A glass-carbon hybrid composite preform, a foam sandwich composite material, and a method for preparing the same.
By using a method for preparing glass-carbon hybrid composite preforms, a three-dimensional network structure is formed through needle punching, and skin fiber hooks are incorporated into the foam core material. This method solves the problems of interlaminar shear and bending failure in composite materials, improves interlaminar strength and modulus, and is suitable for applications such as rail transit and wind turbine blades.
Patent Information
- Application Number
- CN202611336837.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing composite materials suffer from severe interlaminar shear and bending failures in fields such as rail transit and wind turbine blades. Existing solutions, such as layup processes, have low shear strength, stitching processes damage fibers, three-dimensional weaving equipment is expensive and difficult to promote on a large scale, foam sandwich structures are prone to debonding at the interface, and there is a lack of effective non-destructive reinforcement methods.
The method of preparing glass-carbon hybrid composite preforms involves symmetrically and alternately laying glass fiber layers and carbon fiber layers and then needle-punching them to form a three-dimensional network structure. The skin fiber hooks are then incorporated into the foam core material to form an integrated mechanical anchoring structure, which solves the problems of insufficient interlaminar shear strength and flexural modulus.
It significantly improves the interlaminar shear strength and flexural modulus of composite materials, solves the problem of debonding at the skin-core interface of foam sandwich structures, and does not add extra weight, making it suitable for lightweight structural components.
Smart Images

Figure CN123104172A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lightweight composite material technology, specifically relating to a glass-carbon hybrid composite preform, a foam sandwich composite material, and its preparation method. Background Technology
[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
[0003] In composite material structures such as rail transit and wind turbine blades, interlaminar shear and bending failures are the main damage modes. Existing solutions each have their drawbacks: Layup process: interlaminar bonding relies solely on resin, resulting in low shear strength (only about 32.5 MPa) and easy peeling; Stitching process: suture puncture severely damages in-plane fibers (tensile strength reduction of 21.6%), and microcracks easily form at the suture / resin interface; 3D weaving: excellent performance but expensive equipment and low efficiency, making large-scale promotion difficult; Foam sandwich: existing technologies rely on adhesive film bonding between the skin and foam core material, and the interface is prone to debonding under humid heat aging and impact loads, lacking effective non-destructive reinforcement methods.
[0004] There is very little existing research on glass-carbon hybrid needle punching. Some studies involve needle punching carbon / carbon composite materials, but the layup structures are different and do not involve glass-carbon hybrids; others involve hybrid composite material layups, but do not employ needle punching. In particular, no patents or documents disclose a technical solution of "using needle punching to bring the skin's own fiber hooks into the foam core material to form an integrated anchor". Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a glass-carbon hybrid composite preform, a foam sandwich composite material, and a method for preparing the same. The invention discloses a glass-carbon hybrid composite preform and its preparation method, and a foam sandwich composite material and its preparation method. The preparation method includes: symmetrically alternating glass fiber layers and carbon fiber layers are laid down and needle-punched to form a three-dimensional network structure. Further, the layup is placed on the surface of a foam core material, and the needle penetration extends into the foam interior. The needles are used to guide the fiber hooks of the skin into the foam core material, and after curing, an integrated mechanical anchoring structure with Z-direction fiber rivets is formed. This invention significantly improves the interlaminar shear strength and flexural modulus of the composite material, while fundamentally solving the industry problem of skin-core interface debonding in foam sandwich structures, without adding extra weight. It is suitable for lightweight structural components in fields such as rail transportation, wind power, and aviation.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows: In a first aspect, the present invention provides a glass-carbon hybrid composite material preform, which is a multi-layer composite symmetrical layup structure, consisting of, from bottom to top: carbon fiber mesh, glass fiber woven fabric, carbon fiber unidirectional fabric, carbon fiber mesh, glass fiber woven fabric, glass fiber woven fabric, carbon fiber mesh, carbon fiber unidirectional fabric, glass fiber woven fabric, and carbon fiber mesh. The ply structure contains anchoring fiber bundles of the same material and origin as the skin fibers, and the pinholes are filled with cured resin.
[0007] Secondly, the present invention provides a method for preparing the above-mentioned glass-carbon hybrid composite material preform, comprising the following steps: A multilayer structure is formed by alternating layers of carbon fiber mesh as a spacer layer with fiberglass woven fabric and carbon fiber unidirectional fabric in a specific symmetrical order. The product is obtained by needle-punching and then shaping and solidifying it.
[0008] Thirdly, the present invention provides a foam sandwich composite material, comprising a foam core material and the above-mentioned glass-carbon hybrid composite material preform or the glass-carbon hybrid composite material preform prepared by the above-mentioned preparation method; Among them, the foam core material serves as the middle interlayer in the glass-carbon hybrid composite preform; The foam core contains anchoring fiber bundles of the same material and origin as the skin fiber, and the pinholes are filled with cured resin.
[0009] Fourthly, the present invention provides a method for preparing the above-mentioned foam sandwich composite material, comprising the following steps: A layered structure with a foam core material is formed by alternating layers of carbon fiber mesh as a spacer layer with fiberglass woven fabric and carbon fiber unidirectional fabric in a specific symmetrical order. The foam is needled to penetrate into its interior, and then solidified.
[0010] One or more of the above technical solutions have the following advantages or beneficial effects: (1) This invention prepares a glass-carbon hybrid composite preform by combining a specific symmetrical layup of glass-carbon fiber (including alternating mesh / unidirectional fabric / grid fabric) with an optimized needle punching process, which solves the problem of insufficient interlaminar shear and flexural strength of traditional layup composites. This invention can save material costs caused by structural thickening and improve the component's resistance to interlaminar cracking.
[0011] (2) In the preparation of glass-carbon hybrid composite preforms, the needle-punching density is 15~25 needles / cm 2 The needle-punching depth of 8-12mm (solid) and needle-punching speed of 70-90 needles / min, among other process parameters, have a synergistic effect. This is because a density of 20 needles / cm² is used. 2The needle punching introduces Z-axis fibers between layers to construct a three-dimensional network, thus overcoming the defect of weak interlayer adhesion in the layup process, thereby achieving a significant effect of increasing shear strength by 31.2% and flexural modulus by 48.5%. Because a depth of 10mm and a speed of 80 needles / min are used in conjunction with 36# needles, excessive carbon fiber breakage is reduced, so the tensile strength loss is controlled within 26.6%, achieving an excellent balance of performance.
[0012] (3) Based on the glass-carbon hybrid composite preform, this invention further provides a composite material containing a foam interlayer. Fiber layups are placed on the surface of the foam core layer, and needle punching is used to hook the skin's own fibers into the foam core material to form an integrated anchor. In this solution, the needle punching depth extends into the interior of the foam core material, and the needle hooks hook the skin's own fibers into the foam core material. After curing, a Z-axis mechanical anchoring structure is formed that is continuous and integrated with the skin, solving the industry pain point of easy debonding at the skin-core interface of the foam interlayer structure, without adding any external medium or extra weight. Furthermore, the fatigue resistance and damage tolerance are significantly better than Z-pin or stitching solutions.
[0013] (4) The technical solution provided by this invention can be implemented independently without relying on complex external equipment or special materials. It can be modified and implemented on existing VARI (vacuum-assisted resin infusion) production lines by simply adding a needle punching process. Its core function is to improve the interlaminar failure resistance of composite materials under shear and bending loads, as well as the peel resistance of foam sandwich structures. These indicators are key limiting factors for the service life of composite structural components (such as wind turbine blade webs and rail transit bogie components). This solution can replace the costly three-dimensional weaving and easily damaged fiber stitching processes, and has important engineering substitution value.
[0014] (5) The technical solution provided by this invention has good market applicability and market value. The target market covers aerospace (fairing, tail fin), rail transit (body plate, bogie), wind turbine blades (web plate, beam cap), and ships (deck, bulkhead), etc. These fields have an urgent need for lightweight, high shear / bending strength, and high peel resistance composite materials. The cost increase of this solution is extremely low (only needle punching process, no additional materials), but the performance improvement is significant (shear strength +31%, bending modulus +48%, which can reduce the redundant thickness of the structure or extend the service life, and the overall cost of each large component is expected to be reduced by 10%~20%). Combined with the feature of no weight increase, it has obvious advantages in weight-sensitive scenarios such as the top cover of the battery pack of new energy vehicles and the interior panel of high-speed rail.
[0015] (6) This technical solution is expected to have long-term application value in the field of composite materials for at least 10 to 15 years. With the decline in carbon fiber prices and the development of new energy equipment (wind power, hydrogen energy storage and transportation) and high-speed transportation vehicles (magnetic levitation, eVTOL), the usage of hybrid composite materials will continue to grow. As a basic process improvement, this solution does not depend on specific short-term materials or policies and has a long life cycle.
[0016] (7) Furthermore, this invention covers two core aspects: "specific layup + needle punching parameter combination" and "skin fiber hooks introduced into foam anchoring". The product features (anchored fiber bundles inside the foam) are easy to prove, which can effectively limit competitors from achieving the same performance with low-cost needle punching methods. Although similar solutions (three-dimensional weaving, Z-pin) have been disclosed in the prior art, their costs are much higher than those of this invention. Therefore, this invention can build significant technical and cost barriers. Attached Figure Description
[0017] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0018] Figure 1 This is a schematic diagram of the preform obtained before needle punching in the preparation of the needle-punched laminated structure, showing only the layup and no needle punching. Figure 2 This is a schematic diagram of the structural design of the needled preform formed after layer-by-layer needle punching in Example 1; Figure 3 Photographs of the appearance of the three preforms (lay-up, needle punching, and needle punching + stitching) in Example 1, Comparative Example 1, and Comparative Example 2; Figure 4 This is a schematic diagram of the preform obtained before needle punching when preparing the needle-punched foam sandwich structure, with only the layers laid up. Figure 5 This is a schematic diagram of the structural design of the needled foam sandwich preform formed after layup needle punching in Example 2. Detailed Implementation
[0019] In existing technologies, glass-carbon hybrid composite materials mostly employ simple layup or stitching processes: layup processes rely solely on resin bonding between layers, resulting in low shear strength (≤35MPa); while stitching processes enhance interlayer bonding, suture punctures severely damage in-plane fibers (tensile strength reduction of 15%~25%) and introduce heterogeneous interface defects. Although some publicly available literature discusses needle punching processes, there are no reports on combinations of glass-carbon hybrid systems + specific symmetrical layups (including alternating carbon fiber mesh / unidirectional fabric / grid fabric) + fine needle punching parameters (density, depth, and speed coordination). Furthermore, there are no reports on using needle punching to hook skin fibers into foam core materials to form an integrated anchorage. This invention is the first to systematically study the mechanical property enhancement mechanism under this specific combination and creatively extends the needle punching principle to foam sandwich structures, achieving Z-axis anchorage "without external medium," which has significant technical differences from prior art. The implementation method and effect are both groundbreaking and non-obvious.
[0020] In one typical embodiment, the present invention provides a glass-carbon hybrid composite material preform, which is a multi-layered composite symmetrical layup structure, consisting of, from bottom to top: carbon fiber mesh, glass fiber woven fabric, carbon fiber unidirectional fabric, carbon fiber mesh, glass fiber woven fabric, glass fiber woven fabric, carbon fiber mesh, carbon fiber unidirectional fabric, glass fiber woven fabric, and carbon fiber mesh. The ply structure contains anchoring fiber bundles of the same material and origin as the skin fibers, and the pinholes are filled with cured resin.
[0021] In some embodiments of this implementation, the carbon fiber mesh layup density is 20~100g / m², whether in the surface layer or the intermediate structure. 2 Specifically, it can be 20g / m 2 30g / m 2 40g / m 2 45g / m 2 50g / m 2 55g / m 2 60g / m 2 65g / m 2 70g / m 2 75g / m 2 80g / m 2 90g / m 2 100g / m 2 The preferred concentration is 30~80g / m³. 2 The preferred value is 40~60g / m 2 During the experiments of this invention, the 30g / m 2 50g / m 2 and 80g / m 2 The needle-punching process is thin (30g / m²). 2 The needle of this type carries in relatively few fibers, and the thicker ones (80g / m²) are less likely to introduce fibers.2 The needle introduces a large amount of non-directional fibers, resulting in a fluffy texture after needling, with a weight of only 50g / m². 2 The carbon fiber mesh has better processability; therefore, the optimal laying density of the carbon fiber mesh in this invention is 50 g / m². 2 .
[0022] In some embodiments of this implementation, the fiberglass woven fabric and / or unidirectional carbon fiber fabric adjacent to the surface carbon fiber mesh have a laying density of 100~300g / m². 2 Specifically, 100g / m 2 110g / m 2 120g / m 2 130g / m 2 140g / m 2 150g / m 2 160g / m 2 170g / m 2 180g / m 2 190g / m 2 200g / m 2 210g / m 2 220g / m 2 230g / m 2 240g / m 2 250g / m 2 260g / m 2 270g / m 2 280g / m 2 290g / m 2 300g / m 2 The preferred concentration is 150~250 g / m³. 2 More preferably, it is 190~210g / m 2 The optimal value is 200g / m 2 In this process, there are no special requirements for the basis weight of the layup. The fiber type, basis weight, and weave structure (twill, plain, unidirectional, etc.) are selected according to the application and design requirements.
[0023] Carbon fiber unidirectional fabric can be replaced with carbon fiber woven fabric, or glass fiber woven fabric can be replaced with glass fiber unidirectional fabric, but the layup symmetry must be maintained; the position of the mesh layer can be slightly adjusted, but it must be retained at the critical interlayer interface.
[0024] The fiberglass woven fabric adjacent to the surface carbon fiber mesh is laid at an angle of 0 / 90°.
[0025] The layup angle of the unidirectional carbon fiber fabric adjacent to the surface carbon fiber mesh is 0° or 90°. Specifically: the layup angle of the unidirectional carbon fiber fabric adjacent to the lower surface carbon fiber mesh is 0°, and the layup angle of the unidirectional carbon fiber fabric adjacent to the upper surface carbon fiber mesh is 90°. The layup design principle is symmetrical. The asymmetrical layup of 0° and 90° in this embodiment is due to the small number of layers. In order to balance the stress, it provides strength in both the 0° and 90° directions and prevents the template from warping and deforming.
[0026] In some embodiments of this implementation, the laying density of the two layers of fiberglass woven fabric between the upper and lower carbon fiber mesh in the middle part is 300~500g / m². 2 Specifically, 300g / m 2 310g / m 2 320g / m 2 330g / m 2 340g / m 2 350g / m 2 360g / m 2 370g / m 2 380g / m 2 390g / m 2 400g / m 2 410g / m 2 420g / m 2 430g / m 2 440g / m 2 450g / m 2 460g / m 2 470g / m 2 480g / m 2 490g / m 2 500g / m 2 The preferred concentration is 350~450 g / m³. 2 More preferably, it is 390~410 g / m 2 The optimal value is 400g / m 2 The two layers of fiberglass woven fabric between the upper and lower carbon fiber mesh in the middle section are laid at an angle of 0 / 90°.
[0027] In one typical embodiment, the present invention provides a method for preparing the above-mentioned glass-carbon hybrid composite material preform, comprising the following steps: A multilayer structure is formed by alternating layers of carbon fiber mesh as a spacer layer with fiberglass woven fabric and carbon fiber unidirectional fabric in a specific symmetrical order. The product is obtained by needle-punching and then shaping and solidifying it.
[0028] During installation, positioning fixtures are used to ensure no wrinkles and precise orientation.
[0029] In some embodiments of this implementation, the acupuncture process is: a density of 15-25 needles / cm. 2 A depth of 8-12mm and a speed of 70-90 stitches / min can both achieve a certain enhancement effect, but 20 stitches / cm can achieve the best results. 2 The optimal needle penetration rate is 10mm and 80 needles / min. The needles penetrate all the layers.
[0030] Furthermore, the acupuncture needles used are #36, #38, or #40 fine-toothed needles with hooks. The depth needs to be adjusted accordingly for different needles to avoid excessive damage. The hooked needles are those commonly used in this industry.
[0031] In some embodiments of this implementation, the VARI molding process is used, in which the needled preform is placed in a mold, vacuum sealed, resin and curing agent are injected, and then cured to obtain the final product.
[0032] Furthermore, the vacuum degree of the vacuum seal is ≤-0.095MPa.
[0033] Furthermore, the resin includes BST-C760 epoxy resin or other low-viscosity epoxy / vinyl resin, as long as it is suitable for the VARI process. The resin ratio can follow the existing conventional TDS operating requirements, such as a resin to curing agent mass ratio of (90~110):(10~20), preferably 100:15, and vacuum degassing is also required, such as degassing for 10~30 minutes.
[0034] Furthermore, the curing conditions are as follows: heating at 50~70℃ for 1~3 hours, then heating at 80~90℃ for 3~5 hours, wherein the heating rate is 1~5℃ / min. Preferably, curing is carried out at 60℃ / 2 hours and 85℃ / 4 hours (heating rate 2℃ / min).
[0035] Preferred method for preparing glass-carbon hybrid composite preform includes the following steps: Step 1: Lamination Lay in a specific symmetrical order from bottom to top: 40~60g / m² 2 Carbon fiber mesh tire → 150~250g / m 2 Fiberglass woven fabric (0 / 90°) → 150~250g / m 2 Carbon fiber unidirectional fabric (0°) → 40~60g / m 2 Carbon fiber mesh tire → 350~450g / m 2 Fiberglass woven fabric (0 / 90°) → 350~450g / m 2 Fiberglass woven fabric (0 / 90°) → 40~60g / m 2 Carbon fiber mesh tire → 150~250g / m 2Carbon fiber unidirectional fabric (90°) → 150~250g / m 2 Fiberglass woven fabric (0 / 90°) → 40~60g / m 2 Carbon fiber mesh tire.
[0036] Step 2: Acupuncture Using a #36 needle (with a hook), 15-25 needle insertions per cm. 2 The needle preform is formed by repeated punctures at a depth of 8-12mm (through all layers) and a speed of 70-90 needles / min to create a three-dimensional network structure.
[0037] Step 3: VARI molding The preform is placed in a mold, vacuum sealed, a mixture of resin and curing agent is injected, heated to cure, and then cut and sampled after cooling.
[0038] In one typical embodiment, the present invention provides a foam sandwich composite material, comprising a foam core material and the above-mentioned glass-carbon hybrid composite material preform; wherein, the foam core material is the middle sandwich layer in the glass-carbon hybrid composite material preform; The foam core contains anchoring fiber bundles of the same material and origin as the skin fiber, and the pinholes are filled with cured resin.
[0039] In one typical embodiment, the present invention provides a method for preparing the above-mentioned foam sandwich composite material, comprising the following steps: Carbon fiber mesh is used as a spacer layer, and it is laid alternately with fiberglass woven fabric and carbon fiber unidirectional fabric in a specific symmetrical order to form a laminated structure with foam core material as the center; then it is needle-punched, with the needle-punching depth extending into the interior of the foam, and finally it is molded and cured to obtain the final product.
[0040] In some embodiments of this implementation, a symmetrical upper half layer is first laid on the foam core material and then needled; then a symmetrical lower half layer is laid and needled.
[0041] In some embodiments of this implementation, the acupuncture process is as follows: density 15~25 needles / cm. 2 The solid portion has a depth of 8-12mm (preferably 10mm), and the interlayer portion penetrates the foam 5-15mm (preferably 10mm). A speed of 70-90 stitches / min can achieve a certain reinforcing effect, but 20 stitches / cm is less effective. 2 The optimal insertion depth is 20mm and the needle rate is 80 needles / min.
[0042] In foam sandwich composite materials, the needle penetration depth is increased to 15-20mm (ensuring that after piercing a 10mm layup, it penetrates 5-15mm into the foam interior, preferably 10mm). During the return stroke of the needle, the hook pulls out the fiber bundle from the layup and retains it in the foam needle hole; after subsequent glue injection and curing, this fiber bundle forms a skin-foam Z-axis anchoring structure. The upper and lower sides can be needled separately or simultaneously.
[0043] The needle penetration extends into the foam, using the needle hooks to bring the skin's own fibers into the foam, forming a Z-axis mechanical anchoring structure that is continuous and integrated with the skin without external media.
[0044] Foam sandwich composite materials can be needled on one or both sides. Needling can be done on only one side of the tension side, or simultaneously on both sides to form an X-shaped staggered anchorage.
[0045] Foam core materials include one or more of PET and PMI foams.
[0046] Preferably, the structure of the foam sandwich composite material, arranged symmetrically from bottom to top, is as follows: 50 g / m³ 2 Carbon fiber mesh tire → 200g / m 2 Fiberglass woven fabric (0 / 90°) → 200g / m 2 Carbon fiber unidirectional fabric (0°) → 50g / m 2 Carbon fiber mesh tire → 400g / m 2 Fiberglass woven fabric (0 / 90°) → Foam core material → 400g / m 2 Fiberglass woven fabric (0 / 90°) → 50g / m 2 Carbon fiber mesh tire → 200g / m 2 Carbon fiber unidirectional fabric (90°) → 200g / m 2 Fiberglass woven fabric (0 / 90°) → 50g / m 2 Carbon fiber mesh tire.
[0047] In this invention, unless otherwise specified, all other test materials and instruments are conventional test materials in the field and can be purchased through commercial channels.
[0048] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.
[0049] Example 1 - Glass-carbon hybrid composite preform (solid laminate material) Step 1: Laying out layers Lay the soil from bottom to top in a symmetrical order as shown in Table 1: 50g / m 2 Carbon fiber mesh tire → 200g / m 2 Fiberglass woven fabric (0 / 90°) → 200g / m 2Carbon fiber unidirectional fabric (0°) → 50g / m 2 Carbon fiber mesh tire → 400g / m 2 Fiberglass woven fabric (0 / 90°) → 400g / m 2 Fiberglass woven fabric (0 / 90°) → 50g / m 2 Carbon fiber mesh tire → 200g / m 2 Carbon fiber unidirectional fabric (90°) → 200g / m 2 Fiberglass woven fabric (0 / 90°) → 50g / m 2 Carbon fiber mesh tire. Positioning fixtures are used to ensure no wrinkles and precise orientation.
[0050] Step 2: Acupuncture Using a #36 lancet (with a hook), the needle density is 20 needles / cm. 2 The needle penetration depth is 10mm (through all layers), the needle penetration speed is 80 needles / min, and the reciprocating puncture forms a three-dimensional network interwoven structure to obtain the needle-punched preform.
[0051] Step 3: VARI molding Place the preform in the mold, vacuum seal it (vacuum degree ≤ -0.095MPa), inject BST-C760 epoxy resin (mixed with curing agent at a ratio of 100:15, vacuum degassing for 15min), and cure it at 60℃ / 2h + 85℃ / 4h (heating rate 2℃ / min). After cooling, cut and take samples.
[0052] Example 2 - Foam Sandwich Composite Material Unlike Example 1, the step of "providing a foam core material (PET)" is added before step 1; the fiber layup is laid on the surface of the foam core material; in step 2, the needle penetration depth is increased to 20mm (ensuring that after piercing a 10mm layup, it penetrates 10mm into the foam interior), and during the needle return stroke, the hook pulls out the fiber bundle from the layup and retains it in the foam needle hole; after subsequent glue injection and curing, the fiber bundle forms a skin-foam Z-axis anchoring structure. The upper and lower sides can be needled separately or simultaneously.
[0053] The specific steps for preparing foam sandwich composite materials are as follows: First, a symmetrical upper half layer is laid on the foam core material and then needle-punched; then, a symmetrical lower half layer is laid and needle-punched. The fiber layup is placed on the surface of the foam core material, and the structure of the foam sandwich composite material, arranged symmetrically from bottom to top, is: 50 g / m². 2 Carbon fiber mesh tire → 200g / m 2 Fiberglass woven fabric (0 / 90°) → 200g / m 2 Carbon fiber unidirectional fabric (0°) → 50g / m 2 Carbon fiber mesh tire → 400g / m 2Fiberglass woven fabric (0 / 90°) → Foam core material → 400g / m 2 Fiberglass woven fabric (0 / 90°) → 50g / m 2 Carbon fiber mesh tire → 200g / m 2 Carbon fiber unidirectional fabric (90°) → 200g / m 2 Fiberglass woven fabric (0 / 90°) → 50g / m 2 Carbon fiber mesh tire. Positioning fixtures are used to ensure no wrinkles and precise orientation.
[0054] Comparative Example 1 Unlike Example 1, the acupuncture step was omitted, resulting in the "control group" in Table 1.
[0055] Comparative Example 2 Unlike Example 1, a manual suturing method was added to the needle-punched preform, resulting in the "needle-punching + suturing group" shown in Table 1. Suturing parameters: the horizontal and vertical spacing were both 5mm, forming a uniform mesh-like connection; to improve the wrapping effect of the sutures and fibers and enhance connection stability, a modified lockstitch method was used, with the suture trajectory at a 45° angle to the fiber direction to reduce the impact on the directional mechanical properties of the reinforcing phase.
[0056] Table 1 Ply Information Table
[0057] The data in Tables 2 through 4 correspond to the tensile, bending, and shear test data of the three groups in Table 1: "Control Group," "Needle Puncture," and "Needle Puncture + Suture." It is understood that the multiple numbers assigned to each treatment group indicate that the sample underwent repeated experiments multiple times.
[0058] Table 2 Tensile Properties
[0059] Table 3 Bending properties
[0060] Table 4 Shear Properties
[0061] The control group (layout process) exhibited the best tensile properties (tensile strength 413.82 MPa, elastic modulus 29.95 GPa), due to the absence of mechanical damage to the fibers, the integrity of the continuous load-bearing path, and the highest load transfer efficiency. However, its flexural strength (359.91 MPa) and interlaminar shear strength (32.50 MPa) were the lowest among the three groups. This is because the interlaminar bond relies solely on resin adhesion, leading to easy delamination in the tension zone, fiber buckling in the compression zone, and relative slippage between layers under shear loads. Therefore, while the layup process offers good in-plane properties, its interlaminar properties are weak, making it unsuitable for service conditions dominated by interlaminar stress.
[0062] The needle-punched group showed a 26.64% decrease in tensile strength (303.6 MPa) and a 18.82% decrease in elastic modulus, attributed to partial carbon fiber breakage and fiber orientation deviation from the principal stress direction caused by needle punching. However, flexural strength increased by 14.73%, flexural elastic modulus by 48.50%, and interlaminar shear strength by 31.21% (42.58 MPa). The three-dimensional interwoven fiber network formed by needle punching replaces part of the resin bonding force, suppressing interlaminar delamination, fiber buckling, and interlaminar slippage, and resulting in a more uniform load distribution. Therefore, needle punching achieves a comprehensive improvement in interlaminar properties with limited in-plane performance loss, making it the process with the highest interlaminar reinforcement efficiency and the best overall performance among the three groups.
[0063] Needle puncture + suture group: tensile strength 324.62 MPa ( 21.56%), elastic modulus 23.47 GPa ( 21.65%), the suture puncture cuts part of the fiber and forms a resin flow dead zone and stress concentration at the suture-resin interface; the flexural strength decreases instead of increasing (300.9 MPa, (16.40%), suture defects became the initiation source of bending fracture; the interlaminar shear strength was only 34.77 MPa (+6.99%), far lower than that of the needle-punched group. This was because the 5 mm suture spacing was too large, the bridging constraint was limited, and the 12K T300 suture had high rigidity and weak bonding with the resin interface. Therefore, under the suture parameters of this invention, the negative effects of suture offset and weakened the reinforcing effect of needle punching. The matching of suture process parameters (spacing, suture specifications) with the VARI process is the key to determining its reinforcing effect and needs further optimization.
[0064] In summary, the comparison of the three sets of data shows that the control group (layered process) sample has good fiber continuity and the best tensile properties (tensile strength 413.82 MPa, elastic modulus 29.95 GPa), but the interlayer bonding relies solely on the adhesive strength of the resin, with the lowest flexural strength (359.91 MPa) and interlayer shear strength (32.50 MPa), indicating weak interlayer bonding and poor uniformity. The needle-punched group showed a 26.64% decrease in tensile strength (303.6 MPa), but its flexural strength, flexural elastic modulus, and interlayer shear strength increased by 14.73%, 48.50%, and 31.21% respectively (reaching 42.58 MPa), indicating that the needle-punched three-dimensional network structure significantly strengthened interlayer constraints. The tensile strength of the "needle-punched + sutured group" was 324.62 MPa. 21.56%), bending strength is 300.9 MPa ( The interlaminar shear strength was 34.77 MPa (only +6.99%), with a 16.40% increase in fiber strength and interfacial defects introduced by suturing offsetting the reinforcing effect of needle punching. Overall, the needle punching group showed the most significant advantages in interlaminar performance and data stability, making it the optimal process for balancing interlaminar reinforcement and overall load-bearing capacity.
[0065] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A glass-carbon hybrid composite material preform, characterized in that, It is a multi-layered composite symmetrical layup structure, consisting of the following layers from bottom to top: carbon fiber mesh, fiberglass woven fabric, unidirectional carbon fiber fabric, carbon fiber mesh, fiberglass woven fabric, fiberglass woven fabric, carbon fiber mesh, unidirectional carbon fiber fabric, fiberglass woven fabric, and carbon fiber mesh. The ply structure contains anchoring fiber bundles of the same material and origin as the skin fibers, and the pinholes are filled with cured resin.
2. The glass-carbon hybrid composite preform according to claim 1, characterized in that, The laying density of carbon fiber mesh is 20~100g / m². 2 The preferred value is 40~60g / m 2 .
3. The glass-carbon hybrid composite preform according to claim 1, characterized in that, The fiberglass woven fabric and / or unidirectional carbon fiber fabric adjacent to the surface carbon fiber mesh have a laying density of 100~300g / m². 2 The preferred value is 150~250g / m 2 ; Preferably, the fiberglass woven fabric adjacent to the surface carbon fiber mesh is laid at an angle of 0 / 90°. Preferably, the laying angle of the unidirectional carbon fiber fabric adjacent to the surface carbon fiber mesh is 0° or 90°; more preferably, the laying angle of the unidirectional carbon fiber fabric adjacent to the lower surface carbon fiber mesh is 0°, and the laying angle of the unidirectional carbon fiber fabric adjacent to the upper surface carbon fiber mesh is 90°.
4. The glass-carbon hybrid composite preform according to claim 1, characterized in that, In the middle section of the ply structure, the two layers of fiberglass woven fabric between the upper and lower carbon fiber mesh have a laying density of 300~500g / m². 2 The preferred value is 350~450g / m 2 ; Preferably, the laying angle of the two layers of fiberglass woven fabric between the upper and lower carbon fiber mesh in the middle part is 0 / 90°.
5. A method for preparing a glass-carbon hybrid composite preform according to any one of claims 1 to 4, characterized in that, Includes the following steps: A multilayer structure is formed by alternating layers of carbon fiber mesh as a spacer layer with fiberglass woven fabric and carbon fiber unidirectional fabric in a specific symmetrical order. The product is obtained by needle-punching and then shaping and solidifying it.
6. The preparation method according to claim 5, characterized in that, The needle-punching technique has a density of 15-25 needles / cm. 2 Depth 8~12mm, speed 70~90 stitches / min; preferably 20 stitches / cm 2 10mm, 80 needles / min; Preferably, the needle penetrates all the layers; Preferably, the needle is a 36# needle, a 38# fine-toothed needle, or a 40# fine-toothed needle with hooks.
7. The preparation method according to claim 5, characterized in that, The VARI molding process is used to place the needled preform into a mold, vacuum seal it, inject resin and curing agent, and then cure it to obtain the final product. The curing conditions are: heating at 50~70℃ for 1~3h, then heating at 80~90℃ for 3~5h, wherein the heating rate is 1~5℃ / min; preferably, curing is carried out at 60℃ / 2h and 85℃ / 4h, with a heating rate of 2℃ / min.
8. A foam sandwich composite material, characterized in that, Includes foam core material, and glass-carbon hybrid composite preform as described in any one of claims 1 to 4 or glass-carbon hybrid composite preform prepared by the preparation method described in any one of claims 5 to 7; Among them, the foam core material serves as the middle interlayer in the glass-carbon hybrid composite preform; The foam core contains anchoring fiber bundles of the same material and origin as the skin fiber, and the pinholes are filled with cured resin.
9. A method for preparing the foam sandwich composite material according to claim 8, characterized in that, Includes the following steps: Carbon fiber mesh is used as a spacer layer, and it is laid alternately with fiberglass woven fabric and carbon fiber unidirectional fabric in a specific symmetrical order to form a laminated structure with foam core material as the center; then it is needle-punched, with the needle-punching depth extending into the interior of the foam; finally, it is molded and cured to obtain the final product.
10. The preparation method according to claim 9, characterized in that, First, lay symmetrical upper layers on the foam core material and then needle-punch them; then lay symmetrical lower layers and needle-punch them. Preferably, the needle-punching process has a density of 15-25 needles / cm. 2 The solid layup depth is 8-12mm, and the foam interlayer penetrates 5-15mm into the foam, at a speed of 70-90 stitches / min; preferably, the density is 20 stitches / cm. 2 The depth of the solid layer is 10mm, the foam layer is inserted into the foam 10mm, and the speed is 80 needles / min.