping, the stability of rail clamping and centering at the turnout welding site can be improved. By collecting welding current, welding voltage, moving clamp displacement, and system hydraulic pressure during flash welding, and distinguishing between welding continuity and abnormal welding states, a state-based judgment of the welding process can be made. By sequentially performing upsetting, weld bead removal, medium-frequency induction normalizing, and air cooling after the welding procedure is completed, the welding, post-weld heat treatment, and cooling processes can be continuously connected, thereby reducing quality fluctuations in railway turnout rail welded joints caused by inconsistencies in pre-weld contact conditions, clamping conditions, welding process conditions, and post-weld heat treatment conditions.
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the protection scope of the present invention.
Claims
1. A method of flash butt welding a railway turnout, characterized in that, include: Before welding, the rails of the railway turnout are confirmed to be in a state of readiness. The conductive contact area of the rail ends and rail webs is ground, with the grinding range not less than 670mm from the rail end face. The straightness of the rails is also checked. When the conductive contact area shows a metallic luster and the sagitta of the rails is less than 0.5mm, the rails are ready to be welded. In the weldable preparation state, the welding head of the mobile welding machine is moved to the turnout welding station, the rail to be welded is centered and clamped, and a clamping force of 1600kN to 2000kN is used to form the clamping position. In the clamped position state, continuous flash welding or pulsed flash welding is started according to the rail type and end face condition of the rail to be welded, and the welding current, welding voltage, moving clamp displacement and system oil pressure are collected; when the welding current, welding voltage, moving clamp displacement and system oil pressure are all within the set welding process range of the corresponding welding stage, a welding continuation state is formed; when at least one of the welding current, welding voltage, moving clamp displacement or system oil pressure exceeds the set welding process range of the corresponding welding stage and continues to reach the abnormal confirmation time, a welding abnormal state is formed. After the welding continuation state is formed and the welding procedure is completed, upsetting is performed with an upsetting force of 700kN to 800kN, and weld beads at the weld are removed to form a post-weld heat treatment state. In the post-weld heat treatment state, the normalizing assembly is moved to the weld and the normalizing coil is closed to perform medium-frequency induction normalizing on the weld. The normalizing is terminated when the rail top temperature reaches 850℃~920℃. After normalizing, the weld is cooled by air spraying to lower the rail top temperature to below 300°C, thus completing the flash welded joint of the railway turnout.
2. The railway switch flash butt welding process of claim 1 wherein, The aforementioned flash welding process for railway turnouts employs a mobile integrated welding machine to perform the welding operation. This mobile integrated welding machine is integrated into a container and installed on a dual-purpose road-rail vehicle. The mobile integrated welding machine includes a welding head, a hanger assembly, a hydraulic pump station, a generator set, a chiller unit, an air compressor, an air tank, and an electrical control cabinet.
3. The railway switch flash butt welding process of claim 2, wherein, The welding head includes a pressure clamping cylinder, a push-button cylinder, a short-side clamp, a long-side clamp, an upsetting cylinder, a push-button cutter, and a normalizing assembly. When the clamping position is reached, the welding head is moved to the turnout welding station via the hanger assembly. After the welding head is aligned with the rail to be welded, the short-side clamp and the long-side clamp are driven by the pressure clamping cylinder to clamp the rail to be welded.
4. The railway switch flash butt welding process of claim 3, wherein, The pre-welding status confirmation includes: grinding the protruding marks or text on the web of the rail to be welded until they are flush with the web surface, and not entering the weldable preparation state if the conductive contact area does not show a metallic luster or the sag of the rail to be welded is not less than 0.5mm.
5. The railway switch flash butt welding process of claim 4 wherein, After starting continuous flash welding or pulsed flash welding, welding control is executed through a dual-CPU control system. The main CPU collects and stores welding current, welding voltage, moving clamp displacement and system oil pressure. The CPU executes welding timing control and adjusts the moving clamp feed speed through a proportional directional valve.
6. The railway switch flash butt welding process of claim 5 wherein, The forming of the welding abnormal state comprises: when at least one of the welding current, the welding voltage, the tongs displacement or the system oil pressure exceeds the set welding process range, and the exceeding state lasts for the abnormal confirmation time, it is determined that the current welding joint is unqualified, an alarm record is generated, and after the unqualified weld is cut off, the welding program is re-entered.
7. The railway switch flash butt welding process of claim 6 wherein, The upsetting distance of the upsetting is 12mm-16mm; after the upsetting is completed, the push-bump oil cylinder drives the push-bump cutter to move along the weld to remove the weld bumps formed after the upsetting.
8. The railway switch flash butt welding process of claim 7, wherein, The normalizing assembly comprises a normalizing transformer, a bus bar, a first normalizing coil and a second normalizing coil; when the normalizing assembly is moved to the weld and the normalizing coil is closed, the first normalizing coil is first flipped to the closed position with the horizontal center line of the first normalizing coil as the axis, and then the second normalizing coil is rotated to the closed position with the vertical center line of the second normalizing coil as the axis, and the weld is closed and wrapped by the first normalizing coil and the second normalizing coil.
9. The railway switch flash butt welding process of claim 8 wherein, When the rail top temperature reaches 850-920℃, the normalizing is terminated; when the weld is cooled by air blowing, compressed air is blown to the weld after the normalizing is completed, so that the rail top temperature is cooled to below 300℃.
10. The railway switch flash butt welding process of claim 9, wherein, The railway turnout flash butt welding process method is suitable for 50kg / m, 60kg / m or 75kg / m rails; when the rail type of the to-be-welded rail is replaced, the welding machine electrode, the limiting block and the centering gasket matching the to-be-welded rail type are replaced.
Citation Information
Patent Citations
High manganese steel frog and rail flash butt welding method
CN101474713A