A method for preparing anthracite silicon-carbon anode material

By using anthracite to prepare silicon-carbon anode materials, and combining gradient carbonization, steam activation and fluidized bed CVD processes, the volume expansion and cycle performance problems of silicon-based anode materials have been solved, realizing high-capacity, low-expansion and long-life lithium-ion battery anode materials, which are suitable for power batteries, consumer batteries and energy storage batteries.

CN123105633APending Publication Date: 2026-11-17JIANGSU MICRO CARBON TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611394301.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicon-based anode materials in lithium-ion batteries suffer from rapid pulverization and detachment due to volume expansion, resulting in poor cycle performance. Furthermore, traditional carbon carrier raw materials are costly and difficult to control in terms of pore structure, limiting their application scenarios and performance.

Method used

Industrial anthracite is used to replace high-cost carbon sources. A graded porous carbon carrier is constructed by combining gradient carbonization and steam activation processes. Silicon source is deposited by fluidized bed CVD, and then asphalt coating is used to form a uniform carbon shell, which buffers volume expansion and improves conductivity.

Benefits of technology

A high-specific-capacity, low-expansion, and long-cycle anthracite silicon-carbon anode material has been developed, which can be used alone as a lithium battery anode. This improves the structural stability and electrochemical performance of the material and makes it suitable for various lithium-ion battery applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application relates to the field of new energy storage electrode materials technology, specifically disclosing a method for preparing anthracite silicon-carbon anode materials. The method includes the following steps: first, the raw coal is crushed, screened, and subjected to composite acid washing and deashing pretreatment; then, it undergoes gradient carbonization treatment at 700-1800℃; followed by steam activation treatment to create pores; acid-base neutralization to remove impurities; airflow pulverization and fluidized bed CVD silicon deposition; finally, the silicon-carbon is coated with pitch to obtain the final product. The anthracite silicon-carbon anode material prepared by the method of this application combines the high specific capacity of silicon with the high conductivity and structural stability of carbon materials, exhibiting electrochemical performance superior to traditional commercial silicon-carbon materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of new energy storage electrode materials technology, and more specifically, it relates to a method for preparing anthracite silicon-carbon anode material. Background Technology

[0002] Lithium-ion batteries, due to their high energy density, long cycle life, and excellent safety performance, are now widely used in smartphones, laptops, new energy vehicles, low-altitude aircraft, and grid energy storage. As downstream end-products continue to upgrade, the industry is placing higher demands on the energy density, cycle stability, and production cost of lithium batteries.

[0003] Traditional graphite anodes have a theoretical specific capacity of only 372 mAh / g, which is close to the theoretical upper limit and cannot meet the development requirements of high-energy-density batteries. Silicon-based anodes have a theoretical specific capacity of up to 4200 mAh / g and are the core material for next-generation high-capacity anodes. However, silicon undergoes a volume expansion of up to about 300% during lithium-ion insertion and extraction, which easily causes the active material of the electrode to pulverize and fall off, ultimately leading to a rapid decline in battery cycle performance and restricting the large-scale application of pure silicon anodes.

[0004] Currently, the mainstream solution in the industry is to use chemical vapor deposition (CVD) combined with porous carbon supports to prepare silicon-carbon composite materials. The spatial confinement effect of the carbon support buffers the volume deformation of silicon, and this route has achieved initial industrialization. Regarding the aforementioned technologies, the inventors believe that existing commercial silicon-carbon materials generally have technical defects. First, carbon supports mostly use raw materials such as petroleum coke and resin, resulting in high raw material costs. Second, controlling the pore structure of carbon supports is difficult, and the purification process is complex. Furthermore, existing finished silicon-carbon products cannot be used alone as a negative electrode; they can only be added to graphite at a ratio of 3-15% as an auxiliary material, limiting their application scenarios and performance. Summary of the Invention

[0005] This application aims to provide a method for preparing anthracite silicon-carbon anode material. The prepared anthracite silicon-carbon anode material can have high specific capacity, low expansion and long cycle characteristics, and can be used alone as a lithium battery anode.

[0006] Firstly, this application provides a method for preparing anthracite-based silicon-carbon anode material, employing the following technical solution: A method for preparing anthracite-based silicon-carbon anode material includes the following steps: S1: Industrial anthracite is selected as raw material. After mechanical crushing and screening, anthracite particles with uniform particle size are obtained. Then, they are soaked in an acid solution, and then washed and dried to obtain pretreated anthracite particles. S2: Under the protection of an inert gas atmosphere, the pretreated anthracite particles are subjected to gradient carbonization treatment at 700-1800℃; S3: Under the protection of an inert gas atmosphere, the carbonized anthracite particles are activated by steam to obtain the activated product; S4: Add dilute acid to the activated product and stir, then wash and dry to obtain a porous carbon support. S5: The porous carbon support is subjected to ultrafine pulverization and then fed into a fluidized bed CVD equipment. Carrier gas and silicon source gas are introduced, and a vapor phase deposition reaction is carried out at 600-900℃ to obtain anthracite-based silicon-carbon anode material.

[0007] This application selects industrial anthracite to replace traditional high-cost carbon sources such as petroleum coke and resins. The raw materials are abundant and inexpensive, significantly reducing the raw material cost of silicon-carbon anodes from the source, making it suitable for large-scale industrial production. By adopting the above technical solution, a gradient carbonization process is combined with a steam activation process to construct a hierarchical porous matrix with graphitized crystalline regions and non-graphitized carbon regions. The gradient carbonization process simultaneously enhances the graphitization of the pore walls and retains the non-graphitized active sites, providing a stable matrix structure for subsequent activation and pore formation. The steam activation process directionally constructs a hierarchical porous structure, buffering the volume expansion during silicon charging and discharging through a three-dimensional spatial confinement effect. This effectively improves the problems of silicon-based material pulverization and rapid degradation due to cycling at the structural root, ensuring both the conductivity and flexibility of the matrix.

[0008] By utilizing fluidized bed CVD vapor deposition technology, uniform contact of the entire surface and pores of porous carbon particles is achieved through fluidization. The silicon source can be deposited deep into the pores of the particles. Compared with traditional fixed bed CVD deposition, the deposition is more uniform and the silicon loading is controllable. It makes full use of the internal space of porous carbon, providing a capacity basis for the finished anthracite-based silicon-carbon anode material to be used as a standalone anode.

[0009] Preferably, the anthracite-based silicon-carbon anode material obtained in step S5 is subjected to a surface coating treatment using asphalt: At 120-190℃, 5-8% of the mass of the anthracite-based silicon-carbon anode material asphalt is mixed with the anthracite-based silicon-carbon anode material, and the mixture is kept warm and stirred for 10-30 minutes to obtain a pre-coated material. Then, the pre-coated material is subjected to gradient heating heat treatment under an inert gas protective atmosphere, cooled, crushed, and sieved to obtain the final product.

[0010] Preferably, the gradient heating heat treatment includes the following steps: First, heat the temperature to 200-300℃ at a heating rate of 2-5℃ / min, and hold for 30-60 minutes. Then, heat the temperature to 600-800℃ at a rate of 3-8℃ / min and hold for 2-4 hours.

[0011] Through the above technical solution, a dry asphalt melting pre-coating process is adopted. After the asphalt melts, a uniform pre-coating film is formed on the surface of silicon-carbon particles. Subsequent heat treatment carbonizes the asphalt into an amorphous carbon shell. On the one hand, this effectively isolates the direct contact between the silicon active material and the electrolyte, stabilizes the SEI electrolyte membrane, and reduces capacity loss during charging and discharging, thereby improving the cycle life of the material. On the other hand, the carbon layer after asphalt carbonization can improve the overall electronic conductivity of the particles, accelerate the lithium-ion transport rate, improve the rate performance of the material, and at the same time, as an additional physical barrier, it helps to buffer the volume expansion of silicon and further inhibits particle pulverization and shedding.

[0012] The anthracite-based silicon-carbon anode material coated with asphalt is carbonized by a gradient heating method. The asphalt can be fully melted and evenly spread on the particle surface, avoiding direct pyrolysis of the asphalt or discontinuity of the coating layer caused by rapid heating. This prevents the particles from agglomerating due to thermal stress during heat treatment, as well as the problem of silicon reacting with carbon at high temperature to form insulating SiC, which leads to loss of active capacity.

[0013] Preferably, the acid solution in step S1 is a hydrofluoric acid solution with a mass fraction of 10-20%.

[0014] Preferably, step S2, the gradient carbonization process, specifically includes the following steps: First, heat to 700-1000℃ at a heating rate of 3-8℃ / min, and then carbonize at a constant temperature for 0.5-1h. Then continue heating to 1000-1400℃ and carbonize at a constant temperature for 0.5-1 hour; Finally, continue heating to 1400-1800℃ and carbonize at a constant temperature for 1-3 hours.

[0015] By employing the above technical solution, preliminary carbonization is first completed at 700-1000℃ to remove volatiles from the raw coal, forming an initial microporous structure and activation sites. The temperature is then increased to 1000-1400℃ to further densify the carbon framework, improving the stability of the matrix structure and effectively preventing the collapse of the pore structure during subsequent high-temperature activation. Finally, the temperature is increased to 1400-1800℃ to enhance the graphitization degree of the pore walls, strengthening the electronic conductivity and structural strength of the carbon support and providing a high-strength framework to buffer the volume expansion of silicon. The composite structure of graphitized rigid framework and non-graphitized active sites formed by the three-stage gradient carbonization ensures both the conductivity of the carbon matrix and retains sufficient active reaction sites, providing an optimal matrix structure for the subsequent steam activation to prepare a controllable hierarchical pore structure.

[0016] Preferably, the activation temperature of the steam activation treatment in step S3 is 850-1050℃.

[0017] Preferably, the total pore volume of the porous carbon support obtained in step S4 is 0.2-0.5 cm³. 3 / g.

[0018] By adopting the above technical solution, 0.2-0.5 cm³ / g is the optimal pore volume range for silicon-carbon anode materials. It can provide sufficient internal space to load nano-silicon and reserve space for volume expansion during silicon intercalation and deintercalation, thereby suppressing the problem of silicon powdering and shedding from the root. It can also ensure that the carbon skeleton has sufficient structural strength and will not crack due to silicon expansion. This allows the finished product to be used as an anode on its own without the need for a large amount of graphite doping.

[0019] Preferably, the volumetric flow rate ratio of the carrier gas to the silicon source gas in step S5 is (8-15):1, and the deposition time is 2-5 hours.

[0020] Secondly, this application provides a method for preparing anthracite silicon-carbon anode material, which is prepared by the method for preparing anthracite silicon-carbon anode material of this application.

[0021] In summary, this application has the following beneficial effects: 1. This application utilizes a combination of gradient carbonization and steam activation to directionally prepare materials with a total pore volume of 0.2-0.5 cm³. 3 The / g hierarchical porous anthracite-based carbon support combines the graphitized structure of carbon-based supports with a three-dimensional hierarchical porous structure. Relying on the spatial confinement effect, it effectively buffers the volume expansion during the silicon intercalation and deintercalation process, effectively solving the problem of silicon-based material pulverization and shedding. The material's cycle stability is significantly improved, and its electrical cycle life is effectively enhanced.

[0022] 2. The porous carbon support obtained in this application has a pore volume of 0.2-0.5 cm³ / g, which is the optimal pore volume range for silicon-carbon anode materials. It can provide sufficient internal space to load nano-silicon and reserve space for volume expansion during silicon intercalation and deintercalation, thereby suppressing the problem of silicon powdering and shedding from the root. It can also ensure that the carbon skeleton has sufficient structural strength and will not crack due to silicon expansion, so that the finished product can be used as an anode on its own without the need for a large amount of graphite doping.

[0023] 3. The anthracite silicon-carbon anode material prepared by the method of this application does not require a large amount of graphite to be mixed in. It can be used directly as a lithium-ion battery anode material alone, or it can be used in combination with a small amount of graphite according to product requirements. It is suitable for various application scenarios such as power batteries, consumer batteries and energy storage batteries. The finished anthracite silicon-carbon anode material combines the high specific capacity of silicon with the high conductivity and structural stability of carbon materials. Its electrochemical performance is better than that of traditional commercial silicon-carbon materials. Detailed Implementation

[0024] The present application will be further described in detail below with reference to embodiments and comparative examples. Example

[0025] Example 1: A method for preparing anthracite-based silicon-carbon anode material, comprising the following steps: S1: Select conventional industrial anthracite as raw material, first crush it with a jaw crusher, then crush it with a ball mill, and finally classify it through a vibrating screen to remove large particles, irregular particles and fine debris, so as to obtain anthracite particles with uniform particle size. Anthracite particles were placed in a 10% hydrofluoric acid solution and soaked at room temperature for 6 hours for acid washing and deashing. After acid washing, they were washed repeatedly with deionized water in a countercurrent manner until the pH of the washing solution was 6-7. Then, they were dried in an 80℃ oven for 8 hours to obtain pretreated anthracite particles with a final carbon purity of 99.9%. S2: Place the pretreated anthracite particles in a carbonization furnace under a nitrogen atmosphere, and set the heating rate to 3℃ / min for gradient carbonization. First, heat to 700℃ and carbonize at a constant temperature for 1 hour; then continue to heat to 1000℃ and carbonize at a constant temperature for 1 hour; finally, continue to heat to 1400℃ and carbonize at a constant temperature for 3 hours. S3: The carbonized anthracite particles are placed in an activation furnace under a nitrogen atmosphere, heated to 850°C, and saturated steam is introduced for steam activation treatment for 4 hours. After activation, the gas supply is stopped, and the activated product is obtained after natural cooling. S4: Add 10% dilute hydrochloric acid to the activated product, stir and neutralize at room temperature for 2 hours, then wash with deionized water until the washing solution is neutral, and dry at 100℃ for 8 hours to obtain a porous carbon support. S5: A fluidized bed air jet mill was used to pulverize the porous carbon support into ultrafine particles. The working pressure of the equipment was 0.6 MPa, and the particle size was controlled by matching the speed of the classifier wheel. The resulting powder had a D50 of 5-15 μm. The powder was then fed into a fluidized bed CVD reactor, and nitrogen and silane were introduced at a volume flow ratio of 8:1. The furnace temperature was controlled at 600℃ for vapor phase deposition reaction, and the deposition time was 5 hours to obtain anthracite-based silicon-carbon anode material. S6: Mix 5% (by weight) of the anthracite-based silicon-carbon anode material with the anthracite-based silicon-carbon anode material at 120℃, keep warm and stir for 10 min to obtain the pre-coated material. Then, under a nitrogen atmosphere, perform gradient heating heat treatment on the pre-coated material. First, heat to 200℃ at a heating rate of 2℃ / min and keep warm for 60 min; then heat to 600℃ at a heating rate of 3℃ / min and keep warm for 4 h. After natural cooling, crush and sieve to obtain the final product.

[0026] Example 2: A method for preparing anthracite-based silicon-carbon anode material, comprising the following steps: S1: Select conventional industrial anthracite as raw material, first crush it with a jaw crusher, then crush it with a ball mill, and finally classify it through a vibrating screen to remove large particles, irregular particles and fine debris, so as to obtain anthracite particles with uniform particle size. Anthracite particles were placed in a 20% hydrofluoric acid solution and soaked at room temperature for 2 hours for acid washing and deashing. After acid washing, they were washed repeatedly with deionized water in a countercurrent manner until the pH of the washing solution was 6-7. Then, they were dried in a 100℃ oven for 8 hours to obtain pretreated anthracite particles with a final carbon purity of 99.9%. S2: Place the pretreated anthracite particles in a carbonization furnace under a nitrogen atmosphere, and set the heating rate to 4℃ / min for gradient carbonization. First, heat to 700℃ and carbonize at a constant temperature for 1 hour; then continue to heat to 1000℃ and carbonize at a constant temperature for 1 hour; finally, continue to heat to 1400℃ and carbonize at a constant temperature for 3 hours. S3: The carbonized anthracite particles are placed in an activation furnace under a nitrogen atmosphere, heated to 850°C, and saturated steam is introduced for steam activation treatment for 4 hours. After activation, the gas supply is stopped, and the activated product is obtained after natural cooling. S4: Add 10% dilute hydrochloric acid to the activated product, stir and neutralize at room temperature for 2 hours, then wash with deionized water until the washing solution is neutral, and dry at 120℃ for 4 hours to obtain a porous carbon support. S5: The porous carbon support was ultra-finely pulverized using a fluidized bed air jet mill. The working pressure of the equipment was 0.7 MPa, and the particle size was controlled by matching the speed of the classifier wheel. The resulting powder had a D50 of 5-15 μm. The powder was then fed into a fluidized bed CVD reactor, and nitrogen and silane were introduced at a volume flow ratio of 10:1. The furnace temperature was controlled at 700℃ for vapor phase deposition reaction, and the deposition time was 4 hours to obtain anthracite-based silicon-carbon anode material. S6: Mix 5% (by weight) of the anthracite-based silicon-carbon anode material with the anthracite-based silicon-carbon anode material at 120℃, keep warm and stir for 10 min to obtain the pre-coated material. Then, under a nitrogen atmosphere, perform gradient heating heat treatment on the pre-coated material. First, heat to 300℃ at a heating rate of 5℃ / min and keep warm for 30 min; then heat to 800℃ at a heating rate of 8℃ / min and keep warm for 2 h. After natural cooling, crush and sieve to obtain the final product.

[0027] Example 3: A method for preparing anthracite-based silicon-carbon anode material, comprising the following steps: S1: Select conventional industrial anthracite as raw material, first crush it with a jaw crusher, then crush it with a ball mill, and finally classify it through a vibrating screen to remove large particles, irregular particles and fine debris, so as to obtain anthracite particles with uniform particle size. Anthracite particles were placed in a 10% hydrofluoric acid solution and soaked at room temperature for 4 hours for acid washing and deashing. After acid washing, they were washed repeatedly with deionized water in a countercurrent manner until the pH of the washing solution was 6-7. Then, they were dried in a 90℃ oven for 6 hours to obtain pretreated anthracite particles with a final carbon purity of 99.9%. S2: Place the pretreated anthracite particles in a carbonization furnace under a nitrogen atmosphere, and set the heating rate to 6℃ / min for gradient carbonization. First, heat to 700℃ and carbonize at a constant temperature for 1 hour; then continue to heat to 1000℃ and carbonize at a constant temperature for 1 hour; finally, continue to heat to 1400℃ and carbonize at a constant temperature for 3 hours. S3: The carbonized anthracite particles are placed in an activation furnace under a nitrogen atmosphere, heated to 850°C, and saturated steam is introduced for steam activation treatment for 4 hours. After activation, the gas supply is stopped, and the activated product is obtained after natural cooling. S4: Add 10% dilute hydrochloric acid to the activated product, stir and neutralize at room temperature for 2 hours, then wash with deionized water until the washing solution is neutral, and dry at 110℃ for 6 hours to obtain a porous carbon support. S5: The porous carbon support was ultra-finely pulverized using a fluidized bed air jet mill. The working pressure of the equipment was 0.7 MPa, and the particle size was controlled by matching the speed of the classifier wheel. The resulting powder had a D50 of 5-15 μm. The powder was then fed into a fluidized bed CVD reactor, and nitrogen and silane were introduced at a volume flow ratio of 12:1. The furnace temperature was controlled at 800℃ for vapor phase deposition reaction, and the deposition time was 3 hours to obtain anthracite-based silicon-carbon anode material. S6: Mix 5% (by weight) of the anthracite-based silicon-carbon anode material with the anthracite-based silicon-carbon anode material at 120℃, keep warm and stir for 10 min to obtain a pre-coated material. Then, under a nitrogen atmosphere, perform gradient heating heat treatment on the pre-coated material. First, heat to 200℃ at a heating rate of 4℃ / min and keep warm for 40 min; then heat to 700℃ at a heating rate of 4℃ / min and keep warm for 3 h. After natural cooling, crush and sieve to obtain the final product.

[0028] Example 4: A method for preparing anthracite-based silicon-carbon anode material, comprising the following steps: S1: Select conventional industrial anthracite as raw material, first crush it with a jaw crusher, then crush it with a ball mill, and finally classify it through a vibrating screen to remove large particles, irregular particles and fine debris, so as to obtain anthracite particles with uniform particle size. Anthracite particles were placed in a 20% hydrofluoric acid solution and soaked at room temperature for 4 hours for acid washing and deashing. After acid washing, they were washed repeatedly with deionized water in a countercurrent manner until the pH of the washing solution was 6-7. Then, they were dried in a 100℃ oven for 5 hours to obtain pretreated anthracite particles with a final carbon purity of 99.9%. S2: Place the pretreated anthracite particles in a carbonization furnace under a nitrogen atmosphere, and set the heating rate to 8℃ / min for gradient carbonization. First, heat to 700℃ and carbonize at a constant temperature for 1 hour; then continue to heat to 1000℃ and carbonize at a constant temperature for 1 hour; finally, continue to heat to 1400℃ and carbonize at a constant temperature for 3 hours. S3: The carbonized anthracite particles are placed in an activation furnace under a nitrogen atmosphere, heated to 850°C, and saturated steam is introduced for steam activation treatment for 4 hours. After activation, the gas supply is stopped, and the activated product is obtained after natural cooling. S4: Add 10% dilute hydrochloric acid to the activated product, stir and neutralize at room temperature for 2 hours, then wash with deionized water until the washing solution is neutral, and dry at 120℃ for 5 hours to obtain a porous carbon support. S5: The porous carbon support was ultra-finely pulverized using a fluidized bed air jet mill. The working pressure of the equipment was 0.8 MPa, and the particle size was controlled by matching the speed of the classifier wheel. The resulting powder had a D50 of 5-15 μm. The powder was then fed into a fluidized bed CVD reactor, and nitrogen and silane were introduced at a volume flow ratio of 15:1. The furnace temperature was controlled at 900℃ for vapor phase deposition reaction, and the deposition time was 2 hours to obtain anthracite-based silicon-carbon anode material. S6: Mix 5% (by weight) of the anthracite-based silicon-carbon anode material with the anthracite-based silicon-carbon anode material at 120℃, keep warm and stir for 10 min to obtain the pre-coated material. Then, under a nitrogen atmosphere, perform gradient heating heat treatment on the pre-coated material. First, heat to 250℃ at a heating rate of 5℃ / min and keep warm for 50 min; then heat to 750℃ at a heating rate of 6℃ / min and keep warm for 3.5 h. After natural cooling, crush and sieve to obtain the final product.

[0029] Example 5: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S3 specifically involves: The carbonized anthracite particles were placed in an activation furnace under a nitrogen atmosphere and heated to 950°C. Saturated steam was then introduced for steam activation treatment for 3 hours. After activation, the gas supply was stopped, and the product was obtained after natural cooling.

[0030] Example 6: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S3 specifically involves: The carbonized anthracite particles were placed in an activation furnace under a nitrogen atmosphere and heated to 1050°C. Saturated steam was then introduced for steam activation treatment for 2 hours. After activation, the gas supply was stopped, and the product was obtained after natural cooling.

[0031] Example 7: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S3 specifically involves: The carbonized anthracite particles were placed in an activation furnace under a nitrogen atmosphere and heated to 800°C. Saturated steam was then introduced for steam activation treatment for 4 hours. After activation, the gas supply was stopped, and the product was obtained after natural cooling.

[0032] Example 8: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S3 specifically involves: The carbonized anthracite particles were placed in an activation furnace under a nitrogen atmosphere and heated to 1100°C. Saturated steam was then introduced for steam activation treatment for 2 hours. After activation, the gas supply was stopped, and the product was obtained after natural cooling.

[0033] Example 9: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S2 is specifically as follows: The pretreated anthracite particles were placed in a carbonization furnace under a nitrogen atmosphere, and a gradient carbonization process was carried out with a heating rate of 3℃ / min. First, the temperature was raised to 850℃ and carbonized at a constant temperature for 0.8h; then the temperature was raised to 1200℃ and carbonized at a constant temperature for 0.8h; finally, the temperature was raised to 1600℃ and carbonized at a constant temperature for 2h.

[0034] Example 10: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S2 specifically involves: The pretreated anthracite particles were placed in a carbonization furnace under a nitrogen atmosphere, and a gradient carbonization process was carried out with a heating rate of 3℃ / min. First, the temperature was raised to 1000℃ and carbonized at a constant temperature for 0.5h; then the temperature was raised to 1400℃ and carbonized at a constant temperature for 0.5h; finally, the temperature was raised to 1800℃ and carbonized at a constant temperature for 1h.

[0035] Example 11: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S6 specifically involves: At 150℃, 6.5% (by weight) of pitch was mixed with anthracite-based silicon-carbon anode material and stirred at the same temperature for 10 minutes to obtain a pre-coated material. Then, under a nitrogen atmosphere, the pre-coated material was subjected to gradient heating heat treatment. First, the temperature was increased to 200℃ at a heating rate of 2℃ / min and held for 60 minutes. Then, the temperature was increased to 600℃ at a heating rate of 3℃ / min and held for 4 hours. After natural cooling, the material was crushed and sieved to obtain the final product.

[0036] Example 12: A smokeless coal silicon-carbon anode material, differing from Example 1 only in that step S6 specifically involves: At 190℃, 8% (by weight) of pitch was mixed with anthracite-based silicon-carbon anode material and stirred for 10 min to obtain a pre-coated material. Then, under a nitrogen atmosphere, the pre-coated material was subjected to gradient heating heat treatment. First, the temperature was increased to 200℃ at a heating rate of 2℃ / min and held for 60 min. Then, the temperature was increased to 600℃ at a heating rate of 3℃ / min and held for 4 h. After natural cooling, the material was crushed and sieved to obtain the final product.

[0037] Example 13: An anthracite-based silicon-carbon anode material, the only difference from Example 1 is that the anthracite-based silicon-carbon anode material obtained in step S5 was not subjected to the pitch coating modification step in step S6.

[0038] Performance testing The following performance tests were conducted on the anthracite silicon-carbon anode materials obtained in Examples 1-13. Each test was performed three times, and the average value of the final test results was taken as the final result and recorded in Table 1.

[0039] 1. Total pore volume: The static volumetric nitrogen adsorption-desorption method was used. 100 mg of the porous carbon support sample obtained in step S4 was weighed and degassed under vacuum at 200 °C for 6 h. The nitrogen adsorption-desorption isotherm was tested at liquid nitrogen temperature (77 K). The adsorption amount under different nitrogen relative pressures (P / P0) was measured, and the adsorption-desorption isotherm was plotted. Finally, the total pore volume inside the material was obtained by converting the saturated adsorption amount. 2. Electrochemical Performance: The anthracite-silicon-carbon anode materials obtained in Examples 1-13 were used to assemble and test coin cells. First, the anode material to be tested, the conductive agent SuperP, and the binder PVDF were mixed in NMP solvent at a mass ratio of 8:1:1 to prepare a slurry. The slurry was coated on copper foil and dried under vacuum at 80°C for 12 hours. The dried electrode sheet was rolled and punched into a circular electrode sheet with a diameter of 12 mm. CR2032 coin cells were assembled in an argon-filled glove box, using the prepared electrode sheet as the working electrode, a lithium metal sheet as the counter electrode, and a Celgard 2400 membrane as the separator. The electrolyte was a solution of 1 M LiPF6 dissolved in EC, DEC, and DMC (volume ratio 1:1:1). Electrochemical performance was tested using a battery testing system within a voltage window of 0.01-1.5V. The initial charge-discharge test was conducted at a current density of 0.1C (1C = 2000mA / g), and the initial discharge specific capacity and initial coulombic efficiency were calculated. Cycle performance testing was performed 500 times at a current density of 1C, and the capacity retention rate was calculated. In rate performance testing, the battery was charged at 0.1C and discharged at current densities of 0.1C, 0.2C, 0.5C, 1C, 2C, and 5C. The electrode thickness after cycling was measured using a thickness gauge, and the thickness expansion rate was calculated.

[0040] Table 1

[0041] According to the performance test results in Table 1, the anthracite-based silicon-carbon anode material of this application has an initial discharge specific capacity of 1850-2020 mAh / g, an initial coulombic efficiency (ICE) ≥82%, a capacity retention rate ≥74.5% after 500 cycles at 1C, a capacity retention rate ≥78.2% at 5C / 0.1C, and an electrode thickness expansion rate ≤86%. As can be seen, this application combines gradient carbonization with steam activation to construct a hierarchical porous matrix with graphitized crystalline regions and non-graphitized carbon regions. The three-dimensional spatial confinement effect buffers the volume expansion during silicon charging and discharging, effectively improving the problems of silicon-based materials pulverization and rapid degradation at the structural root. This ensures both the conductivity and flexibility of the matrix. The fluidized bed CVD vapor deposition process utilizes fluidization to achieve uniform contact across the entire surface and pores of the porous carbon particles. The silicon source can penetrate deep into the pores of the particles for deposition, and the silicon loading is controllable. This fully utilizes the internal space of the porous carbon, providing a capacity basis for the finished anthracite-based silicon-carbon anode material to be used alone as an anode. The finished anthracite-based silicon-carbon anode material combines the high specific capacity of silicon with the high conductivity and structural stability of carbon materials. It can be used directly as a lithium-ion battery anode material or combined with a small amount of graphite according to product requirements. It is suitable for various application scenarios such as power batteries, consumer batteries, and energy storage batteries, and its electrochemical performance is superior to traditional commercial silicon-carbon materials.

[0042] Based on the performance test results of Examples 1 and 5-8, it can be seen that steam activation at 850-1050℃ to create pores, directionally constructing a hierarchical porous structure, and forming a three-dimensional confined space, results in the best battery performance and the best silicon expansion buffering capacity when used as an anode material. Example 7 had insufficient activation temperature, resulting in low carbon matrix vaporization and insufficient micropore development, making it impossible to achieve high energy density and use as a standalone anode material. Example 8 underwent high-temperature overactivation, excessively ablating the carbon skeleton, thinning the carbon walls, and significantly reducing both the skeleton's mechanical properties and the battery performance.

[0043] Based on the performance test results of Examples 1 and 11-13, it can be seen that the dry asphalt melting pre-coating process forms a uniform pre-coating film on the surface of silicon-carbon particles after the asphalt melts. Subsequent heat treatment carbonization transforms it into an amorphous carbon shell. On the one hand, this effectively stabilizes the SEI electrolyte membrane, reduces capacity loss during charging and discharging, and thus improves the cycle life of the material. On the other hand, the carbon layer after asphalt carbonization can improve the overall electronic conductivity of the particles, accelerate the lithium-ion transport rate, improve the rate performance of the material, and at the same time, as an additional physical barrier, it helps to buffer the volume expansion of silicon and further inhibits particle pulverization and shedding.

[0044] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A method for preparing anthracite-based silicon-carbon anode material, characterized in that, Includes the following steps: S1: Industrial anthracite is selected as raw material. After mechanical crushing and screening, anthracite particles with uniform particle size are obtained. Then, they are soaked in an acid solution, and then washed and dried to obtain pretreated anthracite particles. S2: Under the protection of an inert gas atmosphere, the pretreated anthracite particles are subjected to gradient carbonization treatment at 700-1800℃; S3: Under the protection of an inert gas atmosphere, the carbonized anthracite particles are activated by steam to obtain the activated product; S4: Add dilute acid to the activated product and stir, then wash and dry to obtain a porous carbon support. S5: The porous carbon support is subjected to ultrafine pulverization and then fed into a fluidized bed CVD equipment. Carrier gas and silicon source gas are introduced, and a vapor phase deposition reaction is carried out at 600-900℃ to obtain anthracite-based silicon-carbon anode material.

2. The method for preparing anthracite-silicon-carbon anode material according to claim 1, characterized in that, The anthracite-based silicon-carbon anode material obtained in step S5 is subjected to surface coating post-treatment using asphalt: At 120-190℃, 5-8% of the mass of the anthracite-based silicon-carbon anode material asphalt is mixed with the anthracite-based silicon-carbon anode material, and the mixture is kept warm and stirred for 10-30 minutes to obtain a pre-coated material. Then, the pre-coated material is subjected to gradient heating heat treatment under an inert gas protective atmosphere, cooled, crushed, and sieved to obtain the final product.

3. The method for preparing anthracite-silicon-carbon anode material according to claim 2, characterized in that, The gradient heating heat treatment includes the following steps: First, heat the temperature to 200-300℃ at a heating rate of 2-5℃ / min, and hold for 30-60 minutes. Then, heat the temperature to 600-800℃ at a rate of 3-8℃ / min and hold for 2-4 hours.

4. The method for preparing anthracite-silicon-carbon anode material according to claim 1, characterized in that, The acid solution mentioned in step S1 is a hydrofluoric acid solution with a mass fraction of 10-20%.

5. The method for preparing anthracite-silicon-carbon anode material according to claim 1, characterized in that, Step S2, the gradient carbonization process, specifically includes the following steps: First, heat to 700-1000℃ at a heating rate of 3-8℃ / min, and then carbonize at a constant temperature for 0.5-1h. Then continue heating to 1000-1400℃ and carbonize at a constant temperature for 0.5-1 hour; Finally, continue heating to 1400-1800℃ and carbonize at a constant temperature for 1-3 hours.

6. The method for preparing anthracite-silicon-carbon anode material according to claim 1, characterized in that, The activation temperature for the steam activation treatment in step S3 is 850-1050℃.

7. The method for preparing anthracite-silicon-carbon anode material according to claim 1, characterized in that, The total pore volume of the porous carbon support obtained in step S4 is 0.2-0.5 cm³. 3 / g.

8. The method for preparing anthracite-silicon-carbon anode material according to claim 1, characterized in that, In step S5, the volumetric flow rate ratio of the carrier gas to the silicon source gas is (8-15):1, and the deposition time is 2-5 hours.

9. A smokeless coal-silicon-carbon anode material, characterized in that, The anthracite silicon-carbon anode material is prepared by any one of claims 1-8.