A CVD preparation method for all-carbon single-layer-multilayer graphene PN junctions
By adjusting the hydrogen flow rate to control the partial pressure and transport of methane, an all-carbon single-layer to multi-layer graphene PN junction was prepared, solving the problem of graphene layer thickness control and achieving controllable and highly reproducible PN junction fabrication, which is suitable for the construction of devices such as field-effect transistors and photodetectors.
Patent Information
- Application Number
- CN202611520620.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing chemical vapor deposition (CVD) methods are difficult to achieve uniform control of graphene layer thickness, resulting in random coexistence of single-layer and multi-layer structures, making it impossible to controllably prepare PN junctions. Furthermore, the mechanism by which hydrogen flow affects carbon source transport is unclear, leading to poor steepness and low reproducibility of homojunction interfaces.
By adjusting the hydrogen flow rate to change the methane partial pressure and transport efficiency in the reaction system, adjacent monolayer and multilayer graphene regions were formed on the liquid copper surface. The sample was then transferred to a SiO2/Si substrate using a polymethyl methacrylate-assisted transfer method to prepare an all-carbon monolayer-multilayer graphene PN junction.
It achieves precise regional control of graphene layer thickness, constructs a clear PN junction interface, improves repeatability, solves the problem of random and uncontrollable layer thickness in traditional processes, and establishes a correlation mechanism between hydrogen flow rate, carbon concentration, and layer thickness distribution, which is applicable to the fabrication of devices such as field-effect transistors and photodetectors.
Smart Images

Figure CN123105618A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nanomaterial preparation technology, and in particular to a CVD preparation method for an all-carbon single-layer-multilayer graphene PN junction. Background Technology
[0002] Graphene's excellent electrical, mechanical, and thermal properties make it a promising candidate for applications in high-frequency transistors, flexible sensors, and transparent conductive films. The thickness of graphene layers directly determines its band structure: monolayer graphene is a zero-bandgap half-metal, bilayer graphene can have its bandgap opened by electric field modulation, and multilayer graphene approximates the bulk properties of graphite. Therefore, constructing monolayer-multilayer PN junctions within the same graphene domain enables in-situ integration of different functional regions, forming the core foundation for fabricating high-performance graphene-based heterogeneous integrated devices.
[0003] Currently, chemical vapor deposition (CVD) is the mainstream technology for preparing large-area, high-quality graphene, but existing growth processes generally suffer from the following problems: (1) The uniformity of graphene layer thickness is difficult to control. Single-layer and multi-layer structures are mostly randomly coexisting, making it impossible to achieve controllable preparation of PN junctions. (2) Layer thickness control relies on the adjustment of a single parameter, such as carbon source concentration and growth temperature, and lacks precise control of the fluid transport process, resulting in poor steepness of the homojunction interface and low reproducibility. (3) Hydrogen is the main gas in CVD growth, but the mechanism by which its flow rate affects carbon source transport and substrate surface reaction kinetics is not yet clear, which limits its application in layer thickness control. Summary of the Invention
[0004] The purpose of this invention is to provide a CVD preparation method for all-carbon single-layer to multi-layer graphene PN junctions, which achieves regional precise control of graphene layer thickness by adjusting the hydrogen flow rate to change the methane partial pressure and transport efficiency in the reaction system.
[0005] To achieve the above objectives, this invention provides a CVD preparation method for an all-carbon single-layer / multilayer graphene PN junction, comprising the following steps: S1. Graphene is grown in a dual-temperature tube furnace using chemical vapor deposition with liquid copper as the growth substrate and methane as the carbon source. During the graphene growth process, the hydrogen flow rate is controlled to form adjacent single-layer and multi-layer graphene regions on the surface of the liquid copper. S2. After growth, the sample is cooled and removed. The sample is then transferred to a SiO2 / Si substrate using a polymethyl methacrylate-assisted transfer method to obtain a chemically doped all-carbon monolayer-multilayer graphene PN junction.
[0006] Preferably, step S1 includes the following: S11. Send the quartz tube into the dual-temperature tube furnace, place the quartz boat containing copper foil and tungsten sheets in the center of the high-temperature zone downstream of the carrier gas flow, and connect the methane gas interface to the gas inlet of the quartz tube. S12. Seal the dual-temperature tube furnace, evacuate to a system pressure of 0.1 Pa, and introduce 500 sccm of high-purity argon gas to atmospheric pressure; repeat the evacuation and argon filling to atmospheric pressure 3-5 times to remove air and impurity gases from the system. S13. Set a heating program for the high-temperature zone of the dual-temperature tube furnace to melt the copper foil into a liquid copper growth substrate. During the growth stage, hydrogen is introduced as a reducing gas, while methane is introduced as a carbon source and argon as a carrier gas. The effective concentration of methane in the reaction chamber is controlled by adjusting the hydrogen flow rate to carry out graphene growth.
[0007] Preferably, in S13, the temperature is raised to 1100℃ to melt the copper foil, and 200 sccm of hydrogen is introduced to reduce the liquid copper for 40 min; during the growth stage, 10 sccm of methane and 500 sccm of argon are introduced, and the hydrogen flow rate is 50~150 sccm, and the temperature is maintained for 15 min; after the growth is completed, it is naturally cooled to room temperature.
[0008] Preferably, in S1, the hydrogen flow rate is adjusted as follows: In the low hydrogen flow mode, with a hydrogen flow rate of 60 sccm, a large area of monolayer graphene was obtained, while a small amount of multilayer graphene formed by carbon enrichment was found at the edge of the copper foil. In the medium hydrogen flow mode, with a hydrogen flow rate of 100 sccm, an all-carbon PN junction with alternating single-layer and multi-layer graphene was obtained. In the high hydrogen flow mode, with a hydrogen flow rate of 150 sccm, a large-area multilayer graphene substrate was obtained, as well as a single-layer island-like graphene structure formed locally at the edge of the copper foil due to carbon depletion.
[0009] Preferably, the tungsten sheet is used to support the copper foil wetting process, and the tungsten sheet can be replaced by a molybdenum sheet; all gas sources have a purity of ≥99.999%.
[0010] The present invention also provides an all-carbon single-layer to multi-layer graphene PN junction prepared by the method, comprising a SiO2 / Si substrate and a graphene PN junction located on the SiO2 / Si substrate; the graphene PN junction is an in-situ integrated structure of single-layer graphene regions and double-layer or more multi-layer graphene regions within the same continuous crystal domain, the surface potential difference between the single-layer graphene regions and the multi-layer graphene regions is 40~60meV, and an in-plane PN junction is formed at the interface; the PN junction is an all-carbon PN junction and does not contain heterogeneous element chemical doping.
[0011] In this invention, graphene growth is achieved through variations in hydrogen flow rate. By controlling the methane partial pressure and the diffusion length of carbon atoms on the substrate surface, the nucleation density and layer thickness of the graphene are determined. Specifically, the effect of hydrogen flow rate on the layer distribution of CVD graphene is as follows: Under low hydrogen partial pressure conditions, the reduction degree of the liquid copper substrate is moderate, and active carbon species are mainly used for the in-plane growth of graphene grains in the lateral direction. Secondary nucleation is effectively suppressed, resulting in a high proportion of monolayer graphene. Under medium hydrogen flow rate conditions, the degree of methane cracking increases, and some active carbon on the liquid copper surface undergoes secondary nucleation on the already formed graphene surface, resulting in the coexistence of monolayer and multilayer graphene. Under high hydrogen flow rate conditions, hydrogen further promotes methane cracking, and the strong reduction effect causes carbon dissolved in the liquid copper to precipitate, reconstructing the copper-carbon interface and causing local atomic height fluctuations on the liquid copper surface. A large amount of active carbon induces secondary nucleation on the graphene surface, driving vertical stacking growth, with the sample mainly consisting of multilayer graphene. Although hydrogen atoms have an etching effect on graphene, this etching preferentially removes small, unstable nuclei and cannot suppress the secondary nucleation of multiple layers on the surface of large graphene domains. Ultimately, this results in the growth of long monolayers with low hydrogen flow rates, long mono-multilayers with medium hydrogen flow rates, and long multilayers with high hydrogen flow rates.
[0012] Therefore, the CVD preparation method for an all-carbon single-layer-multilayer graphene PN junction described above has the following beneficial effects: 1) By adjusting the hydrogen flow rate on the liquid copper surface to change the methane partial pressure and transport dynamics in the reaction system, in-situ integration of single-layer and multi-layer graphene within the same crystal domain was achieved. The PN junction interface is clear and highly repeatable, solving the problem of random and uncontrollable layer thickness in traditional processes.
[0013] 2) The correspondence between hydrogen flow rate, carbon concentration, and layer thickness distribution was clarified, and the correlation mechanism between fluid parameters and graphene growth kinetics was established, providing a new approach for the controllable preparation of two-dimensional materials.
[0014] 3) The process is compatible with existing CVD equipment, is simple to operate, and has strong scalability. The prepared graphene PN junction can be used to construct devices such as field-effect transistors and photodetectors, and has broad application prospects.
[0015] 4) It provides an ideal material model for studying the thickness-dependent physical properties of graphene layers, and can also be extended to other two-dimensional materials (such as h-BN and transition metal chalcogenides), and has universal applicability.
[0016] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0017] Figure 1This is a schematic diagram of the mechanism of growing single-layer and multi-layer graphene on a copper substrate after high-temperature melting treatment in the embodiments of the present invention, and optical micrographs under different hydrogen flow rates. Figure 2 These are optical micrographs and area ratio comparison diagrams of the growth of single-layer graphene and multi-layer graphene under different hydrogen flow rates in the embodiments of the present invention. Figure 3 These are the optical morphology, Raman spectrum, and Raman surface scan of the all-carbon single-layer-multilayer graphene PN junction in this embodiment of the invention. Figure 4 This is a schematic diagram of the potential distribution, potential curve, and band structure of the all-carbon single-layer-multilayer graphene PN junction in an embodiment of the present invention. Figure 5 This is a schematic diagram of the structure and electrical test curves of the all-carbon single-layer-multilayer graphene PN junction device in an embodiment of the present invention, where 1, 1', 2, and 2' are all electrodes. Detailed Implementation
[0018] The technical solutions of the present invention will be further described below with reference to the accompanying drawings and embodiments. Unless otherwise defined, the technical or scientific terms used in this invention should be understood in their ordinary sense by those skilled in the art. The described embodiments are some, but not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0019] In this invention, the all-carbon monolayer-multilayer graphene PN junction refers to a structure in which monolayer graphene regions and double-layer or higher multilayer graphene regions coexist within the same continuous graphene domain. Both monolayer and multilayer graphene are graphene materials without heterogeneous element doping, thus belonging to an all-carbon structure. Due to the differences in work function and surface potential between monolayer and multilayer graphene, band bending occurs at their interface, thereby forming an in-plane PN junction.
[0020] like Figure 1 The diagram shows the mechanism of growing monolayer and multilayer graphene on a copper substrate after high-temperature melting treatment under different hydrogen flow rates, as well as optical micrographs under different hydrogen flow rates. Low hydrogen flow rate results in monolayer graphene as the main component; medium hydrogen flow rate results in a coexistence of monolayer and multilayer graphene; and high hydrogen flow rate results in multilayer graphene as the main component.
[0021] Example 1: Preparation of monolayer graphene with low hydrogen flow rate.
[0022] This embodiment uses a low hydrogen flow rate mode to prepare monolayer graphene. The specific steps are as follows: S11, Substrate loading: Fix a 50μm thick copper foil onto a tungsten sheet (the tungsten sheet can be replaced with a molybdenum sheet) and place it in a quartz boat; push the quartz boat into the center of the high-temperature zone of the dual-temperature tube furnace, which is located downstream of the carrier gas flow; connect the methane gas inlet to the inlet end of the quartz tube.
[0023] S12. Vacuuming and Purging: In a sealed dual-temperature tube furnace, evacuate to a system pressure of 0.1 Pa; then introduce 500 sccm of high-purity argon gas to atmospheric pressure; repeat the evacuation and argon purging to atmospheric pressure three times to remove air and impurities from the system. All gas sources used must have a purity ≥99.999% to avoid interference from impurities on the quality of the graphene.
[0024] S13. Heating and Reduction: Set a heating program for the high-temperature zone of the dual-temperature tube furnace, heating to 1100℃ at 20℃ / min, so that the copper foil is immersed and melted on the tungsten sheet to form a liquid copper growth substrate; introduce 200 sccm of hydrogen gas to reduce the liquid copper for 40 min.
[0025] S14. Graphene Growth: After reduction, 10 sccm of methane was introduced as the carbon source and 500 sccm of argon as the carrier gas, while the hydrogen flow rate was adjusted to 60 sccm. The system was kept at room temperature for 15 minutes. The system was kept at atmospheric pressure during the growth process.
[0026] S15. Cooling and Transfer: After growth, the sample was naturally cooled to room temperature and removed. The graphene sample was transferred to a SiO2 / Si substrate using a conventional polymethyl methacrylate-assisted transfer method to obtain all-carbon monolayer graphene.
[0027] Example 2: Preparation of all-carbon monolayer-multilayer graphene PN junctions with alternating monolayer and multilayer distributions using medium hydrogen flow rate.
[0028] This embodiment uses a medium hydrogen flow rate mode to prepare all-carbon single-layer-multilayer graphene PN junctions. The pretreatment steps are the same as in Example 1, except that the hydrogen flow rate in S14 is adjusted to 100 sccm, and the remaining growth parameters, including growth temperature, methane flow rate, argon flow rate, and growth time, are completely consistent with those in Example 1 to ensure that the hydrogen flow rate is the only variable.
[0029] Example 3: Preparation of graphene with multilayer structure and localized single-layer island structure by high hydrogen flow rate.
[0030] This embodiment uses a high hydrogen flow rate mode to prepare multilayer graphene. The pretreatment steps are the same as in Example 1, except that the hydrogen flow rate in S14 is adjusted to 150 sccm, and the remaining growth parameters, including growth temperature, methane flow rate, argon flow rate, and growth time, are completely consistent with those in Example 1 to ensure that the hydrogen flow rate is the only variable.
[0031] The products prepared in Examples 1-3 were tested, and it was found that the area ratio of single-layer graphene to multilayer graphene could be changed by adjusting the hydrogen flow rate during the chemical vapor deposition process. Figure 2 As shown, when the hydrogen flow rate is 60 sccm, the area ratio of monolayer graphene is close to 100%; multilayer graphene mainly appears at local edges or in carbon-rich regions. When the hydrogen flow rate is 100 sccm, the area ratio of monolayer graphene is approximately 40%, and the area ratio of multilayer graphene is approximately 60%, with both monolayer and multilayer graphene coexisting; when the hydrogen flow rate is 150 sccm, the area ratio of multilayer graphene is close to 100%. Therefore, by changing the hydrogen flow rate, adjacent monolayer and multilayer graphene regions can be controllably formed on the same liquid copper surface, with a chemically undoped all-carbon PN junction formed between the two regions.
[0032] The morphology and structure of the prepared single-layer graphene and multi-layer graphene were characterized. Figure 3 Figure a shows an optical microscope image of hexagonal graphene grains on a silicon wafer substrate. Single-layer and multi-layer graphene exhibit hexagonal grain morphology, and the yellow dashed box indicates the selected area for Raman testing. Figure 3 Figure b shows typical Raman spectra of monolayer graphene (black curve) and multilayer graphene (red curve). The Raman spectra show that both monolayer and multilayer graphene have G peaks and 2D peaks, but their peak shapes and intensities differ, which can be used to distinguish between monolayer and multilayer graphene. Different layer thicknesses are specifically shown in the Raman spectra as follows: in monolayer regions, the 2D peak is symmetrical, and the half-maximum width is <40 cm⁻¹. -1 The 2D / G intensity ratio is >2; the 2D peak in the bilayer region is broadened to fit the Lorentz peak, and the 2D / G intensity ratio is 1~2; the 2D peak in the three-layer and above regions is further broadened, and the 2D / G intensity ratio is <1; the absence of obvious D peaks indicates that the graphene sample has good crystallization quality. Figure 3 Figure c shows the 2D peak half-width (FWHM) Raman surface scan imaging of graphene domains. The blue area represents monolayer graphene, and the red-yellow area corresponds to multilayer graphene. The Raman surface scan image can intuitively show the distribution of monolayer and multilayer regions.
[0033] like Figure 4 As shown, surface potential scanning was performed on single-layer graphene and multilayer graphene. Figure 4 Figure a shows an optical microscope image of the graphene sample, with the white dashed box indicating the Kelvin probe force microscopy (KPFM) test area. Figure 4 Figure b shows the surface potential scan of the corresponding region using KPFM, with a potential scan range of -115.8 mV to 130.0 mV. The white dashed line corresponds to the surface potential line scan curve across the monolayer-multilayer graphene interface. Furthermore, the potential variation curve with position shows that the potential difference between the monolayer graphene region and the multilayer graphene region is 55 meV. Figure 4(Figure c in the diagram). Based on the schematic diagram of band bending ( Figure 4 As shown in Figure d, there is a shift in the Fermi level, conduction band, and valence band between monolayer graphene and multilayer graphene. This band shift causes monolayer graphene and multilayer graphene to form a PN junction.
[0034] Example 4: Fabrication and Electrical Verification of All-Carbon Single-Layer / Multi-Layer Graphene PN Junction Devices This embodiment uses the medium hydrogen flow rate sample prepared in Example 2 as an example to construct an all-carbon monolayer-multilayer graphene PN junction device and perform electrical verification. The all-carbon monolayer-multilayer graphene PN junction sample transferred to a SiO2 / Si substrate was photolithographically etched, and electrodes were set to obtain the all-carbon monolayer-multilayer graphene PN junction device. For example... Figure 5 As shown, the device includes four electrodes: electrode 1, electrode 1', electrode 2, and electrode 2'. Electrode 1 and electrode 1' form a first electrode pair, and electrode 2 and electrode 2' form a second electrode pair. Figure 5 Figure a shows an optical microscope image of the fabricated PN junction device; the three-dimensional structure of the device is as follows. Figure 5 As shown in b, it consists of a SiO2 / Si substrate, a graphene conductive channel, and a gold contact electrode.
[0035] Electrical testing: The electrical transport characteristics of the device are tested using a semiconductor parameter analyzer. For example... Figure 5 As shown in Figure c, the output characteristic curves of different electrode pairs exhibit a linear relationship in the range of -1V to 1V, indicating that a good ohmic contact is formed between the metal electrode and the graphene. (Fixed source-drain voltage V) DS =0.5V, and test the transfer characteristic curves of different electrode pairs. For example Figure 5 As shown in d, the electrode pair across the monolayer-multilayer graphene interface exhibits double Dirac points, proving that P-type and N-type regions exist simultaneously within the graphene channel, i.e., an in-plane PN junction has been successfully formed between the monolayer graphene region and the multilayer graphene region.
[0036] Therefore, this invention employs the aforementioned CVD preparation method for all-carbon monolayer-multilayer graphene PN junctions. By controlling only the hydrogen flow rate—a single variable—it alters the methane partial pressure on the liquid copper surface and the transport and diffusion behavior of carbon species. This allows for the controllable formation of adjacent monolayer and multilayer graphene regions within the same continuous graphene domain, constructing a chemically doped all-carbon in-plane PN junction. This method eliminates the need for heteroelement doping, resulting in a clear and highly reproducible PN junction interface. It effectively solves the problems of random coexistence of monolayer and multilayer graphene and the difficulty in controlling the layer thickness in traditional CVD processes. Furthermore, it establishes a correspondence between hydrogen flow rate, carbon concentration, and layer thickness distribution. The process is compatible with existing CVD equipment, simple to operate, and highly scalable. The prepared all-carbon monolayer-multilayer graphene PN junctions can be directly used in graphene-based electronic devices such as field-effect transistors and photodetectors, providing a new material foundation and approach for the controllable preparation and homogeneous integration of two-dimensional material homojunctions.
[0037] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A CVD preparation method for an all-carbon single-layer / multilayer graphene PN junction, characterized in that, Includes the following steps: S1. Graphene is grown in a dual-temperature tube furnace using chemical vapor deposition with liquid copper as the growth substrate and methane as the carbon source. During the graphene growth process, the hydrogen flow rate is controlled to form adjacent single-layer and multi-layer graphene regions on the surface of the liquid copper. S2. After growth, the sample is cooled and removed. The sample is then transferred to a SiO2 / Si substrate using a polymethyl methacrylate-assisted transfer method to obtain a chemically doped all-carbon monolayer-multilayer graphene PN junction.
2. The CVD preparation method for an all-carbon single-layer / multilayer graphene PN junction according to claim 1, characterized in that, Step S1 includes the following: S11. Send the quartz tube into the dual-temperature tube furnace, place the quartz boat containing copper foil and tungsten sheets in the center of the high-temperature zone downstream of the carrier gas flow, and connect the methane gas interface to the gas inlet of the quartz tube. S12. Seal the dual-temperature tube furnace, evacuate to a system pressure of 0.1 Pa, and introduce 500 sccm of high-purity argon gas to atmospheric pressure; repeat the evacuation and argon filling to atmospheric pressure 3-5 times to remove air and impurity gases from the system. S13. Set a heating program for the high-temperature zone of the dual-temperature tube furnace to melt the copper foil into a liquid copper growth substrate. During the growth stage, hydrogen is introduced as a reducing gas, while methane is introduced as a carbon source and argon as a carrier gas. The effective concentration of methane in the reaction chamber is controlled by adjusting the hydrogen flow rate to carry out graphene growth.
3. The CVD preparation method for an all-carbon single-layer / multilayer graphene PN junction according to claim 2, characterized in that, In S13, the temperature is raised to 1100℃ to melt the copper foil, and 200 sccm of hydrogen gas is introduced to reduce the liquid copper for 40 min. During the growth stage, 10 sccm of methane and 500 sccm of argon gas are introduced, and the hydrogen gas flow rate is 50~150 sccm. The temperature is maintained for 15 min. After the growth is completed, the temperature is naturally cooled to room temperature.
4. The CVD preparation method for an all-carbon single-layer / multilayer graphene PN junction according to claim 1, characterized in that, In S1, the hydrogen flow rate is specifically controlled as follows: In the low hydrogen flow mode, with a hydrogen flow rate of 60 sccm, a large area of monolayer graphene was obtained, while a small amount of multilayer graphene formed by carbon enrichment was found at the edge of the copper foil. In the medium hydrogen flow mode, with a hydrogen flow rate of 100 sccm, an all-carbon PN junction with alternating single-layer and multi-layer graphene was obtained. In the high hydrogen flow mode, with a hydrogen flow rate of 150 sccm, a large-area multilayer graphene substrate was obtained, as well as a single-layer island-like graphene structure formed locally at the edge of the copper foil due to carbon depletion.
5. The CVD preparation method for an all-carbon single-layer / multilayer graphene PN junction according to claim 2, characterized in that, The tungsten sheet is used to support the copper foil wetting process; the tungsten sheet can be replaced by a molybdenum sheet; the purity of all gas sources is ≥99.999%.
6. A fully carbon monolayer-multilayer graphene PN junction prepared by the method according to any one of claims 1 to 5, characterized in that, It includes a SiO2 / Si substrate and a graphene PN junction located on the SiO2 / Si substrate; the graphene PN junction is an in-situ integrated structure of a single-layer graphene region and a double-layer or more multi-layer graphene region within the same continuous crystal domain, the surface potential difference between the single-layer graphene region and the multi-layer graphene region is 40~60meV, and an in-plane PN junction is formed at the interface; the PN junction is an all-carbon PN junction and does not contain heterogeneous element chemical doping.