A long-lasting wood protectant, its process and application

By generating an inorganic silicate crystalline framework inside the wood, the problem of early gelation of silicate wood preservatives hindering penetration is solved, achieving long-term protection for the wood and improving dimensional stability and resistance to biodegradation.

CN123103822APending Publication Date: 2026-11-17GUANG DONG INCH WATER IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611436778.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicate wood preservatives exhibit early gelation on the wood surface, hindering deep penetration and resulting in insufficient internal effective components and a decline in protective effect over time.

Method used

The mineralization and crystallization process of silicates is controlled by a latent rare earth catalyst. By keeping rare earth complex ions dispersed in an alkaline system, the silicates are promoted to form an inorganic silicate crystal framework inside the wood, forming a three-dimensional mineralization network. Combined with preservatives, the silicates are fixed in the crystal lattice, inhibiting water penetration and providing mechanical support.

Benefits of technology

It improves the dimensional stability and biodegradability of wood, reduces preservative loss, improves penetration depth and uniformity of crystal distribution, and reduces the risk of cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103822A_ABST
    Figure CN123103822A_ABST
Patent Text Reader

Abstract

This invention relates to the field of wood modification and protection technology, and discloses a long-lasting wood protectant, its process, and its application. The protectant raw materials, by weight, include: 60-70 parts silicate, 20-40 parts deionized water, 2-6 parts latent rare earth catalyst, and 1-2 parts preservative. The treatment process includes diluting the protectant, cleaning and pre-wetting the wood, using alternating pressure difference to allow the protectant to penetrate and immerse itself in the wood, followed by constant temperature and humidity treatment, stepped temperature increase and dehumidification, and conventional static curing, which promotes in-situ mineralization and crystallization of silicate within the wood's micropores. This invention utilizes the rare earth catalyst to maintain the initial low viscosity of the solution to promote deep penetration. The inorganic crystalline framework generated in-situ within the wood fills moisture migration channels and binds with the preservative, thereby improving the dimensional stability and biodegradability of wood products, while reducing drying cracking defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wood modification and protection technology, specifically to a long-lasting wood protectant, its process, and its application. Background Technology

[0002] Wood, as a natural biomass material, is widely used in construction engineering, outdoor furniture, and landscaping due to its renewable, high specific strength, and ease of processing characteristics. However, because wood has a large number of pores and its cell wall components contain abundant hydrophilic groups, it will absorb and desorb moisture when the temperature and humidity of the environment change, which will cause the wood to expand and shrink. At the same time, untreated wood will be eroded by decay fungi, molds, and insects in suitable environments, resulting in material degradation and shortened service life.

[0003] To improve the dimensional stability and biodegradability of wood, chemical impregnation is often used in industry for modification. Among these methods, impregnating wood with inorganic silicate systems is a promising environmentally friendly protective measure. However, existing silicate wood modification technologies struggle to balance the relationship between chemical penetration and in-situ curing in practical applications. Conventional silicate solutions, after penetrating the surface of the wood, undergo premature gelation and condensation reactions in the shallow layers due to some water evaporation and contact with the slightly acidic environment inside the wood. This rapid precipitation of inorganic substances from the surface blocks the wood's pores and capillary networks, creating a surface sealing effect that hinders subsequent penetration of the chemical solution into deeper tissues such as the heartwood, resulting in insufficient effective protective components remaining inside the wood.

[0004] To delay the early gelation of the chemical solution and facilitate penetration, some existing technologies reduce the concentration of the silicate solution. However, this method results in a low amount of inorganic matter deposited in the wood pores, failing to form a physical support framework with sufficient mechanical strength. This makes it difficult to restrict the penetration channels of water. In a long-term humid environment, inorganic salt components that have not formed a complete network structure will hydrolyze and seep out of the wood with free water, causing the anti-corrosion and dimensional stability effects to gradually decrease over time. In addition, during the wood drying process after impregnation, conventional dehumidification processes have difficulty controlling the rate of internal moisture diffusion. Rapid moisture migration often leads to the accumulation of free salts on the wood surface, forming appearance defects. At the same time, the local stress concentration caused by the rapid vaporization of internal moisture can cause cracking of the wood tissue, affecting the overall quality and mechanical properties of the wood products. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a long-lasting wood protectant, its process, and its application, solving the problem that existing silicate wood protectants gel early on the wood surface, hindering deep penetration, resulting in insufficient internal effective ingredients and a decrease in protective effect.

[0006] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides a long-lasting wood protectant, which is made from raw materials comprising the following parts by weight: 60 to 70 parts of silicate; 20 to 40 parts of deionized water; 2 to 6 parts of latent rare earth catalyst; and 1 to 2 parts of preservative.

[0007] By adopting the above technical solutions, a latent rare earth catalyst is introduced to control the mineralization and crystallization process of silicates, generating an inorganic silicate crystal framework in situ inside the pores and cell cavities of wood. This restricts water penetration channels and improves the dimensional stability and resistance to biodegradation of wood. Specifically, the latent rare earth catalyst contains rare earth complex ions, and the multidentate coordination groups shield the high charge on the surface of rare earth ions. This helps to maintain dispersion in the alkaline silicate system and prevents early precipitation reactions, thereby giving the protective agent system a lower viscosity to facilitate penetration and a certain degree of storage stability.

[0008] When the preservative penetrates into the wood, the acid-base neutralization effect occurs due to the migration of water molecules and the presence of slightly acidic groups in the wood cell walls. The coordination equilibrium of rare earth complex ions is reversed, and the system slowly dissociates and releases rare earth cations. These released rare earth cations act as crystal nucleation sites, which can lower the energy barrier for crystallization and accelerate the dehydration and condensation reaction of free silicate anions. Subsequent hydrolysis and condensation reactions generate polysilicate crystals, which grow in the wood cell cavities, pits, and fiber gaps, forming a three-dimensional inorganic mineralized framework. The physical framework fills the internal free water channels, inhibits the penetration of external water, generates mechanical support to resist cell wall deformation, and fixes the preservative in the crystal lattice network, reducing the loss of effective ingredients.

[0009] Preferably, the wood long-lasting protectant is prepared by a method comprising the following steps: stirring the silicate and deionized water at a speed of 150 to 200 rpm for 10 to 15 min to form a matrix solution; while maintaining stirring, adding the latent rare earth catalyst solution to the matrix solution at a rate of 10 to 15 L / min using a metering device; subsequently adding the preservative, continuing to stir for 15 to 20 min, and filtering through a filter screen to obtain the wood long-lasting protectant.

[0010] By adopting the above technical solution, the matrix solution is prepared at a set rotation speed, and the latent rare earth catalyst is added dropwise at a constant flow rate. This reduces the probability of instantaneous agglomeration or gelation caused by excessively high concentrations in local areas, which is beneficial for the dispersion of rare earth complex ions in the silicate solution. The subsequent filtration step aims to remove large particles that may initially agglomerate in the solution, so as to facilitate the penetration of the final protective agent into the micropores of the wood.

[0011] Preferably, the silicate is one of sodium silicate or potassium silicate; the preservative is one of 2-methyl-4-isothiazolin-3-one or iodopropynyl butylcarbamate.

[0012] By adopting the above technical solutions, sodium silicate and potassium silicate have moderate water solubility and low initial degree of polymerization, which is conducive to early penetration into the deep layers of wood and the formation of inorganic polymers after water evaporation. 2-Methyl-4-isothiazolin-3-one and iodopropynyl butylcarbamate have good compatibility with weakly basic silicate systems. After the inorganic skeleton is formed, they are distributed in the interstitial spaces of the crystal lattice and can exert an inhibitory effect on decay fungi and molds.

[0013] Preferably, the latent rare earth catalyst is made from raw materials comprising the following parts by weight: 10 to 15 parts deionized water; 1 to 5 parts rare earth salt; 1 to 5 parts chelating agent; wherein the rare earth salt is at least one of lanthanum chloride or cerium nitrate; and the chelating agent is one of sodium citrate, disodium ethylenediaminetetraacetate, or glycerol.

[0014] By adopting the above technical solutions, lanthanum chloride and cerium nitrate dissociate into lanthanum ions and cerium ions with catalytic activity. Sodium citrate, disodium ethylenediaminetetraacetate, and glycerol provide a multidentate coordination structure. This coordination structure forms coordination bonds with rare earth ions, which helps to control the hydration state and reactivity of rare earth ions, delays the induction period of silicate polymerization mineralization, and promotes the mineralization and crystallization process to occur more within the wood.

[0015] Preferably, the preparation method of the latent rare earth catalyst solution includes: adding deionized water and rare earth salt to a reaction vessel equipped with a heating and stirring device, and stirring at a speed of 200 to 300 rpm to completely dissolve them; adjusting the system temperature to 40 to 50°C, and slowly adding the chelating agent to the solution; maintaining a constant temperature of 40 to 50°C, and continuing the reaction at a speed of 300 to 500 rpm for 30 to 60 minutes, and cooling to room temperature to obtain the solution.

[0016] By adopting the above technical solution, the chelating agent is slowly added under heating conditions and the stirring speed is increased to promote the coordination reaction, so that the chelating agent can fully complex rare earth ions, reduce the number of free metal cations in the system, and thus improve the compositional uniformity and structural stability of the latent rare earth catalyst.

[0017] Secondly, the present invention provides a process for a long-lasting wood protectant, the process comprising the following steps: Prepare the wood long-lasting protective agent according to the formula ratio, and mix and dilute it with deionized water at a volume ratio to obtain a diluted protective solution; After cleaning and pre-wetting the surface of the wood to be treated, allow the diluted protective solution to penetrate and immerse itself in the wood. Once the wood is saturated with water, drain the excess solution. After soaking, the wood is placed naturally until there is no free water on the surface, and then sent into a temperature and humidity controlled kiln for constant temperature and humidity treatment. After the constant temperature and humidity treatment is completed, the wood is heated in stages to remove moisture until the core moisture content of the wood drops to the target range before it is removed from the kiln. After the wood comes out of the kiln, it is transferred to a conventional ventilated warehouse for static curing to complete the in-situ mineralization and crystallization process of silicates in the wood pores, thus obtaining wood that has undergone long-term protective treatment.

[0018] By adopting the above technical solutions, pre-wetting treatment reduces the surface tension of wood and establishes water molecule diffusion channels; dilution operation is used to control the overall viscosity of the agent and promote the penetration of the solution from the surface layer of the wood to the core layer; constant temperature and humidity treatment maintains the liquid phase environment inside the wood and provides reaction conditions for silicate hydrolysis and condensation; stepwise heating and dehumidification accelerate the diffusion of internal moisture to the outer layer, causing the concentration of the internal system to cross the supersaturation critical point and triggering in-situ mineralization reaction; static curing helps to relieve residual internal stress and allows the inorganic skeleton and wood fiber to form an interlocking structure.

[0019] Preferably, the process of allowing the diluted protective liquid to penetrate and immerse itself in the wood includes: placing the wood to be treated into a pressure-resistant impregnation tank, evacuating to -0.08 to -0.09 MPa and maintaining it for 10 to 20 minutes, using negative pressure to draw the diluted protective liquid into the impregnation tank until the wood is completely submerged, releasing the vacuum and using a pressure pump to increase the positive pressure inside the tank to 0.6 to 0.8 MPa for constant pressure penetration; when the constant pressure penetration time reaches 30 to 80 minutes, quickly opening the exhaust valve, rapidly reducing the pressure inside the tank to 0.05 to 0.1 MPa within 15 to 20 seconds and maintaining the low pressure state for 1 to 1.5 minutes, and then repressurizing to 0.6 to 0.8 MPa; performing the alternating pressure difference cycle 1 to 3 times, and draining the liquid after the total soaking time reaches 45 to 120 minutes.

[0020] By adopting the above technical solutions, vacuuming is used to remove the closed air in the cell cavities and pits, reducing the initial penetration resistance. Positive pressure promotes the liquid to penetrate the tissue structure and enter the heartwood. The pressure drop operation creates an internal and external pressure gradient in a short time, causing the closed substances blocking the pits to undergo microscopic displacement, which drives the large molecular solutes remaining on the shallow surface to move inward. Multiple alternating pressure differential cycles are beneficial to increasing the liquid absorption and three-dimensional distribution uniformity of the liquid inside the wood that is difficult to impregnate, and improving the distribution of subsequent crystals inside the wood.

[0021] Preferably, the constant temperature and humidity treatment and the step-by-step heating and dehumidification process include: starting the heating to raise the kiln temperature to 40 to 50°C, while continuously injecting water vapor to forcibly maintain the relative humidity inside the kiln at 85% to 95% and maintain a constant temperature and humidity state for 12 to 24 hours; then stopping the steam injection, and performing step-by-step heating and dehumidification according to a gradient of 5 to 10°C every 2 to 4 hours, and strictly controlling the highest kiln temperature at 65 to 70°C, until the core moisture content of the wood stabilizes at 12% to 14% before it is removed from the kiln.

[0022] By adopting the above technical solutions, the high humidity and medium temperature environment in the early stage inhibits the rapid evaporation of surface moisture, slows down the tendency of silicate to precipitate prematurely on the shallow surface of wood and produce a surface sealing effect, and balances the capillary conduction rate and evaporation diffusion rate of moisture by step-by-step heating and dehumidification, controls the rate of crystal nucleation and growth, reduces the risk of wood cracking or loosening of crystal structure caused by rapid vaporization of internal moisture, and controls the maximum kiln temperature to reduce the thermal degradation of lignin and the volatilization and failure of preservative components caused by high temperature.

[0023] Preferably, the volume ratio of the wood long-lasting protectant to deionized water is 1:1 to 1:2; during the pre-wetting process of the wood surface to be treated, the amount of deionized water used is 0.05 to 0.15 kg / m³. 2 .

[0024] By adopting the above technical solutions, the dilution ratio balances the penetration resistance of the working solution and the total amount of effective inorganic components introduced, reducing the problem of increased fluid viscosity caused by high concentration of the original solution. The amount of pre-wetting ensures that the capillaries on the surface of the wood are in a moderately saturated wetted state, and the capillary pull guides the subsequent solution to penetrate deeper, reducing the situation where the drying surface directly contacts the high concentration of salt solution and causes micropore blockage.

[0025] Thirdly, the present invention provides an application of a wood long-lasting protective agent in the dimensional stabilization treatment or anti-biodegradation treatment of wood products.

[0026] By adopting the above technical solutions, the inorganic skeleton generated by the internal mineralization of the protective agent covers the water absorption binding sites on part of the wood cell wall, hindering the contact pathway of external water vapor and affecting the wood's own moisture absorption and desiccation cycle, thereby improving the dimensional stability of wood products against expansion and shrinkage. At the same time, the nutrient pores are filled by inorganic minerals and combined with preservative components, compressing the living space and nutrient acquisition matrix of decay fungi and molds, giving the wood a certain degree of resistance to biodegradation.

[0027] This invention provides a long-lasting wood protectant, its process, and its application. It offers the following beneficial effects: 1. This invention improves the dimensional stability and biodegradability of wood. The latent rare earth catalyst introduced in the formula dissociates after penetrating into the wood. The released rare earth ions promote the hydrolysis and condensation reaction of silicates in the cell cavities and micropores of the wood. The inorganic polymer crystals generated in situ fill part of the water migration channels and provide mechanical support, thereby reducing the swelling and shrinkage deformation of the wood due to water absorption. At the same time, the skeleton structure can adsorb and bind preservative components, reducing the probability of wood being attacked by decay fungi and mold.

[0028] 2. This invention reduces the risk of premature gelation of the protective liquid in the shallow layer of wood, which could lead to blockage of the permeable pores. The latent rare earth catalytic liquid utilizes the coordination effect of chelating agents and rare earth ions to keep the rare earth catalytic components stably dispersed in an alkaline silicate matrix solution, thereby maintaining a low viscosity state in the initial stage of the mixed solution. The stable coordination state is conducive to the treatment liquid passing smoothly through the capillary network of the wood surface and entering the deeper internal areas during the pretreatment and impregnation stages, thereby improving the overall penetration depth and saturation of the working liquid.

[0029] 3. The processing technology of this invention improves the distribution of mineralized crystals inside the wood and reduces related drying defects. The alternating pressure difference operation used in the impregnation stage uses the instantaneous pressure gradient to promote the penetration of the solution into the difficult-to-impregnate areas, increasing the uniformity of inorganic components in the internal structure of the wood. The subsequent constant temperature and humidity and step-by-step heating and dehumidification steps coordinate the rate relationship between the diffusion of moisture inside the wood and the nucleation and growth of silicates, limit the excessively rapid vaporization of moisture, and reduce the situation of wood cracking or loose crystalline structure caused by local stress concentration. Attached Figure Description

[0030] Figure 1 This is a dynamic evolution curve of the protective liquid in Example 2 of the present invention under a simulated slightly acidic environment; Figure 2 The Fourier transform infrared spectra of the wood treated in Example 2 and Comparative Example 5 of the present invention are shown below. Figure 3 Comparative comparison charts of the weight gain rate, fixation rate and absolute loss of the chemical solution in the wood treated by Example 2 and Comparative Examples 2 to 4 of the present invention; Figure 4 This is a comparative chart showing the peak heat release rate, residual mass rate, and total smoke emission of each group of samples in this invention. Figure 5 This is a comprehensive evaluation diagram of the biodegradation resistance of Examples 2 and 4 of the present invention and the blank untreated substrate; Figure 6 This is a comparative chart showing the water absorption swelling rate and swelling resistance rate of Embodiments 2 and 4 of the present invention and the corresponding blank substrates. Detailed Implementation

[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.

[0033] Sodium silicate, CAS No. 1344-09-8, commercially available, with a modulus of 2.5 to 3.5 and a solid content of 30 wt% to 45 wt%. Potassium silicate, CAS No. 1312-76-1, commercially available, with a modulus of 2.5 to 3.2 and a solid content of 30 wt% to 40 wt%. Lanthanum chloride, CAS No. 10099-58-8, commercially available; Cerium nitrate, CAS No. 10108-73-3, commercially available product; 2-Methyl-4-isothiazolin-3-one, CAS No. 2682-20-4, commercially available aqueous microemulsion, solid content 10 wt%; Iodopropynyl butylcarbamate, CAS No. 55406-53-6, is a commercially available aqueous microemulsion with a solid content of 10 wt%.

[0034] In this invention, the units of measurement for all materials and solvents are uniformly referred to as parts by weight.

[0035] Preparation Example 1: This preparation example provides a method for preparing a latent rare earth catalyst solution, including the following steps: Add 15 parts of deionized water to a reactor equipped with a heating and stirring device, followed by 1 part of lanthanum chloride. Stir at 200 rpm until completely dissolved. Adjust the system temperature to 40°C and slowly add 1.2 parts of sodium citrate to the solution. Maintain a constant temperature of 40°C and continue the reaction at 300 rpm for 30 minutes. Cool to room temperature to obtain a latent rare earth catalyst solution, hereinafter referred to as latent rare earth catalyst solution A.

[0036] Preparation Example 2: This preparation example provides a method for preparing a latent rare earth catalyst solution, including the following steps: Add 12 parts of deionized water to a reactor equipped with a heating and stirring device, followed by 3 parts of cerium nitrate. Stir at 250 rpm until completely dissolved. Adjust the system temperature to 45°C and slowly add 4.5 parts of disodium ethylenediaminetetraacetate to the solution. Maintain a constant temperature of 45°C and continue the reaction at 400 rpm for 45 minutes. Cool to room temperature to obtain a latent rare earth catalyst solution, hereinafter referred to as latent rare earth catalyst solution B.

[0037] Preparation Example 3: This preparation example provides a method for preparing a latent rare earth catalyst solution, including the following steps: Add 10 parts of deionized water to a reactor equipped with a heating and stirring device, followed by 2.5 parts of lanthanum chloride and 2.5 parts of cerium nitrate. Stir at 300 rpm until completely dissolved. Adjust the system temperature to 50°C and slowly add 5 parts of glycerol to the solution. Maintain a constant temperature of 50°C and continue the reaction at 500 rpm for 60 minutes. Cool to room temperature to obtain a latent rare earth catalyst solution, hereinafter referred to as latent rare earth catalyst solution C. Example

[0038] This embodiment provides a process for a long-lasting wood protectant, including the following steps: S1. Add 60 parts of sodium silicate to a reaction vessel and add 36 parts of deionized water. Stir at 150 rpm for 10 min at 25°C to form a matrix solution. Then, while maintaining stirring, slowly add 2 parts of latent rare earth catalyst A to the matrix solution at a rate of 10 L / min through a metering device. Finally, add 2 parts of 2-methyl-4-isothiazolin-3-one and continue stirring for 15 min. Filter through a 200-mesh filter to obtain a long-lasting wood protectant. S2. Clean the surface of the 0.5mm thick bamboo veneer thoroughly, and rinse with deionized water at a concentration of 0.05kg / m³. 2 The amount of product used is used to pre-wet the surface of the bamboo and wood veneer. The wood long-lasting protectant is diluted on-site with deionized water at a volume ratio of 1:1 to obtain a diluted protective solution. S3. Apply the diluted protective solution evenly to the surface of the bamboo and wood patch and soak it under normal pressure for 30 minutes. After removing it, let it air dry until there is no free water on the surface. S4. Send the bamboo and wood veneer into the temperature and humidity controlled kiln and start heating to raise the kiln temperature to 40°C. At the same time, continuously spray water vapor to force the relative humidity inside the kiln to be 85% and maintain a constant temperature and humidity state for 12 hours. Then stop the steam injection and raise the kiln temperature stepwise by increasing the temperature by 5°C every 4 hours until the core moisture content of the bamboo and wood veneer drops to 12% before it is taken out of the kiln. S5. After the bamboo and wood veneers are removed from the kiln, they are transferred to a conventionally ventilated warehouse for static curing for 21 days to complete the silicate mineralization and crystallization process in the pores, thus obtaining wood that has undergone long-term protective treatment. Example

[0039] This embodiment provides a process for a long-lasting wood protectant, including the following steps: S1. Add 70 parts of sodium silicate to a reaction vessel and add 23 parts of deionized water. Stir at 200 rpm for 15 min at 25°C to form a matrix solution. Then, while maintaining stirring, slowly add 6 parts of latent rare earth catalyst B to the matrix solution at a rate of 15 L / min through a metering device. Finally, add 1 part of iodopropynyl butylcarbamate and continue stirring for 20 min. Filter through a 200-mesh filter to obtain a wood long-lasting protectant. S2. Clean the surface of the 10cm thick high-density hardwood load-bearing column thoroughly with deionized water at a concentration of 0.15kg / m². 2 The amount of the agent was used to pre-wet the hardwood surface. The wood long-lasting protectant was diluted on-site with deionized water at a volume ratio of 1:2 to obtain the diluted protective solution. S3. Place the hardwood load-bearing column into the pressure-resistant impregnation tank, evacuate to -0.09MPa and maintain for 20 minutes. Use negative pressure to draw the diluted protective liquid into the impregnation tank until the liquid surface completely submerges the wood. Release the vacuum and use a pressure pump to raise the positive pressure in the tank to 0.8MPa for constant pressure permeation. When the constant pressure permeation time reaches 80 minutes, quickly open the exhaust valve to drop the pressure in the tank to 0.05MPa within 15 seconds and maintain the low pressure state for 1 minute. Then repressurize to 0.8MPa and perform the alternating pressure difference cycle 3 times. After the total soaking time reaches 120 minutes, drain the solution. S4. After soaking, place the hardwood load-bearing column in a ventilated place for 7 days until there is no free water on the surface. Then, put it into a temperature and humidity controlled kiln and start heating to raise the kiln temperature to 50°C. At the same time, continuously spray water steam to force the relative humidity inside the kiln to be maintained at 95% and keep it in a constant temperature and humidity state for 24 hours. Then, stop spraying steam and raise the kiln temperature in stages by 10°C every 2 hours to remove moisture. Strictly control the maximum kiln temperature at 70°C until the core moisture content of the wood stabilizes at 14% before taking it out of the kiln. S5. After the hardwood load-bearing columns are removed from the kiln, they are transferred to a conventional ventilated warehouse for static curing for 28 days to complete the in-situ nucleation and mineralization of silicates in the pores, thus obtaining wood that has undergone long-term protective treatment. Example

[0040] This embodiment provides a process for a long-lasting wood protectant, including the following steps: S1. Add 65 parts of potassium silicate to a reaction vessel and add 30.5 parts of deionized water. Stir at 180 rpm for 12 min at 25°C to form a matrix solution. Then, while maintaining stirring, slowly add 3 parts of latent rare earth catalyst C to the matrix solution at a rate of 12 L / min through a metering device. Finally, add 1.5 parts of 2-methyl-4-isothiazolin-3-one and continue stirring for 18 min. Filter through a 200-mesh filter to obtain a long-lasting wood protectant. S2. Clean the surface of the 5cm thick cedar landscape board, and rinse it with deionized water at a concentration of 0.1kg / m². 2 The amount of the agent was used to pre-wet the surface of the fir wood. The wood long-lasting protectant was diluted on-site with deionized water at a volume ratio of 1:1 to obtain the diluted protective solution. S3. Place the fir landscape board into the pressure-resistant impregnation tank, evacuate to -0.08MPa and maintain for 15 minutes. Use negative pressure to draw the diluted protective liquid into the impregnation tank until the wood is submerged. Release the vacuum and use a pressure pump to raise the positive pressure in the tank to 0.6MPa for constant pressure penetration. When the constant pressure penetration time reaches 40 minutes, quickly open the exhaust valve to drop the pressure in the tank to 0.1MPa within 20 seconds and maintain the low pressure state for 1.5 minutes. Then repressurize to 0.6MPa and perform the alternating pressure difference cycle once. After the total soaking time reaches 60 minutes, drain the liquid. S4. After soaking, place the cedar landscape boards in a ventilated place for 3 days until there is no free water on the surface. Then, put them into a temperature and humidity controlled kiln and start heating to raise the kiln temperature to 45°C. At the same time, continuously spray water vapor to force the relative humidity inside the kiln to be maintained at 90% and keep it in a constant temperature and humidity state for 18 hours. Then, stop spraying steam and raise the kiln temperature stepwise by 8°C every 3 hours to remove moisture. Control the maximum kiln temperature at 65°C until the core moisture content of the wood drops to 13% before taking it out of the kiln. S5. After the cedar landscape boards are removed from the kiln, they are transferred to a conventionally ventilated warehouse for static curing for 24 days to complete the mineralization and crystallization process, thus obtaining wood that has undergone long-term protective treatment. Example

[0041] This embodiment provides a process for a long-lasting wood protectant, including the following steps: S1. Add 68 parts of sodium silicate to a reaction vessel and add 25 parts of deionized water. Stir at 150 rpm for 10 min at 25°C to form a matrix solution. Then, while maintaining stirring, slowly add 5 parts of latent rare earth catalyst B to the matrix solution through a metering device. Finally, add 2 parts of iodopropynyl butylcarbamate and continue stirring for 15 min. Filter through a 200-mesh filter to obtain a wood long-lasting protectant. S2. Clean the surface of a 2cm thick standard bamboo board, and rinse it with deionized water at a concentration of 0.1kg / m². 2The amount of wood pre-wetting agent was used to pre-wet the surface. The wood long-lasting protectant was diluted on-site with deionized water at a volume ratio of 1:1 to obtain a diluted protective solution. S3. Place the bamboo board into a pressure-resistant impregnation tank, evacuate to -0.085MPa and maintain for 10 minutes. Use negative pressure to draw in diluted protective liquid until the board is submerged. Release the vacuum and pressurize to 0.7MPa for constant pressure impregnation. When the constant pressure impregnation time reaches 30 minutes, quickly open the exhaust valve to drop the pressure in the tank to 0.08MPa and maintain for 1 minute. Then repressurize to 0.7MPa. Repeat the alternating pressure difference cycle twice. After the total soaking time reaches 45 minutes, drain the liquid. S4. After soaking, place the bamboo boards in a ventilated place for 5 days until there is no free water on the surface. Then, put them into a temperature and humidity controlled kiln and start heating to raise the kiln temperature to 48°C. At the same time, spray water steam to force the relative humidity inside the kiln to be 92% and keep it in a constant temperature and humidity state for 20 hours. Then, stop spraying steam and carry out step-by-step heating and dehumidification until the core moisture content of the wood drops to 12% before taking it out of the kiln. S5. After the bamboo boards are removed from the kiln, they are transferred to a conventionally ventilated warehouse for static curing for 25 days to complete the mineralization and crystallization process, thus obtaining wood that has undergone long-term protective treatment.

[0042] Comparative Example 1: Compared with Example 2, the difference is that in S1, the latent rare earth catalyst B is not used, but the same mass of free cerium nitrate is directly added to the matrix solution. All other aspects are the same.

[0043] Comparative Example 2: Compared with Example 2, the difference is that in S3, the alternating pressure differential cycle operation is not performed. Instead, the constant pressure of 0.8MPa is maintained throughout the process until the total soaking time reaches 120min before the solution is drained. All other aspects are the same.

[0044] Comparative Example 3: Compared with Example 2, the difference is that in S4, water vapor is not continuously sprayed to force a high humidity state, but conventional industrial hot air is directly used to dry and remove moisture from the wood until the core moisture content stabilizes at 14%. All other aspects are the same.

[0045] Comparative Example 4: Compared with Example 2, the difference is that in S2, the high-density hardwood load-bearing column is first soaked and boiled in a strong alkaline solution to remove the natural slightly acidic substances inside, and then dried after completely destroying the slightly acidic environment inside the wood before subsequent protective treatment. All other operations are the same.

[0046] Comparative Example 5: Compared with Example 2, the difference is that S5 is omitted, that is, the wood after leaving the kiln is directly used as the finished product, without the static curing and mineralization crystallization process in the conventional ventilated warehouse, and the rest are the same.

[0047] Test Example 1: Take 200 mL of each of the protective liquids prepared in Examples 1 to 4 and Comparative Example 1, and measure the initial viscosity of each group of protective liquids at an ambient temperature of 25°C using a rotational viscometer (rotor No. 1) at a speed of 60 rpm.

[0048] Each group of protective liquids was placed in a sealed glass bottle and left to stand at 25°C for 24 hours. The viscosity after storage was measured again under the same test conditions, the data were recorded, and the changes in state were observed.

[0049] Take 150 mL of the protective liquid prepared in Example 2 and place it in a beaker with a magnetic stirrer. Set the stirring speed to 200 rpm and immerse the tip of the burette, the pH composite electrode, and the immersion transmittance fiber optic probe of the automatic potentiometric titrator below the liquid surface.

[0050] Start the titrator and add 0.1 mol / L acetic acid solution at a rate of 0.5 mL / min. Record the pH value and transmittance of the system in real time. At the same time, take 3 mL samples at different pH points and use a rheometer to measure the instantaneous viscosity to obtain the dynamic evolution data of the system under simulated slightly acidic environment.

[0051] Table 1. Viscosity changes of each group of protective fluids before and after storage:

[0052] According to Table 1 and Figure 1 It can be seen that Comparative Example 1, without the addition of a complexing agent, experienced precipitation during the preparation stage, resulting in increased system viscosity and decreased fluidity. Examples 1 to 4, by introducing ligands to form a complex masking structure, suppressed early precipitation side reactions and maintained the liquid at a low viscosity. As the pH value of the system decreased, when the pH value dropped below 8.5, the transmittance of the protective liquid in Example 2 decreased sharply, while the system viscosity increased, exhibiting characteristics of a transition from fluid to gel state. This phenomenon indicates that acidic environmental conditions can promote the dissociation of the coordination structure, suggesting that the protective liquid, under the influence of the wood's intrinsic slightly acidic environment, has the tendency to release metal ions and trigger in-situ gelation and cross-linking of the silicate system.

[0053] Test Example 2: Core wood blocks measuring 10mm × 10mm × 10mm were cut from the geometric center of the wood after processing in Example 2 and Comparative Example 5, respectively. The blocks were then crushed using a pulverizer, and the wood powder that passed through a 100-mesh standard sieve was collected.

[0054] The collected wood powder was placed in a vacuum drying oven at 60°C and dried continuously for 24 hours to remove physically adsorbed water from the material.

[0055] Weigh out 2.1 mg of dried wood flour from Example 2 and 2.3 mg of dried wood flour from Comparative Example 5, respectively, and add 203.5 mg and 205.1 mg of dried potassium bromide powder to each. Grind them evenly in a mortar and then press them into thin tablets using a tablet press at a pressure of 15 MPa.

[0056] The thin slices were placed in the optical path of the Fourier transform infrared spectrometer, and the test wavenumber range was set to 4000 cm⁻¹. -1 Up to 400cm -1 The resolution is 4cm. -1 The scan was performed 32 times to collect test data.

[0057] Table 2. Transmittance values ​​at characteristic wavenumbers for Example 2 and Comparative Example 5:

[0058] According to Table 2 and Figure 2 It can be seen that, without static curing, Comparative Example 5 was at 966cm. -1 The area exhibits a relatively obvious characteristic absorption peak of Si-OH groups, corresponding to lower transmittance, while at 1083 cm⁻¹... -1 798cm -1 and 463cm -1 The characteristic absorption of Si-O-Si groups at this location is relatively weak, suggesting that more uncrosslinked hydrated silanol or oligomeric silica gel structures are retained inside the wood pores at this time; in contrast, after 28 days of static curing, the absorption at 966 cm⁻¹ in Example 2 is relatively weak. -1 The absorption intensity of the Si-OH characteristic peak at 1083 cm⁻¹ decreased, indicating an increase in transmittance. -1 798cm -1 and 463cm -1 The absorption intensity of the Si-O-Si characteristic peak at the location is correspondingly enhanced, that is, the transmittance decreases. The change in spectral data indicates that during the dehydration and curing stage, the sol and primary gel in the wood fiber network have a tendency to undergo dehydration condensation reaction, reflecting the process of silicate unit into inorganic silicate in a three-dimensional network structure. The test results are consistent with the expected law of mineralization and crystallization reaction.

[0059] Test Example 3: Wood substrate samples of the corresponding types in Examples 1 to 4 and Comparative Examples 2, 3 and 4 before treatment were selected and dried in an electric heating oven at 101 to 105°C until the mass was constant. The initial oven-dry mass of each sample was weighed and recorded using an analytical balance.

[0060] The samples were processed according to the process steps described in Examples 1 to 4 and Comparative Examples 2 to 4. After completing the static curing process, they were placed in an electric heating drying oven at 101 to 105°C to dry until the mass was constant. The oven-dried mass after processing was weighed and recorded.

[0061] According to relevant standards, an extraction loss test was conducted. The dried samples were placed in glass beakers, and deionized water with a volume of 10 times the sample volume was added. The samples were kept statically immersed in a 25°C water bath. The deionized water was replaced every 24 hours, and the extraction was carried out continuously for 14 days.

[0062] Take out the sample after the extraction treatment, wipe off the surface moisture, and dry it again in a drying oven at 101 to 105°C until constant weight. Weigh and record the oven-dry mass after the loss test.

[0063] Based on the formula WPG=[(Oven-dried mass after treatment - Oven-dried mass before treatment) / Oven-dried mass before treatment]×100% and the corresponding fixation rate formula, calculate the drug liquid weight gain rate WPG and the effective component fixation rate of each sample.

[0064] Table 3. Quality data and test results of treated wood for each group:

[0065] According to Table 3 and Figure 3 It can be seen that, comparing the data of Example 2 and Comparative Example 2, Comparative Example 2, which did not use the alternating pressure differential circulation process, had a relatively lower drug solution weight gain rate under the same total soaking time, suggesting that single constant pressure penetration is limited by the structural characteristics of wood, while the alternating pressure differential circulation process used in the examples showed a trend of promoting drug solution penetration into the wood interior; comparing the data of Example 2 and Comparative Example 3, although the initial drug solution weight gain rate of Comparative Example 3, which used conventional hot air drying, was similar to that of Example 2, the fixation rate decreased; This indicates that high humidity conditions are conducive to the migration and action of endogenous acidic substances in wood, thereby affecting the gelation process of the protective liquid inside, leading to the precipitation of some incompletely cross-linked components in the loss test. Comparing the data of Example 2 and Comparative Example 4, the fixation rate of Comparative Example 4, which pre-modified the slightly acidic environment of wood, was further reduced, and a more obvious loss phenomenon was observed. The results suggest that the endogenous slightly acidic environment of wood plays an active guiding role in promoting the release of complexed ions and in-situ gelation reaction, indicating that the synergy of each process step helps to effectively fix inorganic components inside the wood.

[0066] Test Example 4: The wood treated in Examples 1 to 4, Comparative Example 2, and the corresponding blank untreated wood, i.e., taking the hardwood substrate corresponding to Example 2 as an example, samples were cut off, a portion of the samples were ground and crushed, wood powder with a particle size of less than 0.2 mm was collected, and dried in a vacuum drying oven at 60°C for 24 hours for later use; another portion of the samples were cut and processed into standard board samples of 100 mm × 100 mm × 10 mm and dried under the same conditions.

[0067] Weigh approximately 5.2 mg of each group of wood flour samples and place them in an alumina crucible. Place the crucible in a thermogravimetric analyzer and set the test environment to air atmosphere with a gas flow rate of 50 mL / min. Heat the samples from 30 °C to 800 °C at a heating rate of 10 °C / min. Record the mass change data with temperature, generate a thermogravimetric loss curve, and record the final residual mass percentage at 800 °C.

[0068] The standard plate sample was placed horizontally on the sample holder of the cone calorimeter. The bottom and sides of the sample were covered with aluminum foil to suppress edge effects. The incident thermal radiation flux of the heating cone was set to 50 kW / m². 2 .

[0069] The evacuation and data acquisition system of the cone calorimeter is activated. The combustible gas generated on the surface of the sample is ignited using an electric spark igniter. The heat release rate during the combustion process is measured in real time, and the peak heat release rate and total smoke volume are calculated and recorded. The test continues until the sample no longer produces open flame and the mass tends to be constant.

[0070] Table 4. Test data of thermal stability and flame retardant performance of each group of samples:

[0071] According to Table 4 and Figure 4 It can be seen that the blank untreated wood exhibits significant weight loss when heated in air and has a low final residual amount. In the cone calorimetry test, it shows a high peak heat release rate accompanied by a large amount of smoke release. In contrast, Comparative Example 2, due to the lack of alternating pressure differential cycling process, has its protective components more confined to the shallow layer of wood. Although it can delay the ignition time to some extent in the early stage of the test, as the surface structure is damaged by heat, the internal substrate is exposed and a significant second exothermic peak is formed, showing certain limitations in the flame retardant improvement effect. The final residual mass percentage at 800℃ was improved in Examples 1 to 4, while the peak heat release rate and total smoke emission showed a significant decreasing trend; combined with Figure 4The continuous monitoring curves show that the heat release peak in Example 2 tends to be flat during the heating process, and the cumulative rate of smoke emission is also suppressed. The test results suggest that the inorganic crystals distributed in the deep pores of the wood will undergo phase transformation under high temperature conditions to form a continuous inorganic layer with a certain covering effect. The physical barrier helps to prevent external oxygen penetration and internal heat conduction, slow down the release of flammable volatiles, and thus play a comprehensive protective role in flame retardancy and smoke suppression for the wood substrate.

[0072] Test Example 5: Test blocks with a processing size of 20mm×20mm×10mm were cut from the finished wood products of Examples 1 to 4 and the corresponding four blank untreated substrates. They were placed in an electric heating drying oven and dried until the mass was constant. The initial absolute dry weight of each test block was recorded. Then, all test blocks were sterilized with ethylene oxide gas for later use.

[0073] Potato glucose agar medium was prepared and autoclaved. The medium was poured into petri dishes and cooled to solidify. Under aseptic conditions, *Cladosporium glomeratum* (representing brown rot fungi) and *Cladosporium variegatum* (representing white rot fungi) were inoculated and placed in an incubator until the mycelia completely covered the surface of the medium.

[0074] The sterilized test blocks were placed on the isolation pads in the culture dishes covered with test hyphae, and then transferred to a constant temperature and humidity incubator with the temperature controlled at 28°C and the relative humidity maintained at 80% for 12 consecutive weeks of inoculation culture.

[0075] After the culture period is over, remove the test block and carefully scrape off the mycelial network attached to the surface. Rinse it with deionized water, place it in a drying oven and dry it again until constant weight. Record the mass after the test to calculate the mass loss rate.

[0076] Select spare sterilized test blocks of the same size to conduct a termite forced feeding experiment. A 3cm thick layer of sterilized river sand with a moisture content of 20% was laid at the bottom of a cylindrical glass container with ventilation holes. The test blocks were placed on the sand surface, and 200 Formosan subterranean termites of the same physiological state were introduced into each container. The containers were left to stand for 28 days in the dark at a temperature of 26°C.

[0077] After the trial period, the container was dissected to count the number of surviving termites, calculate the termite mortality rate, and rate the degree of termite infestation of the test blocks according to relevant standards.

[0078] Table 5. Data on biodegradation resistance evaluation of each group of test blocks:

[0079] According to Table 5 and Figure 5It was found that untreated blank hardwood and blank bamboo boards showed a relatively high susceptibility to wood-decaying fungi and termites during environmental cultivation, with a relatively high mass loss rate and a low termite mortality rate, and the test blocks showed a certain degree of structural damage. In contrast, the mass loss rate of the substrates in Examples 1 to 4 was effectively controlled after experiencing the same infection and forced feeding conditions, and the termite colonies that fed on the wood showed a high mortality rate. The test data were consistent with the protection pattern expected by the process, suggesting that the silicate inorganic crystals generated in the gaps between wood fibers during the process occupy the permeation space of water and extracellular enzymes, thereby constructing an isolation structure at the physical level. This structure is conducive to hindering the pathways for fungi and termites to obtain natural cellulose components, showing a tendency to help improve the biodegradability of treated wood.

[0080] Test Example 6: Cube samples with a processing size of 20mm×20mm×20mm were cut from the hardwood of Example 2, the bamboo board of Example 4, and the corresponding blank untreated hardwood and blank untreated bamboo board.

[0081] Each group of samples was dried in an electric heating drying oven at 101 to 105°C until the mass was constant. The samples were then removed and cooled to room temperature in a desiccator. The initial dimensions of each sample in the radial, chordal, and longitudinal directions were measured using a vernier caliper with an accuracy of 0.02 mm. The data were recorded and the initial absolute dry volume and initial chordal thickness of each sample were calculated.

[0082] Each group of samples was placed in a constant temperature water bath containing deionized water at 18 to 22°C. The samples were then completely submerged 50 mm below the water surface using a stainless steel pressure mesh. The samples were kept submerged for 192 hours to allow the wood to reach a state of water saturation.

[0083] Remove the sample from the water and use qualitative filter paper to quickly absorb the free water adhering to the sample surface. Immediately use vernier calipers to measure the three-dimensional dimensions of the sample after it has absorbed water to saturate, and calculate the saturated volume and saturated chordal thickness after immersion.

[0084] The volume expansion rate and thickness expansion rate of each group of samples were calculated based on the dimensional data before and after immersion in water; at the same time, the expansion resistance rate of Example 2 and Example 4 was calculated using the corresponding blank substrate data as a reference.

[0085] Table 6. Data on water absorption swelling rate and dimensional stability of each group of samples:

[0086] According to Table 6 and Figure 6It can be seen that untreated blank hardwood and blank bamboo boards exhibited obvious water absorption and swelling characteristics under long-term water immersion conditions, suggesting that water molecules can enter the wood cell wall and combine with cellulose hydroxyl groups, thereby causing the cells to swell in volume. The wood treated in Examples 2 and 4, with no obvious external coating on the surface, showed a significant decrease in volume swelling rate and thickness swelling rate compared with the corresponding blank group. The calculated volume swelling resistance rate and thickness swelling resistance rate both reached more than 70%. In Table 6, "-" indicates that the blank substrate is used as the calculation benchmark for the anti-swelling rate and does not have a corresponding anti-swelling rate value. The trend of the test data is consistent with the expected protective mechanism, suggesting that the silicate mineralization and crystallization process that occurs in the pores and cell cavities of the wood will partially fill the entry channels of free water at the physical level, which will help reduce the penetration of water into the capillary pores of the fiber network. At the same time, the rigid inorganic silicate three-dimensional skeleton generated will build a supporting structure inside the cells, which will help resist the deformation stress generated by the cellulose molecular chains after absorbing water. The results show that the corresponding treatment process has the potential to improve the internal structural waterproofing and enhance the dimensional stability of the material without relying on the external sealing film and while basically preserving the original appearance of the substrate.

[0087] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A long-lasting wood protectant, characterized in that, The wood long-lasting protectant is made from the following raw materials in parts by weight: 60 to 70 parts silicate; 20 to 40 parts deionized water; 2 to 6 parts latent rare earth catalyst; and 1 to 2 parts preservative.

2. The wood long-lasting protectant according to claim 1, characterized in that, The wood long-lasting protective agent is prepared by a method including the following steps: The silicate and the deionized water are stirred at a speed of 150 to 200 rpm for 10 to 15 minutes to form a matrix solution; While maintaining stirring, the latent rare earth catalyst solution is added to the matrix solution at a rate of 10 to 15 L / min using a metering dosing device. Then add the preservative, continue stirring for 15 to 20 minutes, and filter through a filter screen to obtain the wood long-lasting protectant.

3. The wood long-lasting protectant according to claim 1, characterized in that, The silicate is either sodium silicate or potassium silicate; the preservative is either 2-methyl-4-isothiazolin-3-one or iodopropynyl butylcarbamate.

4. The wood long-lasting protective agent according to claim 1, characterized in that, The latent rare earth catalyst solution is made from raw materials comprising the following parts by weight: 10 to 15 parts deionized water; 1 to 5 parts rare earth salt; and 1 to 5 parts chelating agent. The rare earth salt is at least one of lanthanum chloride or cerium nitrate; the chelating agent is one of sodium citrate, disodium ethylenediaminetetraacetate, or glycerol.

5. The wood long-lasting protectant according to claim 4, characterized in that, The preparation method of the latent rare earth catalyst solution includes: adding deionized water and rare earth salt to a reaction vessel equipped with a heating and stirring device, and stirring at a speed of 200 to 300 rpm until completely dissolved; adjusting the system temperature to 40 to 50°C, and slowly adding the chelating agent to the solution; maintaining a constant temperature of 40 to 50°C, and continuing the reaction at a speed of 300 to 500 rpm for 30 to 60 minutes, and cooling to room temperature to obtain the solution.

6. A process for a wood long-lasting protective agent according to any one of claims 1 to 5, characterized in that, The process includes the following steps: Prepare the wood long-lasting protective agent according to the formula ratio, and mix and dilute it with deionized water at a volume ratio to obtain a diluted protective solution; After cleaning and pre-wetting the surface of the wood to be treated, allow the diluted protective solution to penetrate and immerse itself in the wood. Once the wood is saturated with water, drain the excess solution. After soaking, the wood is placed naturally until there is no free water on the surface, and then sent into a temperature and humidity controlled kiln for constant temperature and humidity treatment. After the constant temperature and humidity treatment is completed, the wood is heated in stages to remove moisture until the core moisture content of the wood drops to the target range before it is removed from the kiln. After the wood comes out of the kiln, it is transferred to a conventional ventilated warehouse for static curing to complete the in-situ mineralization and crystallization process of silicates in the wood pores, thus obtaining wood that has undergone long-term protective treatment.

7. The process for the wood long-lasting protective agent according to claim 6, characterized in that, The process of allowing the diluted protective solution to penetrate and immerse the wood includes: placing the wood to be treated into a pressure-resistant impregnation tank, evacuating to -0.08 to -0.09 MPa and maintaining it for 10 to 20 minutes, using negative pressure to draw the diluted protective solution into the impregnation tank until the wood is completely submerged, releasing the vacuum and using a pressure pump to increase the positive pressure inside the tank to 0.6 to 0.8 MPa for constant pressure penetration; when the constant pressure penetration time reaches 30 to 80 minutes, quickly opening the exhaust valve, rapidly reducing the pressure inside the tank to 0.05 to 0.1 MPa within 15 to 20 seconds and maintaining the low pressure state for 1 to 1.5 minutes, and then repressurizing to 0.6 to 0.8 MPa; performing the alternating pressure differential cycle 1 to 3 times, and draining the solution after the total soaking time reaches 45 to 120 minutes.

8. The process for the wood long-lasting protective agent according to claim 6, characterized in that, The constant temperature and humidity treatment and the step-by-step heating and dehumidification process include: starting the heating to raise the kiln temperature to 40 to 50°C, while continuously injecting water vapor to force the relative humidity inside the kiln to be between 85% and 95% and maintaining a constant temperature and humidity state for 12 to 24 hours; then stopping the steam injection, and carrying out step-by-step heating and dehumidification according to a gradient of 5 to 10°C every 2 to 4 hours, and strictly controlling the highest kiln temperature at 65 to 70°C, until the core moisture content of the wood stabilizes at 12% to 14% before it is removed from the kiln.

9. The process for the wood long-lasting protective agent according to claim 6, characterized in that, The wood long-lasting protective agent is diluted with deionized water at a volume ratio of 1:1 to 1:2; during the pre-wetting process of the wood surface to be treated, the amount of deionized water used is 0.05 to 0.15 kg / m³. 2 .

10. The application of a wood long-lasting protectant as described in any one of claims 1 to 5 in the dimensional stabilization treatment or anti-biodegradation treatment of wood products.