Lithium iron phosphate recovery methods
By combining pretreatment and heat treatment, the problems of complex hydrometallurgical processes and large amounts of wastewater were solved, enabling the recovery of high-purity iron phosphate and lithium oxide composite materials, reducing costs and wastewater generation.
Patent Information
- Application Number
- CN202611333642.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing hydrometallurgical processes for recovering lithium iron phosphate are complex, consume large amounts of materials, and generate a large amount of complex industrial wastewater, making it difficult to obtain high-purity recovered products.
By removing water and carbon dioxide from lanthanum oxide through pretreatment, and combining heat treatment and sieving steps, waste lithium iron phosphate cathode material is reacted with zirconium dioxide and lanthanum oxide to prepare lithium oxide composite material and iron phosphate. The separation and purification are carried out by utilizing the temperature gradient difference of heat treatment.
The process enabled the recovery of high-purity iron phosphate and lithium oxide composite materials, reducing industrial wastewater generation, lowering preparation costs, and improving the utilization rate of iron and lithium sources.
Abstract
Description
Technical Field
[0001] This application relates to the field of battery cathode material recycling technology, and in particular to a method for recycling lithium iron phosphate. Background Technology
[0002] Currently, the recycling of cathode materials from spent lithium iron phosphate batteries mainly relies on hydrometallurgical processes to prepare lithium salts. Hydrometallurgical methods primarily depend on a cascade of strong acid leaching and chemical precipitation. While this can extract lithium, it requires the continuous addition of various chemical reagents, such as reducing agents, pH adjusters, and precipitants, resulting in high material consumption and complex processes. Furthermore, these hydrometallurgical processes generate significant amounts of complex industrial wastewater, leading to high treatment costs.
[0003] Therefore, there is an urgent need for a method to recover lithium iron phosphate that can simplify the process, reduce wastewater generation, and obtain high-purity recovered products. Summary of the Invention
[0004] Therefore, it is necessary to provide a method for recovering lithium iron phosphate that can obtain high-purity lithium oxide composite materials and iron phosphate, and the process is simple and reduces the generation of industrial wastewater.
[0005] The first aspect of this application provides a method for recovering lithium iron phosphate, comprising the following steps:
[0006] Lanthanum oxide is pretreated to remove water and carbon dioxide.
[0007] Waste cathode material, including lithium iron phosphate, is mixed with zirconium dioxide and subjected to a first heat treatment to prepare a first intermediate.
[0008] The first intermediate was mixed with the pretreated lanthanum oxide and subjected to a second heat treatment. After purging and sieving, crude lithium oxide composite material and iron phosphate were prepared.
[0009] The crude lithium oxide composite material is subjected to a third heat treatment, crushed, and sieved to prepare the lithium oxide composite material.
[0010] The temperature of the third heat treatment is higher than the temperature of the second heat treatment.
[0011] In some embodiments, the mass ratio of the waste cathode material including lithium iron phosphate to zirconium dioxide is (1.13~1.52):1; and / or, the mass ratio of the waste cathode material including lithium iron phosphate to lanthanum oxide is (0.80-2.09):1.
[0012] In some embodiments, the waste cathode material comprising lithium iron phosphate has a lithium iron phosphate content of 65% to 99.5% by mass.
[0013] In some embodiments, the pretreatment step includes: subjecting lanthanum oxide to infrared heating treatment in a protective atmosphere at a temperature of 300°C to 980°C; optionally, the infrared heating treatment time is 5 min to 300 min.
[0014] In some embodiments, the temperature of the first heat treatment is 400°C to 800°C; optionally, the first heat treatment is performed in air; optionally, the time of the first heat treatment is 30 min to 240 min.
[0015] In some embodiments, the temperature of the second heat treatment is 300°C to 750°C; optionally, the second heat treatment is performed in a protective gas atmosphere; optionally, the time of the second heat treatment is 120 min to 480 min.
[0016] In some embodiments, the temperature of the third heat treatment is 1050°C to 1600°C; optionally, the third heat treatment is carried out in a protective atmosphere; optionally, the time of the third heat treatment is 15 min to 480 min.
[0017] In some embodiments, the first heat treatment and / or the second heat treatment is carried out in a rotary kiln at a rotation speed of 2 to 30 revolutions per minute.
[0018] In some embodiments, the recycling method includes at least one of the following features:
[0019] (1) The particle size of the iron phosphate particles is smaller than the particle size of the crude lithium oxide composite material;
[0020] (2) The particle size of the iron phosphate particles is 3 μm ~ 130 μm;
[0021] (3) The particle size of the lithium oxide composite material is 10 mm to 30 mm.
[0022] In some embodiments, the iron-to-phosphorus ratio of the iron phosphate is 0.95 to 1; and / or, the lithium oxide composite material comprises lithium lanthanum zirconium oxide.
[0023] The lithium iron phosphate recycling method of this application can directly react waste cathode materials including lithium iron phosphate with zirconium oxide and pretreated lanthanum oxide to recycle and prepare iron phosphate and lithium oxide composite materials. It makes reasonable use of iron source and the prepared iron phosphate has high purity. At the same time, it can also make reasonable use of lithium source, that is, use lithium source in waste cathode materials to replace lithium source raw materials such as lithium hydroxide and lithium carbonate required in the traditional preparation steps of lithium oxide composite materials, so as to maximize the utilization and recycling of lithium source, reduce the preparation cost of lithium oxide composite materials, and the prepared lithium oxide composite materials have high purity. Detailed Implementation
[0024] The present application will be further described in detail below with reference to the embodiments and examples. It should be understood that these embodiments and examples are for illustrative purposes only and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to enable a more thorough and comprehensive understanding of the disclosure of the present application. It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various modifications or alterations without departing from the spirit of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. For example, features described or illustrated as part of one embodiment can be combined in a suitable manner in another embodiment to produce new embodiments. Furthermore, numerous details are set forth in the following description to provide a more complete understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for descriptive purposes only and is not intended to be limiting of the application.
[0026] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:
[0027] The terms “and / or,” “or / and,” and “and / or” as used herein include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. “Any and all combinations” includes any two related listed items, any more related listed items, or a combination of all related listed items. For example, “A and / or B” includes three parallel options: A, B, and “a combination of A and B.”
[0028] In this application, the terms "multiple", "various", "multiple times", "several", "several", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more or more.
[0029] In this application, "optionally", "optional", and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without".
[0030] In this application, the technical features or solutions described in open-ended language include both closed-ended technical features or solutions consisting of the listed contents and open-ended technical features or solutions that include the listed contents.
[0031] In this application, where the method flow involves multiple steps, unless otherwise explicitly stated herein, there is no strict order restriction on the execution of these steps; they can be executed in any order other than those described. Moreover, any step may include multiple sub-steps or multiple stages, which are not necessarily completed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be performed alternately or simultaneously with other steps or parts of the sub-steps or stages of other steps.
[0032] In this document, when referring to numerical intervals (i.e., numerical ranges), unless otherwise specified, the distribution of selectable values within a numerical interval is considered continuous, and includes the two endpoints (i.e., the minimum and maximum values) of the numerical interval, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which is equivalent to directly listing every integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all subranges included therein. The "numerical value" in this numerical interval can be any quantitative value, such as a number, percentage, ratio, etc. The term "numerical interval" can be broadly included to include percentage intervals, ratio intervals, proportion intervals, and other numerical interval types.
[0033] In this application, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.
[0034] The traditional preparation process of iron phosphate is to react iron or ferrous sulfate with phosphoric acid or phosphate. The synthesis process of lithium oxide composite material is to prepare lithium hydroxide, lanthanum oxide and zirconium dioxide by high-temperature solid-state reaction. Both products are widely used in new energy, fine chemical and other fields, but the traditional production processes have disadvantages such as high production cost, high energy consumption and high output of hazardous waste.
[0035] Based on this, the first aspect of this application provides a method for recovering lithium iron phosphate, comprising the following steps:
[0036] Lanthanum oxide is pretreated to remove water and carbon dioxide.
[0037] Waste cathode material, including lithium iron phosphate, is mixed with zirconium dioxide and subjected to a first heat treatment to prepare a first intermediate.
[0038] The first intermediate was mixed with pretreated lanthanum oxide and subjected to a second heat treatment. After purging and sieving, crude lithium oxide composite material and iron phosphate were prepared.
[0039] The crude lithium oxide composite material is subjected to a third heat treatment, crushed, and sieved to prepare lithium oxide composite material.
[0040] The temperature of the third heat treatment is higher than that of the second heat treatment.
[0041] If untreated lanthanum oxide is directly subjected to a first heat treatment with waste cathode material (including lithium iron phosphate) and zirconium dioxide, the resulting lithium oxide composite material has low purity. The inventors discovered that pretreatment to remove water and carbon dioxide from the lanthanum oxide before the first heat treatment reduces side reactions and improves the purity of the lithium oxide composite material. During the second heat treatment, lithium enters the crystal lattice of lanthanum oxide and zirconium dioxide, accompanied by the initial fusion of the two oxides. After the second heat treatment, the particle size difference between the crude lithium oxide composite material and iron phosphate allows for effective separation through purging and sieving, which improves iron source recovery and the purity of both products. A third heat treatment, at a higher temperature than the second, further promotes molecular-scale fusion of the lithium-incorporated lanthanum oxide and zirconium dioxide. After crushing and sieving, the lithium oxide composite material product is obtained.
[0042] Therefore, the lithium iron phosphate recycling method of this application can directly react waste cathode materials including lithium iron phosphate with zirconium oxide and pretreated lanthanum oxide to recover and prepare iron phosphate and lithium oxide composite materials. This method boasts high iron source utilization, high purity of the prepared iron phosphate, and low production cost. Simultaneously, the lithium source utilization rate of this method is also high. By rationally utilizing the lithium source in the waste cathode materials, the method maximizes lithium source utilization and recycling, reducing the production cost of lithium oxide composite materials, and producing lithium oxide composite materials with high purity. Furthermore, the recycling method of this application is simple and can reduce the generation of industrial wastewater.
[0043] This application does not impose any particular limitation on the above-mentioned purging method, as long as it can achieve the purpose of this application. In some embodiments, the purging process is adjusted so that the purging angle is perpendicular to the screen, which is beneficial to promote the full separation of the iron phosphate and lithium oxide composite materials, thereby improving the recovery rate of the iron source and promoting the improvement of the purity of the iron phosphate and lithium oxide composite materials.
[0044] This application does not impose any particular restrictions on the conditions used for the purging described above, as long as the purpose of this application can be achieved. For example, the purging gas can be one or more of nitrogen, helium, neon, argon, and hydrogen. When the protective atmosphere includes hydrogen, the volume ratio of hydrogen to other gases in the protective atmosphere is (5~15):(85~95). The relative humidity of the purging is less than 25%.
[0045] In some embodiments, the mass ratio of spent lithium iron phosphate cathode material to zirconium dioxide is (1.13-1.52):1. Specifically, the mass ratio of spent lithium iron phosphate cathode material to zirconium dioxide includes, but is not limited to: 1.13:1, 1.21:1, 1.29:1, 1.36:1, 1.44:1, 1.52:1, or any range between the two aforementioned.
[0046] In some embodiments, the mass ratio of spent lithium iron phosphate cathode material to lanthanum oxide is (0.80-2.09):1. Specifically, the mass ratio of spent lithium iron phosphate cathode material to lanthanum oxide includes, but is not limited to: 0.8:1, 1.06:1, 1.32:1, 1.57:1, 1.83:1, 2.09:1, or any range between the two aforementioned.
[0047] In some embodiments, the waste cathode material including lithium iron phosphate contains lithium iron phosphate at a mass percentage of 65% to 99.5%. Specifically, the mass percentage of lithium iron phosphate includes, but is not limited to: 65%, 71.9%, 78.8%, 85.7%, 92.6%, 99.5%, or any range between the foregoing.
[0048] In some embodiments, the pretreatment step includes: subjecting lanthanum oxide to infrared heating treatment in a protective atmosphere at a temperature of 300°C to 980°C. In some embodiments, the infrared heating treatment time is 5 min to 300 min. In some embodiments, the pretreatment is performed in an infrared calcination furnace. By employing the above pretreatment method and controlling the pretreatment conditions within the aforementioned range, water and carbon dioxide in lanthanum oxide can be effectively removed while reducing the content of water and carbon dioxide introduced by the external atmosphere. This further helps to reduce the generation of by-products and improve the purity of the lithium oxide composite material and the recovery rate of the lithium source. Specifically, the infrared heating treatment temperature includes, but is not limited to, 300°C, 470°C, 640°C, 810°C, 980°C, or any two of the aforementioned ranges. Specifically, the infrared heating treatment time includes, but is not limited to, 5 min, 64 min, 123 min, 182 min, 241 min, 300 min, or any two of the aforementioned ranges.
[0049] In some embodiments, the temperature of the first heat treatment is 400°C to 800°C. In some embodiments, the first heat treatment is performed in air. In some embodiments, the duration of the first heat treatment is 30 min to 240 min. By controlling the conditions of the first heat treatment within the above range, impurities such as conductive agents and binders in the waste cathode material, including lithium iron phosphate, can be removed, and the carbon content in the waste cathode material and zirconium dioxide can be reduced. This helps to reduce the probability of side reactions between lanthanum oxide and carbon during the subsequent second heat treatment of the above materials mixed with lanthanum oxide, thereby improving the purity of the prepared iron phosphate and lithium oxide composite material. Specifically, the temperature of the first heat treatment includes, but is not limited to: 400°C, 480°C, 560°C, 640°C, 720°C, 800°C, or any two of the above. Specifically, the duration of the first heat treatment includes, but is not limited to: 30 min, 72 min, 114 min, 156 min, 198 min, 240 min, or any two of the above.
[0050] In some embodiments, the first heat treatment is carried out in a rotary kiln with a rotation speed of 2 to 30 revolutions per minute. Specifically, the rotation speed of the rotary kiln includes, but is not limited to, 2, 9, 16, 23, 30 revolutions per minute or any range between the two.
[0051] In some embodiments, the temperature of the second heat treatment is 300°C to 750°C. In some embodiments, the second heat treatment is performed in a protective gas atmosphere. In some embodiments, the duration of the second heat treatment is 120 min to 480 min. Specifically, the temperature of the second heat treatment includes, but is not limited to: 300°C, 390°C, 480°C, 570°C, 660°C, 750°C, or any range between the foregoing. Specifically, the duration of the second heat treatment includes, but is not limited to: 120 min, 210 min, 300 min, 390 min, 480 min, or any range between the foregoing. For example, the protective atmosphere can be at least one of nitrogen, argon, neon, helium, and hydrogen. When the protective atmosphere includes hydrogen, the volume ratio of hydrogen to other gases in the protective atmosphere is (5 to 15):(85 to 95).
[0052] In some embodiments, the particle size of the iron phosphate particles is smaller than that of the particles in the coarse lithium oxide composite product.
[0053] In some embodiments, the particle size of the ferric phosphate is 3 μm to 130 μm. Specifically, the particle size of the ferric phosphate includes, but is not limited to: 3 μm, 24 μm, 45 μm, 67 μm, 88 μm, 109 μm, 130 μm, or any range between the two aforementioned.
[0054] In this application, the particle size of lithium iron phosphate particles can be controlled by adjusting the conditions of the second heat treatment. For example, the higher the temperature and the longer the time of the second treatment, the smaller the particle size of the prepared lithium iron phosphate particles; conversely, the smaller the particle size, the lower the temperature and the longer the time.
[0055] In some embodiments, the second heat treatment is carried out in a rotary kiln with a rotation speed of 2 to 30 revolutions per minute. Specifically, the rotation speed of the rotary kiln includes, but is not limited to, 2, 9, 16, 23, 30 revolutions per minute or any range between the two.
[0056] In some embodiments, the iron-to-phosphorus ratio of ferric phosphate is 0.95 to 1. An iron-to-phosphorus ratio within this range indicates that the recovery method of this application introduces fewer impurities, resulting in higher purity ferric phosphate. Specifically, the iron-to-phosphorus ratio of ferric phosphate includes, but is not limited to, 0.95, 0.96, 0.97, 0.98, 0.99, 1, or any combination thereof.
[0057] In some embodiments, the temperature of the third heat treatment is 1050°C to 1600°C. In some embodiments, the third heat treatment is performed in a protective atmosphere. In some embodiments, the duration of the third heat treatment is 15 min to 480 min. Specifically, the temperature of the third heat treatment includes, but is not limited to: 1050°C, 1160°C, 1270°C, 1380°C, 1490°C, 1600°C, or any range between the foregoing. Specifically, the duration of the third heat treatment includes, but is not limited to: 15 min, 108 min, 201 min, 294 min, 387 min, 480 min, or any range between the foregoing. For example, the protective atmosphere may include at least one of nitrogen, argon, neon, helium, and hydrogen. When the protective atmosphere includes hydrogen, the volume ratio of hydrogen to other gases in the protective atmosphere is (5 to 15):(85 to 95).
[0058] In some embodiments, the particle size of the lithium oxide composite material is 10 mm to 30 mm. Specifically, the particle size of the lithium oxide composite material includes, but is not limited to, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, or any range between the two mentioned above.
[0059] In some embodiments, the lithium oxide composite material comprises lithium lanthanum zirconium oxide. In some embodiments, the lithium oxide composite material has a mass percentage of lithium lanthanum zirconium oxide greater than or equal to 99%.
[0060] In this application, the particle size of the lithium oxide composite material can be controlled as needed by adjusting the crushing and sieving conditions after the third heat treatment.
[0061] Lanthanum oxide and zirconium dioxide used in this application can be obtained by purchase.
[0062] The waste positive electrode material including lithium iron phosphate in this application can be obtained by purchase; or it can be prepared by the following method: dismantling waste lithium iron phosphate batteries, taking out positive electrode sheets, scraping off the positive electrode material layer, crushing, and preparing waste positive electrode material including lithium iron phosphate.
[0063] The embodiments of this application will be described in detail below with reference to some examples. It should be understood that these embodiments are only for illustrating this application and are not intended to limit the scope of this application. For experimental methods in the following embodiments where conditions are not specified, please refer to the guidelines given in this application first, or follow experimental manuals or conventional conditions in the art, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the art.
[0064] In the following examples, the measurement parameters of the raw material components may have slight deviations within the weighing accuracy range unless otherwise specified. Temperature and time parameters are subject to acceptable deviations due to instrument testing accuracy or operational precision.
[0065] Test method:
[0066] Test method for phosphorus-to-iron ratio:
[0067] Referring to the test method for the iron-phosphorus ratio in HG / T4701-2021 "Iron Phosphate for Batteries", the prepared iron phosphate was dissolved and the phosphorus content was determined by the quinomolybdate-limonene weighing method, and the iron content was determined by redox titration. The iron-phosphorus ratio can be obtained by calculating the measured phosphorus content and iron content.
[0068] Methods for testing the mass percentage of lithium, lanthanum, and zirconium in lithium oxide composite materials:
[0069] The contents of lithium, lanthanum, zirconium, and metallic impurities were detected by inductively coupled plasma atomic emission spectrometry (ICP-AES).
[0070] In lithium oxide composite materials, the mass percentage of lithium, lanthanum, and zirconium = the sum of the contents of lithium, lanthanum, and zirconium / (the sum of the contents of lithium, lanthanum, and zirconium + the sum of the contents of metallic impurity elements).
[0071] In this application, the reaction is that in lithium oxide composite materials, the higher the mass percentage content of lithium, lanthanum, and zirconium, the higher the purity of lithium, lanthanum, zirconium, and oxygen; conversely, the lower the mass percentage content, the lower the purity.
[0072] In the embodiments and comparative examples of this application, the mass percentage of lithium iron phosphate in the waste cathode material includes lithium iron phosphate, as described in the specific embodiments; in addition to lithium iron phosphate, it also includes aluminum, copper, and carbon.
[0073] Example 1
[0074] (1) Take 11 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 300℃ for calcination for 120 minutes before transferring it to a rotary calcining furnace 2.
[0075] (2) Take 23 kg of waste cathode material powder containing lithium iron phosphate (lithium iron phosphate mass percentage is 99%) and 17 kg of zirconium dioxide mass percentage of 98% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, calcinate at a speed of 15 rpm at the first heat treatment temperature of 500℃ for 120 minutes and then transfer them to rotary calcining furnace 2;
[0076] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 2.09:1; the mass ratio of waste cathode material to zirconium dioxide is 1.35:1) for a second heat treatment: at a speed of 20 rpm, in a nitrogen atmosphere, calcined at 650°C for 360 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the purging atmosphere is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 45 μm.
[0077] The test results showed that the iron content in the obtained iron phosphate product was 36.3%, the phosphorus content was 20.5%, and the iron-phosphorus molar ratio was 0.980.
[0078] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1200°C for 120 minutes in a nitrogen atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 21 mm.
[0079] Testing revealed that the lithium oxide composite material contained 99.3% lithium lanthanum zirconium oxide by mass.
[0080] Example 2
[0081] (1) Take 21 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 900℃ for calcination for 90 minutes before transferring it to a rotary calcining furnace 2.
[0082] (2) Take 27 kg of waste cathode material powder containing lithium iron phosphate (lithium iron phosphate mass percentage is 98%) and 19 kg of zirconium dioxide mass content of 98% into a mixer, mix them evenly and then transfer them into a rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into the rotary calcining furnace 1, turn on the heating, and calcinate at a speed of 20 rpm at a first heat treatment temperature of 600℃ for 180 minutes and then transfer them into a rotary calcining furnace 2.
[0083] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.29:1; the mass ratio of waste cathode material to zirconium dioxide is 1.42:1) for a second heat treatment: at a speed of 20 rpm, in an argon atmosphere, calcined at 600°C for 240 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the purging atmosphere is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 60 μm.
[0084] The test results showed that the iron content in the obtained iron phosphate product was 36.1%, the phosphorus content was 20.3%, and the iron-phosphorus molar ratio was 0.984.
[0085] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1350°C for 180 minutes in an argon atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 18 mm.
[0086] Testing revealed that the lithium oxide composite material contained 99.4% lithium lanthanum zirconium oxide by mass.
[0087] Example 3
[0088] (1) Take 31 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 600℃ for calcination for 180 minutes before transferring it to a rotary calcining furnace 2.
[0089] (2) Take 41 kg of waste cathode material powder including lithium iron phosphate (lithium iron phosphate mass percentage is 98%) and 27 kg of zirconium dioxide mass percentage of 98% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, and calcine at a speed of 30 rpm at a first heat treatment temperature of 450℃ for 60 minutes, and then transfer it to rotary calcining furnace 2;
[0090] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.32:1; the mass ratio of waste cathode material to zirconium dioxide is 1.52:1) for the second heat treatment: at a speed of 10 rpm, in a nitrogen atmosphere, calcined at 620°C for 180 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the atmosphere used for purging is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 47 μm.
[0091] The test results showed that the iron content in the obtained iron phosphate product was 36.7%, the phosphorus content was 20.9%, and the iron-phosphorus molar ratio was 0.972.
[0092] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1500°C for 150 minutes in an argon atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 25 mm.
[0093] Testing revealed that the lithium oxide composite material contained 99.2% lithium lanthanum zirconium oxide by mass.
[0094] Example 4
[0095] (1) Take 14 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 700℃ for calcination for 45 minutes before being transferred to a rotary calcining furnace 2.
[0096] (2) Take 23 kg of waste cathode material powder including lithium iron phosphate (lithium iron phosphate mass percentage is 93%) and 17 kg of zirconium dioxide mass content of 95% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, and calcine at a speed of 30 rpm at the first heat treatment temperature of 800℃ for 240 minutes, and then transfer them to rotary calcining furnace 2;
[0097] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.64:1; the mass ratio of waste cathode material to zirconium dioxide is 1.35:1) for a second heat treatment: at a speed of 20 rpm, in a mixed atmosphere of hydrogen and nitrogen (the volume ratio of hydrogen to nitrogen is 5:95), calcined at 750°C for 120 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the atmosphere used for purging is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 37.5 μm.
[0098] The test results showed that the iron content in the obtained iron phosphate product was 36.3%, the phosphorus content was 20.1%, and the iron-phosphorus molar ratio was 1.00.
[0099] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1200°C for 120 minutes in an argon atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 16 mm.
[0100] Testing revealed that the lithium oxide composite material contained 99.4% lithium lanthanum zirconium oxide by mass.
[0101] Example 5
[0102] (1) Take 15 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 800℃ for calcination for 15 minutes before transferring it to a rotary calcining furnace 2.
[0103] (2) Take 17 kg of waste cathode material powder including lithium iron phosphate (lithium iron phosphate mass percentage is 95%) and 15 kg of zirconium dioxide mass content of 96.5% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, and calcine at a speed of 5 rpm at the first heat treatment temperature of 450℃ for 120 minutes before transferring it to rotary calcining furnace 2;
[0104] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.13:1; the mass ratio of waste cathode material to zirconium dioxide is 1.13:1) for a second heat treatment: at a speed of 20 rpm, in a nitrogen atmosphere, calcined at 550°C for 120 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the atmosphere used for purging is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 23.6 μm.
[0105] The test results showed that the iron content in the obtained iron phosphate product was 36.6%, the phosphorus content was 20.1%, and the iron-phosphorus molar ratio was 1.00.
[0106] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1600°C for 15 minutes in a neon atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 14.5 mm.
[0107] Testing revealed that the lithium oxide composite material contained 99.6% lithium lanthanum zirconium oxide by mass.
[0108] Example 6
[0109] (1) Take 18 kg of lanthanum oxide with a mass content of 97% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 450℃ for calcination for 180 minutes before transferring it to a rotary calcining furnace 2.
[0110] (2) Take 24 kg of waste cathode material powder including lithium iron phosphate (lithium iron phosphate mass percentage is 93%) and 18 kg of zirconium dioxide mass content of 98% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, calcinate at a speed of 20 rpm at the first heat treatment temperature of 570℃ for 180 minutes and then transfer them to rotary calcining furnace 2;
[0111] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.33:1; the mass ratio of waste cathode material to zirconium dioxide is 1.33:1) for a second heat treatment: at a speed of 10 rpm, in a mixed atmosphere of hydrogen and argon (the volume ratio of hydrogen to argon is 10:90), after calcination at 650°C for 120 minutes, the materials are transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the atmosphere used for purging is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 126.3 μm.
[0112] The test results showed that the iron content in the obtained iron phosphate product was 35.8%, the phosphorus content was 20.3%, and the iron-phosphorus molar ratio was 0.977.
[0113] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1100°C for 22 minutes in a helium atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 27.3 mm.
[0114] Testing revealed that the lithium oxide composite material contained 99.2% lithium lanthanum zirconium oxide by mass.
[0115] Example 7
[0116] (1) Take 30 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 600℃ for calcination for 300 minutes before transferring it to a rotary calcining furnace 2.
[0117] (2) Take 24 kg of waste lithium iron phosphate cathode material powder (lithium iron phosphate mass percentage is 94%) and 16 kg of zirconium dioxide mass content of 98% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, calcinate at a speed of 20 rpm at the first heat treatment temperature of 650℃ for 240 minutes and then transfer them to rotary calcining furnace 2.
[0118] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 0.8:1; the mass ratio of waste cathode material to zirconium dioxide is 1.5:1) for the second heat treatment: at a speed of 18 rpm, in a nitrogen atmosphere, calcined at 600°C for 180 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the atmosphere used for purging is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 98.3 μm.
[0119] The test results showed that the iron content in the obtained iron phosphate product was 36.5%, the phosphorus content was 20.4%, and the iron-phosphorus molar ratio was 0.993.
[0120] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1080°C for 180 minutes in an argon atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 28 mm.
[0121] Testing revealed that the lithium oxide composite material contained 99.6% lithium lanthanum zirconium oxide by mass.
[0122] Example 8
[0123] (1) Take 16 kg of lanthanum oxide with a mass content of 96% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 980℃ for calcination for 20 minutes before transferring it to a rotary calcining furnace 2.
[0124] (2) Take 25 kg of waste cathode material powder including lithium iron phosphate (lithium iron phosphate mass percentage is 90%) and 19 kg of zirconium dioxide mass content of 98% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, and calcine at a speed of 15 rpm at the first heat treatment temperature of 750℃ for 120 minutes, and then transfer it to rotary calcining furnace 2;
[0125] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.56:1; the mass ratio of waste cathode material to zirconium dioxide is 1.32:1) for a second heat treatment: at a speed of 20 rpm, in an argon atmosphere, calcined at 650°C for 360 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the purging atmosphere is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 68.7 μm.
[0126] The test results showed that the iron content in the obtained iron phosphate product was 36.2%, the phosphorus content was 20.2%, and the iron-phosphorus molar ratio was 0.991.
[0127] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1200°C for 270 minutes in an argon atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 14.5 mm.
[0128] Testing revealed that the lithium oxide composite material contained 99.2% lithium lanthanum zirconium oxide by mass.
[0129] Example 9
[0130] (1) Take 21 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 300℃ for calcination for 120 minutes before transferring it to a rotary calcining furnace 2.
[0131] (2) Take 23 kg of waste cathode material powder including lithium iron phosphate (lithium iron phosphate mass percentage is 85%) and 17 kg of zirconium dioxide mass content of 92% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, and calcine at a speed of 15 rpm at the first heat treatment temperature of 400℃ for 180 minutes, and then transfer it to rotary calcining furnace 2;
[0132] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.10:1; the mass ratio of waste cathode material to zirconium dioxide is 1.35:1) for a second heat treatment: at a speed of 15 rpm, in a nitrogen atmosphere, calcined at 750°C for 120 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the atmosphere used for purging is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 35.8 μm.
[0133] The test results showed that the iron content in the obtained iron phosphate product was 35.9%, the phosphorus content was 20.7%, and the iron-phosphorus molar ratio was 0.962.
[0134] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1100°C for 120 minutes in a nitrogen atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 18.4 mm.
[0135] Testing revealed that the lithium oxide composite material contained 99.0% lithium lanthanum zirconium oxide by mass.
[0136] Example 10
[0137] (1) Take 11 kg of lanthanum oxide with a mass content of 92% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 100℃ for calcination for 120 minutes before transferring it to a rotary calcining furnace 2.
[0138] (2) Take 23 kg of waste cathode material powder including lithium iron phosphate (lithium iron phosphate mass percentage is 70%) and 17 kg of zirconium dioxide mass content of 92% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, calcinate at a speed of 5 revolutions per minute at the first heat treatment temperature of 80°C for 120 minutes and then transfer them to rotary calcining furnace 2;
[0139] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 2.09:1; the mass ratio of waste cathode material to zirconium dioxide is 1.35:1) for a second heat treatment: at a speed of 20 rpm, in an air atmosphere, calcined at 250°C for 60 minutes, then transferred to a rolling screen for sieving. The purging angle is adjusted to be perpendicular to the screen, and the purging atmosphere is the same as that used in the second heat treatment. The crude lithium oxide composite material and iron phosphate are separated. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 11.6 μm.
[0140] The test results showed that the iron content in the obtained iron phosphate product was 33.2%, the phosphorus content was 19.8%, and the iron-phosphorus molar ratio was 0.930.
[0141] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1100°C for 180 minutes in an air atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 12.7 mm.
[0142] Testing revealed that the lithium oxide composite material contained 97.3% lithium lanthanum zirconium oxide by mass.
[0143] Example 11
[0144] (1) Take 10 kg of lanthanum oxide with a mass content of 99% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 1000℃ for calcination for 5 minutes before transferring it to a rotary calcining furnace 2.
[0145] (2) Take 23 kg of waste lithium iron phosphate cathode material powder (lithium iron phosphate mass percentage is 65%) and 17 kg of zirconium dioxide mass content of 99% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, and calcine at a speed of 15 rpm for 60 minutes at the first heat treatment temperature of 950℃, and then transfer it to rotary calcining furnace 2.
[0146] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 2.3:1; the mass ratio of waste cathode material to zirconium dioxide is 1.92:1) for a second heat treatment: calcined at 900°C for 360 minutes at a speed of 20 rpm in a nitrogen atmosphere, and then transferred to a rolling screen for sieving to separate the crude lithium oxide composite material and iron phosphate. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 24.5 μm.
[0147] The test results showed that the iron content in the obtained iron phosphate product was 38.5%, the phosphorus content was 15.5%, and the iron-phosphorus molar ratio was 1.38.
[0148] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1800°C for 5 minutes in an argon atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 28.4 mm.
[0149] Testing revealed that the lithium oxide composite material contained 91.2% lithium lanthanum zirconium oxide by mass.
[0150] Example 12
[0151] (1) Take 20 kg of lanthanum oxide with a mass content of 98% and place it in an infrared calcining furnace for pretreatment. Nitrogen gas is continuously introduced and the temperature is raised to 100℃ for calcination for 120 minutes before transferring it to a rotary calcining furnace 2.
[0152] (2) Take 13 kg of waste lithium iron phosphate cathode material powder (lithium iron phosphate mass percentage is 92%) and 8 kg of zirconium dioxide mass content of 98% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment to prepare the first intermediate: continuously introduce air into rotary calcining furnace 1, turn on the heating, and calcinate at a speed of 15 rpm at the first heat treatment temperature of 870℃ for 120 minutes and then transfer them to rotary calcining furnace 2.
[0153] (3) The materials obtained in steps (1) and (2) are transferred into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 0.65:1; the mass ratio of waste cathode material to zirconium dioxide is 1.625:1) for a second heat treatment: calcined at 150°C for 360 minutes at a speed of 20 rpm in an air atmosphere, and then transferred to a rolling screen for sieving to separate the crude lithium oxide composite material and iron phosphate. The material on the screen is the crude lithium oxide composite material, and the material under the screen is collected to prepare iron phosphate. The particle size of iron phosphate is 26.9 μm.
[0154] The test results showed that the iron content in the obtained iron phosphate product was 32.0%, the phosphorus content was 22.3%, and the iron-phosphorus molar ratio was 0.936.
[0155] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace for the third heat treatment: calcined at 1700°C for 20 minutes in an air atmosphere, then transferred to a pulverizer for crushing and sieving, and the sieve material is collected to prepare the lithium oxide composite material. The particle size of the lithium oxide composite material is 8.7 mm.
[0156] Testing revealed that the lithium oxide composite material contained 90.3% lithium oxide by mass.
[0157] Comparative Example 1 (Comparison of the effects of using air in the first heat treatment versus not treating lanthanum oxide)
[0158] (1) Take 18 kg of lithium iron phosphate powder (lithium iron phosphate mass percentage is 99.5%) and 8 kg of zirconium dioxide mass content of 98% in a mixer, mix them evenly and then transfer them to rotary calcining furnace 1 for the first heat treatment: continuously introduce air, turn on the heating, calcinate at a speed of 10 rpm for 10 minutes and then transfer them to rotary calcining furnace 2.
[0159] (2) Take 11 kg of lanthanum oxide with a mass content of 98% and put it directly into rotary calcining furnace 2 (the mass ratio of waste cathode material to lanthanum oxide is 1.64:1; the mass ratio of waste cathode material to zirconium dioxide is 2.25:1); at a rotation speed of 5 rpm, calcined at 650℃ for 60 minutes, and then transferred to a rolling screen for screening. The material on the screen is the crude product of lithium oxide composite material. The material under the screen is collected to obtain iron phosphate with a particle size of 7.4 μm.
[0160] The tested product contained 33.0% iron and 19.3% phosphorus, with an iron-to-phosphorus ratio of 0.832.
[0161] (3) After purging the crude lithium oxide composite material collected in step (2), it is transferred to a pit furnace and calcined at 800°C for 30 minutes. Then it is transferred to a pulverizer for crushing and sieving. The sieve material is collected to obtain the lithium oxide composite material with a mass percentage of 73.1% of lithium, lanthanum, zirconium and oxygen.
[0162] Comparative Example 2
[0163] (1) Take 15 kg of lanthanum oxide with a mass content of 98% and pretreat it in an infrared calcining furnace. Nitrogen gas is continuously introduced and the temperature is raised to 100℃ for calcination for 60 minutes before transferring it to a rotary calcining furnace 2.
[0164] (2) Take 13 kg of lithium hydroxide octahydrate with a mass content of 98.5% and 19 kg of zirconium dioxide with a mass content of 98% in a mixer, mix them evenly, and then transfer them to rotary calcining furnace 1. Nitrogen gas is continuously introduced and heating is turned on. Calcine at 120°C for 180 minutes at a speed of 15 rpm, and then transfer them to rotary calcining furnace 2.
[0165] (3) Transfer the material obtained in steps (1) and (2) into the rotary calcining furnace 2. At a rotation speed of 15 revolutions per minute, calcine it at 750°C with air for 120 minutes. Collect the product, which is the crude product of lithium oxide composite material.
[0166] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace and calcined at 1050°C for 5 minutes. After pulverizing and sieving, the material under the sieve is collected to prepare the lithium oxide composite material with a mass percentage of 45.3% of lithium, lanthanum, zirconium and oxygen.
[0167] Comparative Example 3
[0168] (1) Take 17.5 kg of lanthanum oxide with a mass content of 98.1% and put it in an infrared calcining furnace. Nitrogen gas is continuously introduced and the temperature is raised to 120℃ for calcination for 60 minutes. Then transfer it to a rotary calcining furnace 2.
[0169] (2) Take 25 kg of lithium carbonate with a mass content of 99.5% and 16 kg of zirconium dioxide with a mass content of 97.5% in a mixer, mix them evenly, and then transfer them to rotary calcining furnace 1. Continuously introduce air, turn on the heating, and calcine at 180°C for 135 minutes at a speed of 15 rpm. Then transfer them to rotary calcining furnace 2.
[0170] (3) Transfer the material obtained in steps (1) and (2) into the rotary calcining furnace 2. Calcinate at 700°C for 160 minutes at a rotation speed of 15 rpm. The collected product is the crude lithium oxide composite material.
[0171] (4) After purging the crude lithium oxide composite material collected in step (3), it is transferred to a pit furnace and calcined at 1100℃ for minutes. Then it is transferred to a pulverizer for crushing and sieving. The sieve material is collected to prepare lithium oxide composite material with a mass percentage of 65.4% of lithium, lanthanum, zirconium and oxygen.
[0172] As can be seen from Examples 1-12 and Comparative Examples 1-3, the recovery method of this application yields iron phosphate with a suitable iron-to-phosphorus ratio and high purity lithium oxide composite material. The preparation method of Comparative Example 1 does not include the step of heat-treating lanthanum oxide. In the preparation methods of Comparative Examples 2-3, lithium iron phosphate is not included as a raw material, resulting in lower purity of lithium lanthanum zirconium oxide in the prepared lithium oxide composite product, and higher cost. This demonstrates that the preparation method of this application can recover lithium iron phosphate at a low cost, with high utilization of lithium and iron sources, and can produce high-purity iron phosphate and lithium lanthanum zirconium oxide.
[0173] The temperature and / or time of infrared heating treatment affect the iron-to-phosphorus ratio of ferric phosphate and the purity of lithium lanthanum zirconium oxide. As can be seen from Examples 1 to 12, by adjusting the temperature and / or time of infrared heating treatment within the range of this application, the prepared ferric phosphate has a suitable iron-to-phosphorus ratio, and the purity of lithium lanthanum zirconium oxide is relatively high. This demonstrates that adjusting the temperature and / or time of infrared heating treatment within the range of this application is beneficial for obtaining ferric phosphate with a suitable iron-to-phosphorus ratio and lithium lanthanum zirconium oxide with high purity. The temperature and / or time of the first heat treatment also affect the iron-to-phosphorus ratio of ferric phosphate and the purity of lithium lanthanum zirconium oxide. As can be seen from Examples 1 to 12, by adjusting the temperature and / or time of the first heat treatment within the range of this application, the prepared ferric phosphate has a suitable iron-to-phosphorus ratio, and the purity of lithium lanthanum zirconium oxide is relatively high. This demonstrates that adjusting the temperature and / or time of the first heat treatment within the range of this application is beneficial for obtaining ferric phosphate with a suitable iron-to-phosphorus ratio and lithium lanthanum zirconium oxide with high purity.
[0174] The temperature and / or time of the second heat treatment affect the iron-to-phosphorus ratio of ferric phosphate and the purity of lithium lanthanum zirconium oxide. As can be seen from Examples 1 to 12, by adjusting the temperature and / or time of the second heat treatment within the range of this application, the particle size of the prepared ferric phosphate particles is within the range of this application, the iron-to-phosphorus ratio is suitable, and the purity of lithium lanthanum zirconium oxide is high. This demonstrates that adjusting the temperature and / or time of the second heat treatment within the range of this application is beneficial for obtaining ferric phosphate with a suitable iron-to-phosphorus ratio and lithium lanthanum zirconium oxide with high purity.
[0175] The temperature and / or time of the third heat treatment affect the purity of lithium lanthanum zirconium oxide. As can be seen from Examples 1 to 12, by adjusting the temperature and / or time of the third heat treatment within the range of this application, the particle size of the prepared lithium lanthanum zirconium oxide particles is within the range of this application, and the purity is consistently high. This demonstrates that adjusting the temperature and / or time of the third heat treatment within the range of this application is beneficial for obtaining lithium lanthanum zirconium oxide with high purity.
[0176] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0177] The embodiments described above are merely examples of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for recovering lithium iron phosphate, characterized in that, Includes the following steps: Lanthanum oxide is pretreated to remove water and carbon dioxide. Waste cathode material, including lithium iron phosphate, is mixed with zirconium dioxide and subjected to a first heat treatment to prepare a first intermediate. The first intermediate was mixed with the pretreated lanthanum oxide and subjected to a second heat treatment. After purging and sieving, crude lithium oxide composite material and iron phosphate were prepared. The crude lithium oxide composite material is subjected to a third heat treatment, crushed, and sieved to prepare the lithium oxide composite material. The temperature of the third heat treatment is higher than the temperature of the second heat treatment.
2. The recycling method according to claim 1, characterized in that, The mass ratio of the waste cathode material including lithium iron phosphate to zirconium dioxide is (1.13~1.52):1; and / or, the mass ratio of the waste cathode material including lithium iron phosphate to lanthanum oxide is (0.80~2.09):
1.
3. The recycling method according to claim 1, characterized in that, The waste cathode material including lithium iron phosphate has a lithium iron phosphate content of 65% to 99.5% by mass.
4. The recycling method according to claim 1, characterized in that, The pretreatment step includes: subjecting lanthanum oxide to infrared heating treatment in a protective atmosphere at a temperature of 300°C to 980°C; optionally, the infrared heating treatment time is 5 min to 300 min.
5. The recycling method according to claim 1, characterized in that, The temperature of the first heat treatment is 400℃~800℃; optionally, the first heat treatment is carried out in air; optionally, the time of the first heat treatment is 30min~240min.
6. The recycling method according to claim 1, characterized in that, The temperature of the second heat treatment is 300℃~750℃; optionally, the second heat treatment is carried out in a protective atmosphere; optionally, the time of the second heat treatment is 120min~480min.
7. The recycling method according to claim 1, characterized in that, The temperature of the third heat treatment is 1050℃~1600℃; optionally, the third heat treatment is carried out in a protective atmosphere; optionally, the time of the third heat treatment is 15min~480min.
8. The recycling method according to any one of claims 1 to 7, characterized in that, The first heat treatment and / or the second heat treatment are carried out in a rotary kiln, the rotary kiln rotating at a speed of 2 rpm to 30 rpm.
9. The recycling method according to any one of claims 1 to 7, characterized in that, The recycling method includes at least one of the following features: (1) The particle size of the iron phosphate particles is smaller than the particle size of the crude lithium oxide composite material; (2) The particle size of the iron phosphate particles is 3μm~130μm; (3) The particle size of the lithium oxide composite material is 10 mm to 30 mm.