An interface reinforcement method for continuous fiber thermoplastic composites integrating automated layup and 3D printing

By depositing a resin transition layer on the surface of an automated filament-laying substrate and setting precise printing parameters, the problem of low interfacial bonding strength when combining automated layup and 3D printing processes is solved, achieving high-precision, low-cost integrated manufacturing of composite materials and improving the anti-delamination ability of composite structures.

CN123104052APending Publication Date: 2026-11-17TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611618600.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, it is difficult to effectively combine automated placement and 3D printing processes, resulting in low interfacial bonding strength and easy delamination, which severely restricts the load-bearing capacity and reliability of composite structures.

Method used

By depositing a resin transition layer on the surface of an automated filament-laying substrate and forming an integrated composite structure using continuous fiber 3D printing, the interfacial bonding strength can be controlled, including the precise setting of parameters such as the linewidth, spacing, and thickness of the resin transition layer, as well as printing temperature and speed.

Benefits of technology

It achieves precise control of the interface bonding strength, improves manufacturing precision and process controllability, reduces costs, is applicable to a wide range of application scenarios, and enhances the anti-delamination ability of composite structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104052A_ABST
    Figure CN123104052A_ABST
Patent Text Reader

Abstract

This invention provides a method for enhancing the interface of continuous fiber thermoplastic composite materials by integrating automated fiber placement and 3D printing. The method includes: step S1, providing an automated fiber placement substrate; step S2, depositing a resin transition layer on the surface of the automated fiber placement substrate using a 3D printing process, wherein the resin transition layer is made of the same matrix material as the automated fiber placement substrate; and step S3, depositing a continuous fiber reinforced thermoplastic composite material on the surface of the resin transition layer using a continuous fiber 3D printing process, forming an integrated composite structure with the automated fiber placement substrate. Therefore, this method for enhancing the interface of continuous fiber thermoplastic composite materials by integrating automated fiber placement and 3D printing achieves precise control of the interface bonding strength from weak to strong by designing the pattern structure and printing parameters of the resin transition layer. It has significant advantages such as high manufacturing precision, strong process controllability, low cost, and wide applicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of additive manufacturing technology, and more specifically to a method for enhancing the interface of continuous fiber thermoplastic composites that integrates automated layup and 3D printing. Background Technology

[0002] Continuous carbon fiber reinforced thermoplastic composites, with their advantages of high specific strength, good toughness, and recyclability, have become core materials for lightweight structures in aerospace, rail transportation, and new energy equipment. The emergence of additive manufacturing technology has further promoted the high-end application of continuous fiber composites. Automated fiber placement (including Automated Fiber Placement, ATP, and Automated Fiber Placement, AFP) is the mainstream technology for efficient and high-precision manufacturing of thermoplastic composites. The automated placement process relies on multi-axis robots and laser / infrared online heating to achieve precise stacking, in-situ melting, and rapid consolidation of continuous fiber prepregs / tapes. The resulting components exhibit controllable fiber orientation, high fiber volume fraction, and stable mechanical properties, meeting the manufacturing needs of large-size, high-load-bearing, and complex functional integrated carbon fiber composites. It is particularly suitable for the mass production of large main load-bearing structures such as panels, skins, and beams. Laser-assisted automated placement, through precise temperature control and pressure coupling, significantly improves interlayer fusion quality and reduces porosity, giving the fiber-placed board excellent in-plane stiffness and interlayer stability. However, automatic placement is limited by movement trajectory and stacking mode, and lacks flexibility in manufacturing complex configurations such as local reinforcement, irregular features, lattice structures, and pipeline integration, making it difficult to achieve integrated structural-functional design and manufacturing.

[0003] Continuous fiber reinforced composite 3D printing, based on additive manufacturing principles, enables moldless, digital, and free-form molding, breaking through the manufacturing constraints of traditional processes on complex structures. It allows for on-demand fiber path placement, maximizing lightweighting and load-bearing efficiency. Continuous fiber 3D printing retains the long-range continuous load-bearing characteristics of fibers, balancing the high performance of composite materials with the high flexibility of additive manufacturing, making it suitable for the rapid manufacturing of complex and detailed structures such as ribs, joints, and irregularly shaped reinforcements. However, the layer-by-layer deposition, lack of high-pressure consolidation, and rapid cooling characteristics of continuous fiber 3D printing result in components with low density, weak interlayer bonding, and significant anisotropy. Overall stiffness and stability are inferior to automatically laid-out sheets, making it difficult to independently bear the main load-bearing function.

[0004] Using laser-assisted PA6 / CF automated filament placement as a high-rigidity substrate, and integrating it with 3D-printed continuous fiber complex functional structures, the two processes can complement each other: the automated substrate placement provides the foundation for overall load-bearing capacity, dimensional stability, and efficient manufacturing, while 3D printing enables local reinforcement, functional integration, and free manufacturing of complex configurations, thus constructing a high-performance composite structure with "main load-bearing capacity + local functions," solving the industry pain point that it is difficult to integrate the complex features of large components.

[0005] Preliminary experiments show that directly depositing 3D-printed continuous fibers onto the surface of an automated filament placement plate results in extremely low interfacial bonding strength and a tendency for delamination, severely limiting the load-bearing capacity and reliability of the composite structure. Currently, existing technologies cannot effectively combine these two processes. The fundamental reason is that the automated filament placement plate undergoes in-situ solidification under high temperature and pressure, forming a dense, low-energy skin layer with high crystallinity and poor wettability. The rapid cooling of the 3D-printed melt and insufficient molecular chain diffusion make it difficult to form effective chain entanglement and thermal fusion with the substrate. In addition, factors such as mismatched molding stress, weak boundary layers, and surface contamination make the interface the weakest link in the composite structure. Summary of the Invention

[0006] This invention is made to solve the above-mentioned problems, and aims to provide a method for interface reinforcement of continuous fiber thermoplastic composites that integrates automated layup and 3D printing.

[0007] This invention provides a method for interface reinforcement of continuous fiber thermoplastic composite materials that integrates automated fiber placement and 3D printing, characterized by the following steps: Step S1, providing an automated fiber placement substrate; Step S2, depositing a resin transition layer on the surface of the automated fiber placement substrate using a 3D printing process, wherein the resin transition layer is made of the same matrix material as the automated fiber placement substrate; Step S3, depositing a continuous fiber reinforced thermoplastic composite material on the surface of the resin transition layer using a continuous fiber 3D printing process, thereby forming an integrated composite structure with the automated fiber placement substrate.

[0008] The method for interface reinforcement of continuous fiber thermoplastic composite materials that integrates automated placement and 3D printing provided by the present invention may also have the following feature: wherein, in step S2, the resin transition layer is deposited in a striped pattern, and the printing parameters of the resin transition layer include line width, spacing and thickness.

[0009] The interface reinforcement method for continuous fiber thermoplastic composite materials that integrates automatic lay-up and 3D printing provided by the present invention may also have the following characteristics: the line width ranges from 0.4 to 6 mm, the spacing ranges from 1 to 10 mm, and the thickness ranges from 0 to 0.3 mm.

[0010] The method for interface reinforcement of continuous fiber thermoplastic composite materials that integrates automatic lay-up and 3D printing provided by the present invention may also have the following feature: wherein the parameters of the 3D printing process include printing temperature, substrate temperature and printing speed.

[0011] The interface reinforcement method for continuous fiber thermoplastic composite materials that integrates automatic lay-up and 3D printing provided by the present invention may also have the following characteristics: wherein the printing temperature ranges from 220 to 260°C, the base plate temperature ranges from 30 to 100°C, and the printing speed ranges from 5 to 10 mm / s.

[0012] The method for enhancing the interface of continuous fiber thermoplastic composite material that integrates automated fiber placement and 3D printing provided by the present invention may also have the following feature: wherein, in step S1, the surface of the automated fiber placement substrate is subjected to polishing and plasma treatment before depositing the resin transition layer.

[0013] The interface reinforcement method for continuous fiber thermoplastic composite materials that integrates automatic lay-up and 3D printing provided by this invention may also have the following features: the grinding process uses 40-300 grit sandpaper, the plasma treatment power is 60-120W, the ambient pressure is 5-15Pa, and the treatment time is 200-300s.

[0014] The method for interface reinforcement of continuous fiber thermoplastic composite materials that integrates automatic lay-up and 3D printing provided by the present invention may also have the following features: step S4, placing the integrated composite structure in a constant temperature environment and slowly cooling it to room temperature to obtain an integrated composite structural component.

[0015] The interface reinforcement method for continuous fiber thermoplastic composite materials that integrates automatic fiber placement and 3D printing provided by the present invention may also have the following features: wherein the automatic fiber placement substrate is a laser-assisted PA6 / CF automatic fiber placement substrate, and the resin transition layer is a PA6 resin transition layer.

[0016] The role and effect of invention

[0017] The interface reinforcement method for continuous fiber thermoplastic composite materials integrating automated fiber placement and 3D printing according to the present invention includes: step S1, providing an automated fiber placement substrate; step S2, depositing a resin transition layer on the surface of the automated fiber placement substrate using a 3D printing process, wherein the resin transition layer is made of the same matrix material as the automated fiber placement substrate; and step S3, depositing a continuous fiber reinforced thermoplastic composite material on the surface of the resin transition layer using a continuous fiber 3D printing process, forming an integrated composite structure with the automated fiber placement substrate. Therefore, the interface reinforcement method for continuous fiber thermoplastic composite materials integrating automated fiber placement and 3D printing of the present invention achieves precise control of the interface bonding strength from weak to strong by designing the pattern structure and printing parameters of the resin transition layer, and has outstanding advantages such as high manufacturing precision, strong process controllability, low cost, and wide applicability. Attached Figure Description

[0018] Figure 1 This is a schematic flowchart of an interface reinforcement method for continuous fiber thermoplastic composite materials that integrates automated layup and 3D printing, as described in an embodiment of the present invention.

[0019] Figure 2 This is a schematic diagram illustrating the principle of the continuous fiber thermoplastic composite interface reinforcement method that integrates automated placement and 3D printing in an embodiment of the present invention.

[0020] Figure 3 This is a schematic diagram illustrating the design principle of the resin transition layer in an embodiment of the present invention.

[0021] Figure 4 This is a schematic diagram of the test sample in an embodiment of the present invention.

[0022] Figure 5 This is a metallographic image of the side of the molded sample in an embodiment of the present invention.

[0023] Figure 6 This is a schematic diagram comparing the force-displacement curves and interlaminar shear strength of different treatment methods when the resin transition layer is 2:3 and the layer thickness is 0.1mm in an embodiment of the present invention.

[0024] Figure 7 This is a schematic diagram showing the shear strength of different thicknesses when the resin transition layer is 2:3 in an embodiment of the present invention.

[0025] Figure 8 This is a schematic diagram of shear strength under different line widths and spacing ratios for the same layer thickness in an embodiment of the present invention. Detailed Implementation

[0026] To make the technical means, creative features, objectives and effects of this invention easy to understand, the following embodiments, in conjunction with the accompanying drawings, specifically illustrate the interface reinforcement method for continuous fiber thermoplastic composite materials that integrates automatic layup and 3D printing.

[0027] Example

[0028] Figure 1 This is a schematic flowchart of an interface reinforcement method for continuous fiber thermoplastic composite materials that integrates automated layup and 3D printing, as described in an embodiment of the present invention.

[0029] Figure 2 This is a schematic diagram illustrating the principle of the continuous fiber thermoplastic composite interface reinforcement method that integrates automated placement and 3D printing in an embodiment of the present invention.

[0030] like Figure 1 and Figure 2 As shown, this embodiment provides a method for interface reinforcement of continuous fiber thermoplastic composites that integrates automated layup and 3D printing, including:

[0031] Step S1: Provide an automated filament-laying substrate. The surface of the automated filament-laying substrate is then subjected to polishing and plasma treatment.

[0032] The polishing process uses 40-300 grit sandpaper, the plasma treatment power is 60-120W, the ambient pressure is 5-15Pa, and the treatment time is 200-300s. This activates the surface functional groups and improves the bond-to-bond connection.

[0033] Step S2: A resin transition layer is deposited on the surface of the automated filament-laying substrate using a 3D printing process. The resin transition layer is made of the same substrate material as the automated filament-laying substrate.

[0034] In step S2, the resin transition layer is deposited in a striped pattern. The printing parameters of the resin transition layer include linewidth, spacing, and thickness. The linewidth ranges from 0.4 to 6 mm, the spacing ranges from 1 to 10 mm, and the thickness ranges from 0 to 0.3 mm. The width (linewidth) of the printed extruded resin strips and the spacing between adjacent strips together determine the surface coverage of the transition layer. A linewidth that is too narrow will result in low single-pass spreading efficiency and a tendency for breakpoints to occur, while a linewidth that is too wide will reduce the stability of resin extrusion. The spacing ensures that adjacent resin strips overlap, allowing air bubbles in the resin transition layer to escape during printing, achieving complete coverage of the resin transition layer and forming a continuous, dense transition layer film.

[0035] Figure 3 This is a schematic diagram illustrating the design principle of the resin transition layer in an embodiment of the present invention.

[0036] like Figure 3As shown, the thickness of the resin transition layer determines the interfacial stress buffering capacity and thermal conductivity efficiency. If the thickness is too thin, it is difficult to cover the microscopic unevenness of the substrate, and the amount of resin is insufficient to support sufficient molecular chain diffusion. However, it can fill some of the gaps generated by 3D printing and can also facilitate interfacial bonding to some extent. If the resin transition layer is too thick, it will introduce additional thermal resistance and may generate new internal stress due to resin shrinkage. Furthermore, the interlayer failure mode will shift towards resin cohesive failure, while also increasing unnecessary printing time.

[0037] In this embodiment, the automated fiber placement substrate is a laser-assisted PA6 / CF automated fiber placement substrate, and the resin transition layer is a PA6 resin transition layer.

[0038] The parameters of the 3D printing process include printing temperature, substrate temperature, and printing speed. The printing temperature ranges from 220 to 260°C, the substrate temperature ranges from 30 to 100°C, and the printing speed ranges from 5 to 10 mm / s.

[0039] Printing temperature directly affects the resin's melt flowability, molecular chain diffusion ability, and fiber wetting effect. PA6 resin has a melting point of approximately 220℃, and the printing temperature needs to be higher than the melting point to ensure sufficient melt flow. Too low a temperature will result in excessively high resin viscosity, failing to adequately wet the fiber bundles and leading to poor interlayer bonding. Too high a temperature may cause thermal oxidative degradation of the PA6 molecular chains, thereby weakening its mechanical properties.

[0040] The substrate temperature affects the thermal history and crystallization behavior of the transition layer during deposition. The substrate temperature is set above the glass transition temperature of PA6 but below its melting point. Appropriately increasing the substrate temperature can slow down the cooling rate of the transition layer, providing a more sufficient diffusion time window for the resin molecular chains at the interface, while reducing warping deformation caused by rapid cooling. However, excessively high temperatures can cause the already spread transition layer to soften excessively, affecting the dimensional accuracy of subsequent fiber deposition.

[0041] Printing speed affects the residence time of the extruded melt at the interface and the spreading and compaction effect. Printing speed needs to be set in conjunction with printing temperature. At low temperatures, a low printing speed (e.g., 5 mm / s) is required to ensure sufficient melting and spreading time. At high temperatures, the printing speed can be appropriately increased (e.g., 10 mm / s). Excessive speed can lead to ineffective compaction of the extruded resin, reduced bonding strength between deposition channels, and potentially uneven surface quality.

[0042] Step S3: On the surface of the resin transition layer, a continuous fiber reinforced thermoplastic composite material is deposited using a continuous fiber 3D printing process to form an integrated composite structure with the automated fiber layup substrate.

[0043] In this embodiment, the continuous fiber reinforced thermoplastic composite material is a continuous carbon fiber reinforced PA6 composite material.

[0044] Step S4: Place the integrated composite structure in a constant temperature environment and slowly cool it to room temperature to obtain the integrated composite structural component.

[0045] In this embodiment, the preferred parameter combinations are shown in Table 1.

[0046] Table 1 Parameter Setting Table

[0047]

[0048] Under different combinations of the above parameters, the resin transition layer can achieve good surface coverage and resin spreading, and the interfacial bonding quality between the fiber deposition layer and the substrate can be quantitatively verified by interlayer shear strength testing.

[0049] In this embodiment, the specific operation steps are as follows:

[0050] First, a laser-assisted heating method is used to lay PA6 / CF prepreg filaments layer by layer on the surface of the mold to prepare a substrate with a thickness of about 1.5 mm.

[0051] The surface of the filament-lay substrate is sanded with P80 sandpaper to create a rougher microstructure. The substrate is then treated with appropriate plasma conditions. 3D printing begins immediately after treatment.

[0052] Using the same PA6 resin as the matrix material, a resin transition layer is printed and spread on the surface of an automated filament spreader according to a preset trajectory through the structured path design of the 3D printing equipment.

[0053] Above the resin transition layer, a coaxial printhead is used to deposit continuous carbon fiber reinforced PA6 prepreg filaments onto a set path to complete the 3D printing of complex functional structures and obtain an integrated composite structure.

[0054] In this embodiment, the geometric parameters of the resin transition layer are set as follows: resin transition layer linewidth: 0.4mm, 2mm, 4mm; resin transition layer spacing: 1mm, 3mm, 5mm, 6mm; resin transition layer thickness: 0, 0.05mm, 0.1mm, 0.2mm. The 3D printing process parameters are set as follows: printing temperature: 250℃; substrate temperature: 70℃; printing speed: 5mm / s, 10mm / s.

[0055] 3D printing cannot be performed at a speed of 10 mm / s. The polyamide transition layer has enough heat to melt, but the high speed and low pressure prevent the printing filaments from bonding. Therefore, it is best to choose a speed of around 5 mm / s for 3D printing.

[0056] After printing, the integrated composite structural component is placed in a constant temperature environment and slowly cooled to room temperature to avoid stress concentration caused by rapid cooling, and finally an integrated composite structural component with a total thickness of about 3 mm is obtained.

[0057] Finally, according to ASTM D2344 standard, a short beam shear test was conducted on the molded part, and the interlaminar shear strength value was used as a quantitative evaluation index of the interface bonding effect.

[0058] Figure 4 This is a schematic diagram of the test sample in an embodiment of the present invention.

[0059] The principle is as follows: a short beam specimen is placed on an interlaminar shear test fixture, and a concentrated load P is applied at the mid-span through an indenter, with the span-to-thickness ratio strictly adhering to 4:1. This causes the specimen to fail at the interlaminar section in the form of shear failure (interlaminar delamination / cracking) rather than bending failure, thus characterizing the bonding interface and interlaminar bond quality of the specimen. This method is often used to compare the effects of different ply structures, transition layer designs, and molding / compacting processes on interlaminar bonding.

[0060] The formula for calculating interlaminar shear strength is:

[0061]

[0062] In the formula, Interlaminar shear strength, in MPa. The maximum load at which the specimen fails is expressed in Newton-hours (N). The width of the sample is in mm. The thickness of the sample is in mm.

[0063] Figure 5 This is a metallographic image of the side of the molded sample in an embodiment of the present invention. For example... Figure 5 As shown, there is a clear transition layer between the upper continuous fiber 3D printed structure and the lower automatic fiber placement structure.

[0064] Figure 6 This is a schematic diagram comparing the force-displacement curves and interlaminar shear strength of different treatment methods when the resin transition layer is 2:3 and the layer thickness is 0.1mm in an embodiment of the present invention.

[0065] like Figure 6 As shown, the micro-roughness of sandpaper treatment creates a stronger mechanical interlocking effect, enabling more efficient load transfer in the initial stage of stress. In contrast, plasma treatment may reduce interface roughness due to the etching effect, resulting in a lack of effective physical anchoring in the initial stage and exhibiting lower stiffness characteristics.

[0066] Figure 7 This is a schematic diagram showing the shear strength of different thicknesses when the resin transition layer is 2:3 in an embodiment of the present invention.

[0067] Figure 8 This is a schematic diagram of shear strength under different line widths and spacing ratios for the same layer thickness in an embodiment of the present invention.

[0068] like Figure 7 and Figure 8 As shown in the figure, experiments have demonstrated that the transition layer design can significantly improve interlayer shear performance, but its effect is closely related to the thickness of the transition layer. There is a synergistic effect between the proportion and thickness of the transition layer, which can maintain interfacial bonding performance comparable to that of the all-adhesive system while significantly reducing the amount of adhesive, thus achieving synergistic optimization of lightweight and high performance.

[0069] Compared to direct 3D printing, the interlayer shear strength of the molded parts produced by the method in this embodiment is significantly improved, and the interface peeling failure phenomenon is fundamentally improved. These tests verify the feasibility and superiority of the new method of step-by-step printing of resin transition layers to enhance the interface. The presence of the transition layer makes it more controllable to construct high-performance composite structures with main load-bearing capacity and local complex structures, solving the industry pain point that it is difficult to integrally mold the complex features of large components.

[0070] The role and effect of the embodiments

[0071] According to the interface enhancement method for continuous fiber thermoplastic composite materials integrating automatic fiber placement and 3D printing involved in this embodiment, it includes: step S1, providing an automatic fiber placement substrate; step S2, depositing a resin transition layer on the surface of the automatic fiber placement substrate using a 3D printing process, wherein the resin transition layer is made of the same matrix material as the automatic fiber placement substrate; step S3, depositing a continuous fiber reinforced thermoplastic composite material on the surface of the resin transition layer using a continuous fiber 3D printing process, forming an integrated composite structure with the automatic fiber placement substrate. Therefore, the interface enhancement method for continuous fiber thermoplastic composite materials integrating automatic fiber placement and 3D printing of the present invention achieves precise control of the interface bonding strength from weak to strong by designing the pattern structure and printing parameters of the resin transition layer, and has outstanding advantages such as high manufacturing precision, strong process controllability, low cost, and wide applicability.

[0072] This embodiment also achieves precise control of the interface bonding strength. By adjusting the geometric parameters such as the line width, spacing, and height of the transition layer pattern, as well as the process parameters such as the continuous fiber printing temperature, layer thickness, and speed, the gradient and programmable precise control of the interface shear strength is realized, meeting the differentiated requirements of bonding strength under different working conditions.

[0073] This embodiment utilizes the buffering effect of the resin transition layer to effectively alleviate the thermo-mechanical parameter conflict caused by the difference in thermal expansion coefficient and crystallization gradient between the automatic placement and 3D printing processes, thereby improving the stability of integrated manufacturing of large components.

[0074] This embodiment can complete the preparation of the resin transition layer and the continuous fiber deposition molding in a single device, eliminating intermediate processes such as workpiece transfer and secondary clamping, shortening the overall molding cycle, and reducing material costs and process complexity.

[0075] The molecular diffusion and buffering mechanism of the resin transition layer in this embodiment improves the interfacial peel strength by more than 40%, effectively enhancing the anti-delamination capability of the composite structure under service loads, and making it suitable for high reliability requirements in fields such as aerospace, automotive, and high-end equipment.

[0076] Those skilled in the art should understand that this invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to this invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.

Claims

1. A method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing, characterized in that, include: Step S1: Provide an automated wire-laying substrate; Step S2: On the surface of the automated filament-laying substrate, a resin transition layer is deposited using a 3D printing process. The resin transition layer is made of the same substrate material as the automated filament-laying substrate. Step S3: On the surface of the resin transition layer, a continuous fiber reinforced thermoplastic composite material is deposited using a continuous fiber 3D printing process to form an integrated composite structure with the automated fiber placement substrate.

2. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 1, characterized in that: in, In step S2, the resin transition layer is deposited in a striped pattern, and the printing parameters of the resin transition layer include line width, spacing and thickness.

3. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 2, characterized in that: in, The line width ranges from 0.4 to 6 mm, the spacing ranges from 1 to 10 mm, and the thickness ranges from 0 to 0.3 mm.

4. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 1, characterized in that: in, The parameters of the 3D printing process include printing temperature, substrate temperature, and printing speed.

5. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 4, characterized in that: in, The printing temperature range is 220~260℃, the base plate temperature range is 30~100℃, and the printing speed range is 5~10mm / s.

6. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 1, characterized in that: in, In step S1, before depositing the resin transition layer, the surface of the automated filament-laying substrate is polished and subjected to plasma treatment.

7. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 6, characterized in that: in, The polishing process uses 40-300 grit sandpaper, the plasma treatment has a power of 60-120W, an ambient pressure of 5-15Pa, and a treatment time of 200-300s.

8. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 1, characterized in that, Also includes: Step S4: Place the integrated composite structure in a constant temperature environment and slowly cool it to room temperature to obtain the integrated composite structural component.

9. The method for interface reinforcement of continuous fiber thermoplastic composites integrating automated layup and 3D printing according to claim 1, characterized in that: in, The automated fiber placement substrate is a laser-assisted PA6 / CF automated fiber placement substrate, and the resin transition layer is a PA6 resin transition layer.