A method for simultaneously producing ammonium-based and iron-based ferric phosphate, ferric phosphate and its applications

By simultaneously producing iron phosphate using both ammonium and iron methods, the problem that existing iron phosphate production processes cannot meet the demands of high-end LiFePO4 cathode materials has been solved. This approach improves high compaction performance and raw material adaptability while reducing costs and energy consumption.

CN123105579APending Publication Date: 2026-11-17TIANJIN GUOAN MGL NEW MATERIALS TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611538184.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing iron phosphate production process is difficult to flexibly meet the diversified needs of high-end, high-pressure LiFePO4 cathode materials, and has problems such as inconsistent raw material sources, unstable product performance, high investment costs and high energy consumption.

Method used

A method for simultaneously producing ammonium-based and iron-based ferric phosphate is adopted. Through steps such as iron dissolution reaction, pH adjustment, aging crystallization, and oxidative dehydration, the co-production of iron-based and ammonium-based ferric phosphate is achieved, avoiding the use of oxidants, reducing energy consumption, and recovering the high-value byproduct ammonium sulfate.

Benefits of technology

The co-production of iron phosphate and ammonium phosphate by iron-based and ammonium-based methods has been achieved, ensuring the consistency of raw materials and the stability of products, reducing investment costs and energy consumption, and improving high-compaction performance and raw material adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105579A_ABST
    Figure CN123105579A_ABST
Patent Text Reader

Abstract

This invention provides a method for simultaneously producing ammonium-based and iron-based ferric phosphate, ferric phosphate, and its applications. The method includes: (1) dissolving an iron source in an acidic solution containing at least phosphoric acid to obtain a ferrous dihydrogen phosphate solution; (2) adjusting the pH of the ferrous dihydrogen phosphate solution obtained in step (1) and aging it to obtain a first ferrous phosphate octahydrate filter cake and an ammonium dihydrogen phosphate filtrate; (3) oxidizing and dehydrating the first ferrous phosphate octahydrate filter cake obtained in step (2) to obtain ferric phosphate prepared by the iron method; (4) mixing the ammonium dihydrogen phosphate filtrate obtained in step (2) and an iron salt solution, reacting to obtain a second ferrous phosphate octahydrate filter cake and an ammonium sulfate filtrate, and recovering the ammonium sulfate filtrate to obtain ammonium sulfate; (5) oxidizing and dehydrating the second ferrous phosphate octahydrate filter cake obtained in step (4) to obtain ferric phosphate prepared by the ammonium method. The method provided by this invention takes into account multiple requirements such as high compaction performance, raw material adaptability, and production line economy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of battery cathode material preparation, and relates to a method for simultaneously producing ammonium-based iron phosphate and iron-based iron phosphate, iron phosphate and its applications. Background Technology

[0002] Lithium iron phosphate (LiFePO4, LFP) or lithium manganese iron phosphate (LMFP) are widely used in new energy vehicles and energy storage fields as cathode materials for lithium-ion batteries due to their advantages such as long cycle life, good safety performance, and relatively low cost. Iron phosphate (FePO4), as the main precursor for the synthesis of LiFePO4, can also be used as the main precursor for lithium manganese iron phosphate. Its physicochemical properties (such as particle size, morphology, specific surface area, and iron-phosphorus ratio) have a decisive influence on the electrochemical performance and processing performance of the final cathode material, especially its compaction density.

[0003] With the market's continuous increase in demand for battery volumetric energy density, improving the powder compaction density of LiFePO4 cathode materials has become one of the core directions of current technological development. Currently, the industry has widely begun shipping fourth-generation high-compaction LiFePO4 products (powder compaction density ≥ 2.6 g / cm³). 3 As a mass production target, existing improvement methods include blending iron phosphate raw materials obtained by different processes in a specific ratio, and using the gradation effect of particles of different sizes to increase the compaction density of LiFePO4.

[0004] However, the production processes of different iron phosphate manufacturers are often relatively simple, and they usually need to purchase iron phosphate raw materials from different suppliers with different processes for blending. This has an adverse impact on the consistency of raw material sources and the stability control of the final product performance. In particular, for LiFePO4 material manufacturers aiming to achieve integrated production, they not only face huge upfront investment costs, but also need to have complex technical reserves.

[0005] The current production processes for iron phosphate mainly include two routes: the iron method and the ammonium method. Both have significant limitations. The iron method involves processes such as iron dissolution and oxidation. Its drawbacks are: (1) The oxidant (such as H2O2) used in the oxidation process constitutes a major hazard source and must be constructed according to explosion-proof standards, resulting in huge upfront investment pressure; (2) Since mass production, the process has almost stagnated, and the particle size control capability of the product is insufficient, making it difficult to meet the needs of high-pressure compaction applications. The ammonium method has a relatively longer process flow, involving processes such as dissolution, oxidation, multiple filtration and washing, and acid adjustment and aging. Its drawbacks are: (1) The iron source used is an industrial by-product, and its source is constrained by upstream capacity. The procurement cost has increased significantly, and the supply is difficult to increase in sync with the expansion of iron phosphate production; (2) The product obtained by this process has high activity, which is beneficial for crystal reconstruction in the subsequent synthesis process, but it is difficult to prepare the small particle size raw materials required for high-pressure compaction, and the overall water and energy consumption is higher.

[0006] In summary, the existing processes and production lines for producing iron phosphate are insufficient to flexibly meet the diversified market demand for high-end, high-compaction LiFePO4 products. There is an urgent need to develop a new iron phosphate preparation process that can take into account high-compaction performance, raw material adaptability, and production line economy. Summary of the Invention

[0007] To address the shortcomings of existing technologies, the present invention aims to provide a method for simultaneously producing ammonium-processed ferric phosphate and ferric-processed ferric phosphate, as well as ferric phosphate and its applications. The method provided by this invention eliminates the traditional process requiring additional oxidation agents and other oxidation steps, and can simultaneously produce ammonium-processed and ferric-processed ferric phosphate. This ensures consistency in raw material sources and stable control over the performance of the final product, while also yielding the high-value byproduct ammonium sulfate, thus satisfying multiple requirements for high-compaction performance, raw material adaptability, and production line economics.

[0008] To achieve this objective, the present invention adopts the following technical solution:

[0009] In a first aspect, the present invention provides a method for simultaneously producing ammonium-processed ferric phosphate and iron-processed ferric phosphate, the method comprising the following steps:

[0010] (1) The iron source is subjected to an iron dissolution reaction using an acid solution containing at least phosphoric acid to obtain a ferrous dihydrogen phosphate solution;

[0011] (2) The ferrous dihydrogen phosphate solution described in step (1) is adjusted for pH and aged to obtain ferrous phosphate filter cake octahydrate and ammonium dihydrogen phosphate filtrate.

[0012] (3) The first ferrous phosphate filter cake in step (2) is oxidized and dehydrated to obtain ferric phosphate prepared by the iron method;

[0013] (4) Mix the ammonium dihydrogen phosphate filtrate and iron salt solution from step (2) and react to obtain ferrous phosphate octahydrate filter cake and ammonium sulfate filtrate. The ammonium sulfate filtrate is recovered to obtain ammonium sulfate.

[0014] (5) The second ferrous phosphate filter cake from step (4) is oxidized and dehydrated to obtain ferric phosphate prepared by the ammonium method.

[0015] In one embodiment of the present invention, the iron dissolving reaction in step (1) is carried out under a protective atmosphere.

[0016] In one embodiment of the present invention, the iron source in step (1) includes elemental iron and / or divalent iron.

[0017] In one embodiment of the present invention, the mixed gas obtained after the iron dissolution reaction in step (1) is recovered by absorption-spraying to obtain an acid solution, which is then reused in the iron dissolution reaction preparation process, and the remaining gas after recovery is discharged as tail gas; or, the mixed gas obtained after the iron dissolution reaction in step (1) is recovered by absorption-spraying to obtain an acid solution, which is then reused in the iron dissolution reaction preparation process, and the remaining gas after recovery is recycled and reused.

[0018] In one embodiment of the present invention, in step (2), an ammonia solution is added to adjust the pH value.

[0019] In one embodiment of the present invention, in step (2), the pH value is adjusted to 4.5~6.5.

[0020] In one embodiment of the present invention, the aging temperature in step (2) is 40℃~50℃, and the aging time in step (2) is 2h~6h.

[0021] In one embodiment of the present invention, after aging in step (2), a first ferrous phosphate octahydrate slurry is obtained. The first ferrous phosphate octahydrate slurry is then filtered under a protective atmosphere to obtain a first ferrous phosphate octahydrate filter cake and an ammonium dihydrogen phosphate filtrate.

[0022] In one embodiment of the present invention, in step (3), the first ferrous phosphate filter cake octahydrate is first dried at low temperature and then oxidized and dehydrated. The temperature of the low-temperature drying is ≤60℃.

[0023] In one embodiment of the present invention, in step (3), the method of oxidation dehydration includes flash cyclone separation drying, and the drying temperature of the flash cyclone separation drying method is 250℃~350℃.

[0024] In one embodiment of the present invention, the reaction in step (4) includes: adding an ammonia solution to adjust the pH value to 4.5~6.5 for aging and crystallization.

[0025] In one embodiment of the present invention, the temperature of the reaction in step (4) is 40℃~50℃, and the reaction time of the reaction in step (4) is 2h~6h.

[0026] In one embodiment of the present invention, after the reaction described in step (4), a second ferrous phosphate octahydrate slurry is obtained. The second ferrous phosphate octahydrate slurry is then filtered under a protective atmosphere to obtain a second ferrous phosphate octahydrate filter cake and an ammonium sulfate filtrate.

[0027] In one embodiment of the present invention, in step (5), the second ferrous phosphate filter cake is first dried at low temperature and then oxidized and dehydrated. The temperature of the low-temperature drying is ≤60℃.

[0028] In one embodiment of the present invention, in step (5), the method of oxidation dehydration includes flash cyclone separation drying, and the drying temperature of the flash cyclone separation drying method is 250℃~350℃.

[0029] In a second aspect, the present invention provides an iron phosphate, which is prepared by the method described in the first aspect.

[0030] Thirdly, the present invention provides a cathode material, wherein the raw materials for preparing the cathode material include iron phosphate as described in the second aspect, and the cathode material includes lithium iron phosphate cathode material and / or lithium manganese iron phosphate cathode material.

[0031] Fourthly, the present invention also provides a battery comprising the positive electrode material described in the third aspect.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] This invention provides a method for simultaneously producing ammonium-processed ferric phosphate and iron-processed ferric phosphate, achieving co-production of these two processes. During the production process, neither the iron-process nor the ammonium-process requires the introduction of additional oxidants (such as hydrogen peroxide), avoiding the storage and use of oxidants and thus eliminating the use of major hazardous sources, significantly reducing investment costs. Furthermore, the method of this invention does not require excessively high temperatures in the aging and crystallization process, the reaction process, or the subsequent oxidation and dehydration stages, significantly reducing energy consumption. Due to the lower oxidation and dehydration temperature, expensive kilns are no longer required. In addition, this invention yields a high-value byproduct, ammonium sulfate, during the production process, which can offset costs. This results in the final iron-processed and ammonium-processed ferric phosphate products exhibiting raw material consistency and high product stability. Attached Figure Description

[0034] Figure 1 This is a schematic diagram of the process flow for the method of simultaneously producing ammonium-based ferric phosphate and iron-based ferric phosphate, as provided in Embodiment 4 of the present invention.

[0035] Figure 2 This is a schematic diagram of the process flow for the conventional iron method for preparing iron phosphate, as provided in Comparative Example 1 of the present invention.

[0036] Figure 3 This is a schematic diagram of the process flow for the conventional ammonium method for preparing iron phosphate, provided in Comparative Example 2 of the present invention. Detailed Implementation

[0037] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0038] The "range" disclosed in this invention can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. This type of range definition can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be arbitrarily combined, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for specific parameters, it is understood that ranges of 60~110 and 80~120 are also expected. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this invention, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0" and "5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, when a parameter is described as an integer selected from "2~10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0039] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.

[0040] The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this invention can be combined with other embodiments.

[0041] In this invention, open-ended technical features or solutions described using terms such as "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or exclude additional members. This can be considered as providing both technical features or solutions where "A is composed of a1, a2, and a3" or "A is selected from a1, a2, and a3," and technical features or solutions where "A includes not only a1, a2, and a3, but also other members."

[0042] In this invention, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a group consisting of A, B, and "a combination of A and B". "Containing A and / or B" can mean "containing A, containing B, and containing A and B", or "containing A, containing B, or containing A and B", and can be appropriately understood according to the context.

[0043] In this invention, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on the quantity.

[0044] In this invention, "room temperature" generally refers to 4℃~35℃, and can refer to 20℃±5℃. In some embodiments of this invention, room temperature refers to 20℃~30℃.

[0045] In one embodiment, the present invention provides a method for simultaneously producing ammonium-processed ferric phosphate and iron-processed ferric phosphate, the method comprising the following steps:

[0046] (1) The elemental iron and the ferrous iron source are dissolved in an acid solution containing at least phosphoric acid to obtain a ferrous dihydrogen phosphate solution;

[0047] (2) The ferrous dihydrogen phosphate solution described in step (1) is adjusted for pH and aged to obtain ferrous phosphate filter cake octahydrate and ammonium dihydrogen phosphate filtrate.

[0048] (3) The first ferrous phosphate filter cake in step (2) is oxidized and dehydrated to obtain ferric phosphate prepared by the iron method;

[0049] (4) Mix the ammonium dihydrogen phosphate filtrate and iron salt solution from step (2) and react to obtain ferrous phosphate octahydrate filter cake and ammonium sulfate filtrate. The ammonium sulfate filtrate is recovered to obtain ammonium sulfate.

[0050] (5) The second ferrous phosphate filter cake from step (4) is oxidized and dehydrated to obtain ferric phosphate prepared by the ammonium method.

[0051] To address the limitations of existing ferric phosphate preparation processes, which struggle to flexibly meet the diverse market demands for high-end, high-compaction LiFePO4 products and fail to achieve a novel ferric phosphate that balances high-compaction performance, raw material adaptability, and production line economics, this invention provides a method for simultaneously producing ammonium-based and ferric-based ferric phosphate, enabling co-production of both methods. During the production process, neither the ferric nor the ammonium method requires the introduction of additional oxidants (such as hydrogen peroxide), avoiding the storage and use of oxidants and thus eliminating the use of major hazardous sources, significantly reducing investment costs. Furthermore, the method of this invention eliminates the need for excessively high temperatures in the aging and crystallization process, the reaction process, and the subsequent oxidation and dehydration stages, resulting in significantly reduced energy consumption. The lower oxidation and dehydration temperature also eliminates the need for expensive kilns. In addition, this invention yields a high-value byproduct, ammonium sulfate, during production, which can offset costs. This ensures that the final ferric and ammonium-based ferric phosphate products exhibit raw material consistency and high product stability.

[0052] The existing iron-based process for producing iron phosphate dihydrate is mostly thick, layered, and difficult to process, making it hard to achieve breakthroughs in the iteration of high-end lithium iron phosphate. Furthermore, the conversion rate is low during the aging and crystallization process, which affects the yield.

[0053] The main chemical reactions involved in the preparation process of this invention are as follows:

[0054] (1) Iron dissolution reaction:

[0055] FeO+2H3PO4→Fe(H2PO4)2+H2O.

[0056] Fe + 2H3PO4 → Fe(H2PO4)2 + H2.

[0057] (2) Iron-based aging and crystallization:

[0058] 3Fe(H2PO4)2+4NH3·H2O+4H2O→Fe3(PO4)2·8H2O+4NH4H2PO4.

[0059] (3) Oxidative dehydration:

[0060] 4Fe3(PO4)2·8H2O+3O2+4H3PO4→12FePO4+38H2O.

[0061] (4) Ammonium process reaction and aging crystallization:

[0062] 3FeSO4+2NH4H2PO4+4NH3·H2O+4H2O→Fe3(PO4)2·8H2O+3(NH4)2SO4.

[0063] (5) Ammonium oxidation dehydration:

[0064] 4Fe3(PO4)2·8H2O+3O2+4H3PO4→12FePO4+38H2O.

[0065] In some embodiments, the acid solution in step (1) can be a pure phosphoric acid solution or a mixed acid solution of phosphoric acid and other acids, including inorganic acids and / or organic acids, wherein the inorganic acids include nitric acid and / or sulfuric acid, and the organic acids include oxalic acid, etc.

[0066] In some embodiments, the mass concentration of the acid solution in step (1) is 25% to 35%, such as 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34% or 35%, etc., and the amount of acid used in the acid solution is 1 to 1.3 times the theoretical molar amount, such as 1, 1.1, 1.2 or 1.3 times.

[0067] In some embodiments, the iron-dissolving reaction in step (1) is carried out under a protective atmosphere.

[0068] It is understood that the protective atmosphere in this invention refers to a gaseous atmosphere that does not participate in the reaction but only serves a protective function, such as a nitrogen atmosphere and / or an inert gas atmosphere. The inert gas is an inert gas defined by the periodic table, such as argon and / or helium. Those skilled in the art can make adaptive selections and adjustments according to actual needs.

[0069] In some implementations, the iron source in step (1) includes elemental iron and / or divalent iron.

[0070] In some embodiments, the divalent iron source includes, but is not limited to, ferrous sulfate and / or ferrous oxide.

[0071] In the iron dissolution reaction process in step (1) of this invention, the introduction of a ferrous iron source is beneficial to control the iron dissolution reaction rate, avoid excessively vigorous reaction leading to local overheating, and at the same time, can adjust the particle size distribution and morphology of the final iron phosphate product; furthermore, the molar ratio of elemental iron to ferrous iron source is 1:0.2~1:0.8, for example 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7 or 1:0.8, etc.

[0072] In some embodiments, the mixed gas obtained after the iron dissolution reaction in step (1) is recovered by absorption-spraying to obtain an acid solution, which is then reused in the iron dissolution reaction preparation process, and the remaining gas after recovery is discharged as tail gas; or, the mixed gas obtained after the iron dissolution reaction in step (1) is recovered by absorption-spraying to obtain an acid solution, which is then reused in the iron dissolution reaction preparation process, and the remaining gas after recovery is recycled and reused.

[0073] In some embodiments, the gas after the iron dissolution reaction in step (1) is a protective gas containing acid mist. After acid mist recovery, the protective gas can be recycled and reused.

[0074] In the method of step (1) of the present invention, when the iron source contains elemental iron, hydrogen gas containing acid mist and protective gas are generated at the same time as the iron dissolution reaction generates ferrous dihydrogen phosphate solution. The acid mist can be absorbed by the absorption-spraying method to obtain acid-containing spray water, which can then be reused in the iron dissolution preparation process. The reuse process can be adjusted according to the amount of target acid solution. The remaining mixture of hydrogen gas and protective gas can be discharged as tail gas.

[0075] When the iron source is ferrous iron, the reaction between phosphoric acid and ferrous iron does not produce hydrogen gas. At this time, the iron dissolution reaction produces ferrous dihydrogen phosphate solution, and at the same time, a protective gas containing acid mist is obtained. The acid mist can be absorbed by the absorption-spraying method to obtain acid-containing spray water, which can then be reused in the iron dissolution preparation process. The reuse process can be adjusted according to the amount of target acid solution used. The remaining protective gas can be reused in the system after dehydration.

[0076] In some implementations, in step (2), an ammonia solution is added to adjust the pH value.

[0077] This invention does not limit the specific mass concentration of the ammonia solution; conventional industrial ammonia solution is sufficient.

[0078] In some implementations, in step (2), the pH value is adjusted to 4.5 to 6.5, for example, 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9 or 6.

[0079] In some embodiments, the aging temperature in step (2) is 40°C to 50°C, for example, 40°C, 45°C or 50°C.

[0080] In the iron-based process of the present invention, the aging and crystallization temperature in step (2) is much lower than that of the existing traditional iron-based process. The aging temperature of the traditional iron-based process is mostly 70℃~95℃, while the present application can obtain ferrous phosphate octahydrate at 40℃~50℃. This reaction temperature condition is mild and ferrous phosphate octahydrate with high conversion rate is obtained.

[0081] In some implementations, the aging time in step (2) is 2h to 6h, for example 2h, 3h, 4h, 5h or 6h.

[0082] In the preparation process of step (2) of this invention, there is no need to introduce a protective gas, and the PO4 in the system... 3- Excessive amounts, even with slight oxidation, will only produce FePO4·2H2O, ensuring the final yield of iron phosphate produced by the iron-based process.

[0083] In some embodiments, after aging in step (2), a first ferrous phosphate octahydrate slurry is obtained. The first ferrous phosphate octahydrate slurry is then filtered under a protective atmosphere to obtain a first ferrous phosphate octahydrate filter cake and an ammonium dihydrogen phosphate filtrate.

[0084] In step (2) of the present invention, a protective gas is introduced during the filtration process to avoid the product from hydrolyzing and generating ferric hydroxide due to excessively high pH value in the aged slurry.

[0085] This invention does not limit the specific means of filtration. Without departing from the overall technical concept of this invention, conventional filtration methods under a protective atmosphere are applicable to this invention; for example, they can be performed in a closed horizontal centrifugal filter press or plate and frame filter press filled with protective gas.

[0086] In some embodiments, in step (3), the first ferrous phosphate filter cake octahydrate is first dried at low temperature and then oxidized and dehydrated. The temperature of the low-temperature drying is ≤60℃, such as 30℃, 35℃, 40℃, 45℃, 50℃, 55℃ or 60℃.

[0087] In step (3) of this invention, low-temperature drying is first performed to initially remove the moisture from the first ferrous phosphate filter cake octahydrate, and the moisture removal can be achieved at a temperature of ≤60℃; while in the conventional iron-based ferric phosphate preparation process, the moisture removal temperature at this stage is often above 450℃.

[0088] In some embodiments, in step (3), the oxidative dehydration method includes flash cyclone separation drying, and the drying temperature of the flash cyclone separation drying method is 250℃~350℃, such as 250℃, 260℃, 270℃, 280℃, 290℃, 300℃, 310℃, 320℃, 330℃, 340℃ or 350℃.

[0089] In step (3) of this invention, the flash cyclone separation drying method can remove the water of crystallization in ferrous phosphate octahydrate. During flash evaporation, the drying speed is too fast, and the water vapor can be quickly extracted, avoiding the hydrolysis process. Thus, it can be directly oxidized and dehydrated in the air atmosphere to produce anhydrous ferric phosphate. Furthermore, the drying temperature of the flash cyclone separation drying method in this invention is much lower than the water of crystallization removal temperature in the existing iron process, which often requires a dehydration temperature of over 650°C. This invention controls the flash temperature within the range of 250°C to 350°C, which on the one hand ensures the full removal of water of crystallization in ferrous phosphate octahydrate and Fe 2+ Complete oxidation avoids residual iron phosphate dihydrate phase and ferrous iron in the product; on the other hand, it can prevent excessive oxidation of the particle surface due to excessive temperature, forming a dense shell that hinders the diffusion of internal moisture, and at the same time avoids agglomeration between particles during sintering, thereby maintaining the product with a suitable specific surface area and particle size distribution, which is beneficial to the subsequent synthesis of lithium iron phosphate and the improvement of compaction density.

[0090] In some embodiments, the reaction in step (4) includes: adding an ammonia solution to adjust the pH value to 4.5-6.5 for aging and crystallization. For example, the pH value can be 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.1, 6.2, 6.3, 6.4 or 6.5, etc.

[0091] In step (4) of this invention, the ammonium dihydrogen phosphate filtrate generated by the iron method can be directly used as the raw material for the ammonium method, without the need for additional procurement, which greatly reduces the production cost.

[0092] In some embodiments, the iron salt in step (4) comprises ferrous sulfate heptahydrate.

[0093] In some embodiments, the temperature of the reaction in step (4) is 40°C to 50°C, for example, 40°C, 45°C or 50°C.

[0094] In some implementations, the reaction time of the reaction in step (4) is 2h to 6h, for example 2h, 3h, 4h, 5h or 6h.

[0095] In some embodiments, after the reaction described in step (4), a ferrous phosphate slurry with second octahydrate is obtained. The ferrous phosphate slurry with second octahydrate is then filtered under a protective atmosphere to obtain a ferrous phosphate filter cake with second octahydrate and an ammonium sulfate filtrate.

[0096] In some embodiments, the filtering process in step (4) of the present invention is the same as the filtering process in step (2).

[0097] In the ammonium reaction process of step (4) of this invention, ammonium sulfate filtrate is obtained. This filtrate can be evaporated and crystallized to obtain high-value ammonium sulfate byproduct ((NH4)2SO4).

[0098] In some embodiments, in step (5), the second ferrous phosphate filter cake is first dried at low temperature and then oxidized and dehydrated. The temperature of the low-temperature drying is ≤60℃, such as 30℃, 35℃, 40℃, 45℃, 50℃, 55℃ or 60℃.

[0099] In some embodiments, in step (5), the oxidative dehydration method includes flash cyclone separation drying, and the drying temperature of the flash cyclone separation drying method is 250℃~350℃, such as 250℃, 260℃, 270℃, 280℃, 290℃, 300℃, 310℃, 320℃, 330℃, 340℃ or 350℃.

[0100] In one embodiment, the present invention provides an iron phosphate, which is prepared by the method described in the above embodiments.

[0101] The present invention, through the methods provided in the above embodiments, yields iron-based iron phosphate and ammonium-based iron phosphate, respectively. These two types of iron phosphate have different particle size distributions and morphological characteristics: iron-based iron phosphate particles are more dense and larger in size, while ammonium-based iron phosphate particles are more porous and smaller in size. Combining the two in a certain proportion can achieve a particle size distribution effect, effectively improving the powder compaction density of subsequent lithium iron phosphate cathode materials, while also considering the material's cycle stability and processing performance.

[0102] In one embodiment, the present invention provides a cathode material, wherein the raw materials for preparing the lithium iron phosphate cathode material include iron phosphate as described in the above embodiments, and the cathode material includes lithium iron phosphate cathode material and / or lithium manganese iron phosphate cathode material.

[0103] It is understood that this invention does not specifically limit the methods for preparing lithium iron phosphate and lithium manganese iron phosphate from iron phosphate. Conventional preparation methods are applicable to this invention without departing from the overall technical concept of the invention.

[0104] In one embodiment, the present invention also provides a battery comprising a positive electrode material as described in the above embodiments.

[0105] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0106] Example 1

[0107] This embodiment provides a method for simultaneously producing ammonium-processed ferric phosphate and iron-processed ferric phosphate, the method being as follows:

[0108] (1) Ferrous oxide is dissolved in a 30% phosphoric acid solution. Nitrogen gas is introduced during the iron dissolution reaction. The amount of phosphoric acid added is 1.2 times the theoretical molar amount. Ferrous dihydrogen phosphate solution and a mixed gas containing acid mist and nitrogen are obtained. The mixed gas containing acid mist and nitrogen is adsorbed and sprayed to obtain phosphoric acid-containing spray water and wet nitrogen. The phosphoric acid-containing spray water is prepared again to form a phosphoric acid solution, which is reused in the iron dissolution reaction. The wet nitrogen is dehydrated and introduced again as a protective gas.

[0109] (2) The ferrous dihydrogen phosphate (Fe(H2PO4)2) solution described in step (1) is added to industrial ammonia water (the mass concentration of ammonia water is 25%) to adjust the pH value to 5.5, and then aged and crystallized to obtain an aged slurry. The aged slurry is filtered in a closed nitrogen-filled plate and frame filter press. After filtration, pure water is introduced into the equipment to wash the material. After the ion conductivity of the effluent is lower than 500 μS / cm, it is thoroughly centrifuged to obtain the first octahydrate ferrous phosphate filter cake and ammonium dihydrogen phosphate filtrate.

[0110] (3) The first ferrous phosphate filter cake in step (2) is dried at low temperature under vacuum at 60°C to form a dry powder. The dry powder is then separated by flash cyclone separation in air at 300°C and rapidly oxidized and dehydrated to obtain anhydrous ferric phosphate prepared by the iron method.

[0111] (4) Mix the ammonium dihydrogen phosphate filtrate and ferrous sulfate heptahydrate solution described in step (2), adjust the iron-phosphorus ratio to 1:1, then add industrial ammonia water (mass concentration of ammonia water is 25%) to adjust the pH value to 5.5 and carry out the reaction to obtain the slurry after reaction. The slurry after reaction is completed in a closed nitrogen-filled plate and frame filter press. After filtration, pure water is introduced into the equipment to wash the material. After the ion conductivity of the water outlet is lower than 500 μS / cm, it is thoroughly centrifuged to obtain the second ferrous phosphate octahydrate filter cake and ammonium sulfate filtrate. The ammonium sulfate filtrate is evaporated and crystallized to recover the by-product ammonium sulfate.

[0112] (5) The second ferrous phosphate filter cake in step (4) is dried at low temperature under vacuum at 60°C to form a dry powder. The dry powder is then subjected to flash cyclone separation in air at 300°C to rapidly oxidize and dehydrate, thereby obtaining ferric phosphate prepared by the ammonium method.

[0113] Example 2

[0114] This embodiment provides a method for simultaneously producing ammonium-processed ferric phosphate and iron-processed ferric phosphate, the method being as follows:

[0115] (1) Ferrous oxide is dissolved in a 30% phosphoric acid solution. Nitrogen gas is introduced during the iron dissolution reaction. The amount of phosphoric acid added is 1.2 times the theoretical molar amount. Ferrous dihydrogen phosphate solution and a mixed gas containing acid mist and nitrogen are obtained. The mixed gas containing acid mist and nitrogen is adsorbed and sprayed to obtain phosphoric acid-containing spray water and wet nitrogen. The phosphoric acid-containing spray water is prepared again to form a phosphoric acid solution, which is reused in the iron dissolution reaction. The wet nitrogen is dehydrated and introduced again as a protective gas.

[0116] (2) The ferrous dihydrogen phosphate (Fe(H2PO4)2) solution described in step (1) is added to industrial ammonia water (the mass concentration of ammonia water is 25%) to adjust the pH value to 4.5, and then aged and crystallized to obtain an aged slurry. The aged slurry is filtered in a closed nitrogen-filled plate and frame filter press. After filtration, pure water is introduced into the equipment to wash the material. After the ion conductivity of the effluent is lower than 500 μS / cm, it is thoroughly centrifuged to obtain the first octahydrate ferrous phosphate filter cake and ammonium dihydrogen phosphate filtrate.

[0117] (3) The first ferrous phosphate filter cake in step (2) is subjected to low-temperature vacuum drying at 45°C to form a dry powder. The dry powder is then subjected to flash cyclone separation in an air environment at 250°C to rapidly oxidize and dehydrate, thereby obtaining anhydrous ferric phosphate prepared by the iron method.

[0118] (4) Mix the ammonium dihydrogen phosphate filtrate and ferrous sulfate heptahydrate solution described in step (2), adjust the iron-to-phosphorus ratio to 1:1.05, then add industrial ammonia water (25% mass concentration of ammonia water) to adjust the pH value to 4.5 for reaction, and obtain the slurry after reaction. The slurry after reaction is completed in a closed nitrogen-filled plate and frame filter press. After filtration, pure water is introduced into the equipment to wash the material. After the ion conductivity of the water outlet is lower than 500 μS / cm, it is thoroughly centrifuged to obtain the second ferrous phosphate octahydrate filter cake and ammonium sulfate filtrate. The ammonium sulfate filtrate is evaporated and crystallized to recover the by-product ammonium sulfate.

[0119] (5) The second ferrous phosphate filter cake from step (4) is dried at a low temperature of 45°C under vacuum to form a dry powder. The dry powder is then subjected to flash cyclone separation in an air environment at 250°C to rapidly oxidize and dehydrate, thereby obtaining ferric phosphate prepared by the ammonium method.

[0120] Example 3

[0121] This embodiment provides a method for simultaneously producing ammonium-processed ferric phosphate and iron-processed ferric phosphate, the method being as follows:

[0122] (1) Ferrous oxide is dissolved in a 30% phosphoric acid solution. Nitrogen gas is introduced during the iron dissolution reaction. The amount of phosphoric acid added is 1.2 times the theoretical molar amount. Ferrous dihydrogen phosphate solution and a mixed gas containing acid mist and nitrogen are obtained. The mixed gas containing acid mist and nitrogen is adsorbed and sprayed to obtain phosphoric acid-containing spray water and wet nitrogen. The phosphoric acid-containing spray water is prepared again to form a phosphoric acid solution, which is reused in the iron dissolution reaction. The wet nitrogen is dehydrated and introduced again as a protective gas.

[0123] (2) The ferrous dihydrogen phosphate (Fe(H2PO4)2) solution described in step (1) is added to industrial ammonia water (the mass concentration of ammonia water is 25%) to adjust the pH value to 6.5, and then aged and crystallized to obtain an aged slurry. The aged slurry is filtered in a closed nitrogen-filled plate and frame filter press. After filtration, pure water is introduced into the equipment to wash the material. After the ion conductivity of the effluent is lower than 500 μS / cm, it is thoroughly centrifuged to obtain the first octahydrate ferrous phosphate filter cake and ammonium dihydrogen phosphate filtrate.

[0124] (3) The first ferrous phosphate filter cake in step (2) is vacuum-dried at 50°C to form a dry powder. The dry powder is then subjected to flash cyclone separation in air at 350°C to rapidly oxidize and dehydrate, thereby obtaining anhydrous ferric phosphate prepared by the iron method.

[0125] (4) Mix the ammonium dihydrogen phosphate filtrate and ferrous sulfate heptahydrate solution described in step (2), adjust the iron-to-phosphorus ratio to 1:1.05, then add industrial ammonia water (25% mass concentration of ammonia water) to adjust the pH value to 6.5 for reaction, and obtain the slurry after reaction. The slurry after reaction is completed in a closed nitrogen-filled plate and frame filter press. After filtration, pure water is introduced into the equipment to wash the material. After the ion conductivity of the water outlet is lower than 500 μS / cm, it is thoroughly centrifuged to obtain the second ferrous phosphate octahydrate filter cake and ammonium sulfate filtrate. The ammonium sulfate filtrate is evaporated and crystallized to recover the by-product ammonium sulfate.

[0126] (5) The second ferrous phosphate filter cake from step (4) is vacuum-dried at 55°C to form a dry powder. The dry powder is then subjected to flash cyclone separation in air at 350°C for rapid oxidation and dehydration to obtain ferric phosphate prepared by the ammonium method.

[0127] Example 4

[0128] like Figure 1 As shown, the difference between this embodiment and embodiment 1 is that in step (1) of this embodiment, ferrous oxide is replaced with elemental iron to obtain ferrous dihydrogen phosphate solution and a mixed gas containing acid mist, hydrogen and nitrogen. The mixed gas is subjected to an adsorption-spraying method to obtain spray water containing phosphoric acid and a mixed gas of wet hydrogen and nitrogen. The spray water containing phosphoric acid is further prepared to form a phosphoric acid solution, which is reused in the iron dissolving reaction process. The mixed gas of wet hydrogen and nitrogen is discharged as tail gas.

[0129] All other conditions remain the same as in Example 1.

[0130] Example 5

[0131] The difference between this embodiment and embodiment 1 is that the pH value in step (2) of this embodiment is 4.

[0132] All other conditions remain the same as in Example 1.

[0133] Example 6

[0134] The difference between this embodiment and embodiment 1 is that the pH value in step (2) of this embodiment is 6.8.

[0135] All other conditions remain the same as in Example 1.

[0136] Example 7

[0137] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, low-temperature drying is not performed, and the first ferrous phosphate filter cake octahydrate is directly separated by flash cyclone separation.

[0138] All other conditions remain the same as in Example 1.

[0139] Example 8

[0140] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the drying temperature of flash cyclone separation is 200℃.

[0141] All other conditions remain the same as in Example 1.

[0142] Example 9

[0143] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the drying temperature of flash cyclone separation is 400℃.

[0144] All other conditions remain the same as in Example 1.

[0145] Example 10

[0146] The difference between this embodiment and embodiment 1 is that in step (3) of this embodiment, the flash cyclone separation and drying is adjusted to air atmosphere in the tube furnace for sintering, and the sintering temperature is 300℃.

[0147] All other conditions remain the same as in Example 1.

[0148] Example 11

[0149] The difference between this embodiment and embodiment 1 is that the pH value in step (4) of this embodiment is 4.

[0150] All other conditions remain the same as in Example 1.

[0151] Example 12

[0152] The difference between this embodiment and embodiment 1 is that the pH value in step (4) of this embodiment is 6.8.

[0153] All other conditions remain the same as in Example 1.

[0154] Example 13

[0155] The difference between this embodiment and embodiment 1 is that in step (5) of this embodiment, low-temperature drying is not performed, and the second ferrous phosphate filter cake is directly separated by flash cyclone separation.

[0156] All other conditions remain the same as in Example 1.

[0157] Example 14

[0158] The difference between this embodiment and embodiment 1 is that in step (5) of this embodiment, the drying temperature of flash cyclone separation is 200℃.

[0159] All other conditions remain the same as in Example 1.

[0160] Example 15

[0161] The difference between this embodiment and embodiment 1 is that in step (5) of this embodiment, the drying temperature of flash cyclone separation is 400℃.

[0162] All other conditions remain the same as in Example 1.

[0163] Comparative Example 1

[0164] This comparative example provides a traditional iron-based method for preparing iron phosphate, such as... Figure 2 As shown, it includes:

[0165] (1) Add iron powder to a 30% phosphoric acid solution and carry out the iron dissolution reaction at 85°C. The amount of phosphoric acid added is 1.1 times the theoretical molar amount. The reaction continues until no obvious bubbles are produced, and ferrous dihydrogen phosphate solution is obtained.

[0166] (2) After filtering the ferrous dihydrogen phosphate solution described in step (1) to remove impurities, heat it to 85°C and slowly add hydrogen peroxide with a mass concentration of 27.5% under stirring to carry out the oxidation reaction. The amount of hydrogen peroxide added is 1.15 times the theoretical molar amount, and the oxidation reaction time is 2 hours to obtain ferric phosphate slurry.

[0167] (3) Adjust the pH value of the ferric phosphate slurry obtained in step (2) to 2.0, and age it at 90°C for 4 hours to obtain ferric phosphate dihydrate slurry;

[0168] (4) Filter the ferric phosphate dihydrate slurry described in step (3) and wash it with pure water until the conductivity of the wash water is less than 500 μS / cm to obtain ferric phosphate dihydrate filter cake.

[0169] (5) The ferric phosphate filter cake obtained in step (4) is flash-dried at 120°C for 4 hours and then calcined at 600°C for 3 hours to obtain anhydrous ferric phosphate.

[0170] Comparative Example 2

[0171] This comparative example provides a traditional ammonium method for preparing iron phosphate, such as... Figure 3 As shown, it includes:

[0172] (1) Mix ammonium dihydrogen phosphate solution and ferrous sulfate solution with a concentration of 1.5 mol / L at an iron-to-phosphorus molar ratio of 1:1.05, heat to 60°C, and slowly add hydrogen peroxide with a mass concentration of 27.5% under stirring to carry out the oxidation reaction. The amount of hydrogen peroxide added is 1.1 times the theoretical molar amount. Adjust the pH value to 1.8 with sulfuric acid. The oxidation reaction time is 2 hours to obtain the oxidized mixture.

[0173] (2) Add 25% ammonia water to the oxidized mixture in step (1) to adjust the pH value to 6.0, stir and precipitate at 50°C for 1 hour to obtain an amorphous precipitate slurry;

[0174] (3) The amorphous precipitate slurry described in step (2) is filtered and washed with pure water until the conductivity of the wash water is less than 500 μS / cm to obtain an amorphous precipitate filter cake and ammonium sulfate filtrate. The ammonium sulfate filtrate is concentrated by evaporation and dried to recover the byproduct ammonium sulfate.

[0175] (4) The amorphous precipitated filter cake described in step (3) is mixed with water to make a slurry with a solid content of 20%. Phosphoric acid and / or sulfuric acid are added to adjust the pH value to 2.0. Phosphoric acid is added to adjust the iron-phosphorus molar ratio to 1:1.05. The mixture is aged and crystallized at 95°C for 3 hours to obtain iron phosphate dihydrate slurry.

[0176] (5) Filter the ferric phosphate dihydrate slurry obtained in step (4), wash it with pure water until the conductivity of the wash water is less than 500 μS / cm, and obtain ferric phosphate dihydrate filter cake. Flash dry the ferric phosphate dihydrate filter cake at 120°C for 4 hours, and then calcine it at 600°C for 3 hours in a rotary kiln to obtain anhydrous ferric phosphate.

[0177] Performance testing

[0178] The iron-phosphate and ammonium-phosphate prepared in each embodiment were used to prepare lithium iron phosphate materials. The iron-phosphate and ammonium-phosphate were mixed uniformly at a mass ratio of 1:1 to obtain compound iron phosphate. The compound iron phosphate, lithium carbonate and glucose were added to pure water at a lithium-iron molar ratio of 1.03:1 and the carbon source was added at 8% of the mass of iron phosphate to prepare a slurry with a solid content of 40%, which was ball-milled for 6 hours. The ball-milled slurry was spray-dried at 120°C to obtain precursor powder. The precursor powder was heated to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere, held at 700°C for 10 hours, and then pulverized after natural cooling to obtain lithium iron phosphate cathode material.

[0179] The iron phosphate prepared by the iron method provided in Comparative Example 1 and the iron phosphate prepared by the ammonium method provided in Comparative Example 2 were used to prepare lithium iron phosphate materials, and the preparation process was consistent with that of the examples.

[0180] The lithium iron phosphate prepared in the examples and comparative examples were tested for compaction density using a powder compaction density meter. 1.5g of sample was weighed and placed in a mold with a diameter of 13mm. The sample was pressed for 30 seconds under a pressure of 3t. The thickness of the compressed tablet was measured and the powder compaction density was calculated. The test results are shown in Table 1.

[0181] Table 1

[0182]

[0183] From Table 1, we can obtain:

[0184] The method provided by this invention abandons the traditional process scheme that requires the addition of oxidants and other oxidation processes, and can simultaneously realize the preparation of ammonium-based ferric phosphate and iron-based ferric phosphate, ensuring the consistency of raw material sources and the stability control of final product performance. At the same time, it also obtains high-value by-product ammonium sulfate, satisfying multiple requirements that take into account high compaction performance, raw material adaptability and production line economy.

[0185] Data analysis of Examples 1 and 5-6 shows that, in the process of preparing ferric phosphate by the iron method, adjusting the pH value of aging and crystallization in step (2) to 4.5-6.5 is more conducive to the full crystallization and grain growth of ferrous phosphate octahydrate, resulting in a more uniform particle size distribution of the obtained ferric phosphate. The compacted density of lithium iron phosphate after compounding can reach 2.60 g / cm³. 3 The above applies; however, when the pH value is too low (such as pH=4.0 in Example 5), ferrous phosphate precipitation is incomplete, and the product yield decreases; when the pH value is too high (such as pH=6.8 in Example 6), ferric hydroxide impurities are easily generated, affecting product purity and electrochemical performance.

[0186] Data analysis of Examples 1 and 7 reveals that, in the iron-based preparation of lithium iron phosphate, failure to perform low-temperature drying of ferrous phosphate octahydrate leads to problems such as excessively high filter cake moisture content and easy agglomeration of materials during flash evaporation. This results in insufficient oxidation and dehydration, residual ferrous iron and water of crystallization in the product, ultimately reducing the compaction density of lithium iron phosphate to 2.50 g / cm³. 3 Furthermore, the stability of product batches has decreased.

[0187] Data analysis of Examples 1 and 8-10 shows that in step (3), the flash cyclone separation drying method can remove the water of crystallization from the ferrous phosphate octahydrate. During flash evaporation, the drying speed is too fast, and the water vapor can be quickly extracted, avoiding the hydrolysis process. Thus, it can be directly oxidized and dehydrated in the air atmosphere to produce anhydrous ferric phosphate. Other oxidative dehydration methods, such as tube furnace sintering dehydration, will lead to excessively long heating time of the material, sintering and agglomeration between particles, and a significant decrease in the specific area. Finally, the compaction density of lithium iron phosphate is only 2.45 g / cm³. 3 Furthermore, the drying temperature of the flash cyclone separation drying method in this invention is much lower than the temperature at which water of crystallization is removed in the existing iron-based method, and is preferably 250℃~350℃. This better leverages the technical advantages of the flash cyclone separation drying method in low-temperature rapid oxidation and dehydration, resulting in high-purity, uniformly sized iron-based lithium phosphate products. After compounding, the compacted density of lithium iron phosphate can reach 2.60 g / cm³. 3 above.

[0188] Data analysis of Examples 1 and 11-12 shows that, in the process of preparing ferric phosphate by ammonium method, the pH value of the aging crystallization in step (4) is adjusted to 4.5-6.5, which more effectively utilizes the phosphorus source in the ammonium dihydrogen phosphate filtrate. The resulting ammonium-processed ferric phosphate particles are small and uniformly distributed, and the gradation effect is significant after compounding with iron-processed ferric phosphate. When the pH value is too low (such as pH=4.0 in Example 11), the precipitation of ammonium-processed ferric phosphate is incomplete, and the phosphorus resource utilization rate decreases. When the pH value is too high (such as pH=6.8 in Example 12), iron hydroxide impurities are easily generated, affecting the purity of the product.

[0189] Data analysis of Examples 1 and 13 reveals that, during the ammonium method for preparing ferric phosphate, failure to perform low-temperature drying of ferrous phosphate dioctahydrate leads to hollow structures and particle breakage during flash evaporation of the ferric phosphate particles. This results in a wider particle size distribution, weakened gradation after compounding, and a decrease in the compacted density of lithium iron phosphate to 2.51 g / cm³. 3 .

[0190] Data analysis of Examples 1 and 14-15 shows that in step (5), the ferrous phosphate dihydrate is also dried using a flash cyclone separation method to remove the water of crystallization. The preferred temperature for this flash cyclone separation method is 250℃~350℃, which better improves the oxidative dehydration efficiency and product consistency of the ammonium-based ferric phosphate. If the flash temperature is too low (e.g., 200℃ in Example 14), the water of crystallization is not completely removed, leaving residual ferric phosphate dihydrate in the product. If the flash temperature is too high (e.g., 400℃ in Example 15), excessive oxidation on the particle surface forms a dense layer, hindering the diffusion of internal moisture, resulting in a higher product moisture content and a decreased specific surface area.

[0191] Data analysis of Example 1 and Comparative Examples 1-2 shows that the method provided by the present invention achieves the co-production of iron-based ferric phosphate and ammonium-based ferric phosphate, and only through a specific preparation process can the high-compaction performance, raw material adaptability and production line economy be taken into account.

[0192] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A method for simultaneously producing ammonium-processed ferric phosphate and iron-processed ferric phosphate, characterized in that, The method includes the following steps: (1) The iron source is subjected to an iron dissolution reaction using an acid solution containing at least phosphoric acid to obtain a ferrous dihydrogen phosphate solution; (2) The ferrous dihydrogen phosphate solution described in step (1) is adjusted for pH and aged to obtain ferrous phosphate filter cake octahydrate and ammonium dihydrogen phosphate filtrate. (3) The first ferrous phosphate filter cake in step (2) is oxidized and dehydrated to obtain ferric phosphate prepared by the iron method; (4) Mix the ammonium dihydrogen phosphate filtrate and iron salt solution from step (2) and react to obtain ferrous phosphate octahydrate filter cake and ammonium sulfate filtrate. The ammonium sulfate filtrate is recovered to obtain ammonium sulfate. (5) The second ferrous phosphate filter cake from step (4) is oxidized and dehydrated to obtain ferric phosphate prepared by the ammonium method.

2. The method for simultaneously producing ammonium-process ferric phosphate and iron-process ferric phosphate according to claim 1, characterized in that, The iron-dissolving reaction in step (1) is carried out under a protective atmosphere; And / or, the iron source in step (1) includes elemental iron and / or divalent iron source; And / or, the mixed gas obtained after the iron dissolution reaction in step (1) is recovered by absorption-spraying method to obtain acid solution, which is reused in the iron dissolution reaction preparation process, and the remaining gas after recovery is discharged as tail gas; Alternatively, the mixed gas obtained after the iron dissolution reaction in step (1) can be recovered by absorption-spraying to obtain an acid solution, which can be reused in the iron dissolution reaction preparation process, and the remaining gas after recovery can be recycled and reused.

3. The method for simultaneously producing ammonium-process ferric phosphate and iron-process ferric phosphate according to claim 1, characterized in that, In step (2), an ammonia solution is added to adjust the pH value; And / or, in step (2), the pH value is adjusted to 4.5~6.5; And / or, the aging temperature in step (2) is 40℃~50℃, and the aging time in step (2) is 2h~6h.

4. The method for simultaneously producing ammonium-process ferric phosphate and iron-process ferric phosphate according to claim 1 or 3, characterized in that, After aging in step (2), a first ferrous phosphate octahydrate slurry is obtained. The first ferrous phosphate octahydrate slurry is then filtered under a protective atmosphere to obtain a first ferrous phosphate octahydrate filter cake and an ammonium dihydrogen phosphate filtrate.

5. The method for simultaneously producing ammonium-process ferric phosphate and iron-process ferric phosphate according to claim 1, characterized in that, In step (3), the first ferrous phosphate filter cake octahydrate is first dried at low temperature and then oxidized and dehydrated. The temperature of the low-temperature drying is ≤60℃. And / or, in step (3), the oxidative dehydration method includes flash cyclone separation drying, wherein the drying temperature of the flash cyclone separation drying method is 250℃~350℃.

6. The method for simultaneously producing ammonium-process ferric phosphate and iron-process ferric phosphate according to claim 1, characterized in that, The reaction in step (4) includes: adding an ammonia solution to adjust the pH to 4.5-6.5 for aging and crystallization; And / or, the temperature of the reaction in step (4) is 40℃~50℃, and the reaction time of the reaction in step (4) is 2h~6h; And / or, after the reaction described in step (4), a second ferrous phosphate octahydrate slurry is obtained. The second ferrous phosphate octahydrate slurry is then filtered under a protective atmosphere to obtain a second ferrous phosphate octahydrate filter cake and an ammonium sulfate filtrate.

7. The method for simultaneously producing ammonium-process ferric phosphate and iron-process ferric phosphate according to claim 1 or 6, characterized in that, In step (5), the filter cake of ferrous phosphate octahydrate is first dried at low temperature and then oxidized and dehydrated. The temperature of the low-temperature drying is ≤60℃. And / or, in step (5), the oxidative dehydration method includes flash cyclone separation drying, wherein the drying temperature of the flash cyclone separation drying method is 250℃~350℃.

8. A type of iron phosphate, characterized in that, The iron phosphate is prepared by the method according to any one of claims 1-7.

9. A positive electrode material, characterized in that, The raw materials for preparing the cathode material include iron phosphate as described in claim 8, and the cathode material includes lithium iron phosphate cathode material and / or lithium manganese iron phosphate cathode material.

10. A battery, characterized in that, The battery comprises the positive electrode material as described in claim 9.