Paraffin-graded alumina carbon nanotube wound slices thermal interface material and preparation method
By introducing graded alumina particles and carbon nanotube films into paraffin-based thermal interface materials, a continuous thermal conduction path is formed, solving the problems of low thermal conductivity and complex preparation. This enables efficient thick-to-thickness heat transfer and transient thermal management, making it suitable for electronic devices operating at different temperatures.
Patent Information
- Application Number
- CN202611457049.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
Smart Images

Figure CN123104168A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermal interface materials and thermal management technology for electronic devices, specifically to a paraffin-graded alumina carbon nanotube wound and sliced thermal interface material and its preparation method. Background Technology
[0002] With the rapid development of advanced packaging, 3D heterogeneous integration, high-performance computing chips, and wide-bandgap power devices, electronic systems are accelerating their evolution towards higher integration, miniaturization, higher power density, and higher reliability. Thermal management has become a key bottleneck restricting device performance and system stability. Taking advanced logic devices as an example, the transistor density at the 7 nm node has reached approximately 10⁸ transistors / mm². 2 Commercial high-performance chips have a heat flux density exceeding 100 W·cm⁻¹. -2 In high-power and three-dimensional integrated scenarios, the heat flux density of local hotspots can reach hundreds or even exceed 1000 W·cm⁻¹. -2 Vertical stacking of devices, limited interlayer thermal diffusion, and thermal expansion mismatch among multiple materials further exacerbate temperature non-uniformity, thermal stress concentration, and thermal crosstalk problems. Studies have shown that temperature-related factors account for approximately 40%-55% of electronic device failures, and interfacial thermal resistance has become a core factor limiting the heat dissipation efficiency and reliability of advanced electronic systems. Therefore, research on high-efficiency thermal interface materials and interfacial thermal transport regulation in complex packaging environments has significant scientific importance and urgent engineering value.
[0003] Current heat dissipation technologies for electronic devices, such as air cooling, water cooling, and heat pipes, face a common bottleneck: the actual effective contact area between electronic components and heat dissipation elements is less than 2% of the apparent contact area, with the remaining 98% of the interface occupied by microscopic gaps filled with air. This is because air has extremely low thermal conductivity at room temperature, only 0.026 W·m. -1 ·K -1 Interfacial voids significantly increase contact thermal resistance, severely limiting heat transfer efficiency and leading to uncontrolled temperature rise in the system. To address this challenge, thermal interface materials (TIMs) have become a key area for breakthrough. Replacing the interfacial air layer with high thermal conductivity TIMs can significantly increase the effective contact area, reduce contact thermal resistance, thereby improving device heat dissipation uniformity and suppressing hotspot formation.
[0004] Traditional thermal interface materials typically improve thermal conductivity by adding highly thermally conductive particles to polymers or other matrices. However, relying solely on steady-state thermal conduction is insufficient to simultaneously meet the requirements of high-power electronic devices for interfacial gap-filling capability and short-term thermal shock buffering capability.
[0005] Paraffin wax possesses a large latent heat of phase change, good chemical stability, a suitable phase change temperature range, and low cost, making it suitable as a matrix for phase change thermal interface materials. Once the device operating temperature reaches the softening or phase change temperature range of paraffin wax, it can improve the material's wetting and gap-filling capabilities on the contact surface, while simultaneously absorbing some heat during the phase change process, thus providing a certain degree of transient thermal buffering.
[0006] However, paraffin itself has low thermal conductivity, making it difficult to meet the rapid heat transfer requirements of high heat flux density electronic devices. Therefore, it is necessary to improve its heat transfer capacity by introducing high thermal conductivity fillers and constructing continuous thermal conduction paths.
[0007] Alumina possesses good thermal stability, electrical insulation, and thermal conductivity, making it a commonly used ceramic filler in thermal interface materials. However, when alumina particles of a single size are randomly dispersed in paraffin, significant matrix gaps may still exist between the particles, leading to insufficient continuity of the thermally conductive network. By using alumina particles of different sizes for particle size gradation, smaller-sized alumina particles can fill some of the gaps between larger-sized particles, which helps to improve the degree of particle packing and the probability of effective thermal contact between particles.
[0008] Research on thermally conductive fillers in composite thermal interface materials has evolved from early random filling of single particles to the collaborative construction of multi-scale, multi-dimensional, and multi-component thermally conductive networks. Studies have shown that simply optimizing the type and size of fillers is insufficient to meet the requirements of efficient heat transport; the spatial continuity and structural integrity of the thermal conductive pathways are equally crucial. Therefore, three-dimensional thermally conductive fillers and their network construction have become a current research hotspot. Ran et al. constructed a vertically oriented graphene microstrip thermally conductive pad by vertically arranging graphene microstrips and encapsulating them with silicone rubber. With a graphene content of 60 wt.%, the out-of-plane thermal conductivity of the sample reached 565.92 W·m. -1 ·K -1 This demonstrates that vertically oriented flexible thermal conductive networks are an effective strategy for achieving both high thermal conductivity and high flexibility in thermal interface materials. Yoshitomi et al. constructed a nanodiamond oriented framework using an ice template, and after vacuum-assisted impregnation with epoxy resin, achieved a thickness-direction thermal conductivity of 1.27 W·m for the composite material when the nanodiamond volume fraction exceeded 3 vol.%. -1 ·K -1 The thermal conductivity is three times that in the in-plane direction. Zeng et al. constructed a 3D-BNNS framework using an ice template and impregnated it with epoxy resin. The resulting composite system exhibited a clearly ordered structure; with a low filler content of 1.67 vol.%, the thermal conductivity of the randomly dispersed sample was only 0.17 W·m. -1 ·K -1The oriented framework samples already exhibited significant orientation dependence. Liu et al. further prepared PAAS / GO hybrid aerogels using bidirectional freezing, and after vacuum impregnation with epoxy resin, achieved a Z-axis thermal conductivity of 20.0 W·m with a graphene content of only 2.3 vol.%. -1 ·K -1 The thermal conductivity of the composite film is approximately 100 times that of pure epoxy resin, demonstrating the significant advantage of bidirectional freezing in enhancing thermal conductivity in the thickness direction. Yuan et al. achieved magnetic responsiveness in the filler by electrostatically compositing negatively charged BNNS with positively charged FeCo nanocubes; when the BNNS content was 50 wt.% and the FeCo content was 30 wt.%, the thermal conductivity of the composite film reached 2.25 W·m. -1 ·K -1 The thermal conductivity was improved by 7 times compared to the unoriented sample and nearly 20 times compared to the pure film, representing an increase of 592%. Ma et al. loaded Fe3O4 onto the surface of carbon fibers and achieved directional construction of carbon fibers under the action of an external magnetic field. The resulting OCF / PDMS composite material achieved a thermal conductivity of 1.51 W·m with 20 wt.% filler. -1 ·K -1 The thermal conductivity was 5.59 times that of pure PDMS and 1.6 times that of unoriented CF / PDMS. Zhang et al. further proposed a strategy of "pre-orienting in air with a magnetic field and then filling with polymer," which increased the thermal conductivity of the composite material to 1.95 W·m under a load of 62.2 wt.%. -1 ·K -1 The thermal conductivity of the composite material is 12 times that of the pure matrix, thus effectively weakening the limitation of the high-viscosity matrix on the orientation effect. Kim et al. endowed the BN surface with dielectric response after depositing TiO2, which increased the thermal conductivity of the composite material in the thickness direction from 0.78 to 1.54 W·m. -1 ·K -1 Meanwhile, the in-plane thermal conductivity decreased from 1.17 to 0.84 W·m. -1 ·K -1 This indicates that external field induction can significantly enhance heat conduction in a specific direction, but it can also exacerbate the directional selectivity of heat transfer.
[0009] Currently, directional heat transfer networks are typically constructed using methods such as template orientation, cryogenic casting, magnetic or electric field induction, and three-dimensional skeleton infiltration. While these methods can improve heat transfer performance in specific directions, some suffer from complex processes, high equipment requirements, difficulties in parameter control, or are not conducive to continuous production.
[0010] Therefore, it is necessary to provide a thermal interface material with a well-defined structure, a relatively simple preparation process, and continuous processing potential. By fully utilizing the high in-plane thermal conductivity of carbon nanotube films through structural design, and at the same time leveraging the synergistic effect of graded alumina particles and paraffin phase change matrix, the thickness-to-thickness heat transfer performance and transient thermal management capability of the thermal interface material can be improved. Summary of the Invention
[0011] The purpose of this invention is to overcome the problems of low thermal conductivity, difficulty in forming continuous thermal conduction pathways in the thickness direction, and complex preparation process of some directional thermal conduction networks in existing paraffin-based thermal interface materials, and to provide a paraffin-graded alumina carbon nanotube film rolled-up slice thermal interface material and its preparation method.
[0012] This invention uses paraffin as a phase change matrix, graded alumina particles of different sizes as particulate thermal conductivity enhancement components, and continuous carbon nanotube films as high thermal conductivity enhancement units. The spatial orientation of the carbon nanotube film in the final thermal interface material is changed through the process of "composite sheet forming - film lamination - winding - hot pressing and shaping - vertical slicing".
[0013] After slicing, the carbon nanotube film extends along the thickness direction of the material in a manner approximately perpendicular to the main surface of the thermal interface material. This allows the original in-plane high thermal conductivity direction of the carbon nanotube film to participate in the heat transfer along the thickness direction of the material, thereby enhancing the thickness-based thermal conductivity of the thermal interface material.
[0014] To achieve the above objectives, the present invention provides a paraffin-graded alumina / carbon nanotube film rolled-up sheet thermal interface material.
[0015] The thermal interface material includes a paraffin-based composite layer and multiple carbon nanotube film segments.
[0016] The paraffin-based composite region includes paraffin wax and graded alumina particles dispersed in the paraffin wax. The graded alumina particles include at least two different particle sizes of alumina particles. The phase transition temperature of the paraffin wax meets the operating temperature and thermal management requirements of electronic devices. The graded alumina particles include at least two different particle sizes of alumina particles.
[0017] Furthermore, the graded alumina is composed of alumina with particle sizes of 3-8 μm and 13-18 μm at a mass ratio of 1:2-3.
[0018] Furthermore, its mass composition is 9%-19% carbon nanotube film, 38%-60% alumina, and the remainder is paraffin. Furthermore, the thickness of the carbon nanotube film is 5-15 μm.
[0019] The paraffin wax used in this invention is not limited to a specific type; it can be selected based on the actual operating temperature, interface temperature, and transient thermal management requirements of the electronic device, and has a corresponding melting point or phase transition temperature range. Paraffin wax enhances the wetting and gap-filling effect of the material at the contact interface and absorbs some heat using the latent heat of phase change, thereby providing a certain transient thermal buffering capacity. Therefore, by selecting paraffin waxes with different phase transition temperature ranges, the adaptability of the thermal interface material to electronic devices operating at different temperature zones can be improved.
[0020] This invention also provides a method for preparing a paraffin-graded alumina carbon nanotube wound and sliced thermal interface material, comprising, Graded alumina suspension was mixed with molten paraffin to obtain a composite slurry; A paraffin-graded alumina composite layer was obtained by using a composite slurry to prepare a film. A composite tape is obtained by laminating carbon nanotube films of the same size with a paraffin-based composite layer and then laminating them together. The composite strip is wound, hot-pressed and shaped, and sliced along a direction perpendicular to the winding axis, so that the paraffin-based composite layer and carbon nanotube film segments are alternately distributed, and the film surface of the carbon nanotube film extends along the thickness direction of the resulting thermal interface material.
[0021] Furthermore, paraffin wax with a corresponding melting point or phase transition temperature range is selected according to the target working temperature of the thermal interface material, and melt composite is carried out at a temperature 10-20 °C above the melting point of the paraffin wax.
[0022] Furthermore, the film is formed by blade coating, the coating platform temperature is 10-20 °C above the melting point of paraffin, and the blade gap is 100-300 μm.
[0023] Furthermore, after lamination, the thickness of the composite sheet is 20-30 μm.
[0024] Furthermore, the hot pressing is carried out at a temperature 10-20°C above the melting point of paraffin and a pressure of 1-10 MPa.
[0025] The present invention also provides the application of the above-mentioned paraffin-graded alumina carbon nanotube wound slice thermal interface material in heat dissipation of electronic devices, wherein the thermal interface material is disposed between the heat-generating device and the heat dissipation element.
[0026] Compared with the prior art, the beneficial effects of the present invention include: 1. Enhance the thickness-to-thickness heat transfer of thermal interface materials This invention uses lamination, winding, and slicing perpendicular to the winding axis to distribute carbon nanotube films radially in the final material, which is beneficial for constructing a thickness-oriented heat transfer path by utilizing the thermal conductivity of the film along its planar direction.
[0027] 2. Graded alumina particles improve the thermal connection between particles. This invention uses alumina particles of different sizes for gradation. Small-sized alumina particles can fill part of the gaps between large-sized particles, increasing the packing degree of the filler and the probability of effective thermal contact between particles, which helps to reduce the heat transfer resistance inside the paraffin-based composite layer.
[0028] 3. Possesses both interfacial wetting and transient phase change endothermic capabilities. Once paraffin reaches its softening or phase change temperature range, it can improve the wetting and gap-filling ability of thermal interface materials on the contact surfaces of devices and heat sinks. At the same time, it absorbs latent heat through phase change, thereby enhancing heat conduction while providing a certain transient thermal buffer function.
[0029] 4. Adaptable to different working temperature zones The paraffin used in this invention is not limited to a single grade. Paraffins with a suitable phase change temperature range can be selected according to the normal operating temperature and thermal management requirements of different devices, thus having good adaptability to application scenarios.
[0030] 5. The preparation process is simple, requires low equipment, and has good potential for continuous production and industrialization. The steps employed in this invention, such as filler dispersion, melt composite, blade coating, lamination, winding, hot pressing, and slicing, are all conventional material processing techniques. They do not rely on special technologies such as freezing templates, strong magnetic field induction, complex aerogel preconstruction, or high-cost in-situ growth. The process flow is relatively simple, has good repeatability, and is highly compatible with existing industrial processing methods such as coating, rolling, winding, and die-cutting. Therefore, it is more conducive to subsequent scale-up preparation and industrialization.
[0031] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description
[0032] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.
[0033] Figure 1 The preparation process of the paraffin-graded alumina carbon nanotube wound slice thermal interface material of the present invention is shown. Figure 2 The changes in thermal conductivity of the thermal interface material under different combinations of alumina particle sizes and different alumina mass fractions are shown. Figure 3 The variation of thermal conductivity of the thermal interface material under different carbon nanotube film mass fractions is shown. Detailed Implementation
[0034] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the invention, are intended to cover non-exclusive inclusion.
[0036] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0037] Paraffin wax is an ideal choice for phase change thermal interface materials due to its wide phase change temperature range, large latent heat, non-toxicity, stability, good thermal / chemical stability, and low price. However, its low thermal conductivity is a key factor limiting its performance. To improve the thermal conductivity of phase change thermal interface materials, high thermal conductivity fillers such as metals, ceramics, and carbon materials are generally added. Among them, carbon materials such as carbon fibers, graphene, and carbon nanotubes not only utilize phonon vibrations for heat conduction but also have external free electrons contributing to heat conduction, resulting in high thermal conductivity and enabling rapid heat transfer. In addition, carbon materials are lightweight and have good electromagnetic shielding effects, thus attracting extensive research. Multi-walled carbon nanotubes, as thermally conductive fillers, have advantages such as high intrinsic thermal conductivity, large aspect ratio, and ease of forming continuous thermally conductive networks, significantly improving the heat transfer capacity of composite materials even with low filler content. Simultaneously, their excellent mechanical properties, thermal stability, and synergistic effects with other fillers make them promising candidates for applications in thermal interface materials, phase change thermal storage materials, and electronic packaging heat dissipation.
[0038] Therefore, this invention is proposed.
[0039] This invention provides a paraffin-graded alumina carbon nanotube wound and sliced thermal interface material, comprising multiple paraffin-based composite layers and carbon nanotube thin film layers; The paraffin-based composite layer includes paraffin wax and graded alumina particles dispersed in the paraffin wax. The graded alumina particles include at least two different particle sizes of alumina particles. The phase transition temperature of the paraffin wax meets the operating temperature and thermal management requirements of electronic devices. The carbon nanotube film layer and the paraffin-based composite layer are alternately distributed; The surface of the carbon nanotube film extends along the thickness direction of the thermal interface material, so that the thermal conduction direction of the carbon nanotube film is along the thickness direction of the thermal interface material.
[0040] In some preferred embodiments, the graded alumina comprises small-diameter alumina particles and large-diameter alumina particles, wherein the small-diameter alumina particles have a diameter of 3-8 μm, and the large-diameter alumina particles have a diameter of 13-18 μm, with a mass ratio of small-diameter to large-diameter alumina particles of 1:2-3. More preferably, the graded alumina particles comprise large-diameter alumina particles with a diameter of 15 μm and small-diameter alumina particles with a diameter of 5 μm, with a mass ratio of large-diameter to small-diameter particles of 2:1.
[0041] Alumina particles of different sizes are graded to adjust their packing and contact state. Smaller particles can fill some of the gaps between larger particles, which helps improve heat transfer between particles. The carbon nanotube film segment extends along the final material thickness direction and works together with the alumina particles to enhance thermal conductivity.
[0042] This invention uses paraffin wax as the phase change matrix. When the operating temperature reaches the softening or phase change temperature range of the selected paraffin wax, the paraffin wax helps to wet the contact surface, fill the interfacial gaps, and improve the interfacial thermal contact; paraffin wax absorbs heat during the phase change process and can provide a certain transient thermal buffering effect.
[0043] In some preferred embodiments, the composition is 9%-19% carbon nanotube film, 38%-60% alumina, and the remainder is paraffin.
[0044] It should be noted that the thicknesses of the paraffin-based composite layer, the carbon nanotube film, and the final slice are defined separately. The carbon nanotube film thickness is measured along a direction perpendicular to the film surface, while the final slice thickness is measured along the direction between its two opposing heat-transfer surfaces.
[0045] In some preferred embodiments, the thickness of the carbon nanotube film is 5-15 μm.
[0046] On the other hand, the present invention also provides a method for preparing a paraffin-graded alumina carbon nanotube wound slice thermal interface material, comprising, Graded alumina suspension was mixed with molten paraffin to obtain a composite slurry; A paraffin-based composite layer was obtained by using a composite slurry to prepare a film. A continuous carbon nanotube film is laminated with the paraffin-based composite layer to obtain a composite tape. The composite strip is wound to form a composite wound body; The composite wound body is hot-pressed for shaping; The hot-pressed composite winding is sliced along a plane perpendicular to the winding axis, so that the paraffin-based composite layer and carbon nanotube film segments are alternately distributed, and the film surface of the carbon nanotube film extends along the thickness direction of the obtained thermal interface material.
[0047] Before winding, a single continuous carbon nanotube (CNT) film is bonded to a composite sheet and then wound together. The diameter of the winding mandrel should be determined based on the rollability of the sheet and the target size of the wound body. The slicing plane is perpendicular to the winding axis, so that the paraffin-based composite layer and the carbon nanotube film are alternately stacked in the radial direction of the slice. The initial slice is cylindrical, and subsequent slices can be made again as needed for the heat dissipation device structure. For a certain slice structure, it can be a local structure of 100μm×100μm×100μm. The number of CNT films (i.e., the number of CNT film layers) and their mass ratio are related to the winding spacing, CNT film thickness, and selection location. The mass fraction of the local CNT film is the sum of the geometric masses of each film segment divided by the total mass of the local structure, and cannot be directly determined by the mandrel diameter alone. The local structure parameters should correspond to the actual geometry after winding, hot pressing, and slicing. The specific dimensional relationships are explained in the corresponding embodiments.
[0048] It should be noted that there is a certain antagonism between the mass ratio of CNT film and the mass ratio of alumina in the same local structure, because an excessive mass ratio of alumina will compress the layer distribution of CNT film in the same size.
[0049] This invention does not require strict limitations on the length and width of the paraffin-graded alumina composite layer and the carbon nanotube film, as long as the subsequent winding, hot pressing, and slicing steps can be carried out effectively.
[0050] In some preferred embodiments, the molten paraffin is obtained by heating paraffin to a melting temperature of 10-20 °C.
[0051] In some preferred embodiments, the film is formed by blade coating, the coating platform temperature is 10-20 °C above the melting point of paraffin, and the blade gap is 100-300 μm; wherein, the blade gap is not directly equivalent to the actual sheet thickness after lamination.
[0052] In some preferred embodiments, the thickness of the composite strip after lamination is 20-30 μm. In some preferred embodiments, the hot pressing is carried out at a temperature 10-20°C above the melting point of paraffin and a pressure of 1-10 MPa.
[0053] The present invention will be further described in detail below through specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0054] The carbon nanotube films of different thicknesses used in the following examples and comparative examples are multi-walled carbon nanotube films, all of which were purchased from Chengdu Jiacai Technology Co., Ltd.
[0055] Example 1 like Figure 1 As shown, a method for preparing a paraffin-graded alumina carbon nanotube wound slice thermal interface material includes the following steps: S1, Raw material ratio Weigh out 4.63 g of No. 58 fully refined paraffin wax, 7.90 g of 15 μm alumina particles, and 3.95 g of 5 μm alumina particles.
[0056] S2, dispersion of alumina particles 15 μm and 5 μm alumina particles were added to 94.8 mL of anhydrous ethanol and pre-dispersed by mechanical stirring at 800 rpm for 30 min. Subsequently, ultrasonic dispersion was performed for 20 min to obtain a uniform graded alumina suspension.
[0057] S3, Paraffin Melting Composite Fully refined paraffin wax (No. 58, melting point approximately 58 ℃) was added to a beaker and heated to 75 ℃ until completely melted. At 75 ℃, a graded alumina suspension was added to the molten paraffin wax while maintaining mechanical stirring at 800 rpm. After addition, stirring continued for 60 min. The mixed slurry was then placed in a vacuum drying oven for solvent removal and degassing. The vacuum level was set to -0.08 MPa, the temperature to 75 ℃, and the processing time to 60 min, yielding a composite slurry.
[0058] S4, Composite Layer Forming The glass coating platform temperature was set to 65 ℃. The composite slurry obtained in S3 was poured onto the release film surface on the glass coating platform and coated using an adjustable coating tool with a doctor blade gap set to 200 μm. After coating, the coated composite film was cooled at 25 ℃ for 30 min to obtain a paraffin-based composite layer.
[0059] S5, carbon nanotube film laminate composite The paraffin-based composite layer and a 5 μm thick carbon nanotube film were preheated on a 65 ℃ heating table for 5 min. After preheating, a continuous carbon nanotube film was laid flat on the surface of a paraffin-graded alumina composite sheet to bond the two together. The two materials were then laminated using a flat plate hot pressing method at a lamination temperature of 65 ℃, a lamination pressure of 2 MPa, and a lamination time of 5 min to obtain the sheet.
[0060] S6, winding The sheet material is wound using a 3 mm diameter stainless steel optical shaft as a winding mandrel to obtain a composite wound body.
[0061] S7, Hot pressing and shaping The composite wound body was placed in a hot press for hot pressing and shaping. The hot pressing temperature was set to 75 ℃, the hot pressing pressure was set to 5 MPa, and the hot pressing time was set to 10 min. After hot pressing, the shaped composite wound body was obtained.
[0062] S8, Vertical Slicing The shaped composite winding was sliced on a plane perpendicular to the winding axis to obtain multiple finished sheets with a thickness of 200 μm. These finished sheets were then sliced again to obtain a local structure with dimensions of 100 μm × 100 μm × 100 μm, in which four layers of 5 μm thick CNT films were stacked along the radial direction of the local structure. In the local structure, the mass fractions of CNT film, alumina, and paraffin were 18.26%, 58.78%, and 22.96%, respectively; the mass fractions of 15 μm alumina particles and 5 μm alumina particles were 39.51% and 19.27%, respectively. Unless otherwise specified in the following examples and comparative examples, the mass ratio of large-size to small-size alumina particles was 2:1.
[0063] Please refer to the preparation method of Example 1 and the amounts of alumina, paraffin, and anhydrous ethanol in Table 1 below to prepare Examples 2-6. In Table 1, the mass fractions represent the mass fractions of "carbon nanotube film / alumina / paraffin". In Examples 1-4, the selected representative local structures were all formed with four layers of carbon nanotube film with a thickness of 5 μm; Examples 5 and 6 were formed with two and three layers of carbon nanotube film with a thickness of 5 μm, respectively. Unless otherwise specified, the mass ratio of 15 μm alumina particles to 5 μm alumina particles was 2:1. The amount of anhydrous ethanol used was 8 mL / g of the liquid-to-solid ratio of the alumina particles.
[0064] Table 1
[0065] Example 2 The difference from Example 1 lies in adjusting the amounts of paraffin wax and graded alumina particles. 5.06 g of fully refined No. 58 paraffin wax, 6.65 g of 15 μm alumina particles, and 3.32 g of 5 μm alumina particles were weighed, with a mass ratio of approximately 2:1 between the 15 μm and 5 μm alumina particles. The two types of alumina particles were dispersed in 79.8 mL of anhydrous ethanol.
[0066] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina and paraffin are 19.67%, 53.28% and 27.05%, respectively; four carbon nanotube film segments with a thickness of 5 μm are formed in the selected representative local structure, and the other preparation conditions are the same as in Example 1.
[0067] Example 3 Compared to Example 1, the difference lies in adjusting the amount of paraffin wax and graded alumina particles added. 5.52 g of No. 58 fully refined paraffin wax, 5.32 g of 15 μm alumina particles, and 2.66 g of 5 μm alumina particles were weighed, with a mass ratio of 2:1 between the 15 μm and 5 μm alumina particles. The two types of alumina particles were dispersed in 63.8 mL of anhydrous ethanol.
[0068] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina and paraffin are 21.43%, 46.43% and 32.14%, respectively; four carbon nanotube film segments with a thickness of 5 μm are formed in the selected representative local structure, and the other preparation conditions are the same as in Example 1.
[0069] Example 4 Compared to Example 1, the difference lies in adjusting the amount of paraffin wax and graded alumina particles added. 5.98 g of No. 58 fully refined paraffin wax, 3.99 g of 15 μm alumina particles, and 1.99 g of 5 μm alumina particles were weighed, with a mass ratio of approximately 2:1 between the 15 μm and 5 μm alumina particles. The two types of alumina particles were dispersed in 47.8 mL of anhydrous ethanol.
[0070] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina and paraffin are 23.53%, 38.24% and 38.24%, respectively; four carbon nanotube film segments with a thickness of 5 μm are formed in the selected representative local structure, and the other preparation conditions are the same as in Example 1.
[0071] Example 5 Compared with Example 1, the amount of 15 μm alumina particles and 5 μm alumina particles added remained unchanged, at 7.90 g and 3.95 g respectively, with a total alumina addition of 11.85 g; the difference was that the amount of paraffin was adjusted to 5.48 g, and the carbon nanotube film in the selected representative local structure was changed from 4 layers to 2 layers, with each layer having a thickness of 5 μm.
[0072] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 9.53%, 61.87%, and 28.60%, respectively. The alumina particles were still dispersed in 94.8 mL of anhydrous ethanol, and the remaining preparation conditions were the same as in Example 1.
[0073] Example 6 Compared with Example 1, the amount of 15 μm alumina particles and 5 μm alumina particles added remained unchanged, at 7.90 g and 3.95 g respectively, with a total alumina addition of 11.85 g; the difference was that the amount of paraffin was adjusted to 5.26 g, and the carbon nanotube film in the selected representative local structure was changed from 4 layers to 3 layers, with each layer having a thickness of 5 μm.
[0074] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 14.15%, 59.47%, and 26.38%, respectively. The alumina particles were still dispersed in 94.8 mL of anhydrous ethanol, and the remaining preparation conditions were the same as in Example 1.
[0075] Examples 5, 6, and 1 correspond to 2-layer, 3-layer, and 4-layer carbon nanotube film structures with a thickness of 5 μm, respectively, and are used to compare the effects of the number of carbon nanotube film layers and their mass fraction on the heat transfer performance of the thermal interface material in the thickness direction.
[0076] Table 2
[0077] Comparative Example 1 Compared to Example 4, the difference lies in replacing the 15 μm alumina particles with 10 μm alumina particles, and using alumina particles of both 10 μm and 5 μm size for gradation. 5.98 g of fully refined paraffin wax (No. 58), 3.99 g of 10 μm alumina particles, and 1.99 g of 5 μm alumina particles were weighed, with a mass ratio of approximately 2:1 between the two particle sizes, and 47.8 mL of anhydrous ethanol was added for dispersion.
[0078] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 23.53%, 38.24%, and 38.24%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 4.
[0079] Comparative Example 2 Compared to Example 3, the difference lies in replacing the 15 μm alumina particles with 10 μm alumina particles, and using alumina particles of both 10 μm and 5 μm size for gradation. 5.52 g of No. 58 fully refined paraffin wax, 5.32 g of 10 μm alumina particles, and 2.66 g of 5 μm alumina particles were weighed, with a mass ratio of the two particle sizes of alumina particles of 2:1, and 63.8 mL of anhydrous ethanol was added for dispersion.
[0080] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 21.43%, 46.43%, and 32.14%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 3.
[0081] Comparative Example 3 Compared to Example 2, the difference lies in replacing the 15 μm alumina particles with 10 μm alumina particles, and using alumina particles of both 10 μm and 5 μm for gradation. 5.06 g of No. 58 fully refined paraffin wax, 6.65 g of 10 μm alumina particles, and 3.32 g of 5 μm alumina particles were weighed, with a mass ratio of approximately 2:1 between the two particle sizes, and 79.8 mL of anhydrous ethanol was added for dispersion.
[0082] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 19.67%, 53.28%, and 27.05%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 2.
[0083] Comparative Example 4 Compared to Example 1, the difference lies in replacing the 15 μm alumina particles with 10 μm alumina particles, and using a gradation of alumina particles with two sizes, 10 μm and 5 μm. 4.63 g of No. 58 fully refined paraffin wax, 7.90 g of 10 μm alumina particles, and 3.95 g of 5 μm alumina particles were weighed, with a mass ratio of the two particle sizes of alumina particles of 2:1, and 94.8 mL of anhydrous ethanol was added for dispersion.
[0084] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 18.26%, 58.78%, and 22.96%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 1.
[0085] Comparative Example 5 Compared to Example 4, the difference is that 10 μm single-particle-size alumina particles were used, and 5 μm alumina particles were not added. 5.98 g of No. 58 fully refined paraffin wax and 5.98 g of 10 μm alumina particles were weighed, and the alumina particles were added to 47.8 mL of anhydrous ethanol for dispersion.
[0086] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 23.53%, 38.24%, and 38.24%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 4.
[0087] Comparative Example 6 Compared to Example 3, the difference is that 10 μm single-particle-size alumina particles were used, and 5 μm alumina particles were not added. 5.52 g of No. 58 fully refined paraffin wax and 7.98 g of 10 μm alumina particles were weighed, and the alumina particles were added to 63.8 mL of anhydrous ethanol for dispersion.
[0088] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 21.43%, 46.43%, and 32.14%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 3.
[0089] Comparative Example 7 Compared to Example 2, the difference is that 10 μm single-particle-size alumina particles were used, and 5 μm alumina particles were not added. 5.06 g of No. 58 fully refined paraffin wax and 9.97 g of 10 μm alumina particles were weighed, and the alumina particles were dispersed in 79.8 mL of anhydrous ethanol.
[0090] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 19.67%, 53.28%, and 27.05%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 2.
[0091] Comparative Example 8 Compared to Example 1, the difference is that 10 μm single-particle-size alumina particles were used, and 5 μm alumina particles were not added. 4.63 g of No. 58 fully refined paraffin wax and 11.85 g of 10 μm alumina particles were weighed, and the alumina particles were added to 94.8 mL of anhydrous ethanol for dispersion.
[0092] In the obtained thermal interface material, the mass fractions of carbon nanotube film, alumina, and paraffin were 18.26%, 58.78%, and 22.96%, respectively. Four carbon nanotube film segments with a thickness of 5 μm were formed in the selected representative local structure, and the remaining preparation conditions were the same as in Example 1.
[0093] Figure 2 The thermal conductivity of Examples 1-4 and Comparative Examples 1-8 was compared under different alumina particle size combinations and different alumina mass fractions. Examples 1-4 used 15 μm and 5 μm alumina particle sizes, Comparative Examples 1-4 used 10 μm and 5 μm alumina particle sizes, and Comparative Examples 5-8 used a single 10 μm alumina particle size. The mass fractions of carbon nanotube film, alumina, and paraffin were consistent in each corresponding group, and four 5 μm thick carbon nanotube film segments were formed in the selected representative local structures. Therefore, these groups could be used to compare the effects of alumina particle size combinations and alumina content on the thermal transfer performance of the materials.
[0094] Depend on Figure 2 It can be seen that under lower alumina mass fraction conditions, the thermal conductivity of the three alumina particle systems is relatively similar. As the alumina mass fraction increases, the thermal conductivity of the two dual-particle-size gradation systems gradually increases, while the thermal conductivity of the 10 μm single-particle-size alumina system changes relatively little. Under higher alumina mass fraction conditions, the 15 μm and 5 μm gradation systems exhibit the highest thermal conductivity, followed by the 10 μm and 5 μm gradation systems, while the 10 μm single-particle-size system has relatively lower thermal conductivity.
[0095] The above results indicate that, compared to alumina particles of a single size, grading alumina particles of different sizes is beneficial for improving particle packing and contact in paraffin. Small-sized alumina particles can fill some of the gaps between large-sized particles, increasing the probability of effective thermal contact between particles; simultaneously, larger-sized particles help shorten the paraffin distance that needs to be traversed during continuous heat transfer. Therefore, the particle size distribution of alumina particles can synergistically work with the carbon nanotube film extending along the material's thickness direction, which is beneficial for enhancing the material's heat transfer. Among them, the gradation of 15 μm and 5 μm alumina particles exhibits better thickness-based thermal conductivity enhancement within the composition range studied in this embodiment.
[0096] Figure 3 The thermal conductivity of Examples 5, 6, and 1 was compared under different numbers and mass fractions of carbon nanotube film layers. Examples 5, 6, and 1 all used 15 μm and 5 μm alumina particle gradations, maintaining the same actual amount of alumina particles added. In the selected representative local structures, 2, 3, and 4 carbon nanotube film segments with a thickness of 5 μm were formed, respectively, corresponding to carbon nanotube film mass fractions of 9.53%, 14.15%, and 18.26%, respectively.
[0097] like Figure 3 As shown, when the mass fraction of the carbon nanotube film is 9.53%, the thermal conductivity of the material is 10.63 W·m. -1 ·K -1 When the mass fraction of carbon nanotube film increased to 14.15%, the thermal conductivity increased to 15.63 W·m. -1 ·K -1 When the mass fraction of the carbon nanotube film was further increased to 18.26%, the thermal conductivity reached 20.64 W·m. -1 ·K -1 Therefore, within the scope studied in this embodiment, the thermal conductivity of the material shows a significant increasing trend with the increase of the number and mass fraction of carbon nanotube film layers.
[0098] The results indicate that extending the carbon nanotube film along the final material thickness direction by winding and vertical slicing increases the number of carbon nanotube film layers, thereby increasing the proportion of the high thermal conductivity film in the thickness-direction heat transfer path. This allows the original in-plane high thermal conductivity direction of the carbon nanotube film to participate more fully in the heat transfer along the material thickness direction, thus improving the material's thickness-directed thermal conductivity. This also demonstrates that the "lamination-winding-vertical slicing" structural design employed in this invention can effectively utilize the high thermal conductivity of carbon nanotube films to achieve control over the thermal transport properties of the thermal interface material.
[0099] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A paraffin-graded alumina carbon nanotube rolled sheet thermal interface material, characterized by, It includes multiple paraffin-based composite layers and carbon nanotube thin film layers; The paraffin-based composite layer includes paraffin wax and graded alumina particles dispersed in the paraffin wax. The graded alumina particles include at least two different particle sizes of alumina particles. The phase transition temperature of the paraffin wax meets the operating temperature and thermal management requirements of electronic devices. The carbon nanotube film layer and the paraffin-based composite layer are alternately distributed; The surface of the carbon nanotube film extends along the thickness direction of the thermal interface material, so that the thermal conduction direction of the carbon nanotube film is along the thickness direction of the thermal interface material.
2. The paraffin-graded alumina carbon nanotube roll good thermal interface material of claim 1, wherein, The graded alumina particles include small-diameter alumina particles and large-diameter alumina particles. The small-diameter alumina particles have a particle size of 3-8 μm, and the large-diameter alumina particles have a particle size of 13-18 μm. The mass ratio of small-diameter alumina particles to large-diameter alumina particles is 1:2-3.
3. The paraffin-graded alumina carbon nanotube roll good thermal interface material of claim 1, wherein, Its mass composition is 9%-19% carbon nanotube film, 38%-60% alumina, and the remainder is paraffin.
4. The paraffin-graded alumina carbon nanotube roll good thermal interface material of any one of claims 1-3, wherein, The thickness of the carbon nanotube film is 5-15 μm.
5. A method of making a paraffin-graded alumina carbon nanotube roll-in- sheet thermal interface material, characterized by, include, Graded alumina suspension was mixed with molten paraffin to obtain a composite slurry; A paraffin-based composite layer was obtained by using a composite slurry to prepare a film. A continuous carbon nanotube film is laminated with the paraffin-based composite layer to obtain a composite tape. The composite strip is wound to form a composite wound body; The composite wound body is hot-pressed for shaping; The hot-pressed composite winding is sliced along a plane perpendicular to the winding axis, so that the paraffin-based composite layer and carbon nanotube film segments are alternately distributed, and the film surface of the carbon nanotube film extends along the thickness direction of the obtained thermal interface material.
6. The method for preparing the paraffin-graded alumina carbon nanotube wound slice thermal interface material according to claim 5, characterized in that, Select paraffin wax with a corresponding melting point or phase transition temperature range according to the target working temperature of the thermal interface material, and perform melt composite at a temperature 10-20 ℃ higher than the melting point of the selected paraffin wax.
7. The method for preparing the paraffin-graded alumina carbon nanotube wound slice thermal interface material according to claim 5, characterized in that, The film is formed by blade coating, with the coating platform temperature being 10-20 ℃ above the melting point of paraffin and the blade gap being 100-300 μm.
8. The method for preparing the paraffin-graded alumina carbon nanotube wound slice thermal interface material according to claim 5, characterized in that, After lamination, the thickness of the composite strip is 20-30 μm.
9. The method for preparing the paraffin-graded alumina carbon nanotube wound slice thermal interface material according to claim 5, characterized in that, The hot pressing is carried out at a temperature 10-20°C above the melting point of paraffin and a pressure of 1-10 MPa.
10. The application of a paraffin-graded alumina carbon nanotube wound-cut thermal interface material as described in any one of claims 1-4 in heat dissipation of electronic devices, characterized in that, The thermal interface material is placed between the heat-generating device and the heat-dissipating element.