An atomic-level structure and a laser method for fabricating atomic-level structures.

By forming a dielectric layer of a predetermined thickness on the substrate surface, the problem of interface separation between the response layer and the substrate under laser scanning is solved, enabling the formation of a continuous and depth-controllable modified layer, thus ensuring the stability and consistency of laser processing.

CN123105541APending Publication Date: 2026-11-17NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611618085.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Under continuous laser scanning conditions, the response layer and the substrate are prone to interface separation due to heating, resulting in inconsistent energy transfer states and making it impossible to form a continuous and depth-controllable modified layer.

Method used

By forming a dielectric layer on the substrate surface, the thickness of the dielectric layer is set to both suppress interface separation and meet the requirements for the formation of the modified layer. The lower and upper limits of the dielectric layer thickness are determined according to the constraint stiffness and laser energy density, respectively, to ensure the stability between the response layer and the substrate and the continuity of the modified layer.

Benefits of technology

Stable connection between the response layer and the substrate was achieved under continuous laser scanning, forming a continuous and depth-controllable modified layer, avoiding interface separation, ensuring consistent energy transfer state at each processing location, and obtaining a continuous atomic-level structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105541A_ABST
    Figure CN123105541A_ABST
Patent Text Reader

Abstract

This application relates to the field of materials processing technology, specifically to an atomic-level structure and a laser-based method for fabricating atomic-level structures. The method includes: forming a response layer on the surface of a substrate; determining a lower limit for the thickness of the dielectric layer based on the constraint stiffness of the dielectric layer to be formed, wherein the minimum constraint stiffness is the minimum value required to suppress interface separation between the response layer and the substrate under the condition of cumulative laser energy received at a single point on the response layer during continuous scanning; determining an upper limit for the thickness of the dielectric layer based on the laser energy density reaching the response layer after passing through the dielectric layer; forming a dielectric layer on the surface of the response layer; performing continuous laser scanning on the dielectric layer and the response layer to form a modified layer of a predetermined depth, wherein the cumulative laser energy received at a single point on the response layer is less than the damage threshold of the response layer and the damage threshold of the dielectric layer; and etching the modified layer to obtain an atomic-level structure, thereby suppressing interface separation under continuous laser scanning conditions and obtaining a continuous atomic-level structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of materials processing technology, specifically an atomic-level structure and a laser atomic-level structure processing method. Background Technology

[0002] Currently, processes for achieving atomic-scale removal typically utilize laser-induced migration of response layer components to the substrate surface to form a modified layer, followed by selective removal to obtain a structure at atomic depth. During continuous scanning processing, laser energy continuously accumulates, and the interface between the response layer and the substrate is prone to bulging, delamination, and other separations due to heating. This results in inconsistent energy transfer states at different processing locations, making it impossible to form a continuous atomic-level structure.

[0003] Therefore, how to suppress the interface separation between the response layer and the substrate under continuous laser scanning conditions, so as to form a continuous and depth-controllable modified layer, is a technical problem that needs to be solved in this field. Summary of the Invention

[0004] To address the above problems, this application provides an atomic-level structure and a laser-based method for fabricating atomic-level structures.

[0005] In a first aspect, this application provides a laser-based atomic-level structure fabrication method, comprising: forming a response layer on the surface of a substrate, the thickness of the response layer being determined based on the total amount of migratable components required for a modified layer to be formed; determining a lower limit for the thickness of the dielectric layer based on the constraint stiffness of the dielectric layer to be formed, wherein the minimum value of the constraint stiffness is the minimum value required to suppress interface separation between the response layer and the substrate under the condition that the cumulative laser energy received at a single point on the response layer during continuous scanning; determining an upper limit for the thickness of the dielectric layer based on the laser energy density reaching the response layer after passing through the dielectric layer, wherein the minimum value of the laser energy density is the minimum value required to form the modified layer; forming the dielectric layer on the surface of the response layer based on the lower limit and the upper limit; performing continuous laser scanning on the dielectric layer and the response layer to cause the migratable components to migrate to the substrate to form the modified layer of a predetermined depth, wherein the laser energy density reaching the response layer is not less than the minimum value of the laser energy density, and the cumulative laser energy received at a single point on the response layer is less than the damage threshold of the response layer and the damage threshold of the dielectric layer; removing the dielectric layer and the response layer, and etching the modified layer to obtain an atomic-level structure.

[0006] In some embodiments, forming a responsive layer on the surface of the substrate includes: determining the number of atomic layers of the modified layer based on the predetermined depth and the interatomic spacing of the substrate; obtaining the total amount of migratable components; determining the thickness of the responsive layer based on the total amount of migratable components; wherein the total amount of migratable components included in the responsive layer is not less than the total amount of migratable components; wherein the absorption ratio of the responsive layer to laser light increases with the increase of the thickness of the responsive layer; and the thickness of the responsive layer is not greater than the thickness corresponding to when the absorption ratio is equal to the thermal instability ratio, wherein the thermal instability ratio is the absorption ratio of the responsive layer when it is thermally unstable.

[0007] In some embodiments, obtaining the total amount of the migratable component and determining the thickness of the response layer based on the total amount of the migratable component includes: establishing an interface model between the response layer and the substrate; loading laser energy into the interface model to simulate the migration process of the migratable component to the substrate; based on the migration process, obtaining a correspondence between the number of modified layers formed in the substrate and the amount of migratable component entering the substrate; determining, based on the correspondence, the minimum content of migratable component required for the substrate to form a modified state that can be selectively removed; and determining the migratable component thickness based on the minimum content and the predetermined depth. Total component amount; the total amount of migratory components included in the response layer is determined based on the atomic number density of the migratory components in the response layer and the thickness of the response layer; when the total amount of migratory components included in the response layer is equal to the total amount of migratory components, the thickness of the response layer is the lower limit of the thickness of the response layer; processing experiments are conducted on response layers of different thicknesses, and the thermal instability ratio is determined based on the fact that the laser cannot form the modified layer at the interface between the response layer and the substrate when the response layer is too thick; the upper limit of the thickness of the response layer is the thickness of the response layer when the absorption ratio of the laser by the response layer is equal to the thermal instability ratio.

[0008] In some embodiments, determining the lower limit of the thickness of the dielectric layer based on the constraint stiffness of the dielectric layer to be formed includes: the constraint stiffness is the bending stiffness per unit width of the dielectric layer, the bending stiffness is positively correlated with the elastic modulus of the dielectric layer and positively correlated with the thickness of the dielectric layer; when the constraint stiffness is equal to the minimum value of the constraint stiffness, the thickness of the dielectric layer is the lower limit of the thickness.

[0009] In some embodiments, the minimum constraint stiffness is determined by: performing a continuous laser scanning comparative test on the response layer with dielectric layers of different thicknesses at multiple cumulative laser energies, and detecting whether interface separation occurs between the response layer and the substrate after each test; at the cumulative laser energy, the minimum constraint stiffness is the constraint stiffness corresponding to the minimum thickness of the dielectric layer where interface separation does not occur between the response layer and the substrate; the minimum constraint stiffness increases with the increase of the cumulative laser energy.

[0010] In some embodiments, determining the upper limit of the thickness of the dielectric layer based on the laser energy density reaching the response layer after passing through the dielectric layer includes: performing a variable energy single-point processing test on the substrate on which the response layer is formed to obtain the correspondence between the modification depth and the laser energy density reaching the response layer, and determining the minimum value of the laser energy density based on the correspondence; the laser energy density decreases as the thickness of the dielectric layer increases; when the laser energy density incident on the dielectric layer is equal to the damage threshold of the dielectric layer and the laser energy density reaching the response layer is equal to the minimum value, the thickness of the dielectric layer is the upper limit of the thickness.

[0011] In some embodiments, the continuous laser scanning of the dielectric layer and the response layer includes: determining the positional offset of the laser focus after passing through the dielectric layer based on the thickness and refractive index of the dielectric layer; correcting the focus based on the positional offset; the focus being located inside the response layer or at the interface between the response layer and the substrate; the damage threshold of the response layer and the damage threshold of the dielectric layer being the cumulative laser energy received at a single point under the same laser conditions as the continuous laser scanning, when the response layer or the dielectric layer is damaged; and performing the continuous laser scanning with a pulse overlap rate not less than a minimum overlap rate, wherein the minimum overlap rate is the minimum value of the pulse overlap rate that allows the effective modified regions of adjacent laser-acting regions to connect with each other.

[0012] In some embodiments, forming the dielectric layer on the surface of the response layer based on the lower thickness limit and the upper thickness limit includes: cleaning the surface of the substrate before forming the response layer; and forming the response layer and the dielectric layer based on electron beam evaporation, magnetron sputtering, or atomic layer deposition.

[0013] In some embodiments, etching the modified layer includes: selective etching, the etching rate ratio of the modified layer to the substrate being not less than 5:1, and the etching stopping or slowing down on the surface of the substrate when the modified layer is removed. The selective etching is at least one of wet etching, dry etching, or short-wave laser desorption.

[0014] Secondly, this application also provides an atomic-level structure, which is fabricated using the laser atomic-level structure processing method described in any of the above embodiments.

[0015] In the atomic-level structure and laser atomic-level structure processing method of this application, on the one hand, the lower limit of the thickness of the dielectric layer ensures that its constraint stiffness is not less than the minimum value of constraint stiffness required to suppress interface separation. The minimum value of constraint stiffness is determined based on the cumulative laser energy received at a single point during continuous scanning. The greater the cumulative laser energy, the greater the constraint stiffness. After the response layer expands due to heat, it must bend the dielectric layer to arch. The constraint stiffness can suppress arching, thereby controlling the interface separation caused by the continuous accumulation of energy. On the other hand, the upper limit of the thickness of the dielectric layer ensures that the laser energy density reaching the response layer through the dielectric layer is still sufficient to form the modified layer. Furthermore, the cumulative laser energy received at a single point during continuous scanning is less than the damage threshold of the response layer and the dielectric layer. The response layer and the dielectric layer remain intact throughout the scanning process. As a result, the energy transfer state at each processing position is consistent, and adjacent effective modified regions are interconnected to form a continuous modified layer with a depth corresponding to the predetermined depth, thereby obtaining a continuous atomic-level structure.

[0016] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0017] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 A schematic diagram of the process flow of a processing method provided in an embodiment of this application; Figure 2 This is a schematic diagram of the overall process of a processing method provided in an embodiment of this application; Figure 3 This is a schematic diagram of the specific process of step 01 in a processing method provided in an embodiment of this application; Figure 4 This is a schematic diagram of the specific process of step 013 in a processing method provided in an embodiment of this application; Figure 5 This is a schematic diagram of the specific process of step 03 in a processing method provided in an embodiment of this application; Figure 6 This is a schematic diagram of the specific process of step 05 in a processing method provided in an embodiment of this application; Figure 7 This is a schematic flowchart of step 07 in a processing method provided in an embodiment of this application; Figure 8This is a schematic diagram of the specific process of step 06 in a processing method provided in an embodiment of this application. Detailed Implementation

[0018] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, the specific embodiments of this application are described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.

[0019] In the description of this application, it should be understood that the terms "center", "length", "upper", "lower", "front", "rear", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0020] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0021] Please see Figure 1 and Figure 2 This application provides a laser atomic-level structure fabrication method, comprising: 01: A responsive layer is formed on the surface of the substrate, the thickness of which is determined based on the total amount of migratable components required for the modified layer to be formed; 03: Determine the lower limit of the thickness of the dielectric layer based on the constraint stiffness of the dielectric layer to be formed. The minimum value of the constraint stiffness is the minimum value required to suppress the interface separation between the response layer and the substrate under the condition that the cumulative laser energy is received at a single point on the response layer during continuous scanning. 05: The upper limit of the thickness of the dielectric layer is determined based on the laser energy density reaching the response layer after passing through the dielectric layer, and the minimum value of the laser energy density is the minimum value required to form the modified layer; 06: Based on the lower and upper thickness limits, a dielectric layer is formed on the surface of the response layer; 07: Perform continuous laser scanning on the dielectric layer and the response layer to allow the migratable components to migrate to the substrate and form a modified layer of a predetermined depth. The laser energy density reaching the response layer is not less than the minimum laser energy density, and the cumulative laser energy received at a single point on the response layer is less than the damage threshold of the response layer and the damage threshold of the dielectric layer. 09: Remove the dielectric layer and response layer, and etch the modified layer to obtain an atomic-level structure.

[0022] Specifically, in the 01 method, the substrate can be a workpiece requiring atomic-scale processing, such as a semiconductor crystal, optical crystal, or optical amorphous material. Semiconductor crystals include, but are not limited to, silicon and sapphire, while optical amorphous materials include, but are not limited to, fused silica. The response layer is a film containing migratable components, which are components capable of leaving the response layer and entering the substrate surface under laser irradiation, such as elemental metals like gold, aluminum, and chromium, or alloys or compounds containing these metals. The modified layer refers to the region formed when the composition, atomic arrangement, or chemical activity of the substrate surface changes after the migratable components enter. The modified layer responds differently to subsequent etching processes than the unmodified substrate, which is the basis for the eventual ability to remove the modified layer separately. The desired modified layer has a predetermined depth, pre-set by the processing target, typically ranging from one to tens of atomic layers. The thickness of the response layer is determined based on the total amount of migratable components required to form a modified layer of the predetermined depth. The formation of the modified layer is essentially a process of doping the substrate surface with migratory components. Insufficient doping leads to inadequate modification, making it impossible for subsequent etching to distinguish the modified layer from the substrate. Therefore, the total amount of migratory components stored in the response layer should be no less than the total amount of migratory components required to form a modified layer of the predetermined depth. In this way, the thickness of the response layer is no longer selected empirically but is determined by the processing target, ensuring that the modified layer reaches the predetermined depth while avoiding material waste and heat accumulation caused by an excessively thick response layer.

[0023] In the method of 03, the dielectric layer is a film formed on the surface of the response layer, allowing laser light to pass through and providing mechanical constraint to the response layer. Its material can be, for example, silicon oxide, aluminum oxide, magnesium fluoride, or other dielectric materials with low absorption at the processing laser wavelength. The thickness of the dielectric layer has a lower and upper limit, with each boundary corresponding to a different failure mode. The lower limit of the dielectric layer thickness is the cumulative laser energy received at a single point on the response layer during continuous laser scanning. That is, as the laser moves along the scanning path, the total laser energy received at the same location on the response layer continuously accumulates throughout the processing. The response layer expands due to heat, but is constrained by the substrate below and the dielectric layer above, limiting expansion and creating compressive stress within the response layer. When the compressive stress accumulates to a certain level, the response layer releases stress by arching upwards. At the arched point, the response layer separates from the substrate, resulting in bulging, delamination, or other interface separation. The arching of the response layer requires bending of the dielectric layer covering it. The greater the dielectric layer's resistance to bending (i.e., constraint stiffness), the greater the resistance the response layer needs to overcome to arch. When the constraint stiffness of the dielectric layer is sufficient to resist the compressive stress buckling caused by the current accumulated laser energy, interface separation is suppressed. Therefore, there exists a minimum value for the constraint stiffness. This minimum value is the minimum required to suppress interface separation between the response layer and the substrate under the condition of receiving accumulated laser energy at a single point on the response layer during continuous scanning. The lower limit of the dielectric layer thickness can be determined based on the minimum value of the constraint stiffness.

[0024] In the method of 05, regarding the upper limit of the dielectric layer thickness, the dielectric layer absorbs or reflects some laser light, and the laser energy density reaching the response layer after passing through the dielectric layer decreases as the dielectric layer thickness increases. To ensure that the laser energy density reaching the response layer is not lower than the minimum value required to form the modified layer, the thickness of the dielectric layer cannot exceed the corresponding upper limit. Thus, the lower limit of thickness ensures that the constraint capability of the dielectric layer matches the thermal accumulation intensity of continuous scanning. The greater the accumulated laser energy, the greater the minimum required constraint stiffness, and the improvement of scanning intensity and the suppression of interface separation can be satisfied simultaneously. The upper limit of thickness ensures that the dielectric layer plays a constraint role without hindering energy transfer. The thickness of the dielectric layer is bidirectionally constrained by two failure modes in opposite directions, eliminating the need for trial and error.

[0025] In methods 06 and 07, a dielectric layer is formed on the surface of the response layer. This can be achieved using film-forming processes such as electron beam evaporation, magnetron sputtering, or atomic layer deposition, ensuring the actual thickness of the dielectric layer falls between its lower and upper limits. Subsequently, continuous laser scanning is performed on the dielectric and response layers: the laser passes through the dielectric layer and acts on the response layer, causing migratable components to migrate towards the substrate under the influence of laser energy, forming a modified layer with a depth corresponding to a predetermined depth. During the scanning process, the laser energy density reaching the response layer is not less than the minimum value required to form the modified layer (i.e., the aforementioned minimum laser energy density) to ensure effective component migration at each scanned location. Simultaneously, the cumulative laser energy received at a single point on the response layer is less than the damage threshold of both the response layer and the dielectric layer. The damage threshold refers to the cumulative laser energy corresponding to irreversible damage such as ablation, cracking, or delamination of the film layer, which can be determined through damage testing under the same laser conditions as the actual processing. In this way, the response layer remains intact throughout the scanning process, the constraint effect of the dielectric layer remains effective, the laser energy transfer state at each processing position is consistent, and the modification depth is uniform; the energy state at adjacent scanning positions does not fluctuate due to interface separation, thus forming a continuous modification layer rather than an isolated lattice.

[0026] Finally, in the method of 09, due to the difference in etching rate between the modified layer and the substrate, etching stops or slows significantly at the substrate surface when the modified layer is completely removed. Therefore, the removal depth is self-limited to the depth of the modified layer, i.e., a predetermined depth, thereby obtaining an atomic-level structure on the substrate surface. An atomic-level structure refers to a surface structure with a depth of one or more atomic layers. Since the modified layer is a continuous region formed by continuous scanning, the obtained atomic-level structure is correspondingly a continuously extending linear or planar structure, thus overcoming the limitation of existing metal film-assisted laser processing methods that can only perform intermittent lattice processing.

[0027] like Figure 1 As shown, the laser atomic-level structure processing method of this application will be described in general below, taking into account the changes in the film structure during the process. Figure 1 As shown in step 1), a response layer is deposited on the surface of the substrate using magnetron sputtering with a metal target as the target material. The metal target is a target material that provides migratable components, such as a gold target or an aluminum target. The thickness of the response layer is determined based on the total amount of migratable components required to form a modified layer of a predetermined depth. Figure 1 As shown in step 2), a dielectric layer is deposited on the surface of the response layer using magnetron sputtering, with the dielectric target serving as the target material. The dielectric target is the material that provides the dielectric layer, such as a quartz target or an alumina target. The thickness of the dielectric layer is not less than the lower limit and not greater than the upper limit. Figure 1 As shown in step 3), the laser continuously scans the response layer through the dielectric layer; as... Figure 1As shown in step 4), the migratable components migrate to the substrate under laser irradiation and diffuse within the substrate surface, forming a continuous modified layer. During the scanning process, the dielectric layer always covers the surface of the response layer. The compressive stress generated by the thermal expansion of the response layer is suppressed by the constraint stiffness of the dielectric layer, and no interface separation occurs between the response layer and the substrate. The energy transfer state remains consistent at each processing location. Figure 1 As shown in step 5), after removing the dielectric layer and the response layer, the modified layer is selectively etched. The etching rate ratio of the modified layer to the substrate is not less than 5:1, and the etching stops or slows down on the substrate surface when the modified layer is completely removed. Figure 1 As shown in step 6), an atomic-level structure is finally obtained on the surface of the substrate. In a second aspect, this application also provides an atomic-level structure, which is fabricated using the laser atomic-level structure processing method of any of the above embodiments. The atomic-level structure is located on the surface of the substrate, has a depth of one or more atomic layers, and extends continuously on the surface of the substrate.

[0028] In the laser atomic-level structure processing method of this application, on the one hand, the lower limit of the thickness of the dielectric layer ensures that its constraint stiffness is not less than the minimum value of constraint stiffness required to suppress interface separation. The minimum value of constraint stiffness is determined based on the cumulative laser energy received at a single point during continuous scanning. The greater the cumulative laser energy, the greater the constraint stiffness. After the response layer expands due to heat, it must bend the dielectric layer to arch. The constraint stiffness can suppress arching, thereby controlling the interface separation caused by the continuous accumulation of energy. On the other hand, the upper limit of the thickness of the dielectric layer ensures that the laser energy density reaching the response layer through the dielectric layer is still sufficient to form the modified layer. Furthermore, the cumulative laser energy received at a single point during continuous scanning is less than the damage threshold of the response layer and the dielectric layer. The response layer and the dielectric layer remain intact throughout the scanning process. As a result, the energy transfer state at each processing position is consistent, and adjacent effective modified regions are interconnected to form a continuous modified layer with a depth corresponding to the predetermined depth, thereby obtaining a continuous atomic-level structure.

[0029] Please see Figure 1 and Figure 3 In some embodiments, a responsive layer is formed on the surface of the substrate, including: 011: Determine the number of atomic layers in the modified layer based on the predetermined depth and the atomic spacing of the substrate; 013: Obtain the total amount of migratable components, determine the thickness of the response layer based on the total amount of migratable components, the total amount of migratable components included in the response layer is not less than the total amount of migratable components, wherein the absorption ratio of the response layer to the laser increases with the increase of the thickness of the response layer, and the thickness of the response layer is not greater than the thickness corresponding to when the absorption ratio is equal to the thermal instability ratio, the thermal instability ratio is the absorption ratio of the response layer when it is thermally unstable.

[0030] Specifically, before forming the response layer on the substrate surface, the focusing method of the laser is determined, and the effective spot size can be expressed as:

[0031] in, This refers to the effective spot size after focusing. The wavelength of the laser. The numerical aperture of the focusing objective is denoted by the target linewidth. The target linewidth refers to the desired linewidth of the atomic-level structure, which is preset by the target being processed. The laser wavelength is determined by the selected laser, such as a 1030nm near-infrared femtosecond laser or a 266nm ultraviolet nanosecond laser. Since the effective spot size determines the lateral size of a single laser-acting region, once the target linewidth is determined, the effective spot size should not exceed the target linewidth. Therefore, the numerical aperture of the focusing objective can be determined according to the above formula: the shorter the laser wavelength and the larger the numerical aperture, the smaller the effective spot size, and the finer the linewidth that can be processed. Thus, the selection of the focusing objective is locked in reverse by the target linewidth and the laser wavelength, and the optical path configuration matches the target being processed, providing an optical basis for the processing accuracy of subsequent continuous scanning.

[0032] In the 011 method, for a crystal substrate, atoms are arranged in a layered periodic pattern, and the number of atomic layers N in the modified layer can be expressed as:

[0033] in, For the predetermined depth, This refers to the atomic layer spacing of the substrate along the processing crystal plane direction. Since the atomic layer spacing varies along different crystal plane directions on the same substrate, and the number of atomic layers corresponds to the same predetermined depth under different crystal plane orientations, the atomic layer spacing should be selected based on the actual crystal plane orientation being processed. For amorphous substrates, atoms are not arranged in periodic layers; therefore, the predetermined depth can be equivalently converted to the number of atomic layers using atomic number density. In this way, the macroscopic predetermined depth is converted to the number of atomic layers, allowing the processing target to be measured at the atomic scale, providing a computational basis for subsequently determining the total amount of transferable components.

[0034] Please see Figure 1 and Figure 4 In the method of 013, obtaining the total amount of transferable components and determining the thickness of the response layer based on the total amount of transferable components includes: 0131: Establish an interface model between the response layer and the substrate, load laser energy into the interface model, and simulate the migration process of the transferable components to the substrate; 0133: Based on the migration process, obtain the correspondence between the number of modified layers formed in the substrate and the amount of migratory components entering the substrate, and determine the minimum content of migratory components required for the substrate to form a modified state that can be selectively removed based on the correspondence. 0135: Determine the total amount of migratable components based on the minimum content and predetermined depth; determine the total amount of migratable components included in the response layer based on the atomic number density of migratable components in the response layer and the thickness of the response layer; 0136: When the total number of mobile components included in the response layer is equal to the total number of mobile components, the thickness of the response layer is the lower limit of the thickness of the response layer; 0137: Processing experiments were conducted on response layers of different thicknesses. The thermal instability ratio was determined based on the fact that the laser could not form a modified layer at the interface between the response layer and the substrate when the response layer was too thick. 0139: The upper limit of the thickness of the response layer is the thickness of the response layer when the absorption ratio of the laser by the response layer is equal to the thermal instability ratio.

[0035] Specifically, an interface model between the response layer and the substrate is established, for example, an interface structure between a 10nm response layer and a 10nm substrate. Laser energy is applied to the interface model to simulate the process of migratable components diffusing through the interface and into the substrate under laser irradiation. The simulated structure is analyzed to obtain the correspondence between the number of modified layers formed in the substrate and the amount of migratable components entering the substrate, i.e., the quantitative proportion by which the number of modified layers in the substrate increases with a certain increase in the amount of migratable components. Based on this correspondence, the minimum content of migratable components required to form a selectively removable modified state per unit volume of substrate is determined. Thus, the minimum content of migratable components... Thickness design can be achieved through simulation calibration rather than extensive trial-and-error processing experiments, significantly reducing the amount of testing required. Furthermore, the simulation directly uses "selective removal" as the modification criterion, ensuring the lowest possible content of migratable components. It is directly linked to the requirements of subsequent etching and removal processes.

[0036] The total amount of migratable components required to form a modified layer of a predetermined depth can be expressed as:

[0037] in, The minimum content of the migratable component refers to the minimum atomic number density of the migratable component required to achieve a selectively removable modified state per unit volume of substrate. The method for obtaining this content will be described in detail below. The predetermined depth; the method for obtaining the total amount of migrateable components will be described in detail below. The total amount of migrateable components stored in the response layer can be expressed as:

[0038] in, The atomic number density of the migratable components in the response layer. The thickness of the response layer. To ensure that the migrateable components stored in the response layer can meet the modification requirements, the lower limit of the response layer thickness should satisfy the following:

[0039] That is, when the total amount of mobile components included in the response layer equals the total amount of mobile components, the thickness of the response layer is its lower limit. On the other hand, a thicker response layer is not necessarily better: the absorption ratio of the laser by the response layer increases with the increase of the response layer thickness, which can be approximated as:

[0040] in, The absorption ratio of the laser by the response layer. The absorption coefficient of the response layer at the processing laser wavelength is given. When the response layer is too thick, a large amount of laser energy is absorbed by the response layer itself. On the one hand, insufficient energy reaches the interface between the response layer and the substrate, while the migration of migratable components occurs precisely at this interface, preventing the effective formation of the modified layer. On the other hand, the accumulated heat absorbed by the response layer causes a sharp increase in interfacial stress, leading to thermal instability of the response layer. Therefore, the thickness of the response layer should not exceed the thickness corresponding to the absorption ratio being equal to the thermal instability ratio. The thermal instability ratio is the absorption ratio of the response layer when thermal instability occurs due to laser absorption, and its acquisition method will be explained in detail below. Thus, the lower limit of the response layer thickness is determined by the modification requirements, and the upper limit is determined by thermal instability failure. The two boundaries correspond to the two failure modes of insufficient material supply and overheating instability, respectively. The thickness of the response layer is bidirectionally constrained without the need for trial and error. Therefore, the thickness of the response layer should not exceed the thickness corresponding to the absorption ratio being equal to the thermal instability ratio, i.e.: , in, The thermal instability ratio refers to the absorption ratio of the response layer when it experiences thermal instability due to laser absorption. This ratio can be determined through processing experiments on response layers of different thicknesses, with the benchmark being that if the response layer is too thick, the laser cannot form a modified layer at the interface. Considering both the lower and upper thickness limits, the thickness hr of the response layer satisfies the following:

[0041] Thus, the lower limit of the response layer thickness is determined by the modification requirements, while the upper limit is determined by the thermal instability failure of the response layer itself. The two boundaries correspond to the two failure modes of "insufficient material supply" and "overheating instability," respectively. The thickness of the response layer is bidirectionally constrained without the need for trial and error. At the same time, the constraint direction of the upper limit of the thickness directly addresses the bulging problem under continuous scanning, avoiding the exacerbation of interface separation due to excessive thickness of the response layer.

[0042] In some implementations, the constraint stiffness is the bending stiffness per unit width of the dielectric layer, which is positively correlated with the elastic modulus of the dielectric layer and also positively correlated with the thickness of the dielectric layer; when the constraint stiffness is equal to the minimum value of the constraint stiffness, the thickness of the dielectric layer is the lower limit of the thickness.

[0043] Specifically, the constraint stiffness is the bending stiffness per unit width of the dielectric layer. Bending stiffness is the ability of a thin plate to resist bending deformation. When the response layer expands due to heat, it releases compressive stress by arching upwards. This arching must bend the dielectric layer covering it; the dielectric layer's ability to resist this bending deformation is the bending stiffness. The bending stiffness per unit width can be expressed as:

[0044] in, The bending stiffness per unit width of the dielectric layer, This refers to the elastic modulus of the dielectric layer, which is the ability of the dielectric layer material to resist elastic deformation. Poisson's ratio is the ratio of the longitudinal expansion of the dielectric layer material when subjected to lateral compression. Let be the thickness of the dielectric layer. As can be seen from the above formula, the bending stiffness is positively correlated with the elastic modulus of the dielectric layer, and also positively correlated with the cube of the dielectric layer thickness. Thus, the quantitative relationship between constraint stiffness and the material and thickness of the dielectric layer is clarified, providing a physical basis for the conversion of the lower limit of thickness.

[0045] When the constraint stiffness equals the minimum constraint stiffness, the thickness of the dielectric layer is the lower limit of the thickness, i.e.:

[0046] in, The minimum value of the constraint stiffness will be determined in detail below. Thus, the lower limit of the thickness is directly calculated from the minimum value of the constraint stiffness through the quantitative relationship of bending stiffness, without the need for trial and error. Furthermore, by selecting a medium material with a higher elastic modulus (such as alumina, whose elastic modulus is higher than that of silicon oxide), the minimum value of the constraint stiffness can be met at a smaller thickness, leaving a larger range of values ​​for the upper limit of the thickness. The material selection and thickness design of the medium layer are thus interconnected.

[0047] Please see Figure 1 and Figure 5 In some implementations, the minimum value of the constraint stiffness is determined in the following manner: 031: Under multiple cumulative laser energies, a continuous laser scanning comparative experiment was conducted on the response layer with a dielectric layer of different thicknesses to detect whether interface separation occurred between the response layer and the substrate after each experiment; 033: Under the cumulative laser energy, the minimum constraint stiffness is the constraint stiffness corresponding to the minimum thickness of the dielectric layer that does not separate from the substrate; the minimum constraint stiffness increases with the increase of cumulative laser energy.

[0048] Specifically, in the 033 method, the cumulative laser energy can be adjusted by changing the laser repetition frequency (i.e., the number of pulses emitted by the laser per unit time), scanning speed (i.e., the speed at which the laser spot moves relative to the substrate), and number of scans (i.e., the number of times the laser repeatedly scans the same scanning path). A higher repetition frequency, slower scanning speed, and more scans result in more laser pulses received at the same location on the response layer, leading to a higher cumulative laser energy. The quantitative relationship between these parameters and the cumulative laser energy will be explained in detail below. At each cumulative laser energy level, samples with multiple dielectric layers of different thicknesses are prepared and continuously laser-scanned. After the experiment, the response layer is observed using an optical microscope, scanning electron microscope, atomic force microscope, or cross-sectional inspection to detect whether bulging, cracks, delamination, cavities, or other phenomena occur, thus detecting whether interface separation has occurred. In this way, through comparative experiments, a correspondence between cumulative laser energy and the occurrence of interface separation is established, providing experimental data for determining the minimum constraint stiffness.

[0049] In the 035 method, at each cumulative laser energy, the minimum constraint stiffness is the constraint stiffness corresponding to the minimum thickness of the dielectric layer that prevents interface separation between the response layer and the substrate. The principle is that during continuous laser scanning, the higher the cumulative laser energy, the more thermal cycles the response layer undergoes, the higher the peak temperature rise, and the greater the compressive stress driving bulging and delamination. Therefore, the constraint stiffness required to suppress interface separation is also greater, and the minimum constraint stiffness increases with increasing cumulative laser energy. Since the constraint stiffness monotonically increases with the thickness of the dielectric layer, there is a one-to-one correspondence between the "minimum thickness without interface separation" and the "minimum constraint stiffness." Therefore, in the comparative experimental results at each cumulative laser energy, the thinnest dielectric layer that just prevents interface separation can be selected, and this thickness can be substituted into the quantitative relationship of bending stiffness to obtain the minimum constraint stiffness corresponding to that cumulative laser energy. For cumulative laser energies between test points, interpolation can be used to determine the corresponding minimum constraint stiffness. In this way, the minimum constraint stiffness is matched to the cumulative thermal intensity of continuous scanning as needed: when the scanning intensity increases, the minimum constraint stiffness increases synchronously, and the lower limit of the dielectric layer thickness increases accordingly; conversely, when the thickness of the dielectric layer is limited by the upper limit and cannot be increased further, the cumulative laser energy can be reduced by decreasing the repetition frequency, increasing the scanning speed, or reducing the number of scans, so that the minimum constraint stiffness is reduced below the actual constraint stiffness of the dielectric layer. The cumulative laser energy, the minimum constraint stiffness, and the lower limit of thickness thus form a series data chain, and the intensity design of continuous scanning and the thickness design of the dielectric layer are mutually constrained, with no room for free trial and error.

[0050] Please see Figure 1 and Figure 6 In some embodiments, the upper limit of the thickness of the dielectric layer is determined based on the laser energy density reaching the response layer after passing through the dielectric layer, including: 051: Perform variable energy single-point processing experiments on the substrate with the formed response layer to obtain the correspondence between the modification depth and the laser energy density reaching the response layer, and determine the minimum value of the laser energy density based on the correspondence. 053: Laser energy density decreases as the thickness of the dielectric layer increases; when the laser energy density incident on the dielectric layer is equal to the damage threshold of the dielectric layer and the laser energy density reaching the response layer is equal to the minimum value, the thickness of the dielectric layer is the upper limit of the thickness.

[0051] Specifically, the material of the dielectric layer is selected based on the processing laser wavelength, the response layer material, the interface bonding state, and the predetermined focal point. Preferably, it is an optical antireflective coating material suitable for the laser wavelength, such as silicon oxide, aluminum oxide, or magnesium fluoride. The dielectric layer material should meet the following conditions: 1. Sufficient transmittance at the processing laser wavelength to ensure that laser energy can effectively reach the response layer; 2. A laser damage threshold higher than the actual processing energy to ensure that the dielectric layer is not damaged during processing; 3. Continuous coverage of the response layer to ensure that mechanical constraints are effective throughout the scanning path. This condition is not mandatory; when the dielectric layer does not cover continuously, the constraint effect is only effective within the covered area; 4. Selective removal in subsequent processes so that the dielectric layer can be removed after processing without damaging the substrate. Thus, the selection of the dielectric layer material is jointly limited by four conditions: energy transfer, self-survival, constraint effectiveness, and removability, providing a clear basis for material selection.

[0052] In the 051 method, before the dielectric layer is formed, a single-point laser processing experiment is performed directly on the substrate sample with the formed response layer. The laser energy density is gradually decreased from high to low until the response layer no longer undergoes a modification reaction. The depth of the modified layer formed at each laser energy density is measured, and a correlation curve between the modification depth and the laser energy density reaching the response layer is obtained. Based on the correlation curve, the laser energy density required to reach the response layer to form a modified layer of a predetermined depth is read, which is the minimum laser energy density. In this way, the minimum laser energy density is obtained through calibration experiments rather than trial and error estimation. Furthermore, since the dielectric layer has not yet formed on the sample during calibration, the calibration yields the actual energy requirement to reach the response layer, providing a unified energy benchmark for subsequent dielectric layer thickness design.

[0053] In the 053 method, the laser energy density reaching the response layer decreases with increasing dielectric layer thickness. Specifically, the transmittance of the dielectric layer to the laser can be expressed as:

[0054] in, The transmittance of the dielectric layer, This is the interfacial transmittance of the dielectric layer, which is the product of the transmittance corresponding to the reflection loss at the two interfaces between the dielectric layer and the dielectric layer. It is independent of the thickness of the dielectric layer. The absorption coefficient of the dielectric layer at the processing laser wavelength is given. The thickness of the dielectric layer; the laser energy density reaching the response layer can be expressed as:

[0055] in, To achieve the laser energy density reaching the response layer, The laser energy density incident on the dielectric layer is defined as follows: When the laser energy density incident on the dielectric layer equals the damage threshold of the dielectric layer, and the laser energy density reaching the response layer equals the minimum laser energy density, the thickness of the dielectric layer is the upper limit. The thicker the dielectric layer, the lower the transmittance, and the lower the laser energy density reaching the response layer. To compensate for energy loss, the laser energy density incident on the dielectric layer needs to be increased. However, the laser energy density incident on the dielectric layer cannot exceed the damage threshold of the dielectric layer; otherwise, the dielectric layer itself will be damaged. Therefore, when the dielectric layer is thickened to the point that even if the laser energy density incident on the dielectric layer reaches the damage threshold, the laser energy density reaching the response layer also drops to the minimum laser energy density, the thickness of the dielectric layer reaches the upper limit. In this way, the thickness of the dielectric layer, the incident laser energy, the damage threshold of the dielectric layer, and the predetermined depth are all locked under the same boundary conditions, and the dielectric layer provides mechanical constraint without hindering energy transfer.

[0056] Please see Figure 1 and Figure 7 In some embodiments, continuous laser scanning is performed on the dielectric layer and the response layer, including: 071: Determine the positional offset of the laser focus after passing through the dielectric layer based on the thickness and refractive index of the dielectric layer, and correct the focus based on the positional offset. The focus is located inside the response layer or at the interface between the response layer and the substrate. 073: The damage threshold of the response layer and the damage threshold of the dielectric layer are the cumulative laser energy received at a single point when the response layer or dielectric layer is damaged under the same laser conditions as continuous laser scanning. Continuous laser scanning is performed with a pulse overlap rate not less than the minimum overlap rate. The minimum overlap rate is the minimum value of the pulse overlap rate that connects the effective modified regions of adjacent laser action regions.

[0057] Specifically, in the method of 071, the laser beam is refracted when it enters the dielectric layer from air. The optical path length within the dielectric layer differs from that of air of the same physical thickness, causing the laser's focal point to shift backward after passing through the dielectric layer. Under paraxial, perpendicular incidence conditions, this positional shift can be approximated as:

[0058] in, This is the position offset. The thickness of the dielectric layer, The refractive index of the dielectric layer is the ratio of the speed of light in a vacuum to the speed of light in the dielectric layer. After correcting the focus based on the position offset, the focus is positioned either inside the response layer or at the interface between the response layer and the substrate. When the focus is at the interface, the laser energy is directly deposited at the location where the migration of the migrating components occurs, resulting in the highest migration efficiency. When the focus is inside the response layer, the energy at the interface is relatively mild, and the migrating components migrate to the substrate via thermal conduction, reducing the risk of interface separation. In actual processing, the focus position can be selected based on a trade-off between migration efficiency and the risk of interface separation. Under high numerical aperture conditions, the accuracy of the above approximate formula decreases, and the focus position and axial light intensity distribution are preferably determined through optical field simulation or layer-by-layer focus scanning experiments. In this way, the focus position is corrected in conjunction with the thickness and refractive index of the dielectric layer, ensuring that the laser energy deposition position during actual processing is consistent with the calibration experiment of 051, and the adjustment of the dielectric layer thickness does not cause a drift in the modification depth.

[0059] In the method of 073, the damage thresholds of the response layer and the dielectric layer are the cumulative laser energy received at a single point when damage occurs in either the response layer or the dielectric layer under the same laser conditions as continuous laser scanning. Specifically, under the same laser wavelength, pulse width, repetition frequency, focal position, and scanning mode as the actual processing, a laser scanning test is performed on the sample to measure the cumulative laser energy received at a single point when irreversible damage such as ablation, delamination, cracking, ablation, or delamination occurs in the response layer or the dielectric layer. This cumulative energy is used as the damage thresholds for the response layer and the dielectric layer, respectively. It should be noted that film damage has a cumulative effect: the more pulses received at the same location, the lower the cumulative laser energy required for film damage. Therefore, the damage threshold should be determined under the same conditions as continuous laser scanning, i.e., based on the number of pulses received at a single point during actual processing, rather than based on a single pulse. In this way, the damage threshold is consistent with the cumulative energy of continuous scanning, avoiding design based on the energy of a single pulse, and preventing film damage due to energy accumulation during continuous scanning. The upper limit of the scanning energy strictly corresponds to the actual working conditions.

[0060] Furthermore, continuous laser scanning is performed with a pulse overlap rate not less than the minimum overlap rate. Specifically, when using pulsed lasers for linear scanning, the equivalent number of pulses received at a single point on the response layer can be approximated as:

[0061] in, The equivalent number of pulses. The repetition frequency, The effective spot size along the scanning direction. The scanning speed is given by the pulse overlap rate along the scanning direction, which can be expressed as:

[0062] in, The pulse overlap ratio is the proportion of laser action areas of adjacent pulses that overlap spatially; the cumulative laser energy received at a single point can be approximated as:

[0063] in, To accumulate laser energy, The laser energy density absorbed by a single pulse. The minimum overlap rate is the minimum pulse overlap rate required to connect the effective modified regions of adjacent laser-acted areas. The effective modified region refers to the area actually modified within a single laser-acted area. A higher pulse overlap rate results in greater overlap of effective modified regions between adjacent pulses. When the pulse overlap rate is not less than the minimum overlap rate, the effective modified regions of adjacent pulses and adjacent scan lines connect, forming a continuous modified layer on the substrate surface. The minimum overlap rate can be determined experimentally, using the point where the effective modified regions just connect as the criterion, and gradually decreasing the pulse overlap rate during scanning experiments. Thus, the repetition frequency, scanning speed, and number of scans are related to the upper limit of scanning energy (damage threshold) and the continuity of the modified layer (minimum overlap rate) through the cumulative laser energy and pulse overlap rate, respectively: the cumulative laser energy determines whether the film survives, and the pulse overlap rate determines whether the modified regions connect. The parameter design for continuous scanning is limited by two independent constraints, thereby forming a continuous modified layer while ensuring the integrity of the film.

[0064] Please see Figure 1 and Figure 8 In some embodiments, a dielectric layer is formed on the surface of the response layer based on a lower thickness limit and an upper thickness limit, including: 061: Clean the surface of the substrate before forming the response layer; 063: The response layer and dielectric layer are formed based on electron beam evaporation, magnetron sputtering or atomic layer deposition.

[0065] Specifically, in method 061, the substrate can be soaked and cleaned using a piranha solution, a mixture of concentrated sulfuric acid and hydrogen peroxide. This solution has strong oxidizing properties, effectively removing organic contaminants from the substrate surface and forming active groups such as hydroxyl groups. After cleaning, the substrate can be rinsed with ultrapure water and dried. The principle is that the bonding strength between the response layer and the substrate directly determines the ease of interfacial separation. Residual contaminants and adsorption layers on the substrate surface weaken the bonding between the response layer and the substrate, causing bulging and delamination at the interface under relatively low compressive stress. After cleaning, the substrate surface is clean and rich in active groups, increasing the bonding strength between the response layer and the substrate, and correspondingly reducing the minimum constraint stiffness required to inhibit interfacial separation. Thus, the bonding between the response layer and the substrate is strengthened from the source, reducing the tendency for interfacial separation and allowing for a larger margin in selecting the lower limit of the dielectric layer thickness.

[0066] In the 063 method, electron beam evaporation refers to a film formation method that uses an electron beam to heat the film material in a high vacuum environment, causing it to evaporate and deposit on the substrate surface. It has a fast film formation rate and is suitable for preparing metal response layers such as gold and aluminum. Magnetron sputtering refers to a film formation method that uses plasma to bombard a target, causing target atoms to sputter and deposit on the substrate surface. It produces dense films with high bonding strength and is suitable for preparing metal response layers and dielectric layers such as silicon oxide and magnesium fluoride. Atomic layer deposition (ALD) refers to a film formation method that uses alternating introduction of precursors to grow the film material layer by layer in units of single atomic layers. It allows for thickness control precision down to the single atomic layer and is suitable for preparing dielectric layers such as alumina. Since the thickness of both the response layer and the dielectric layer is on the nanometer scale and has clearly defined upper and lower thickness limits, the thickness control precision of the film formation method should meet the requirements of the thickness window. The dielectric layer formation method should also ensure that the dielectric layer densely and continuously covers the response layer, avoiding defects such as pinholes that could lead to constraint failure. In this way, the film formation method is matched with the thickness window constraint, ensuring that the actual thickness of the response layer and the dielectric layer falls within the design range, the dielectric layer continuously and densely covers the response layer, and the constraint effect is effective along the entire processing area.

[0067] In some embodiments, the etching is selective etching, and the etching rate ratio of the modified layer to the substrate is not less than 5:1. When the modified layer is removed, the etching on the surface of the substrate stops or slows down. The selective etching is at least one of wet etching, dry etching, or short-wave laser desorption.

[0068] Specifically, selective etching refers to an etching method that utilizes the difference in response between the modified layer and the substrate to the etching process, allowing the etching rate of the modified layer to be significantly higher than that of the substrate. The principle is as follows: after migratable components enter the substrate surface, the chemical activity or defect density of the modified layer is higher than that of the unmodified substrate, thus it is removed more quickly under the same etching conditions. When the etching rate ratio is not less than 5:1, the substrate loss at the moment the modified layer is completely removed does not exceed one-fifth of the modified layer depth. Therefore, the removal depth is limited to the depth of the modified layer, i.e., the predetermined depth, thereby obtaining a structure with atomic-scale precision. The higher the etching rate ratio, the smaller the substrate loss and the higher the depth precision of the structure. When the modified layer is completely removed, the etching stops or slows down on the substrate surface; that is, the etching process has a self-stopping characteristic, eliminating the need for precise control of the etching time. Thus, the final structure depth is limited by the depth of the modified layer, not by the etching time. The precision of depth control is guaranteed by the laser modification stage, and the etching stage does not introduce additional depth errors.

[0069] Furthermore, selective etching includes at least one of wet etching, dry etching, or short-wavelength laser desorption. Wet etching involves immersing the sample in an etching solution, utilizing the difference in dissolution rates between the modified layer and the substrate in the solution for removal. Examples include hydrofluoric acid solution and aqua regia. This method is simple to implement and offers good selectivity. Dry etching utilizes plasma or reactive gases to interact with the modified layer physically or chemically for removal. This method offers good directionality and is suitable for fine structures. Short-wavelength laser desorption utilizes the difference in response thresholds between the modified layer and the substrate to short-wavelength lasers. Laser energy higher than the response threshold of the modified layer but lower than the response threshold of the substrate is used to desorb and remove the modified layer. This is a non-contact removal method. In practical applications, one or a combination of these methods can be selected based on the substrate material, the properties of the modified layer, and the required structural precision. In addition, before etching the modified layer, the dielectric layer and the response layer also need to be removed. These can be removed sequentially or simultaneously using wet etching, dry etching, or physical friction, depending on the differences in the physicochemical properties of the dielectric layer, the response layer, and the substrate. In this way, the removal processes of the dielectric layer, the response layer, and the modification layer are independent of each other but sequentially connected, ultimately leaving only the atomic-level structure of the substrate and its surface.

[0070] The following are two examples.

[0071] Example 1

[0072] Substrate cleaning. An 8×8mm sapphire single wafer (c-side) was selected as the substrate, immersed in piranha solution for 30 minutes, rinsed with ultrapure water and dried with nitrogen to enhance the bonding strength between the subsequently formed response layer and the substrate.

[0073] Determine the thickness of the response layer. Predetermine depth. Set to 1.0 nm; atomic spacing of the sapphire c-plane Approximately 0.22 nm, atomic number of the modified layer Approximately 5. Using gold as the migratable component, the minimum content of the migratable component was determined through molecular dynamics simulations. In, the atomic number density of gold Approximately 5.9 × 10 22 When the total amount of mobile components included in the response layer equals the total amount of mobile components, the lower limit of the response layer thickness is approximately 4 nm; the absorption coefficient of gold at a wavelength of 1030 nm... The thermal instability ratio was determined through processing tests with different film thicknesses. Subsequently, the thickness corresponding to the absorption ratio being equal to the thermal instability ratio is approximately 20 nm. The thickness hr of the response layer is set to 5 nm, falling between the lower and upper thickness limits.

[0074] The thickness of the dielectric layer was determined and a film was formed. Silicon oxide was selected as the dielectric layer. Through continuous laser scanning comparative experiments, the minimum constraint stiffness corresponding to the minimum thickness of the dielectric layer that prevents interfacial separation between the response layer and the substrate at the proposed cumulative laser energy was determined. Substituting this into the bending stiffness relationship, the lower limit of the dielectric layer thickness was calculated to be approximately 30 nm. Through variable energy single-point processing experiments, the correspondence between the modification depth and the laser energy density reaching the response layer was obtained. The minimum laser energy density corresponds to a predetermined depth of 1.0 nm. When the laser energy density incident on the dielectric layer equals the damage threshold of the dielectric layer, the thickness of the dielectric layer corresponding to the minimum laser energy density reaching the response layer is approximately 80 nm, i.e., the upper limit of the thickness. The thickness of the dielectric layer was selected. The thickness is 50nm, which falls between the lower and upper limits of the thickness. A 5nm gold response layer and a 50nm silicon oxide dielectric layer are formed sequentially using electron beam evaporation.

[0075] Continuous laser scanning was employed. A femtosecond laser with a wavelength of 1030 nm, a pulse width of 250 fs, and a repetition rate of 1 MHz was used, focused by an objective lens with a numerical aperture of 0.45, resulting in an effective spot size D of approximately 2.8 μm. The refractive index of silicon oxide at 1030 nm was also measured. Approximately 1.45, position offset The focal length is approximately 15nm, and the focus is adjusted accordingly to position the focal point at the interface between the response layer and the substrate. The scan speed is 1mm / s, and the equivalent number of pulses... Approximately 2800, pulse overlap rate The effective modified regions of adjacent laser-acting regions are interconnected, with the laser energy density reaching the response layer not less than the minimum laser energy density. The cumulative laser energy received at a single point on the response layer is less than the damage threshold of gold and the damage threshold of silicon oxide. No bulging or delamination occurs in the response layer throughout the scanning process, and no cracking, ablation, or delamination occurs in the dielectric layer. A continuous modified layer is formed on the surface of the substrate.

[0076] Removal and Detection. The processed sample was successively immersed in dilute hydrofluoric acid and aqua regia to remove the silicon oxide dielectric layer and the gold response layer. Then, utilizing the difference in response thresholds between the modified layer and the substrate to short-wavelength lasers, a 248nm excimer laser was used to selectively desorb and remove the modified layer, with an etching (desorption) rate ratio greater than 5:1. Atomic force microscopy measurements showed that the processed area formed a continuous linear structure with an average depth of approximately 1.0nm, consistent with the predetermined depth.

[0077] Example 2

[0078] Substrate cleaning. A 5×5mm fused silica polishing disc was selected as the substrate and ultrasonically cleaned sequentially with acetone, anhydrous ethanol, and ultrapure water, followed by nitrogen drying.

[0079] Determine the thickness of the response layer. Predetermine depth. The depth was set at 2.0 nm; fused silica was used as the amorphous substrate, and atomic number density was used to convert the predetermined depth into the equivalent number of atomic layers. Aluminum was used as the migratable component, and the minimum content was calibrated by molecular dynamics simulation. Subsequently, the lower limit of the response layer thickness was approximately 8 nm; after determining the thermal instability ratio through processing experiments with different film thicknesses, the upper limit of the response layer thickness was approximately 25 nm. The thickness of the aluminum response layer was set at 10 nm.

[0080] The thickness of the dielectric layer was determined and a film was formed. Silicon oxide was selected as the dielectric layer. A continuous laser scanning comparative experiment determined the lower limit of the dielectric layer thickness to be approximately 20 nm; a variable energy single-point processing experiment determined the minimum laser energy density, and the upper limit of the thickness was determined to be approximately 60 nm based on the damage threshold of the dielectric layer. The thickness of the silicon oxide dielectric layer was chosen to be 40 nm. A 10 nm aluminum response layer and a 40 nm silicon oxide dielectric layer were sequentially formed using magnetron sputtering.

[0081] Continuous laser scanning. A 266nm nanosecond laser is used, focused through an objective lens with a numerical aperture of 0.2. The refractive index of silicon oxide at 266nm. Approximately 1.50, position offset The focal length is approximately 13 nm. Based on this, the focus is adjusted so that the focal point is located at the interface between the response layer and the substrate (Note: The depth of focus of this objective lens is approximately 6.6 μm, and the correction for the positional offset is within the depth of focus range; the focal point being located at the interface was verified by calibration tests). A continuous laser scan is performed along a preset path using a displacement stage. The pulse overlap rate is not less than the minimum overlap rate, and the cumulative laser energy received at a single point on the response layer is less than the damage threshold of aluminum and silicon oxide, thus forming a continuous modified layer on the substrate surface.

[0082] Removal and Detection. The processed sample was first immersed in dilute hydrofluoric acid to remove the silicon oxide dielectric layer, and then immersed in dilute hydrochloric acid to remove the aluminum response layer (aluminum is soluble in dilute hydrochloric acid, and the removal process and materials are well-matched). Taking advantage of the difference in etching rates between the aluminum-doped modified layer and fused silica in dilute hydrofluoric acid (the etching rate ratio was not less than 5:1), the modified layer was selectively etched using a wet method. Atomic force microscopy measurements revealed a continuous planar structure with an average depth of approximately 2.0 nm, consistent with the predetermined depth.

[0083] The technical features of the above-described embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as the combination of these technical features does not contradict each other, it should be considered within the scope of this specification. Furthermore, other embodiments can be derived from the above embodiments, allowing for structural and logical substitutions and changes without departing from the scope of this disclosure.

[0084] The embodiments described above are merely illustrative of several implementations of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Therefore, the scope of protection of this patent application should be determined by the appended claims.

Claims

1. A method of laser atomic structure processing, characterized by, include: A responsive layer is formed on the surface of a substrate, the thickness of which is determined based on the total amount of migratable components required for the modified layer to be formed; The lower limit of the thickness of the dielectric layer is determined based on the constraint stiffness of the dielectric layer to be formed. The minimum value of the constraint stiffness is the minimum value required to suppress the interface separation between the response layer and the substrate under the condition of the cumulative laser energy received at a single point on the response layer during continuous scanning. The upper limit of the thickness of the dielectric layer is determined based on the laser energy density reaching the response layer after passing through the dielectric layer, and the minimum value of the laser energy density is the minimum value required to form the modified layer; Based on the lower thickness limit and the upper thickness limit, the dielectric layer is formed on the surface of the response layer; Continuous laser scanning is performed on the dielectric layer and the response layer to allow the migratable components to migrate toward the substrate and form the modified layer at a predetermined depth, wherein the laser energy density reaching the response layer is not less than the minimum value of the laser energy density, and the cumulative laser energy received at a single point on the response layer is less than the damage threshold of the response layer and the damage threshold of the dielectric layer. and The dielectric layer and the response layer are removed, and the modified layer is etched to obtain an atomic-level structure.

2. The method of claim 1, wherein The formation of a responsive layer on the surface of the substrate includes: Based on the predetermined depth and the atomic spacing of the substrate, the number of atomic layers of the modified layer is determined; and The total amount of the migratable components is obtained, and the thickness of the response layer is determined based on the total amount of the migratable components. The total amount of migratable components included in the response layer is not less than the total amount of the migratable components. The absorption ratio of the response layer to the laser increases with the increase of the thickness of the response layer. The thickness of the response layer is not greater than the thickness corresponding to when the absorption ratio is equal to the thermal instability ratio. The thermal instability ratio is the absorption ratio of the response layer when it is thermally unstable.

3. The method of claim 2, wherein the laser atomically structured material processing is performed by a laser beam having a wavelength of 10 nm or less. The step of obtaining the total amount of the migratable components and determining the thickness of the response layer based on the total amount of the migratable components includes: An interface model between the response layer and the substrate is established, and laser energy is loaded into the interface model to simulate the migration process of the migratable components to the substrate. Based on the migration process, a correspondence is obtained between the number of modified layers formed in the substrate and the amount of migratory components entering the substrate, and based on the correspondence, the minimum content of migratory components required to form a modified state in the substrate that can be selectively removed is determined. The total amount of the migratable component is determined based on the minimum content and the predetermined depth; the total amount of the migratable component included in the response layer is determined based on the atomic number density of the migratable component in the response layer and the thickness of the response layer; When the total amount of mobile components included in the response layer is equal to the total amount of mobile components, the thickness of the response layer is the lower limit of the thickness of the response layer; Processing experiments were conducted on the response layers of different thicknesses. The thermal instability ratio was determined based on the condition that if the response layer was too thick, the laser could not form the modified layer at the interface between the response layer and the substrate. The upper limit of the thickness of the response layer is the thickness of the response layer when the absorption ratio of the laser by the response layer is equal to the thermal instability ratio.

4. The method of claim 1, wherein, The constraint stiffness is the bending stiffness per unit width of the dielectric layer. The bending stiffness is positively correlated with the elastic modulus of the dielectric layer and also positively correlated with the thickness of the dielectric layer. When the constraint stiffness is equal to the minimum value of the constraint stiffness, the thickness of the dielectric layer is the lower limit of the thickness.

5. The method of claim 1, wherein the laser atomically structured material processing is performed by a laser beam having a wavelength of 10 nm or less. The minimum value of the constraint stiffness is determined in the following way: Under multiple cumulative laser energies, the response layer is subjected to continuous laser scanning comparative tests with dielectric layers of different thicknesses to detect whether interface separation occurs between the response layer and the substrate after each test; and At the accumulated laser energy, the minimum value of the constraint stiffness is the constraint stiffness corresponding to the minimum thickness of the dielectric layer at which no interface separation occurs between the response layer and the substrate; the minimum value of the constraint stiffness increases with the increase of the accumulated laser energy.

6. The method of claim 1, wherein, Determining the upper limit of the thickness of the dielectric layer based on the laser energy density reaching the response layer after passing through the dielectric layer includes: A variable-energy single-point processing experiment was performed on the substrate with the formed response layer to obtain the correspondence between the modification depth and the laser energy density reaching the response layer. Based on the correspondence, the minimum value of the laser energy density was determined; and The laser energy density decreases as the thickness of the dielectric layer increases; when the laser energy density incident on the dielectric layer is equal to the damage threshold of the dielectric layer and the laser energy density reaching the response layer is equal to the minimum value, the thickness of the dielectric layer is the upper limit of the thickness.

7. The method of claim 1, wherein The continuous laser scanning of the dielectric layer and the response layer includes: The positional offset of the laser focus after passing through the dielectric layer is determined based on the thickness and refractive index of the dielectric layer; the focus is corrected based on the positional offset; the focus is located inside the response layer or at the interface between the response layer and the substrate; and The damage threshold of the response layer and the damage threshold of the dielectric layer are the cumulative laser energy received at a single point when the response layer or the dielectric layer is damaged under the same laser conditions as the continuous laser scanning. The continuous laser scanning is performed with a pulse overlap rate not less than the minimum overlap rate, where the minimum overlap rate is the minimum value of the pulse overlap rate that allows the effective modified regions of adjacent laser action regions to connect with each other.

8. The method of claim 1, wherein, The process of forming the dielectric layer on the surface of the response layer based on the lower thickness limit and the upper thickness limit includes: Before forming the response layer, the surface of the substrate is cleaned; and The response layer and the dielectric layer are formed by electron beam evaporation, magnetron sputtering or atomic layer deposition.

9. The method of claim 1, wherein, The etching is selective etching, and the etching rate ratio of the modified layer to the substrate is not less than 5:

1. When the modified layer is removed, the etching stops or slows down on the surface of the substrate. The selective etching is at least one of wet etching, dry etching, or short-wave laser desorption.

10. An atomic structure, characterized in that, The atomic structure is made by the laser atomic structure processing method of any one of claims 1 to 9. The atomic structure is made by the laser atomic structure processing method of any one of claims 1 to 9.