An ultrasonic-assisted acid stripping process for efficient removal of cyanide from cyanide-containing wastewater

By optimizing the ultrasonic parameters in the acidification and stripping separation stages, and synergistically enhancing mass transfer with ultrasonic fields, the problems of low efficiency and poor stability of traditional acidification and stripping processes were solved, achieving efficient cyanide removal and resource recovery.

CN123105933APending Publication Date: 2026-11-17METALLURGICAL LABORATORY BRANCH OF SHANDONG GOLD MINING TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611609690.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing traditional acid stripping processes suffer from low cyanide removal efficiency, incomplete dissociation of complexed cyanide, high gas-to-water ratio, high energy consumption, and poor long-term operational stability. Furthermore, existing ultrasonic-coupled cyanide-containing wastewater treatment processes have technical shortcomings that cannot simultaneously achieve resource recovery and efficient removal.

Method used

The process employs a stepwise coupled ultrasonic field acidification and stripping separation section, utilizing the ultrasonic cavitation effect to enhance mass transfer, thereby achieving efficient removal and resource recovery of cyanide, reducing the gas-water ratio, shortening the processing time, alleviating packing blockage, and reducing energy consumption.

Benefits of technology

It has achieved a significant improvement in cyanide removal rate, increased resource recovery rate, reduced total cyanide concentration in effluent, extended packing blockage cycle, reduced energy consumption, and improved operational stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a process for efficiently removing cyanide from cyanide-containing wastewater using ultrasound-assisted acidification stripping, belonging to the field of cyanide-containing wastewater treatment technology. This invention couples the ultrasonic field stepwise to both the acidification / complex breaking and stripping separation stages. Through five steps—pretreatment, ultrasound-assisted acidification / complex breaking, ultrasound-coupled stripping, alkaline absorption and recovery, and neutralization—it utilizes the ultrasonic cavitation effect to break the liquid film at the gas-liquid interface, enhance mass transfer, and assist in the dissociation of metal cyanide complexes, achieving efficient cyanide removal and resource recovery. This invention achieves full-process synergistic enhancement by stepwise coupling the ultrasound to the acidification / complex breaking and stripping separation stages, improving efficiency from the dissociation of complexed cyanide to HCN stripping, and solving the dual problems of incomplete dissociation and high mass transfer resistance in traditional processes. It is suitable for treating high-concentration cyanide-containing wastewater from gold smelting, electroplating, and other industries, offering both environmental benefits and economic value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of cyanide-containing wastewater treatment and resource recovery technology, specifically involving an ultrasonic-assisted acid stripping process for efficient removal of cyanide from cyanide-containing wastewater. It is mainly applicable to the decyanation treatment and cyanide resource recovery of high-concentration complex cyanide-containing wastewater generated in industries such as gold smelting, electroplating, and metal beneficiation. Background Technology

[0002] Cyanide-containing wastewater mainly originates from industrial production processes such as gold cyanide leaching, electroplating, and metal refining. This wastewater not only contains free cyanide ions but also a large amount of stable complexes formed by cyanide ions with metals such as copper, zinc, and iron. Cyanide is a highly toxic substance, and if discharged directly without effective treatment, it will cause great harm to the ecological environment and human health. At the same time, cyanide, as an industrial production raw material, has high resource recovery value. Therefore, acid stripping processes are often used to recover and remove cyanide from high-concentration cyanide-containing wastewater, taking into account both environmental and economic benefits.

[0003] The core principle of the traditional acid stripping process (AVR process) is to add sulfuric acid to cyanide-containing wastewater to adjust the pH to acidic, causing the metal cyanide complex to dissociate and release cyanide ions. The cyanide ions combine with hydrogen ions to generate volatile hydrogen cyanide (HCN). Then, HCN is transferred from the liquid phase to the gas phase by aeration stripping, and cyanide is regenerated and recovered by alkaline absorption. However, this process has significant drawbacks in practical applications: First, the gas-liquid mass transfer resistance is relatively high, and the liquid film at the gas-liquid interface hinders the escape of HCN from the liquid phase to the gas phase, limiting the stripping efficiency. Conventional processes can only achieve a cyanide removal rate of 90%-95%, which is difficult to improve further. Second, some stable metal cyanide complexes are not completely dissociated, and the residual complexed cyanide cannot be converted into strippable HCN, resulting in a high total cyanide content in the effluent. Third, to ensure removal efficiency, a high gas-to-water ratio and long residence time are required, resulting in high blower energy consumption, large equipment footprint, and long treatment cycles. Fourth, suspended solids and heavy metal precipitates in the wastewater easily adhere to the surface of the stripping tower packing, causing packing blockage and a continuous decline in long-term operating efficiency.

[0004] Existing technologies disclose various patents related to the treatment of cyanide-containing wastewater and ultrasonic-enhanced wastewater treatment. After comparison, similar patents can be divided into three categories: The first category consists of conventional acid stripping and its process improvements, which only optimize process parameters, equipment structure, or supporting recovery processes, without introducing ultrasonic field enhancement, thus still suffering from low mass transfer efficiency and incomplete dissociation of complexed cyanide; the second category consists of patents on ultrasonic-coupled oxidation methods for treating cyanide-containing wastewater, such as ultrasound combined with sodium hypochlorite, zero-valent iron, hydrogen peroxide, etc., to oxidize and degrade cyanide. The core is oxidative cyanide destruction, not... Regarding the resource recovery process for HCN stripping, there is no alkali solution recovery of cyanide, and the oxidation method is prone to waste of cyanide resources, making it unsuitable for resource recovery scenarios of high-concentration cyanide tail liquid; the third type is a patent for general ultrasonic stripping to remove volatile pollutants, which only sets ultrasound in the stripping unit or only targets conventional volatile pollutants such as ammonia nitrogen, without considering the characteristics of cyanide-containing wastewater, coupling ultrasound with acidification and complex breaking and stripping dual units, and without specifically solving industry technical problems such as the dissociation of metal cyanide complexes, closed negative pressure recovery of HCN, and packing anti-clogging.

[0005] For example, Chinese invention patent application CN105776765A discloses a "method for treating cyanide-containing wastewater", which involves a complete process for acid stripping treatment of cyanide-containing wastewater, including acid pH adjustment, stripping tower packing, gas-water ratio control and alkaline absorption and recovery of NaCN. However, it does not introduce ultrasonic enhancement, making it difficult to achieve satisfactory technical results.

[0006] For example, Chinese invention patent application CN106966488A discloses "a sodium hypochlorite-ultrasonic composite treatment system for cyanide-containing wastewater", which is an oxidation destruction process. It uses sodium hypochlorite to oxidize CN⁻ to CNO⁻ under ultrasonic cavitation, and then oxidizes it to CO2 and N2. It does not involve acid stripping, HCN recovery, or alkaline absorption of NaCN.

[0007] For example, Chinese invention patent application CN106977029A discloses "a cyanide gold extraction wastewater treatment and recycling system based on acoustic-chemical composite". The acidification and HCN evaporation are completed in the same tank. In essence, it is a reaction-evaporation integrated process. HCN evaporation is a passive diffusion process, which relies on natural diffusion and airflow carrying in a sealed environment.

[0008] For example, Chinese invention patent application CN1757771A discloses a "method for ultrasonic field-enhanced desorption of cyanide and valuable metals from resin." The treatment target is an acidic desorption solution loaded with resin, and the process route is "resin adsorption - acidic desorption - ultrasonic field-enhanced stripping of HCN-NaOH absorption." Ultrasound is applied to both the resin desorption and the stripping of the desorption solution. This process does not involve acidification or complex disruption of the cyanide-containing wastewater itself. The cyanide has already been enriched on the resin through adsorption, and the cyanide in the desorption solution exists in a relatively simple form, eliminating the dissociation problem of copper, zinc, iron, and other metallic cyanide complexes in the liquid phase.

[0009] In summary, existing related patented technologies either only optimize traditional acid stripping without process enhancement methods, or use ultrasound coupled oxidation instead of resource-based stripping, or only provide ultrasound assistance in a single stage without achieving synergistic enhancement throughout the entire process. Currently, there is no complete process patent that couples ultrasonic field to acidification and complex breaking and stripping separation, achieving both high cyanide removal rate and cyanide resource recovery. Therefore, developing a highly efficient, low-consumption, and thorough cyanide removal ultrasonic-assisted acid stripping process has outstanding technological innovation and engineering application value. Summary of the Invention

[0010] The technical problem to be solved by this invention is to address the shortcomings of existing traditional acid stripping processes, such as low cyanide removal efficiency, incomplete dissociation of complexed cyanide, high gas-to-water ratio, high energy consumption, and poor long-term operational stability, as well as the technical deficiencies of existing ultrasonic-coupled cyanide-containing wastewater treatment processes that cannot simultaneously achieve resource recovery and efficient removal. This invention provides an ultrasonic-assisted acid stripping process for efficient removal of cyanide from cyanide-containing wastewater. By stepwise coupling the ultrasonic field to the dual core sections of acidification and complex breaking and stripping separation, the ultrasonic cavitation effect is used to enhance mass transfer and assist in complex breaking, thereby achieving efficient removal and resource recovery of cyanide. At the same time, the gas-to-water ratio is reduced, the treatment time is shortened, packing blockage is reduced, and energy consumption is decreased.

[0011] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A process for efficiently removing cyanide from cyanide-containing wastewater using ultrasonic-assisted acid stripping includes the following steps: S1. Wastewater pretreatment: The cyanide-containing wastewater is transported to the pretreatment equalization tank and allowed to settle for 1-2 hours. S2. Ultrasonic acidification and complex breaking: The pretreated cyanide-containing wastewater is introduced into an ultrasonic acidification reactor, and an acidic regulator is added to adjust the pH to 2.0-3.0; the reaction temperature is controlled at 25-40℃; the ultrasonic device is turned on and the reaction is carried out for 30-60 minutes. S3, Ultrasonic Coupled Stripping: The acidified cyanide-containing wastewater is introduced into another independent ultrasonic stripping tower. The ultrasonic device is turned on in the tower, and the air-to-water ratio is controlled at 200-400:1 with a negative pressure of -0.02~-0.05MPa. Wastewater is sprayed and air is stripped in a countercurrent manner. The stripping time is 20-40 minutes. S4. Alkali absorption and recovery: The stripping tail gas is absorbed by NaOH solution to recover sodium cyanide; S5. Neutralization treatment: After stripping, the pH of the wastewater is adjusted to 8.0-9.0, and after sedimentation, it is treated to meet the standards.

[0012] Preferably, in step S3, the negative pressure value and the ultrasonic power density of the ultrasonic stripping tower satisfy the following: the ratio of the absolute value of the negative pressure value in MPa to the ultrasonic power density in W / cm² is 0.05-0.25; the ratio of the power density of the ultrasonic stripping tower to the power density of the ultrasonic acidification reactor is 0.25-2.0.

[0013] More preferably, the ratio of the absolute value of the negative pressure in MPa to the ultrasonic power density in W / cm² is 0.075; and the ratio of the power density of the ultrasonic stripping tower to the power density of the ultrasonic acidification reactor is 0.8.

[0014] Preferably, in step S2, the ultrasonic frequency is 20-40kHz and the ultrasonic power density is 0.3-0.8W / cm².

[0015] Preferably, in step S3, the ultrasonic device includes an ultrasonic transducer, the ultrasonic transducer having an ultrasonic frequency of 25-35kHz and an ultrasonic power density of 0.2-0.6W / cm².

[0016] More preferably, the ultrasonic transducers of the ultrasonic stripping tower are arranged in multiple transducer groups at intervals along the axial direction of the tower body. Each group of transducers corresponds to a layer of packing. The transducer groups and the packing are arranged alternately along the axial direction of the tower body, so that each layer of packing is within the sound field coverage range of the two adjacent groups of transducers. The packing is a polypropylene Pall ring, a multi-faceted hollow sphere, or a stepped ring, with a specific surface area ≥300m² / m³.

[0017] Preferably, in step S4, the HCN-containing tail gas discharged from the top of the ultrasonic stripping tower is introduced into an alkaline absorption tower and absorbed countercurrently using a 10%-20% NaOH solution to generate a sodium cyanide solution, which is then recycled back to the production section for reuse.

[0018] Preferably, in step S5, the cyanide-removed wastewater discharged from the bottom of the ultrasonic stripping tower is transported to a neutralization tank, where lime slurry is added to adjust the pH value to 8.0-9.0, and residual heavy metal ions and sulfate ions in the wastewater are precipitated to remove them. After the supernatant meets the standards, it is used for production or discharged after further treatment.

[0019] Preferably, the cyanide-containing wastewater is gold smelting cyanide tailings or electroplating plant cyanide-containing wastewater, with an initial total cyanide concentration ≥500mg / L.

[0020] More preferably, the cyanide-containing wastewater is a gold smelting cyanide tailings solution with an initial total cyanide concentration of 1000-5000 mg / L.

[0021] Compared with the prior art, the present invention has the following beneficial effects: First, this invention applies ultrasound independently to both the acidification and complex-breaking reactor and the stripping tower, and optimizes the ultrasound parameters for different mass transfer requirements in each stage. Unlike existing patents that use single ultrasonic stripping or ultrasonic oxidation, this invention couples ultrasound stepwise to the two core stages of acidification and complex-breaking and stripping separation, achieving synergistic enhancement throughout the entire process. This improves efficiency from the dissociation of complexed cyanide to HCN stripping, solving the dual problems of incomplete dissociation and high mass transfer resistance in traditional processes.

[0022] Secondly, this invention abandons the destruction-type route of ultrasonic coupled oxidation to destroy cyanide, and adopts a resource recovery route of ultrasonic enhanced acid stripping combined with alkaline recovery, which is suitable for the recovery of cyanide from high-concentration cyanide-containing wastewater and avoids the waste of cyanide resources.

[0023] Third, the acidification section of this invention uses a relatively low frequency and medium power density (20-40kHz, 0.3-0.8 W / cm²) to utilize a strong cavitation shock wave to preferentially break the metal-cyanide coordination bond (complex breaking), while avoiding excessively high power density that would cause a large amount of HCN to escape instantaneously due to local overheating, resulting in a load impact on the absorption system. In the stripping section, a frequency of 25-35kHz and a power density of 0.2-0.6 W / cm² are selected. The core of the stripping section is to enhance gas-liquid mass transfer rather than chemical bond breaking, therefore a slightly lower power density is required. This design aims to generate sufficiently strong acoustic flow and microjets to thin the liquid film at the gas-liquid interface, increase the mass transfer area, and simultaneously meet the continuous scouring requirements for online packing anti-clogging.

[0024] Fourth, in the ultrasonic coupling stripping process of this invention, the negative pressure value (absolute value) and the ultrasonic power density of the ultrasonic stripping tower must meet a specific ratio. This specific ratio is determined based on the matching relationship between the gas-liquid equilibrium characteristics of HCN under negative pressure conditions and the ultrasonic cavitation threshold. If the negative pressure value is too large (e.g., exceeding -0.05 MPa), the partial pressure of HCN in the liquid phase will be too low, and the HCN concentration in the bubbles generated by ultrasonic cavitation will be insufficient, affecting the alkali absorption efficiency; if the negative pressure value is too small, the driving force for HCN escape will be insufficient.

[0025] Fifth, in this invention, the power density of the ultrasonic acidification reactor and the ultrasonic stripping tower is designed collaboratively based on the different functional requirements of the two sections. The acidification and complex-breaking section needs to provide sufficient cavitation energy to break the metal-cyanide coordination bonds, and the power density is maintained at a high level. The core function of the stripping section is to enhance gas-liquid mass transfer and prevent packing blockage, requiring a relatively low cavitation intensity. If the power density of the stripping section is too high (more than twice that of the acidification section), energy will be excessively invested in the mass transfer process, and the cavitation wear of the oscillators in the solid-liquid phase will be aggravated. If it is too low (less than 1 / 4 of that of the acidification section), the cavitation intensity will be insufficient to effectively break large bubbles and scour the packing surface. Theoretical analysis shows that controlling the power density ratio of the stripping section to the acidification section within the range of 0.25-2.0 can achieve the optimal balance between complex-breaking efficiency, mass transfer enhancement, and equipment lifespan.

[0026] Sixth, the traditional acid stripping process has a low cyanide removal rate, and the simple ultrasonic oxidation process has no resource recovery. The ultrasonic-assisted process of this invention significantly improves the cyanide removal rate and cyanide resource recovery rate, and the total cyanide concentration in the effluent is much lower than the residual concentration in the effluent of the traditional process, which reduces the load for subsequent deep treatment.

[0027] Seventh, this invention can effectively destroy moderately stable metal cyanide complexes such as copper and zinc through ultrasonic synergistic acidification, solving the problem of incomplete dissociation of complexed cyanide in traditional processes. It can treat wastewater containing cyanide with high complexation state and breaks through the wastewater adaptability limitations of conventional acidification stripping.

[0028] Eighth, the ultrasonic field of this invention can continuously scour the surface of the tower body and packing, inhibit the adhesion of heavy metal precipitates and calcium salt scale, avoid packing blockage, extend equipment service life, reduce maintenance frequency, and solve the industry technical problem of long-term efficiency decline of traditional stripping towers.

[0029] Ninth, this invention operates under a completely closed, slightly negative pressure system, combined with ultrasonic enhancement to rapidly remove HCN, reducing the residence time of HCN in the liquid phase and lowering the risk of highly toxic gas leakage; at the same time, it achieves closed-loop recovery of cyanide without the addition of additional oxidizing agents and without secondary pollution. Detailed Implementation

[0030] The present invention will be further described below with reference to specific embodiments and relevant experimental data. These embodiments are for illustrative purposes only and are not intended to limit the scope of protection of the present invention.

[0031] I. Examples and Comparative Examples

[0032] Example 1 A gold smelter's cyanide tailings initially contained a total cyanide concentration of 2800 mg / L, a copper ion concentration of 120 mg / L, a zinc ion concentration of 45 mg / L, and a pH of 10.5. The following process was employed for treatment: S1. Pretreatment of cyanide tailings: The cyanide tailings are transported to a pretreatment equalization tank, homogenized and allowed to stand for 1.5 hours to remove large suspended solids and silt, and to ensure uniform water quality.

[0033] S2. Ultrasonic acidification and complex breaking: The pretreated cyanide tail liquid is pumped into an ultrasonic acidification reactor, and 25% industrial sulfuric acid is slowly added dropwise to avoid excessive acid consumption due to excessively low local pH value, and to prevent the safety risks caused by the instantaneous release of large amounts of HCN. The pH is adjusted to 2.5; the reaction temperature is controlled at 30℃; and the ultrasonic device is turned on at a frequency of 25kHz and a power density of 0.5W / cm². Intermittent or continuous ultrasonic mode is used, with continuous ultrasonic mode preferred to enhance the complex breaking and mass transfer effect; the reaction is carried out for 45 minutes to dissociate the metal cyanide complex into dissolved hydrogen cyanide.

[0034] S3. Ultrasonic Stripping: The cyanide tailings after ultrasonic acidification are fed into an ultrasonic stripping tower. The ultrasonic transducers in the tower are arranged in multiple transducer groups at intervals along the tower's axial direction. Each group of transducers corresponds to a layer of packing material. The transducer groups and packing layers are arranged alternately along the tower's axial direction, ensuring that each packing layer is within the acoustic field coverage of the adjacent two groups of transducers. The packing material is polypropylene Pall rings with a specific surface area of ​​350 m² / m³.

[0035] The gas-to-water ratio was controlled at 300:1, with a slight negative pressure of -0.03MPa to prevent hydrogen cyanide leakage. The internal spraying and counter-current air stripping functions were activated, allowing the cyanide tail liquid to spray down from the top of the tower, while air was introduced counter-currently from the bottom via a fan. The ultrasonic device was activated, with an ultrasonic frequency of 30kHz and an ultrasonic power density of 0.4W / cm², maintaining an ultrasonic field throughout the process and ensuring full coverage of the wastewater spraying area and packing layer to eliminate mass transfer dead zones. HCN stripping separation was completed under ultrasonic synergy, with a stripping residence time of 30 minutes, achieving hydrogen cyanide gas-phase separation. S4. Alkali absorption: The HCN-containing tail gas discharged from the top of the ultrasonic stripping tower is passed into the alkali absorption tower and absorbed countercurrently using a 15% NaOH solution to generate sodium cyanide solution, which is then recycled back to the production section for reuse.

[0036] S5. Neutralization treatment: The cyanide-removed wastewater discharged from the bottom of the ultrasonic stripping tower is transported to the neutralization tank, and lime milk is added to adjust the pH value to 8.5. The residual heavy metal ions and sulfate ions in the wastewater are removed by precipitation. After the supernatant meets the standards, it is reused in production or discharged after further treatment.

[0037] Results: The packing blockage cycle exceeded 90 days. After 90 days of operation, the tower pressure drop stabilized at 1.8 kPa, an increase of 12.5% ​​compared to the initial pressure drop of 1.6 kPa. After 60 days of continuous operation, the total cyanide concentration in the effluent was approximately 50 mg / L, with a cyanide removal rate of 98.2%, a decrease of 0.7 percentage points compared to the initial level. The results of testing various forms of cyanide after ultrasonic acidification and neutralization treatment are shown in Table 1. The metal ion conversion rate after ultrasonic acidification and the total metal ion removal rate after neutralization and precipitation treatment are also measured, and the results are shown in Table 2.

[0038] Table 1. Detailed detection data of cyanide forms in Example 1

[0039] As shown in Table 1, ultrasonic acidification breaks down the complex, causing weakly complexed cyanide and some stable complexed cyanide to dissociate, thus increasing the content of free cyanide. After ultrasonic stripping, alkaline absorption and neutralization, the removal rates of free cyanide and weakly complexed cyanide reached 98.92% and 98.35%, respectively, the removal rate of stable complexed cyanide reached 61.03%, and the total cyanide removal rate was 98.21%.

[0040] Table 2 Metal ion conversion rate and removal data from Example 1

[0041] As shown in Table 2, under ultrasonic acidification and complex-breaking conditions, Cu 2+ Zn 2+ The cyanide complex dissociation conversion rates were 95.0% and 95.1%, respectively; after neutralization and precipitation with lime slurry, Cu 2+ Zn 2+ The overall removal rates reached 99.33% and 99.11%, respectively.

[0042] Comparative Example 1 (conventional acid stripping, without ultrasonication) The traditional acid stripping process was adopted, without turning on the ultrasonic device. The remaining process parameters were the same as in Example 1: pH 2.5, reaction time 45 min, gas-water ratio 300:1, stripping time 30 min, and the cyanide tail liquid was treated in the same way as in Example 1.

[0043] Treatment results: Total cyanide concentration in the effluent was 210 mg / L, and cyanide removal rate was 92.5%. See Table 3 for the results of the individual tests.

[0044] Table 3. Detailed test data of cyanide forms in Comparative Example 1

[0045] Comparative Example 2 (Ultrasonic Coupling Oxidation Method, No Resource Recovery) The process of ultrasonic coupling sodium hypochlorite oxidation was adopted without acid stripping and alkali recovery. The ultrasonic frequency and power density were the same as those of the ultrasonic acidification reactor in Example 1. Sodium hypochlorite was added in two stages, and the total oxidation time was 60 min. The treatment was the same as that of cyanide tail liquid in Example 1.

[0046] Treatment results: The total cyanide concentration in the effluent was approximately 196 mg / L, the cyanide removal rate was 93%, there was no cyanide recovery, but chlorine-containing secondary pollutants were generated, and the treatment cost was higher than that of Example 1.

[0047] Comparative Example 3 (Ultrasonic stripping tower shut off) The same ultrasonic acidification and alkaline absorption process as in Example 1 was used, except that the ultrasonic device in the ultrasonic stripping tower was turned off. The remaining process parameters were the same as in Example 1: pH 2.5, acidification reaction 45 min, gas-water ratio 300:1, slight negative pressure -0.03 MPa, stripping 30 min, and the same cyanide tail liquid was treated as in Example 1.

[0048] Results: The packing blockage period was 35 days. After 35 days of operation, the tower pressure drop increased from 1.6 kPa to 4.2 kPa, an increase of 162.5%. After 60 days of continuous operation, the total cyanide concentration in the effluent was approximately 193 mg / L, and the cyanide removal rate was 93.1%, a decrease of 5.4 percentage points compared to the initial stage. The results of the sub-items are shown in Table 4.

[0049] Table 4. Detailed test data of cyanide in each form in Comparative Example 3

[0050] Example 2 A high-concentration cyanide-containing wastewater from an electroplating plant, with an initial total cyanide concentration of 1200 mg / L, was treated using the process described in Example 1, with the following parameters adjusted: ultrasonic acidification frequency 20 kHz, power density 0.3 W / cm², pH 2.0, reaction time 30 min, temperature 25 °C; ultrasonic stripping frequency 25 kHz, power density 0.2 W / cm², air-to-water ratio 250:1, stripping time 20 min, and a slight negative pressure of -0.03 MPa.

[0051] Treatment results: After 60 days of continuous operation, the total cyanide concentration in the effluent was approximately 35 mg / L, with a cyanide removal rate of 97.1%. The results of the individual tests are shown in Table 5. The metal ion conversion rate after ultrasonic acidification and the total metal ion removal rate after neutralization and precipitation treatment were also tested, and the results are shown in Table 6.

[0052] Table 5. Detection data of cyanide morphologies in Example 2

[0053] As shown in Table 5, ultrasonic acidification breaks down the complex, causing weakly complexed cyanide and some stable complexed cyanide to dissociate, thus increasing the content of free cyanide. After ultrasonic stripping, alkaline absorption and neutralization, the removal rates of free cyanide and weakly complexed cyanide reached 99.41% and 96.32%, respectively, the removal rate of stable complexed cyanide reached 59.07%, and the total cyanide removal rate was 97.08%.

[0054] Table 6. Metal ion conversion rate and removal data for Example 2

[0055] As can be seen from the above data, Example 2 can still achieve a total cyanide removal rate of 97.1% and Cu removal rate even with lower ultrasonic power density and shorter air-blowing time. 2+ Zn 2+ The acidification conversion rates reached 95.0% and 94.8%, respectively, and the neutralization removal rates reached 99.27% ​​and 99.03%, respectively, indicating that the process also has good effects on complex breaking, stripping and metal removal for electroplating wastewater containing cyanide.

[0056] II. Parameter boundary verification process and results.

[0057] Based on Example 1, and under the premise of treating the same cyanide tail liquid as in Example 1 and keeping other process conditions the same as in Example 1, single-factor boundary verification was performed on the acidification ultrasonic parameters, stripping ultrasonic parameters, the ratio of negative pressure to ultrasonic power density K, and the ratio of stripping tower power density to acidification reactor power density. The results are shown in Tables 7-10.

[0058] Table 7 Boundary Verification of Acidification Ultrasonic Parameters

[0059] As shown in Table 7, when the acidification ultrasonic frequency and power density are too low, the cavitation breaking ability is insufficient; when they are too high, the cavitation bubbles collapse incompletely and HCN escapes too quickly, resulting in incomplete absorption of the alkali solution. Within the range of 20-40 kHz / 0.3-0.8 W / cm², the total cyanide removal rate is not less than 97.3%; outside this range, both the stable complexed cyanide removal rate and the total cyanide removal rate decrease significantly.

[0060] Table 8 Boundary verification of blow-off ultrasonic parameters

[0061] As shown in Table 8, when the ultrasonic frequency and power density are too low, mass transfer enhancement is insufficient, HCN removal is incomplete, and the packing is prone to scaling. When the frequency and power density are too high, the sound field attenuates severely in the packing layer and accelerates scaling on the packing surface. Within the range of 25-35kHz / 0.2-0.6W / cm², the total cyanide removal rate is not less than 97.1%, and the packing blockage cycle is not less than 75 days. Beyond this range, the removal rate and long-term operational stability deteriorate significantly.

[0062] Table 9 Boundary verification of the ratio K of negative pressure value to ultrasonic power density.

[0063] As shown in Table 9, when the K value is too low, the negative pressure is insufficient, resulting in a weak driving force for HCN stripping; when the K value is too high, the negative pressure is too large, the air volume increases, the concentration of HCN in the gas phase decreases, and the alkaline absorption efficiency decreases. Within the K range of 0.05-0.25, the total cyanide removal rate is not less than 96.0%; outside this range, the removal rate decreases significantly.

[0064] Table 10 Boundary verification of the ratio of stripping tower power density to acidification reactor power density

[0065] As shown in Table 10, when the power density ratio is too low, the acidification and complex breaking are strong, but the stripping enhancement is insufficient, and HCN cannot be stripped off in a timely and efficient manner after it is generated. When the power density ratio is too high, the acidification and complex breaking are insufficient, the dissociation rate of stable complexed cyanide is low, and although the subsequent stripping is strong, the total amount of free cyanide that can be stripped is insufficient. When the power density ratio is in the range of 0.25-2.0, the total cyanide removal rate is not less than 96.2%; outside this range, the removal rate further decreases.

[0066] In this embodiment, the ratio of the absolute value of the micro-negative pressure to the power density is 0.075, and the ratio of the power density of the ultrasonic stripping tower to the power density of the ultrasonic acidification reactor is 0.8. This specifically designed ultrasonic field is most effective in inhibiting scaling and sludge adhesion on the packing surface, maintaining long-term stable operation.

[0067] The air-to-water ratio mentioned in this invention refers to the ratio of air volumetric flow rate to wastewater volumetric flow rate.

Claims

1. A process for efficiently removing cyanide from cyanide-containing wastewater using ultrasonic-assisted acid stripping, characterized in that, Includes the following steps: S1. Wastewater pretreatment: The cyanide-containing wastewater is transported to the pretreatment equalization tank and allowed to settle for 1-2 hours. S2. Ultrasonic acidification and complex breaking: The pretreated cyanide-containing wastewater is introduced into an ultrasonic acidification reactor, and an acidic regulator is added to adjust the pH to 2.0-3.0; the reaction temperature is controlled at 25-40℃; the ultrasonic device is turned on and the reaction is carried out for 30-60 minutes. S3, Ultrasonic Coupled Stripping: The acidified cyanide-containing wastewater is introduced into another independent ultrasonic stripping tower. The ultrasonic device is turned on in the tower, and the air-to-water ratio is controlled at 200-400:1 with a negative pressure of -0.02~-0.05MPa. Wastewater is sprayed and air is stripped in a countercurrent manner. The stripping time is 20-40 minutes. S4. Alkali absorption and recovery: The stripping tail gas is absorbed by NaOH solution to recover sodium cyanide; S5. Neutralization treatment: After stripping, the pH of the wastewater is adjusted to 8.0-9.0, and after sedimentation, it is treated to meet the standards.

2. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 1, characterized in that: In step S3, the negative pressure value and the ultrasonic power density of the ultrasonic stripping tower satisfy the following: the ratio of the absolute value of the negative pressure value in MPa to the ultrasonic power density in W / cm² is 0.05-0.25; the ratio of the power density of the ultrasonic stripping tower to the power density of the ultrasonic acidification reactor is 0.25-2.

0.

3. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 2, characterized in that: The ratio of the absolute value of the negative pressure in MPa to the ultrasonic power density in W / cm² is 0.075; the ratio of the power density of the ultrasonic stripping tower to the power density of the ultrasonic acidification reactor is 0.

8.

4. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 1, 2, or 3, characterized in that: In step S2, the ultrasonic frequency is 20-40kHz and the ultrasonic power density is 0.3-0.8W / cm².

5. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 1, 2, or 3, characterized in that: In step S3, the ultrasonic device includes an ultrasonic transducer with an ultrasonic frequency of 25-35kHz and an ultrasonic power density of 0.2-0.6W / cm².

6. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 5, characterized in that: The ultrasonic transducers are arranged in multiple transducer groups at intervals along the axial direction of the ultrasonic stripping tower. Each transducer group corresponds to a layer of packing. The transducer groups and packing are arranged alternately along the axial direction of the tower, so that each layer of packing is within the sound field coverage of the two adjacent transducer groups. The packing is a polypropylene Pall ring, a multi-faceted hollow sphere, or a stepped ring, with a specific surface area ≥300m² / m³.

7. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 1, 2, or 3, characterized in that: In step S4, the HCN-containing tail gas discharged from the top of the ultrasonic stripping tower is passed into an alkaline absorption tower and absorbed countercurrently by a 10%-20% NaOH solution to generate a sodium cyanide solution, which is then recycled back to the production section for reuse.

8. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 1, 2, or 3, characterized in that: In step S5, the cyanide-removed wastewater discharged from the bottom of the ultrasonic stripping tower is transported to a neutralization tank, where lime slurry is added to adjust the pH value to 8.0-9.

0. Residual heavy metal ions and sulfate ions in the wastewater are precipitated and removed. After the supernatant meets the standards, it is used for production or discharged after further treatment.

9. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 1, 2, or 3, characterized in that: The cyanide-containing wastewater is gold smelting cyanide tailings or electroplating plant cyanide-containing wastewater, with an initial total cyanide concentration ≥500mg / L.

10. The process for efficient removal of cyanide from cyanide-containing wastewater by ultrasonic-assisted acid stripping according to claim 9, characterized in that: The cyanide-containing wastewater is a cyanide tailings solution from gold smelting, with an initial total cyanide concentration of 1000-5000 mg / L.

Citation Information

Patent Citations

  • Cyanide-containing wastewater treatment method

    CN105776765A

  • System for performing sodium hypochlorite-ultrasonic composite treatment on cyanide-containing waste water

    CN106966488A

  • Acoustic cavitation complex-based cyanidation gold extraction waste water treatment and recycling system

    CN106977029A

  • Method of stripping cyanide and valuable metal on resin with ultrasonic

    CN1757771A