Inserts and their manufacturing methods, vehicles, and embedded composite components and their manufacturing methods

By setting displacement compensation slits and functional gradient interface coatings on the insert body, the problems of easy cracking, peeling and warping of the bonding interface in steel-aluminum embedded composite components are solved, and the connection strength and stability of embedded composite components are improved.

CN123104786APending Publication Date: 2026-11-17ZHEJIANG GEELY HLDG GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611190451.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In steel-aluminum embedded composite components, the bonding interface is prone to cracking, peeling or debonding, and the embedded composite components may warp and deform, leading to structural strength and stability problems.

Method used

A displacement compensation slit is set on the insert body, and a functional gradient interface coating is applied to the bonding surface. The path and width of the displacement compensation slit are designed to compensate for the material cooling shrinkage difference, thereby improving the bonding strength and stability.

Benefits of technology

It reduces the risk of interface cracking, peeling and debonding, reduces the warping deformation of the embedded composite components, and improves the connection strength and overall structural stability of the steel-aluminum composite components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104786A_ABST
    Figure CN123104786A_ABST
Patent Text Reader

Abstract

This application relates to inserts and their manufacturing methods, vehicles, and cast composite components and their manufacturing methods. Specifically, an insert is provided, comprising an insert body made of a first material, the insert body having a mating surface; a displacement compensation slit is provided on the insert body, the displacement compensation slit penetrating the mating surface; two opposing sidewalls are formed on both sides of the displacement compensation slit along its width direction. Thus, by providing the displacement compensation slit, the relative shrinkage displacement that needs to be compensated at the corresponding position on the mating surface, corresponding to at least part of the cooling shrinkage difference during the cooling process of the casting process, can be compensated. This reduces the risk of cracking, peeling, or debonding at the mating interface and decreases the possibility of warping of the cast composite component after cooling or demolding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metal composite molding technology, and in particular to an insert and its manufacturing method, a vehicle, an embedded composite component and its manufacturing method. Background Technology

[0002] To reduce vehicle weight, body components are mostly made of die-cast aluminum alloy. However, the relatively low structural rigidity and strength of aluminum alloy limits its application in components with extremely high collision safety requirements, such as the front engine compartment. To ensure structural rigidity while avoiding a significant increase in vehicle weight, steel-aluminum interlocking composite components are now widely used. High-strength steel inserts provide load-bearing and deformation resistance, while the aluminum alloy matrix maintains the lightweight advantage.

[0003] However, due to the different coefficients of thermal expansion of steel and aluminum alloy, there is a difference in shrinkage between the steel insert and the aluminum alloy matrix during the cooling process of the inlay casting process. As a result, cracking, peeling or debonding can easily occur at the interface between the two, which may lead to warping deformation of the inlay casting composite component.

[0004] Therefore, how to overcome the aforementioned shortcomings of existing technologies is a technical problem that urgently needs to be solved by all sectors. Summary of the Invention

[0005] The purpose of this application is to solve the technical problem that the bonding interface of the embedded composite component is prone to cracking, peeling or debonding, which may cause the embedded composite component to warp.

[0006] To achieve the above objectives, a first aspect of this application provides an insert, including an insert body made of a first material, the insert body having a mating surface; The insert body is provided with a displacement compensation slit, which penetrates the mating surface. The displacement compensation slit has two opposing sidewalls on both sides along its width direction.

[0007] In some exemplary embodiments, the bonding surface 13 is covered by a second material in a molten state during the casting process, wherein the coefficient of thermal expansion of the first material is different from that of the second material; Preferably, the coefficient of thermal expansion of the first material is less than that of the second material.

[0008] In some exemplary embodiments, multiple displacement compensation slits (11) are provided, and among the multiple displacement compensation slits (11), at least a displacement compensation slit (11) with a straight extension path and a displacement compensation slit (11) with a curved extension path are included; and / or Multiple displacement compensation slits are provided, and at least two of the multiple displacement compensation slits have straight extension paths and different width directions from each other; and / or The extension path of the displacement compensation slit is a curve; and / or The displacement compensation slit has at least two segments with unequal widths along its extension path; and / or The displacement compensation slit penetrates the insert body along its thickness direction; and / or The displacement compensation slit is located at the end of its extension path inside the insert body, and the insert body has an end wall at the end, the end wall being arc-shaped and smoothly transitioning to the two side walls respectively.

[0009] In some exemplary embodiments, the insert body has a guide portion protruding from the bonding surface, the guide portion including a guide surface having an inlet edge connected to and located on the bonding surface.

[0010] The guide surface extends obliquely upward from the inlet edge along a first direction, away from the bonding surface.

[0011] In some exemplary embodiments, along the first direction, the guide portion is located before the displacement compensation slit; The flow guide has a receiving chamber with an opening facing the mating surface.

[0012] In some exemplary embodiments, the first material is steel and the second material is aluminum alloy; The bonding surface is provided with a functionally graded interface coating, which includes, in sequence along the direction away from the insert body, a substrate bonding layer, a thermal expansion buffer layer, a chemical transition layer, and a wetting activation layer.

[0013] In some exemplary embodiments, the total thickness of the functionally graded interface coating is 40–185 μm; and / or The thickness of the substrate bonding layer is 5–25 μm, and it is formed of at least one of Ni, Ni-Fe alloy, Fe-Ni alloy, and Fe-Ni-Co alloy; and / or The thermal expansion buffer layer has a thickness of 10–40 μm and is formed of at least one of Fe-Ni alloy and Fe-Ni-Co alloy; and / or The thickness of the chemical transition layer is 20–80 μm, and includes at least one of the Ni-Al system, Ni-Al-Zn system, and Fe-Ni-Al system, wherein, along the direction away from the insert body, the Ni content in the chemical transition layer shows a decreasing trend, and the Al content shows an increasing trend; and / or The thickness of the wetting and activating layer is 5 to 40 μm, and includes a matrix formed of Zn-Al alloy or Al-Si alloy, and 0.5% to 8% by mass of fluoroaluminate activator particles, wherein the fluoroaluminate activator particles are selected from at least one of KAlF4, K2AlF5 and CsAlF4, and the particle size of the fluoroaluminate activator particles is not greater than 5 μm.

[0014] A second aspect of this application provides a cast composite component including the insert described in the first aspect. The insert includes an insert body made of a first material and a cover made of a second material, wherein the cover at least partially enters a displacement compensation slit provided on the insert body.

[0015] A third aspect of this application provides a vehicle including the cast composite component described in the second aspect.

[0016] The fourth aspect of this application provides an insert manufacturing method, comprising: The thermal expansion coefficient and plastic deformation performance parameters of a first material used to manufacture the insert body, and the thermal expansion coefficient of a second material used to form the coating, are obtained, and it is determined that the thermal expansion coefficients of the first material and the second material are different, wherein the insert body has a bonding surface for being coated by the second material in a molten state; Based on the insert body without displacement compensation slits, the cooling shrinkage difference between the insert body and the second material, the relative shrinkage displacement that needs to be compensated, the interfacial shear force, and the forces on the bonding surface are determined during the cooling process. Based on the cooling shrinkage difference, the relative shrinkage displacement requiring compensation, the interfacial shear force, and the compressive stress on the bonding surface, and constrained by the fact that the insert body after forming the displacement compensation slit meets preset strength and stiffness conditions, the design parameters of the displacement compensation slit are determined. These design parameters include the number and location of the displacement compensation slits, as well as the extension path, local width direction, and width distribution along the extension path of each displacement compensation slit; and The insert body is provided, and each of the displacement compensation slits is formed on the mating surface of the insert body according to the design parameters, wherein the displacement compensation slits penetrate the insert body along the thickness direction of the insert body.

[0017] In some exemplary embodiments, the cooling shrinkage difference, the relative shrinkage displacement that needs to be compensated, the interfacial shear force, and the forces acting on the bonding surface are all obtained through thermo-mechanical coupling analysis.

[0018] In some exemplary embodiments, the coefficient of thermal expansion of the first material is less than that of the second material.

[0019] In some exemplary embodiments, it also includes: The flow process of the second material in the molten state along the bonding surface is analyzed to obtain a predetermined flow path of the second material on the bonding surface, a predetermined flow direction of the predetermined flow path at different positions, and flow state data. Based on the results of the filling analysis, the location and geometric parameters of the guide section are determined. These geometric parameters include the inclination of the guide surface relative to the bonding surface and the protrusion height of the guide section relative to the bonding surface. According to the set position and the geometric parameters, the flow guide portion protruding from the bonding surface is formed on the insert body. The flow guide surface has an inlet edge located on the bonding surface, and the protrusion height of the flow guide surface relative to the bonding surface gradually increases from the inlet edge along the predetermined flow direction.

[0020] In some exemplary embodiments, it also includes: The bonding surface is subjected to surface roughening treatment to achieve a surface roughness Ra of 2.0–6.0 μm; and On the roughened bonding surface, a matrix bonding layer, a thermal expansion buffer layer, a chemical transition layer, and a wetting activation layer are sequentially formed in a direction away from the insert body to form a functional gradient interface coating.

[0021] The fifth aspect of this application provides a method for manufacturing a cast composite component, comprising: An insert is provided, the insert comprising an insert body made of a first material, the insert body having a mating surface, the mating surface having a displacement compensation slit, the insert body having two opposing sidewalls formed on both sides of the displacement compensation slit in the width direction, the first material having plastic deformation capability, and the coefficient of thermal expansion of the first material being less than the coefficient of thermal expansion of the second material. Place the insert into the cavity of the mold; Molten second material is injected into the cavity, so that the molten second material covers the bonding surface; The mold cooling system is turned on to cool the mold, so that the second material solidifies to form a coating, thereby obtaining the embedded composite component.

[0022] In some exemplary embodiments, the insert is prepared by the insert manufacturing method described in the fourth aspect.

[0023] In some exemplary embodiments, the insert located in the cavity is preheated in situ after being placed in the cavity and before the molten second material is injected into the cavity; The in-situ preheating includes: Make the electrode contact the insert body; and A pulsed current is passed through the electrode to heat the insert using Joule heating.

[0024] According to the insert provided in this application, a displacement compensation slit is provided to compensate for at least part of the relative shrinkage displacement that needs to be compensated at the corresponding position on the bonding surface, corresponding to the difference in cooling shrinkage between the first and second materials. This reduces the risk of cracking, peeling, or debonding at the bonding interface and decreases the likelihood of warping of the cast composite component after cooling or demolding. Attached Figure Description

[0025] Figure 1 This is a schematic diagram of an exemplary insert structure of this application; Figure 2 yes Figure 1 Enlarged schematic diagram of the mid-displacement compensation slit; Figure 3 This is a schematic diagram of the displacement compensation slit along the extended path of the curve. Figure 4 This is a schematic diagram showing that the width direction varies in different sections; Figure 4a This is a schematic diagram showing the different width directions of the displacement compensation slits on the surface. Figure 5 This is a schematic diagram showing that the width of the extension path along the displacement compensation slit is not constant; Figure 6a This is a schematic diagram of a displacement compensation slit penetrating the insert body along the thickness direction of the insert body; Figure 6b A schematic diagram showing that the displacement compensation slits are distributed in a matrix in one embodiment; Figure 7a This is a schematic diagram of the flow guide section; Figure 7b A schematic diagram showing that the flow guides are distributed in a matrix in one embodiment; Figure 8 This is a flowchart illustrating the insert manufacturing process; Figure 9 This is a flowchart illustrating the manufacturing method of the embedded composite component.

[0026] Explanation of reference numerals in the attached figures: Insert 10 Displacement compensation slits 11, 11a, 11b, 11c Side wall 111 Insert body 12 End wall 121 bonding surface 13 Guide section 14 Guide surface 141 142 chambers Opening 143 Import Edge 144 Rectangular area 20 First rectangular area 21 Second rectangular area 22 The third rectangular area is 23.

[0027] Unless otherwise stated, the same reference numerals or symbols denote the same elements in the accompanying drawings.

[0028] It should be understood that the accompanying drawings are not necessarily drawn to scale, but rather present simplified representations of various features to illustrate the principles of this application. The specific design features disclosed in this application (including, for example, specific dimensions, orientations, locations, and shapes) will be determined in part by the specific environment in which they will be applied and used.

[0029] Throughout these figures, and across multiple figures, the same reference numerals denote the same or equivalent parts of this application. Detailed Implementation

[0030] Reference will now be made in detail to various embodiments of this application, examples of which are presented in the accompanying drawings and described below. Although this application will be described in conjunction with exemplary embodiments, it should be understood that this specification is not intended to limit this application to these exemplary embodiments. Rather, this application is intended to cover not only these exemplary embodiments, but also various alternatives, modifications, equivalents, and other embodiments that may be included within the spirit of this application and the scope defined by the appended claims.

[0031] The technical solution of this application mainly relates to steel-aluminum composite components. In the field of vehicle manufacturing, in order to reduce the weight of the vehicle body while ensuring the rigidity of the body and the energy absorption performance in a collision, high-stress, high-strain areas with insufficient rigidity or high energy absorption requirements are usually identified based on the stress and strain distribution of the components under target working conditions. These areas are then locally reinforced through steel-aluminum composite design, thereby avoiding the increase in vehicle weight and material waste caused by overall thickening or large-scale reinforcement.

[0032] [Insert] See Figure 1 The first aspect of this application provides an insert 10, wherein the insert 10 includes an insert body 12 made of a first material, the insert body 12 having a bonding surface 13 covered by a molten second material during the casting process. The molten second material flows within the mold cavity to the region where the bonding surface 13 is located, and forms a covering body (not shown) after cooling and solidification. The surface of the covering body that contacts the bonding surface is the covering surface (not shown). The coefficients of thermal expansion of the first material and the second material are different.

[0033] In some exemplary embodiments, the first material is steel, the second material is aluminum alloy, the insert 10 is a steel insert, and the cladding is an aluminum alloy cladding. It should be understood that the first and second materials are not limited to steel and aluminum alloy, but can be other materials that meet the corresponding conditions. Specifically, the first material is suitable for preparing the insert 10 and is at least capable of plastic deformation during the cooling process of the casting process; the first material and the second material have different coefficients of thermal expansion so that the insert 10 made of the first material and the cladding made of the second material produce a shrinkage difference during cooling. For ease of description, the terms "first material" and "second material" will be used consistently below to refer to the respective materials.

[0034] See also Figure 1 and Figure 2 The insert body 12 is provided with a displacement compensation slit 11, which penetrates the mating surface 13 along the thickness direction of the insert body 12. The displacement compensation slit 11 has two opposing sidewalls 111 on both sides along its width direction.

[0035] In this application, see Figure 2 The extension path of the displacement compensation slit 11 can be straight. For a displacement compensation slit 11 with a straight extension path, its width direction is perpendicular to the extension path. (See also...) Figure 3 The extension paths of displacement compensation slits 11a, 11b, and 11c can also be curved. For displacement compensation slits 11a, 11b, and 11c with curved extension paths, their width direction changes along the extension path. That is, the width direction can be different in different sections along the extension path.

[0036] For example, see Figure 4If the extension path of one segment A of the curved displacement compensation slit 11c is a straight line, then the local width direction of segment A is perpendicular to its own extension path, and in this case, the extension direction of segment A coincides with the extension path. For example, if the extension path of another segment B of the curved displacement compensation slit 11c is a curve, then the local width direction of this other segment B is perpendicular to the tangent direction of its own extension path, and in this case, the extension direction of segment B is the tangent direction.

[0037] In this application, see Figure 2 The width of the displacement compensation slit 11 refers to the distance between the two sidewalls 111 measured along its width direction. Exemplarily, the width of the displacement compensation slit 11 may be equal in each segment of its extension path, or, see [reference needed]. Figure 5 The displacement compensation slit 11 has at least two segments with unequal widths along its extension path. For example, at least two segments with unequal widths W1 and W2 along its extension path.

[0038] The aforementioned segments can be either a portion of the displacement compensation slit corresponding to a certain segment of the extension path of the displacement compensation slit, or a displacement compensation slit corresponding to a certain point on the extension path of the displacement compensation slit (in this case, a segment can be understood as a part located on the cross-section of the displacement compensation slit, wherein the cross-section is perpendicular to the extension direction of the displacement compensation slit).

[0039] For example, the thickness of the insert body 12 can be 0.6 mm to 1.5 mm, preferably 0.8 mm to 1.2 mm. The nominal wall thickness of the cover near the insert body 12 can be 2.5 mm to 5.0 mm, preferably 3.0 mm to 4.0 mm. It should be understood that the above dimensions can also be adapted to actual needs.

[0040] The bonding surface 13 of the second material-coated insert body, as referred to herein, includes the case where the coating directly contacts and covers the bonding surface, and also includes the case where the bonding surface is coated, and the coating is bonded to the side of the coating facing away from the bonding surface 13 and covers the area where the bonding surface is located (the case with a coating will be described in detail below). Unless otherwise stated, the following description of the bonding interface and interface cracking mainly uses the embodiment where the bonding surface is not coated and the coating directly forms a bonding interface with the insert body 12 as an example.

[0041] Because the coefficients of thermal expansion of the first material and the second material are different, the difference in their coefficients causes different theoretical shrinkage amounts during the cooling process of the casting process. This results in a shrinkage difference between the insert 10 and the second material used to form the cladding. During the casting process, because the first material (insert 10) and the second material are bonded together, they cannot deform completely according to their respective theoretical shrinkage amounts. Therefore, the shrinkage difference can transmit the force generated by cooling shrinkage to the bonding surface 13 of the cladding towards the insert body 12. This force may cause cracking, peeling, or debonding at the bonding interface between the insert 10 and the cladding, and may cause warping of the composite component after cooling and demolding.

[0042] Because the first material possesses plastic deformation capability, when the force generated by the cooling shrinkage difference between the insert 10 and the covering body is transmitted to the local area on the insert body 12 corresponding to the displacement compensation slit 11, at least a portion of the material in this local area can undergo irreversible plastic deformation. During the irreversible plastic deformation in this local area, the two sidewalls of the displacement compensation slit corresponding to this local area can deform along the width direction (the width direction of the displacement compensation slit). At this time, the width of the displacement compensation slit 11 changes, and the portion of the bonding surface 13 corresponding to the local area is displaced along the direction of the force.

[0043] It is understandable that the displacement compensation slit 11 is used to provide plastic deformation space for a local area, so that the corresponding part of the bonding surface 13 can generate corresponding displacement as the second material cools and contracts, thereby compensating for at least part of the relative contraction displacement that needs to be compensated at the corresponding position of the bonding surface 13 corresponding to the difference in cooling and contraction between the first material and the second material.

[0044] Although the shrinkage difference between the first and second materials does not disappear, localized areas undergo plastic deformation, causing displacement of the corresponding portion of the bonding surface 13. This compensates for at least part of the relative shrinkage displacement, preventing the shrinkage difference from being entirely converted into a force exerted by the second material on the insert body 12. Consequently, the risk of cracking, peeling, or debonding at the bonding interface is reduced, and the likelihood of warping of the cast composite component after cooling or demolding is decreased.

[0045] It should be noted that the local area extends from the corresponding sidewall 111, at least along the local width direction of the displacement compensation slit 11 at the corresponding position, toward the side away from the displacement compensation slit 11.

[0046] It is worth mentioning that after the molten second material is injected into the mold cavity, it can enter the displacement compensation slit 11 and form a mechanical lock with the insert 10 after cooling and solidification, thereby improving the connection strength between the cover and the insert 10. This further avoids phenomena such as interface cracking, peeling, and debonding at the bonding interface.

[0047] In some exemplary embodiments, the coefficient of thermal expansion of the first material is less than that of the second material.

[0048] Specifically, during the cooling process of the inlay casting process, the shrinkage of the second material is greater than that of the first material. The cooling shrinkage of the cladding body transmits a compressive force to the insert body 12, and forms a compressive stress (force) towards the displacement compensation slit 11 in the region where the displacement compensation slit 11 is located.

[0049] The compressive stress causes localized plastic deformation in the insert body 12 that forms at least one sidewall 111 and is adjacent to the sidewall 111, causing the corresponding sidewall 111 to shift and / or change shape toward the interior of the displacement compensation slit 11, and reducing the width of the displacement compensation slit 11.

[0050] The reduction in the width of the displacement compensation slit 11 can manifest as a decrease in the distance between the two sidewalls 111 compared to before the compressive stress, while still maintaining a gap, or it can manifest as the two sidewalls 111 at least partially contacting each other. The reduction in width can occur along the entire extension path of the displacement compensation slit 11, or it can occur only in a portion of the displacement compensation slit 11.

[0051] It is understandable that when the width of the displacement compensation slit 11 decreases, the second material entering the displacement compensation slit 11 can form a closer contact with the insert body 12, thereby improving the clamping and limiting effect of the sidewalls 111 on both sides of the displacement compensation slit 11 on the solidified second material (covering body), which is beneficial to improving the locking strength.

[0052] In some exemplary embodiments, the width direction of the displacement compensation slit 11 is the same as the direction of the compressive stress it bears. The term "same" as used in this application should not be construed as merely geometrically absolute parallelism without any angular deviation, but also includes substantially parallel or approximately parallel.

[0053] When the width direction of the displacement compensation slit 11 is parallel or substantially parallel to the direction of the compressive stress, the relative shrinkage displacement that needs to be compensated, corresponding to the difference in cooling shrinkage between the insert 10 and the covering body, is mainly distributed along the width direction of the displacement compensation slit 11. Therefore, the compressive stress can more effectively induce plastic deformation in at least one of the two sidewalls 111 along the width direction, and compensate for more of the relative shrinkage displacement that needs to be compensated through the width change of the displacement compensation slit 11.

[0054] In some alternative embodiments, the coefficient of thermal expansion of the first material may be greater than that of the second material. In this case, during the cooling process of the casting process, the force transmitted from the cladding to the insert body 12 is tensile stress, which can increase the width of the displacement compensation slit 11.

[0055] The extension path of the displacement compensation slit 11 can be a straight line and / or a curve. For example, the displacement compensation slit 11 with a curved extension path can include a non-closed curve, a closed curve, a circle, or an extension path formed by a combination of straight line segments and curved segments.

[0056] It should be noted that for the displacement compensation slit 11 with a curved extension path, the two sidewalls 111 corresponding to the displacement compensation slit 11 have an arc transition structure at the position where their extension direction changes, thereby avoiding stress concentration.

[0057] In some exemplary embodiments, multiple displacement compensation slits 11 are provided, and at least two of the multiple displacement compensation slits 11 have straight extension paths and different width directions to correspond to compressive stresses in different directions. Exemplarily, multiple displacement compensation slits 11 with straight extension paths can be provided on the insert body 12, and these multiple straight-line displacement compensation slits 11 can be divided into multiple slit groups according to different width directions. The width directions of the displacement compensation slits 11 in each slit group are interconnected and correspond to compressive stresses in the same direction. It is worth noting that the displacement compensation slits 11 in the same slit group may not be adjacent to each other; that is, different displacement compensation slits 11 within the slit group correspond to compressive stresses at different locations, but the direction of the compressive stresses at these different locations is the same.

[0058] In some other exemplary embodiments, at least one displacement compensation slit 11 has a curved extension path. The displacement compensation slit 11 with a curved extension path has a local width direction that varies along its extension path, thereby being able to accommodate compressive stress in different directions.

[0059] In some other exemplary embodiments, multiple displacement compensation slits 11 may be provided. Among the multiple displacement compensation slits 11, at least two types are included: displacement compensation slits 11 with straight extension paths and displacement compensation slits 11 with curved extension paths. The displacement compensation slits 11 with straight extension paths can be located in regions where the compressive stress direction is relatively consistent, while the displacement compensation slits 11 with curved extension paths can be located in regions where the compressive stress direction changes continuously or segmentally.

[0060] It is worth mentioning that displacement compensation slits with curved extension paths include at least the following two types: 1) the extension paths of each segment are all curved; 2) the extension path of at least one segment is curved, while the extension paths of other segments can be straight lines.

[0061] Multiple displacement compensation slits 11 with straight extension paths, multiple displacement compensation slits 11 with curved extension paths, and different slit groups formed by multiple displacement compensation slits 11 can be combined and set according to the magnitude, direction, and spatial distribution of compressive stress. This allows the insert body 12 to have corresponding local plastic deformation capabilities at different positions and in different directions, in order to cope with complex compressive stress states that are multi-directional, non-uniform, or whose direction changes.

[0062] For example, see Figure 4a When the mating surface 13 is subjected to forces along the first, second, and third acting directions, the displacement compensation slit 11 can be configured such that its width direction is along the first, second, and third acting directions, respectively. For example, multiple displacement compensation slits 11 can be provided, each with a straight extension path, and the width direction of each straight extension path displacement compensation slit 11 is along the first, second, and third acting directions, respectively. Alternatively, a displacement compensation slit 11 with a curved extension path can be provided, each including three segments with different width directions, the width directions of which are along the first, second, and third acting directions, respectively. Alternatively, multiple displacement compensation slits 11 can be provided, including displacement compensation slits with straight extension paths and displacement compensation slits with curved extension paths. The width direction of the displacement compensation slit with a straight extension path is along the first action direction, and the displacement compensation slit with a curved extension path includes two segments with different width directions, the width directions of which are along the second action direction and the third action direction, respectively.

[0063] It is understandable that the width of the displacement compensation slit 11 determines the deformation stroke that can be provided when the two sidewalls 111 undergo relative displacement. A larger width can provide a larger amount of deformation to compensate for a larger relative shrinkage displacement corresponding to the cooling shrinkage difference; a smaller width can meet the compensation requirements for a smaller relative shrinkage displacement and reduce the impact of opening the displacement compensation slit 11 on the continuity of the insert body 12.

[0064] In some exemplary embodiments, the displacement compensation slit 11 has at least two segments with unequal widths along its extension path.

[0065] Based on the relative displacement difference between the bonding surface 13 and the covering surface at different sections, the width of the displacement compensation slit 11 along its extension path can be determined. Sections with larger relative displacement differences can have a larger width; sections with smaller relative displacement differences can have a smaller width.

[0066] For example, as the relative displacement difference between the bonding surface 13 and the covering surface gradually increases along the extension path of the displacement compensation slit 11, the width of the displacement compensation slit 11 can gradually increase along the corresponding extension path direction. When the relative displacement difference is maintained within different ranges in different sections, the stress relief joint can be set with different widths in different sections.

[0067] In some alternative implementations, the displacement compensation slit 11 has the same width in each segment along its extension path.

[0068] See Figure 6a In some exemplary embodiments, the displacement compensation slit 11 penetrates the insert body 12 along its thickness direction. Furthermore, it should be understood that the mating surface 13 can be planar or non-planar, depending on the shape of the insert body 12.

[0069] participate Figure 2 and Figure 6a In some exemplary embodiments, the end of the displacement compensation slit 11 along its extension path is disposed inside the insert body 12, and the insert body 12 has an end wall 121 at the end, the end wall 121 being arc-shaped and smoothly transitioning to the two side walls 111 respectively.

[0070] End wall 121 is a solid surface formed at the end of the insert body 12 at the displacement compensation slit 11. End wall 121 connects the two side walls 111 and defines the end boundary of the displacement compensation slit 11. The smooth transition between end wall 121 and side walls 111 means that there are no sharp corners or obvious abrupt changes in contour between them.

[0071] For example, the end wall 121 may be a circular arc surface, an elliptical arc surface, or a composite arc surface formed by the continuous connection of multiple arc surfaces. The end wall 121 may be tangent to or substantially tangent to the two side walls 111 respectively. The fillet radius of the end wall 121 may be 0.15 mm to 1.5 mm, preferably 0.5 mm to 1.5 mm.

[0072] In some exemplary embodiments, the local slotting rate on the insert body 12 is 5% to 45%, preferably 12% to 28%. Here, the local slotting rate of the insert body 12 refers to the area ratio of the displacement compensation slots 11 within the region where the displacement compensation slots 11 are located. Specifically, all displacement compensation slots 11 within the smallest rectangular area are selected, and the ratio of the area of ​​the displacement compensation slots 11 within this rectangular area to the area of ​​the rectangular area is the local slotting rate within that area.

[0073] See Figure 6b In some exemplary embodiments, a plurality of displacement compensation slits 11 arranged in a rectangular array are provided on a local area of ​​the insert body 12. The plurality of displacement compensation slits 11 can be selected by the smallest rectangular area 20. The plurality of displacement compensation slits 11 in the rectangular array are equally spaced along the width and length directions of the rectangular array, and the displacement compensation slits of the rectangular array as a whole compensate for relative contraction displacement along the width direction of the rectangular array. The distance L1 between two adjacent displacement compensation slits 11 along the length direction is 2–20 mm, preferably 4–10 mm, and the distance L2 between two adjacent displacement compensation slits 11 along the width direction is 2–20 mm, preferably 5–12 mm.

[0074] For example, the local opening rates of the displacement compensation slits, arranged in a rectangular array along the width direction, exhibit a gradient. Specifically, the multiple displacement compensation slits are divided into a first rectangular region 21, a second rectangular region 22, and a third rectangular region 23 along the width direction of the rectangular array. The local opening rate of the first rectangular region 21 is 5%–12%, the local opening rate of the second rectangular region 22 is 12%–28%, and the local opening rate of the third rectangular region 23 is 12%–28%. For example, the ratio of the dimensions of the first rectangular region 21, the second rectangular region 22, and the third rectangular region 23 in the width direction (the dimensions of the three in the length direction are the same) is 3:4:3.

[0075] It should be noted that, Figure 6b This is only to illustrate the positional relationship between multiple displacement compensation slits and rectangular regions 20, 21, 22 and 23, and does not reflect the aforementioned proportional relationship.

[0076] In some exemplary embodiments, the extension path of the displacement compensation slit 11 is a straight line, and its length is 4–25 mm, preferably 8–14 mm, and its width is 0.5–1.5 mm, preferably 0.8–1.2 mm. See also [link to exemplary embodiments]. Figure 1 The insert body 12 has a guide portion 14 protruding from the mating surface 13. (See also...) Figure 7aThe flow guiding section 14 includes a flow guiding surface 141, which has an inlet edge connected to and located on the bonding surface 13. The flow guiding surface 141 extends obliquely upward from the inlet edge 144 along a first direction, away from the bonding surface 13. The first direction is a predetermined flow direction of the molten second material on the bonding surface 13.

[0077] Predetermined flow direction (e.g., Figure 1 The direction indicated by the middle arrow is the local extension direction of the predetermined flow path of the molten second material at a certain location on the bonding surface 13, pointing towards the downstream flow side of the second material. Specifically, when the predetermined flow path at a certain location on the bonding surface 13 is a straight line, the predetermined flow direction is the extension direction of that straight line. When the predetermined flow path at a certain location on the bonding surface 13 is a curve, the predetermined flow direction is the tangent direction of the predetermined flow path at that location, pointing towards the flow direction of the molten second material.

[0078] Along the predetermined flow direction, the protrusion height of the guide surface 141 relative to the mating surface 13 gradually increases from the inlet edge. The protrusion height of the guide surface 141 relative to the mating surface 13 at any location refers to the distance between the guide surface 141 and the mating surface 13 measured along the local thickness direction of the insert body 12 at that location. The guide surface 141 connects to the mating surface 13 at the inlet edge, so the protrusion height at the inlet edge is zero or substantially zero.

[0079] The guide surface 141 guides the molten second material to continuously flow along the guide surface 141, making the liquid flow tend towards a quasi-laminar state, thereby reducing turbulence, splashing, and air entrapment, and reducing the formation of an oxide film. In some exemplary embodiments, the guide portion 14 is located upstream of the displacement compensation slit 11 along a predetermined flow direction. The guide is located upstream of the displacement compensation slit 11, so that the molten second material maintains a relatively stable quasi-laminar state when it reaches the displacement compensation slit 11. After the stable flow of the second material (molten state) reaches the displacement compensation slit 11, it can enter the displacement compensation slit 11 relatively smoothly. This facilitates the full entry of the molten second material into the displacement compensation slit 11, and after solidification, it forms a stable mechanical lock with the insert 10.

[0080] In some exemplary embodiments, multiple flow guides 14 are provided. These multiple flow guides 14 can be respectively disposed at different flow positions of the molten second material and extend along a predetermined flow direction at their respective positions. When the predetermined flow path bends or changes direction, the extension directions of the multiple flow guides 141 can be different accordingly; that is, the multiple flow guides 141 may not be parallel to each other.

[0081] In some exemplary embodiments, the flow guide 14 has a receiving chamber 142 with an opening 143 facing the bonding surface. The receiving chamber 142 is a space formed inside the flow guide 14 capable of containing the molten second material. The opening 143 communicates with the receiving chamber 142 and is located near the bonding surface 13, allowing the second material flowing along the bonding surface 13 to enter the receiving chamber 142 through the opening 143. After entering the receiving chamber 142 and cooling and solidifying, the molten second material forms a mechanical lock with the insert 10, thereby improving the connection strength and connection stability between the cover and the insert 10.

[0082] In some exemplary embodiments, multiple flow guides 14 are integrally formed with the insert body 12. Exemplarily, in some exemplary embodiments, a portion of the insert body 12 is stamped to form a cut on one side of the portion. The connecting side of the portion, opposite the cut side, remains connected to the insert body 12, and side edges are formed on both sides of the portion between the cut side and the connecting side. When the portion is flipped up along the thickness direction of the insert body 12, the cut side and portions of the two side edges near the cut side rise relative to the mating surface 13, and the connecting side remains continuous as a connection between the portion and the insert body 12. Thus, the portion protrudes from the mating surface 13 with the connecting side as its root, forming the flow guide 14. After the portion is flipped up, an opening 143 is formed between the cut side and the insert body 12. The flipped portion defines a receiving chamber 142, and the opening 143 communicates with the receiving chamber 142.

[0083] It is understandable that, since the flow guide 14 is formed by stamping and turning up a portion of the material of the insert body 12, the side of the flow guide 14 opposite to the flow guide surface 141 is open. During the casting process, the molten second material located on both sides of the insert body 12 in the thickness direction can enter the receiving chamber 142 and converge within the receiving chamber 142. After the second material cools and solidifies, the second material within the receiving chamber 142 forms a connecting portion and connects to the covering body located on both sides of the insert body 12 in the thickness direction.

[0084] See Figure 7a and Figure 7bIn some exemplary embodiments, the length L3 of the guide portion 14 is 3–20 mm, preferably 6–12 mm, and the width L4 is 0.5–5 mm, preferably 1–3 mm. When the guide surface 141 is planar, the included angle α between the guide surface 141 and the mating surface 13 can be 10°–60°, preferably 25°–40°. The maximum protrusion height H1 of the guide portion 14 relative to the mating surface is less than the single-sided flow channel gap g (i.e., the gap between one side of the insert body 12 along its own thickness direction and the inner wall of the mold cavity), for example, H1 ≤ 0.8g. Exemplarily, the maximum protrusion height H1 can be 0.2 mm–1.2 mm, preferably 0.4 mm–0.8 mm.

[0085] In some exemplary embodiments, multiple guide sections 14 are provided, and the multiple guide sections 14 are distributed in a rectangular array. Furthermore, the distance L5 between two adjacent guide sections 14 in the length and width directions is 3 to 30 mm, preferably 6 to 15 mm.

[0086] For example, the local opening ratio of the flow guide 14 on the insert body 12 is 8% to 18%. Specifically, when multiple flow guides 14 are provided on the insert body 12, the multiple flow guides 14 are selected by the smallest rectangular area, and the ratio of the area occupied by the multiple flow guides 14 to this rectangular area is the local opening ratio.

[0087] [Functional Gradient Interface Coating] In some exemplary embodiments, the first material is steel, the second material is aluminum alloy, and a functionally graded interface coating is provided on the bonding surface. The functionally graded interface coating can promote metallurgical bonding and reduce the risk of excessive growth of brittle Fe-Al intermetallic compound layers. Specifically, the functionally graded interface coating includes, in sequence, a substrate bonding layer, a thermal expansion buffer layer, a chemical transition layer, and a wetting activation layer along the direction away from the insert body.

[0088] Functionally graded interface coatings enhance adhesion stability to the insert body through a substrate bonding layer, mitigate the difference in thermal expansion properties between the first and second materials through a thermal expansion buffer layer, improve the chemical compatibility of the steel and aluminum sides and inhibit the excessive growth of brittle intermetallic compounds through a chemical transition layer, and improve the spreading and wetting of the molten second material on the insert surface through a wetting activation layer. This improves the bonding stability between the insert and the coating, reduces the risk of cracking, peeling, or debonding at the bonding interface, and helps reduce local stress concentration near the interface.

[0089] In some exemplary embodiments, the total thickness of the functionally graded interface coating is 40–185 μm, for example, it can be 150 μm.

[0090] The thickness of the substrate bonding layer can be 5–25 μm, preferably 8–15 μm. The substrate bonding layer can be formed of Ni, Ni-Fe alloy, Fe-Ni alloy, or Fe-Ni-Co alloy.

[0091] The thickness of the thermal expansion buffer layer can be 10–40 μm, preferably 10–25 μm. The thermal expansion buffer layer can be formed of Fe-Ni alloy or Fe-Ni-Co alloy.

[0092] The thickness of the chemical transition layer can be 20–80 μm, preferably 35–60 μm. The chemical transition layer can employ a Ni-Al, Ni-Al-Zn, or Fe-Ni-Al material system. Along the direction away from the insert body, the Ni content in the chemical transition layer decreases while the Al content increases, forming a gradient structure transitioning from the steel-side composition to the aluminum-side composition. For example, the chemical transition layer uses a Ni-Al material system, wherein the Ni content gradually decreases and the Al content gradually increases along the direction away from the insert body. For instance, the content is as follows: near the insert body (Ni 70%–95%, Al 5%–30%), in the middle region (Ni 40%–70%, Al 30%–60%), and near the cladding (Ni 10%–40%, Al 60%–90%).

[0093] The thickness of the wetting and activating layer can be 5–40 μm, preferably 10–25 μm. The wetting and activating layer may include a matrix formed of Zn-Al alloy or Al-Si alloy, and fluoroaluminate activator particles with a mass percentage of 0.5%–8%, preferably 2%–5%. The activator particles may be KAlF4, K2AlF5, or CsAlF4, and the particle size may not be greater than 5 μm.

[0094] When the fluoroaluminate activator particles are heated by the molten second material, they promote the removal of the oxide film on the surface of the bonding region and improve the wetting of the functionally graded interface coating by the molten aluminum. This effect facilitates the continuous coverage of the functionally graded interface coating by the second material and promotes its entry into the receiving chambers of the displacement compensation slit and the guide section.

[0095] In one exemplary embodiment, the total thickness of the functionally graded interface coating is approximately 85 μm. Specifically, the substrate bonding layer has a thickness of approximately 10 μm; the low-expansion buffer layer has a thickness of approximately 15 μm; the chemical transition layer has a thickness of approximately 45 μm; and the wetting activation layer has a thickness of approximately 15 μm. The total thickness is allowed to have an error of ±10 μm.

[0096] [The technical effects of combining functional interface coatings and displacement compensation slits] Functionally graded interface coatings primarily improve the spreading, wetting, and interfacial bonding of the second material in the molten state with the insert, and mitigate the performance differences between steel and aluminum alloys. Displacement compensation slits provide plastic deformation space for localized areas of the insert body to compensate for at least part of the relative shrinkage displacement that needs to be compensated.

[0097] The molten second material can also enter the containment chambers of the displacement compensation slit and the guide section, and form a mechanical lock with the insert after solidification. Therefore, the functionally graded interface coating and the mechanical locking structure can improve the connection stability between the insert and the coating body from the aspects of interface bonding and structural restraint, respectively.

[0098] [Inlaid Composite Components] The second aspect of this application provides a cast composite component.

[0099] The embedded composite component includes an insert provided in the first aspect, the insert including an insert body made of a first material and an encapsulation made of a second material, wherein the encapsulation at least partially enters a displacement compensation slit disposed on the mating surface of the insert.

[0100] During the embedding process, the molten second material flows to the mating surface of the insert and at least partially enters the displacement compensation slit. After the second material cools and solidifies, it forms a cladding, and the second material located within the displacement compensation slit constitutes part of the cladding.

[0101] For example, the covering body may enter only a portion of the depth of the displacement compensation slit, or it may substantially fill the displacement compensation slit along the depth direction of the displacement compensation slit.

[0102] For example, when the displacement compensation slit penetrates the insert body along the thickness direction of the insert body, the second material can also pass through the displacement compensation slit and connect with the second material on the opposite side of the insert body.

[0103] For example, the covering may enter only a portion of the displacement compensation slit along its extension path, or it may enter the entire displacement compensation slit along its extension path.

[0104] [vehicle] The third aspect of this application also provides another vehicle that includes the insert provided in the first aspect, or includes the cast composite component provided in the second aspect.

[0105] [Insert Manufacturing Method] The fourth aspect of this application provides a method for manufacturing an insert.

[0106] The thermal expansion coefficient and plastic deformation performance parameters of a first material used to manufacture the insert body, and the thermal expansion coefficient of a second material used to form the coating, are obtained, and it is determined that the thermal expansion coefficients of the first material and the second material are different, wherein the insert body has a bonding surface for being coated by the second material in a molten state.

[0107] First, two materials with different coefficients of thermal expansion under the casting condition are selected, ensuring that the material with the smaller coefficient of thermal expansion has the ability to undergo plastic deformation during the cooling process under the casting condition. Then, the material with the smaller coefficient of thermal expansion is selected as the first material, and the material with the larger coefficient of thermal expansion is selected as the second material.

[0108] A first material is used to form the insert body, and a second material is injected into the mold cavity in a molten state during the casting process, and after cooling, forms a covering body to cover the insert body made of the first material. Thus, the insert body has a mating surface covered by the covering body, and the covering body has a covering surface connected to the mating surface.

[0109] It should be noted that the connection between the covering surface and the bonding surface means that the covering surface and the bonding surface are in direct contact and bonded, or that a coating is provided on the insert body, and the covering surface is in direct contact with the coating and connected to the bonding surface through the coating.

[0110] Based on the insert body without displacement compensation slits, the cooling shrinkage difference between the insert body and the second material, the relative shrinkage displacement that needs to be compensated, the interfacial shear force, and the forces acting on the bonding surface are determined during the cooling process.

[0111] In some exemplary embodiments, the coefficient of thermal expansion of the first material is less than that of the second material, and in this case, the force acting on the bonding surface is compressive stress.

[0112] In some alternative embodiments, the coefficient of thermal expansion of the first material is greater than that of the second material, in which case the force acting on the bonding surface is tensile stress.

[0113] An insert body without a displacement compensation slit refers to an insert body that has not yet formed a displacement compensation slit. Analyzing this insert body can reveal its initial stress and deformation requirements without a displacement compensation slit, serving as a basis for designing the displacement compensation slit.

[0114] For example, the cooling shrinkage difference, the relative shrinkage displacement that needs to be compensated, the interfacial shear force, and the forces acting on the bonding surface are all obtained through thermo-mechanical coupling analysis.

[0115] Based on the cooling shrinkage difference, the relative shrinkage displacement that needs to be compensated, the interfacial shear force, and the forces acting on the bonding surface, and constrained by the fact that the insert body after forming the displacement compensation slit meets the preset strength and preset stiffness conditions, the design parameters of the displacement compensation slit are determined. The design parameters include the number and location of the displacement compensation slits, as well as the extension path, local width direction, and width distribution along the extension path of each displacement compensation slit.

[0116] The following explanations will be based on the premise that the coefficient of thermal expansion of the first material is less than that of the second material, and that the force acting on the surface is compressive stress.

[0117] Compressive stress is the stress exerted by the covering surface on the mating surface. The relative shrinkage displacement that needs to be compensated refers to the amount of displacement that needs to occur at certain locations on the mating surface, thereby avoiding compressive stress on the mating surface, without presuming that actual relative displacement has already occurred between the insert body and the second material.

[0118] In some exemplary embodiments, a thermo-mechanical coupling analysis is first performed on a reference structure without displacement compensation slits to obtain the cooling shrinkage difference between the first and second materials, the relative shrinkage displacement requiring compensation, the interfacial shear force, and the compressive stress on the bonding surface. Based on the analysis results, the number, location, extension path, local width direction, and width distribution of the displacement compensation slits are preliminarily determined, and a thermo-mechanical coupling analysis is performed again on the structure with candidate displacement compensation slits. Based on the interfacial shear stress, compressive stress on the bonding surface, local plastic deformation, and the strength and stiffness of the insert body obtained from the analysis, at least one of the above parameters is adjusted until all analysis results meet the preset conditions.

[0119] For example, for an insert body with a thickness of 1.0 mm, a set of candidate parameters can be set: six displacement compensation slits are set in the area with high compressive stress; the extension path of each displacement compensation slit is a straight line, and the local width direction is basically parallel to the direction of compressive stress at the corresponding position; the length of each displacement compensation slit is 10 mm, the width is 0.8 mm and remains constant along the extension path; the spacing between adjacent displacement compensation slits is 6 mm.

[0120] Substituting the structure with the aforementioned candidate parameters into a thermo-mechanical coupling analysis, it is determined whether the local plastic deformation near the displacement compensation slit can compensate for the required relative shrinkage displacement, and whether the insert body meets the preset strength and stiffness conditions. If the compensation is insufficient, the number, location, and width of the displacement compensation slits can be adjusted; if the strength or stiffness of the insert body is insufficient, the number of displacement compensation slits can be reduced or the spacing between adjacent displacement compensation slits can be increased. By adjusting and analyzing the candidate parameters, the displacement compensation slit parameters that meet the design requirements are determined.

[0121] The insert body is provided, and each of the displacement compensation slits is formed on the mating surface of the insert body according to the design parameters. The insert body referred to in this step is still an insert body without displacement compensation slits.

[0122] For example, when forming a displacement compensation slit on the insert body, a fiber laser can be used to cut along a predetermined contour, or an ultrafast laser can be used to perform multiple scans or remove material layer by layer to form the displacement compensation slit.

[0123] A filling analysis is performed on the flow process of the second material in the molten state along the bonding surface to obtain a predetermined flow path of the second material on the bonding surface, a predetermined flow direction of the predetermined flow path at different locations, and flow state data.

[0124] The predetermined flow direction is the local extension direction of the predetermined flow path at the corresponding position, pointing towards the downstream flow side of the second material. When the predetermined flow path is a straight line, the predetermined flow direction is the extension direction of that straight line; when the predetermined flow path is a curve, the predetermined flow direction is the tangent direction at the corresponding position, pointing towards the flow side of the second material.

[0125] Flow state data is used to characterize the stability of the flow of the second material along the bonding surface. For example, the flow state data may include the flow direction and the location or trend of turbulence, splashing, or air entrapment. Through filling analysis, the locations where turbulence, splashing, or air entrapment may occur can be determined. Simultaneously, based on the flow direction, the upstream region of the locations on the insert body where turbulence, splashing, or air entrapment may occur can be determined.

[0126] Based on the results of the filling analysis, the location and geometric parameters of the guide section are determined. The geometric parameters include the inclination of the guide surface relative to the bonding surface and the protrusion height of the guide section relative to the bonding surface.

[0127] The guide section can be located upstream of a location where turbulence, splashing, or air entrapment may occur. The geometric parameters of the guide section include its length, width, height, and the angle between the guide surface and the mating surface.

[0128] According to the set position and the geometric parameters, the flow guide portion protruding from the bonding surface is formed on the insert body. The flow guide surface has an inlet edge located on the bonding surface, and the protrusion height of the flow guide surface relative to the bonding surface gradually increases from the inlet edge along the predetermined flow direction.

[0129] In some exemplary embodiments, the guide section is disposed upstream of the displacement compensation slit along a predetermined flow direction. The second material flows through the guide surface before reaching the displacement compensation slit, thereby maintaining a relatively stable quasi-laminar flow state for the second material upon reaching the displacement compensation slit and facilitating the entry of the second material into the displacement compensation slit.

[0130] For example, the length of the guide portion is 3 to 20 mm, preferably 6 to 12 mm, and the width is 0.5 to 5 mm, preferably 1 to 3 mm.

[0131] When the guide surface is planar, the angle between the guide surface and the mating surface can be 10° to 60°, preferably 25° to 40°. The maximum protrusion height of the guide portion relative to the mating surface can be 0.2 mm to 1.2 mm, preferably 0.4 mm to 0.8 mm.

[0132] When determining the maximum protrusion height, the predetermined installation position of the insert in the mold cavity can be combined to maintain a gap between the guide section and the cavity wall facing the guide section for the passage of the second material, so as to avoid the guide section from excessively reducing the flow cross section or blocking the cavity. For example, the minimum distance between the guide section and the cavity is 0.6mm to 2mm.

[0133] When guide sections are provided on both sides of the insert body along the thickness direction, the protrusion height of each guide section can be determined according to the cavity space on both sides, so that a gap is maintained between the guide sections on both sides and the corresponding cavity wall.

[0134] The aforementioned setup and geometric parameters were determined to guide the continuous flow of the second material adhering to the guide surface, making the liquid flow tend to a quasi-laminar state, thereby reducing turbulence, splashing, and air entrapment, and reducing the formation of oxide film.

[0135] For example, a stamping process can be used to process a portion of the insert body material. Stamping creates a notch on one side of the portion of material, while a connecting side opposite the notched side remains connected to the insert body. The connecting side is located upstream of a predetermined flow direction and forms an inlet edge on the mating surface; the notched side is located downstream of the inlet edge.

[0136] During the stamping process, the cut side of the local material and the portion of both sides closest to the cut side located between the cut side and the connecting side are turned up along the thickness direction of the insert body. The connecting side remains continuous as the connection between the local material and the insert body. Thus, the local material protrudes from the mating surface with the connecting side as its root, and integrally forms a guide section with the insert body.

[0137] The upturned local material forms a guide surface. The guide surface connects to the bonding surface at the inlet edge formed on the connecting side, and its protrusion height gradually increases from the inlet edge towards the cut side, thus conforming to the predetermined flow direction, inclination degree and protrusion height determined by the filling analysis.

[0138] After the material is partially turned up, an opening is formed between the cut side and the insert body. The turned-up material and the adjacent portion of the insert body together define a receiving chamber, and the opening communicates with the receiving chamber and is adjacent to the mating surface.

[0139] When the molten second material flows along the bonding surface, it can enter the receiving chamber through the opening under injection pressure. After the second material cools and solidifies in the receiving chamber, it can form a mechanical lock with the insert, thereby improving the connection stability between the insert and the cover.

[0140] In the embodiment where the flow guide is formed by stamping and flipping, the side of the receiving chamber opposite to the flow guide surface is open and communicates with the cavity space on the other side of the insert body in the thickness direction. Therefore, the molten second material located on both sides of the insert body in the thickness direction can enter the receiving chamber and converge within it.

[0141] After the second material cools and solidifies, the second material within the cavity forms a connecting portion. This connecting portion connects the coverings located on both sides of the insert body in the thickness direction and is constrained by both the guide portion and the insert body, thereby forming a mechanical locking structure bridging both sides of the insert body.

[0142] In embodiments where multiple flow guides are provided, multiple local materials of the insert body can be stamped according to the setting position and geometric parameters of each flow guide to form multiple flow guides integrally formed with the insert body.

[0143] In some exemplary embodiments, the method of manufacturing the insert further includes forming a functionally graded interface coating on the bonding surface. The step of forming the functional interface coating may be performed before forming the displacement compensation slit; or it may be performed after forming the displacement compensation slit and before forming the guide portion; or it may be performed after forming the guide portion.

[0144] Before forming a functionally graded interface coating on the bonding surface, the bonding surface is roughened to achieve a surface roughness Ra of 2.0–6.0 μm.

[0145] Surface roughening can be achieved through sandblasting. A roughened bonding surface increases the contact area between the substrate bonding layer and the insert body, and also improves the adhesion stability of the substrate bonding layer.

[0146] For example, the surface can be sandblasted to a surface roughness Ra of not less than 4.0 μm.

[0147] On the roughened bonding surface, a matrix bonding layer, a thermal expansion buffer layer, a chemical transition layer, and a wetting activation layer are sequentially formed in a direction away from the insert body to form a functional gradient interface coating.

[0148] The above layers can be formed by supersonic cold spraying, low-temperature dynamic spraying, plasma spraying, high-speed flame spraying, laser cladding, electroplating, chemical plating, physical vapor deposition, or a combination of the above processes.

[0149] In some preferred embodiments, a substrate bonding layer, a thermal expansion buffer layer, and a chemical transition layer are sequentially formed by ultrasonic cold spraying, and a wetting and activation layer is formed by low-temperature cold spraying or composite coating.

[0150] When forming a chemical transition layer, the feed ratio of Ni and Al in the spraying material can be gradually changed, so that the Ni content gradually decreases and the Al content gradually increases in the direction away from the insert body. This creates a continuous or segmented compositional gradient within the same chemical transition layer.

[0151] [Manufacturing method of embedded composite components] The fifth aspect of this application provides a method for manufacturing a cast composite component.

[0152] An insert is provided. The insert includes an insert body made of a first material, the insert body having a mating surface, the mating surface having a displacement compensation slit, and the insert body having two opposing sidewalls formed on both sides of the displacement compensation slit in the width direction. The first material has plastic deformation capability, and the coefficient of thermal expansion of the first material is less than the coefficient of thermal expansion of the second material.

[0153] The provided insert can be an insert that has already formed a displacement compensation slit. For example, the number, location, extension path, local width direction, and width distribution of the displacement compensation slits can be determined according to the aforementioned insert manufacturing method based on the compressive stress during cooling and the relative shrinkage displacement that needs to be compensated, and the displacement compensation slits can be formed according to the determined parameters.

[0154] The first material possesses plastic deformation capability, enabling localized areas of the insert body that form sidewalls and are adjacent to them to undergo non-fully recoverable plastic deformation during cooling. The coefficient of thermal expansion of the first material is less than that of the second material, giving the second material a greater tendency for free contraction under the same cooling conditions, thus providing a material basis for the displacement compensation slit to tend to close during cooling.

[0155] Place the insert inside the cavity of the mold.

[0156] The placement and orientation of the insert within the cavity can be determined based on the structure of the cast composite component and the area of ​​the mating surface that needs to be covered by the second material. The mating surface faces the cavity space used to form the covering, so that the molten second material can flow to the mating surface.

[0157] In some exemplary embodiments, the insert can be positioned by a positioning structure disposed within the mold to limit its movement during the second material injection process. The positioning structure should not obstruct the flow of the second material to the bonding surface and the area where the displacement compensation slit is located.

[0158] A molten second material is injected into the cavity, so that the molten second material covers the bonding surface.

[0159] After the second material enters the cavity, it flows along the cavity and reaches the mating surface, thereby forming a continuous second material region on the outer side of the mating surface. The term "second material covering the mating surface" as used herein includes the case where the second material directly contacts and covers the mating surface, as well as the case where the mating surface is coated, the second material covers the area of ​​the mating surface, and a bonding relationship is formed with the insert body through the coating.

[0160] In actual manufacturing, the molten second material can at least partially enter the displacement compensation slit. The second material can enter a portion or all of the displacement compensation slit along its extension path; within any entered portion, the second material can penetrate to a certain depth or essentially fill the corresponding portion.

[0161] When the displacement compensation slit penetrates the insert body, the molten second material can also pass through the displacement compensation slit and connect with the second material on the opposite side of the insert body. After the second material solidifies, the portion located within the displacement compensation slit can increase the bonding area between the insert and the covering body, and can form a mechanical lock.

[0162] The mold cooling system is turned on to cool the mold, so that the second material solidifies to form a coating, thereby producing the embedded composite component.

[0163] In some embodiments, since the insert body is located at the innermost part of the entire mold, its heat dissipation is relatively slow. The mold cooling system can perform localized enhanced cooling (i.e., reduce the temperature of the cooling medium in the area where the insert is located so that the temperature is lower than the temperature of the cooling medium in other areas) based on the temperature information fed back by the temperature detection element set in the mold. This reduces the cooling difference between the area where the insert is located and other areas, so that the area where the insert body is bonded to the second material and the adjacent area of ​​the second material tend to solidify synchronously.

[0164] As the second material continues to cool and solidify, a shrinkage difference arises between the insert body and the second material due to their different coefficients of thermal expansion. During this shrinkage process, a local area on the mating surface of the insert body with a displacement compensation slit can undergo plastic deformation toward the displacement compensation slit, thereby compensating for at least part of the relative shrinkage displacement that needs to be compensated for, corresponding to the shrinkage difference between the first and second materials. This reduces the constraint effect of the mating interface, lowers the risk of cracking, peeling, or debonding at the mating interface, and reduces the possibility of warping in the cast composite component.

[0165] The aforementioned plastic deformation is mainly concentrated near the displacement compensation slit, so that the overall contour and macroscopic shape of the insert body remain basically unchanged; even if the insert body undergoes slight overall deformation, the deformation can be controlled within the allowable range.

[0166] In one exemplary embodiment, the initial temperature of the insert body is 450-550°C, and the cooling flow rate of the area where the insert is located can be increased to about 1.8 times that of other areas, so that the cooling rate of the composite area reaches 18-25°C / s, and the steel-aluminum bonding area and the adjacent aluminum alloy area tend to reach the solidus temperature synchronously.

[0167] After the second material has completely solidified, open the mold, remove the embedded composite component, and cool it to room temperature. Subsequently, the embedded composite component can be trimmed, ground, and treated to remove gates, flash, and electrode contact areas formed during in-situ preheating.

[0168] In some implementations, a protective layer can also be formed on the surface of the steel-aluminum bonding area, such as by spraying an anti-corrosion coating or a sealant, to reduce the possibility of external media entering the steel-aluminum bonding interface and improve the corrosion resistance of the embedded composite component in humid, salt spray and other environments.

[0169] The insert provided in this method is prepared by the insert manufacturing method of the fourth aspect.

[0170] In some exemplary embodiments, the insert located within the cavity is preheated in situ after being placed in the cavity and before the molten second material is injected into the cavity. In-situ preheating includes contacting an electrode with the insert and passing a pulsed current through the electrode to the insert to heat it using Joule heating.

[0171] In this design, multiple insulating positioning pins are pre-placed within the cavity of the mold. For example, the multiple insulating positioning pins are located on both sides of the insert's thickness direction, so that there is a gap between the insert and the mold on both sides of the insert's thickness direction. The molten second material can then enter the gaps on both sides of the insert's thickness direction, thereby covering the mating surfaces on both sides of the insert's thickness direction.

[0172] The specific number and position of the insulating positioning pins are determined based on the specific structure of the insert and the mold. While ensuring stable support for the insert, the number of insulating positioning pins should be minimized. For example, the insulating positioning pins are made of Si3N4 ceramic material.

[0173] In-situ preheating refers to heating the insert after it has been placed in the mold cavity. This heating is performed before the injection of the molten second material, ensuring the insert is at a predetermined temperature at the start of the casting process. Ideally, the time interval between the in-situ preheating and the injection of the molten second material should be as short as possible.

[0174] For example, two electrodes can be made to contact different positions on the insert body, and a pulsed current can be passed through the insert body via the two electrodes. When the pulsed current flows through the insert body, the resistance of the insert body itself generates Joule heat, thereby raising the temperature of the insert body.

[0175] In some exemplary embodiments, the electrode contacts the insert body with a contact pressure of approximately 2 MPa, the pulse current is 5500 A to 6500 A, the energizing time is 0.9 s to 1.4 s, and the insert body is heated to 450°C to 550°C. These parameters can be adjusted according to the material, resistance, size, and target temperature of the insert body.

[0176] In-situ preheating can reduce the initial temperature difference between the insert and the molten second material, weaken the chilling effect of the insert, and maintain good fluidity of the second material. This reduces the risk of premature local solidification and cold shuts in the second material, and facilitates the second material's full coverage of the bonding surface and its entry into the displacement compensation slit and containment chamber.

[0177] In-situ preheating is performed after the insert is placed in the mold cavity and before the second material is injected. The second material can be injected immediately after preheating. Compared to prolonged preheating of the insert outside the furnace and subsequent transfer to the mold, this method shortens the contact time between the high-temperature insert and the outside air, reducing the risk of oxidation on the insert surface. Simultaneously, it reduces the exposure time of the insert's bonding surface after heating, which helps suppress the excessive growth of brittle intermetallic compound layers at the steel-aluminum interface. In-situ preheating also causes the insert to pre-expand before the second material is injected. This reduces the shrinkage difference between the insert and the cladding during subsequent cooling, lowering the relative shrinkage displacement that needs to be compensated for.

[0178] In summary, the embedded composite component and its manufacturing method provided in this application contribute to the compensation of relative shrinkage displacement, control of the flow pattern of the molten second material, improvement of the bonding interface, and control of the temperature difference between the insert and the molten second material through displacement compensation slits, flow guides, functionally graded interface coatings, and in-situ preheating. These technical features can be implemented individually or in combination. When implemented in combination, they can improve the filling and wetting quality of the second material, enhance the stability and mechanical locking strength of the bonding interface between the insert and the coating, and compensate for at least part of the relative shrinkage displacement between the first and second materials through plastic deformation of local areas of the insert body. This synergistically reduces the risk of cracking, peeling, or debonding at the bonding interface and decreases the likelihood of warping in the embedded composite component.

[0179] The foregoing description of specific exemplary embodiments of this application is for illustrative and descriptive purposes. It is not intended to be exhaustive, nor to limit the application to the precise forms disclosed; obviously, many changes and variations are possible in accordance with the foregoing teachings. The exemplary embodiments were chosen and described to explain the specific principles of this application and its practical application, thereby enabling others skilled in the art to implement and utilize various exemplary embodiments of this application, as well as their different alternatives and modifications. The scope of this application is defined by the appended claims and their equivalents.

Claims

1. An insert, characterized in that, Includes an insert body (12) made of a first material, the insert body (12) having a bonding surface (13); The insert body (12) is provided with a displacement compensation slit (11), which penetrates the mating surface (13). The displacement compensation slit (11) has two opposing sidewalls (111) on both sides along its width direction.

2. The insert according to claim 1, characterized in that, The bonding surface (13) is covered by a second material in a molten state during the embedding process, wherein the coefficient of thermal expansion of the first material is different from that of the second material; Preferably, the coefficient of thermal expansion of the first material is less than that of the second material.

3. The insert according to claim 1, characterized in that, Multiple displacement compensation slits (11) are provided, and among the multiple displacement compensation slits (11), at least one displacement compensation slit (11) with a straight extension path and a displacement compensation slit (11) with a curved extension path are included; and / or There are multiple displacement compensation slits (11), and at least two of the multiple displacement compensation slits (11) have straight extension paths and have different width directions from each other; and / or The extension path of the displacement compensation slit (11) is curved; and / or The displacement compensation slit (11) has at least two segments with unequal widths along its extension path; and / or The displacement compensation slit (11) penetrates the insert body (12) along the thickness direction; and / or The displacement compensation slit (11) is located at the end of its extension path inside the insert body (12), and the insert body (12) has an end wall (121) at the end, the end wall (121) being arc-shaped and smoothly transitioning to the two side walls (111) respectively.

4. The insert according to claim 2, characterized in that, The insert body (12) has a guide portion (14) protruding from the bonding surface (13), the guide portion (14) includes a guide surface (141), the guide surface (141) has an inlet edge (144) connected to the bonding surface (13) and located on the bonding surface (13). The guide surface (141) extends obliquely upward from the guide edge (144) along the first direction, away from the bonding surface (13).

5. The insert according to claim 4, characterized in that, Along the first direction, the guide section (14) is located before the displacement compensation slit (11); The flow guide (14) has a receiving chamber (142) having an opening (143) facing the bonding surface (13).

6. The insert according to claim 2, characterized in that, The first material is steel, and the second material is aluminum alloy; The bonding surface (13) is provided with a functional gradient interface coating, which includes, in sequence, a substrate bonding layer, a thermal expansion buffer layer, a chemical transition layer and a wetting activation layer along the direction away from the insert body.

7. The insert according to claim 2, characterized in that, The total thickness of the functionally graded interface coating is 40–185 μm; and / or The thickness of the substrate bonding layer is 5–25 μm, and it is formed of at least one of Ni, Ni-Fe alloy, Fe-Ni alloy, and Fe-Ni-Co alloy; and / or The thermal expansion buffer layer has a thickness of 10–40 μm and is formed of at least one of Fe-Ni alloy and Fe-Ni-Co alloy; and / or The thickness of the chemical transition layer is 20–80 μm, and includes at least one of the Ni-Al system, Ni-Al-Zn system, and Fe-Ni-Al system, wherein, along the direction away from the insert body, the Ni content in the chemical transition layer shows a decreasing trend, and the Al content shows an increasing trend; and / or The thickness of the wetting and activating layer is 5 to 40 μm, and includes a matrix formed of Zn-Al alloy or Al-Si alloy, and 0.5% to 8% by mass of fluoroaluminate activator particles, wherein the fluoroaluminate activator particles are selected from at least one of KAlF4, K2AlF5 and CsAlF4, and the particle size of the fluoroaluminate activator particles is not greater than 5 μm.

8. A cast composite component, characterized in that, The insert includes the insert body (12) made of a first material and an overlay made of a second material, wherein the overlay at least partially enters a displacement compensation slit (11) provided on the insert body.

9. A vehicle, characterized in that, Includes the embedded composite component as described in claim 8.

10. A method for manufacturing an insert, characterized in that, include: The thermal expansion coefficient and plastic deformation performance parameters of a first material used to manufacture the insert body, and the thermal expansion coefficient of a second material used to form the coating, are obtained, and it is determined that the thermal expansion coefficients of the first material and the second material are different, wherein the insert body has a bonding surface for being coated by the second material in a molten state; Determine the cooling shrinkage difference between the insert body and the second material during the cooling process, the relative shrinkage displacement that needs to be compensated, the interfacial shear force, and the forces acting on the bonding surface; Based on the cooling shrinkage difference, the relative shrinkage displacement requiring compensation, the interfacial shear force, and the compressive stress on the bonding surface, and constrained by the fact that the insert body after forming the displacement compensation slit meets preset strength and stiffness conditions, the design parameters of the displacement compensation slit are determined. These design parameters include the number and location of the displacement compensation slits, as well as the extension path, local width direction, and width distribution along the extension path of each displacement compensation slit; and The insert body is provided, and each of the displacement compensation slits is formed on the mating surface of the insert body according to the design parameters, wherein the displacement compensation slits penetrate the insert body along the thickness direction of the insert body.

11. The insert manufacturing method according to claim 10, characterized in that, The cooling shrinkage difference, the relative shrinkage displacement that needs to be compensated, the interfacial shear force, and the forces acting on the bonding surface are all obtained through thermo-mechanical coupling analysis.

12. The insert manufacturing method according to claim 9, characterized in that, The coefficient of thermal expansion of the first material is less than that of the second material.

13. The insert manufacturing method according to claim 10, characterized in that, Also includes: The flow process of the second material in the molten state along the bonding surface is analyzed to obtain a predetermined flow path of the second material on the bonding surface, a predetermined flow direction of the predetermined flow path at different positions, and flow state data. Based on the results of the filling analysis, the location and geometric parameters of the guide section are determined. The geometric parameters include the inclination of the guide surface relative to the bonding surface and the protrusion height of the guide section relative to the bonding surface. as well as According to the set position and the geometric parameters, the flow guide portion protruding from the bonding surface is formed on the insert body. The flow guide surface has an inlet edge located on the bonding surface, and the protrusion height of the flow guide surface relative to the bonding surface gradually increases from the inlet edge along the predetermined flow direction.

14. The insert manufacturing method according to claim 10, characterized in that, Also includes: The bonding surface is subjected to surface roughening treatment to make the surface roughness Ra of the bonding surface 2.0 to 6.0 μm; as well as On the roughened bonding surface, a matrix bonding layer, a thermal expansion buffer layer, a chemical transition layer, and a wetting activation layer are sequentially formed in a direction away from the insert body to form a functional gradient interface coating.

15. A method for manufacturing a cast composite component, characterized in that, include: An insert is provided, the insert comprising an insert body made of a first material, the insert body having a mating surface, the mating surface having a displacement compensation slit, the insert body having two opposing sidewalls formed on both sides of the displacement compensation slit in the width direction, the first material having plastic deformation capability, and the coefficient of thermal expansion of the first material being less than the coefficient of thermal expansion of the second material. Place the insert into the cavity of the mold; Molten second material is injected into the cavity, so that the molten second material covers the bonding surface; The mold cooling system is turned on to cool the mold, so that the second material solidifies to form a coating, thereby obtaining the embedded composite component.

16. The method for manufacturing the embedded composite component according to claim 14, characterized in that, The insert is prepared by the insert manufacturing method according to any one of claims 9 to 12.

17. The method for manufacturing the embedded composite component according to claim 15 or 16, characterized in that, After the insert is placed in the cavity and before the molten second material is injected into the cavity, the insert located in the cavity is preheated in situ. The in-situ preheating includes: Make the electrode contact the insert body; and A pulsed current is passed through the electrode to heat the insert using Joule heating.