A process for directional separation and resource utilization of high-salt wastewater from rare earth smelting
By using hydrogen peroxide aqueous solution, ammonia water, and phosphorylated betaine-type chitosan resin, the problems of rare earth loss and low purity of waste salt in the treatment of high-salt wastewater from rare earth smelting were solved, achieving efficient recovery of rare earth elements and resource utilization of waste salt, and reducing evaporation load and equipment scaling risk.
Patent Information
- Application Number
- CN202611636946.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for treating high-salt wastewater from rare earth smelting suffer from problems such as rare earth element loss, low purity of mixed waste salts, high evaporation load, and equipment scaling and corrosion. They also lack coordination and integration between various treatment units, resulting in low resource utilization rates.
Low-valent iron ions are oxidized using hydrogen peroxide aqueous solution, pH is adjusted using ammonia water, anionic polyacrylamide promotes precipitation, and phosphorylated betaine-type chitosan resin enriches rare earth ions; ammonium carbonate aqueous solution and ammonia water form calcium carbonate precipitate, calcium carbonate seed crystals promote crystallization, hydrochloric acid adjusts pH, nanofiltration separates chloride and sulfate, ammonium sulfate and ammonium chloride seed crystals promote directional crystallization, and powdered activated carbon adsorbs organic matter.
It achieves efficient recovery of rare earth elements and resource utilization of waste salt, reduces rare earth loss and mixed waste salt generation, lowers evaporation load and equipment scaling risk, and improves resource utilization rate.
Smart Images

Figure CN123105935A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of rare earth smelting wastewater treatment technology, specifically relating to a process for directional separation and resource utilization of high-salt wastewater from rare earth smelting. Background Technology
[0002] Rare earth elements possess unique optical, electrical, magnetic, and catalytic properties, and are widely used in permanent magnet materials, luminescent materials, hydrogen storage materials, electronic devices, aerospace, and new energy equipment. The processes of acid leaching, salt leaching, extraction separation, back-extraction, precipitation, and washing of rare earth minerals require the use of substances such as ammonium sulfate, ammonium chloride, hydrochloric acid, sulfuric acid, and ammonia, resulting in large quantities of saline wastewater. This type of wastewater typically contains high concentrations of ammonium, sulfate, and chloride ions, while also carrying rare earth ions such as lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, dysprosium, and yttrium, as well as impurity ions such as iron, aluminum, calcium, and magnesium. It is characterized by high salinity, complex ionic composition, significant pH fluctuations, and poor biodegradability. Direct discharge without treatment will not only increase the salinity and ammonia nitrogen load of the receiving water body but also cause the loss of rare earth resources and may adversely affect soil structure, aquatic organisms, and the surrounding ecological environment. Therefore, it is necessary to carry out in-depth treatment and resource utilization of high-salinity wastewater from rare earth smelting.
[0003] Existing methods for treating high-salinity wastewater from rare earth smelting mainly include neutralization precipitation, chemical hardening removal, adsorption, ion exchange, extraction, membrane separation, and evaporation crystallization. Neutralization precipitation can remove iron, aluminum, and some heavy metal ions; however, during the process of increasing pH, rare earth ions in the wastewater are prone to co-precipitation with iron and aluminum hydroxides or being entrained by flocs, causing valuable rare earth elements to enter the sludge and increasing the difficulty of subsequent sludge disposal. Solvent extraction is suitable for treating solutions with high rare earth concentrations, but for low-concentration, high-salinity wastewater, it easily leads to problems such as high extractant consumption, difficulty in oil-water separation, and organic residues. Although ordinary chitosan and ion exchange resins can adsorb rare earth ions, they are easily competed for by ammonium, calcium, magnesium, and other coexisting ions under high ionic strength conditions. Some materials also suffer from swelling in acidic environments, insufficient mechanical strength, and decreased reusability. Nanofiltration can separate monovalent and polyvalent ions by using membrane pores for sieving and charge repulsion. However, calcium, magnesium, iron, aluminum and colloidal substances tend to deposit on the membrane surface, causing a decrease in membrane flux, a reduction in separation selectivity and an increase in cleaning frequency.
[0004] Existing processes typically separate impurity removal, rare earth recovery, membrane separation, and evaporation crystallization, lacking coordination and integration between these units. Some processes involve deep neutralization or softening before residual rare earths are recovered, leading to rare earth elements entering iron-aluminum sludge or calcium-magnesium precipitation. Other processes use large amounts of sodium hydroxide, lime, or calcium-containing defluorinating agents, further introducing sodium and calcium ions into the wastewater, making the final waste salt composition more complex. When sulfate and chloride ions are directly evaporated without directional separation, a mixed waste salt of sulfate, chloride, and impurity salts is easily formed. This mixed waste salt has low purity, significant hygroscopicity, and a tendency to agglomerate, making it difficult to directly return to the rare earth smelting process or utilize as a stable industrial raw material. Furthermore, directly evaporating raw high-salinity wastewater also presents problems such as high evaporation load, equipment scaling and corrosion, and high operating energy consumption. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a process for the directional separation and resource recovery of high-salt wastewater from rare earth smelting, comprising the following steps:
[0006] S1. By weight, filter 900-1100 parts of high-salt wastewater from rare earth smelting, add 0.1-0.5 parts of a 27.5-30% hydrogen peroxide aqueous solution, and stir at 25-35℃; then add 18-22% ammonia water to adjust the pH and continue stirring; add 0.005-0.015 parts of anionic polyacrylamide, stir, let stand, and filter to obtain a purified high-salt clear liquid and iron-aluminum sludge.
[0007] S2. Pack 18-30 parts of phosphorylated betaine-type chitosan resin into an adsorption column, and pass a high-salt purified solution through the column for adsorption to obtain a rare earth removal solution; pass 20-40 parts of deionized water through the column for displacement, and then pass 60-150 parts of 0.8-1.6 mol / L HCl aqueous solution for desorption to obtain a rare earth desorption solution; add 0.1-2.5 parts of oxalic acid and 8-12% ammonia water to the rare earth desorption solution, adjust the pH to 1.6-2.0, stir, age, and filter to obtain a rare earth oxalate precipitate; dry and calcine the rare earth oxalate precipitate to obtain mixed rare earth oxides;
[0008] S3. Add 5-85 parts of ammonium carbonate aqueous solution with a mass fraction of 10-15% to the rare earth removal solution, add ammonia water with a mass fraction of 18-22%, adjust the pH to 8.8-9.2, and stir at 35-45℃; add 0.2-0.5 parts of calcium carbonate seed crystals, continue stirring, let stand, filter, and obtain softened filtrate; add hydrochloric acid with a mass fraction of 8-12% to the softened filtrate, adjust the pH to 6.6-7.0, add 0.2-0.5 parts of powdered activated carbon, stir, filter, and obtain softened high-salt clear solution; subject the softened high-salt clear solution to two-stage nanofiltration to obtain chloride-enriched permeate and sulfate-enriched solution;
[0009] S4. Concentrate the sulfate-enriched solution under reduced pressure to obtain concentrate A; add 0.2-0.5 parts of ammonium sulfate seed crystals to 100 parts of concentrate A, cool to crystallize, and centrifuge to obtain crystal A; rinse crystal A with a saturated aqueous solution of ammonium sulfate and dry to obtain regenerated ammonium sulfate; concentrate the chloride-enriched permeate under reduced pressure to obtain concentrate B; add 0.2-0.5 parts of ammonium chloride seed crystals to 100 parts of concentrate B, cool to crystallize, and centrifuge to obtain crystal B; rinse crystal B with a saturated aqueous solution of ammonium chloride and dry to obtain regenerated ammonium chloride.
[0010] Preferably, in step S1, the pH is adjusted to 4.4-4.8.
[0011] Preferably, in step S2, the flow rate of the purified high-salt solution introduced into the adsorption column is 1.0-3.0 BV / h.
[0012] Preferably, in step S3, the temperature of the secondary nanofiltration is 25-35°C.
[0013] Preferably, in step S4, ammonium sulfate seed crystals are added to concentrate A, the temperature is lowered to 25-30℃, and crystallization is carried out for 1.5-2.5 hours; ammonium chloride seed crystals are added to concentrate B, the temperature is lowered to 20-30℃, and crystallization is carried out for 1.5-2.5 hours.
[0014] Preferably, the preparation steps of the phosphorylated betaine-type chitosan resin include:
[0015] A1. By weight, add 100 parts of chitosan to 2500-3500 parts of an aqueous acetic acid solution with a mass fraction of 1.5-2.5%, stir at 20-30℃, allow to stand to remove bubbles, filter, and obtain chitosan sol; add the chitosan sol dropwise to a coagulation solution composed of 1800-2400 parts of an aqueous NaOH solution with a mass fraction of 8-12% and 750-1050 parts of anhydrous ethanol, stir, solidify, filter, and obtain chitosan microspheres; add the chitosan microspheres to 1000-1500 parts of deionized water, add 15-25 parts of epichlorohydrin, add an aqueous NaOH solution with a mass fraction of 8-12%, adjust the pH to 10.0-11.0, and stir the reaction at 50-60℃; after the reaction is complete, filter to obtain a solid; wash the solid sequentially with anhydrous ethanol and deionized water, dry, and obtain cross-linked chitosan resin microspheres;
[0016] A2. Add 100 parts of cross-linked chitosan resin microspheres to 800-1200 parts of deionized water, add 130-170 parts of formaldehyde aqueous solution with a mass fraction of 37-40% and 80-105 parts of formic acid aqueous solution with a mass fraction of 85-90%, and stir at 30-40℃; then raise the temperature to 80-90℃ to react, cool to room temperature, add NaOH aqueous solution with a mass fraction of 8-12%, adjust the pH to 6.8-7.2, filter to obtain a solid; wash the solid with deionized water and dry to obtain tertiary amination chitosan resin;
[0017] A3. Add 100 parts of tertiary amination chitosan resin to 800-1200 parts of deionized water, add 50-75 parts of sodium chloroacetate, add 8-12% NaOH aqueous solution, adjust the pH to 8.2-8.8, stir the reaction at 65-75℃ to obtain the reaction product; filter the reaction product to obtain the solid product; wash the solid product successively with deionized water and anhydrous ethanol, and vacuum dry at 50-60℃ to obtain carboxymethyl betaine type chitosan resin;
[0018] A4. Add 100 parts of carboxymethyl betaine-type chitosan resin to 400-600 parts of deionized water, add 30-50 parts of 85% phosphoric acid and 20-35 parts of urea, and stir and impregnate at 35-45℃; remove water under reduced pressure, dry at 65-75℃, and then heat to 130-140℃ to react; cool naturally to room temperature to obtain the product; add the product to 400-600 parts of 0.3-0.8% sodium bicarbonate aqueous solution, stir, filter, and obtain a solid; wash the solid with deionized water, and vacuum dry at 50-60℃ to obtain phosphorylated betaine-type chitosan resin.
[0019] Preferably, in step A1, the stirring reaction time at 50-60°C is 3-5 hours.
[0020] Preferably, in step A2, the reaction time at 80-90℃ is 12-16 hours.
[0021] Preferably, in step A3, the stirring reaction time at 65-75°C is 8-10 hours.
[0022] Preferably, in step A4, the reaction time at 130-140℃ is 2-3 hours.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) Hydrogen peroxide aqueous solution is used to oxidize low-valence iron ions in high-salt wastewater from rare earth smelting. Controlling its dosage can reduce the loss of cerium with iron and aluminum sludge after oxidation. Ammonia water is used to adjust the pH so that iron and aluminum impurities can precipitate. Anionic polyacrylamide promotes precipitation and solid-liquid separation, reducing the interference of iron and aluminum impurities on subsequent rare earth adsorption. Phosphorylated betaine-type chitosan resin coordinates with rare earth ions through phosphate groups and carboxylate groups, enriching rare earth ions in a high-salt environment. The rare earth desorption solution obtained by desorption is precipitated with oxalic acid and calcined to obtain mixed rare earth oxides, realizing the recovery of rare earth resources.
[0025] (2) Ammonium carbonate aqueous solution and ammonia water cause calcium ions in the rare earth removal solution to form calcium carbonate precipitate. Calcium carbonate seed crystals provide a crystal growth surface for calcium carbonate, promoting particle growth and facilitating filtration, thus reducing the risk of scaling in the subsequent nanofiltration process. Hydrochloric acid is used to adjust the pH of the softened filtrate and decompose residual carbonate ions, reducing scaling on the nanofiltration membrane; powdered activated carbon is used to adsorb organic matter and colloidal impurities. After nanofiltration treatment, the softened high-salt clear liquid forms chloride-enriched permeate and sulfate-enriched concentrate, achieving directional separation of chloride and sulfate.
[0026] (3) Ammonium sulfate seed crystals and ammonium chloride seed crystals promote the directional crystallization of sulfate enrichment concentrate and chloride enrichment permeate, respectively, improving crystal formation and solid-liquid separation. Saturated aqueous solutions of ammonium sulfate and ammonium chloride are used to rinse the corresponding crystals, removing mother liquor and impurities adhering to the crystal surface, yielding regenerated ammonium sulfate and regenerated ammonium chloride. This process reduces the loss of rare earth elements and the generation of mixed waste salts, improving the resource utilization rate of rare earth elements and waste salts. Attached Figure Description
[0027] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. The drawings are only used to illustrate the implementation methods and are not intended to limit the present invention.
[0028] Figure 1 The infrared spectrum of the phosphorylated betaine-type chitosan resin prepared in Example 1. Detailed Implementation
[0029] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.
[0030] Example 1
[0031] This embodiment provides a process for the directional separation and resource recovery of high-salt wastewater from rare earth smelting, the steps of which include:
[0032] S1. Weigh 1000.0 kg of high-salt wastewater from rare earth smelting, filter it through a filter material with a pore size of 100 μm, add 0.30 kg of 28.75% hydrogen peroxide aqueous solution, and stir for 20 min at 30℃ and 300 r / min; then add 20% ammonia water to adjust the pH to 4.6, and continue stirring at 300 r / min for 40 min; add 0.010 kg of anionic polyacrylamide, stir at 250 r / min for 2 min, then stir at 40 r / min for 10 min, let stand for 60 min, filter, and obtain a purified high-salt clear liquid and iron-aluminum sludge.
[0033] S2. Weigh 24.0 kg of phosphorylated betaine-type chitosan resin and pack it into the adsorption column. Pre-wash the phosphorylated betaine-type chitosan resin with 50.0 kg of deionized water. Introduce the purified high-salt solution obtained in step S1 into the adsorption column at a flow rate of 2.0 BV / h for adsorption. When the total rare earth element concentration at the adsorption column outlet reaches 5% of the total rare earth element concentration at the inlet, switch to a standby adsorption column. Continue this process until the purified high-salt solution is completely treated. Combine the adsorption effluents to obtain the rare earth removal solution. Introduce 30.0 kg of deionized water into the adsorption column for replacement, and then proceed with the next step at a flow rate of 0.75 BV / h. Desorption was performed by passing 105.0 kg of 1.2 mol / L HCl aqueous solution through the solution at a flow rate of / h, and the rare earth desorption solution was collected. 1.30 kg of oxalic acid and 10% ammonia water were added to the rare earth desorption solution to adjust the pH to 1.8. The solution was stirred at 40℃ and 200 r / min for 30 min, allowed to stand for 2 h, filtered, and rare earth oxalate precipitate was obtained. The rare earth oxalate precipitate was washed with 20.0 kg of deionized water, dried at 105℃ for 6 h, calcined at 825℃ for 2 h, and cooled to 25℃ to obtain mixed rare earth oxides.
[0034] S3. Add 45.0 kg of 12.5% ammonium carbonate aqueous solution and 20% ammonia solution to the rare earth removal solution obtained in step S2, adjust the pH to 9.0, and stir for 45 min at 40℃ and 250 r / min; add 0.35 kg of calcium carbonate seed crystals, continue stirring at 200 r / min for 20 min, let stand for 60 min, and filter through 1 μm filter material to obtain a softened filtrate; add 10% salt to the softened filtrate. The pH was adjusted to 6.8, and the mixture was stirred at 40℃ and 200 r / min for 20 min. 0.35 kg of powdered activated carbon was added, and stirring was continued for another 20 min. The mixture was then filtered through a 1 μm filter material to obtain a softened high-salt clear solution. The softened high-salt clear solution was subjected to two-stage nanofiltration at 30℃, 2.75 MPa, and a membrane flow rate of 1.15 m / s, with the total recovery rate controlled at 75%. The nanofiltration permeate and nanofiltration concentrate were collected separately to obtain chloride-enriched permeate and sulfate-enriched solution, respectively.
[0035] S4. The sulfate enrichment solution obtained in step S3 is concentrated under reduced pressure at 75℃ and 45kPa to obtain 260.0 kg of concentrate A. 0.91 kg of ammonium sulfate seed crystals are added to concentrate A, stirred at 50 r / min and cooled to 28℃, kept at this temperature for 2.0 h for crystallization, and then centrifuged to obtain crystal A. Crystal A is washed with 20.0 kg of saturated ammonium sulfate aqueous solution and dried at 80℃ to constant weight to obtain regenerated ammonium sulfate. The chloride enrichment permeate obtained in step S3 is concentrated under reduced pressure at 70℃ and 40kPa to obtain 300.0 kg of concentrate B. 1.05 kg of ammonium chloride seed crystals are added to concentrate B, stirred at 50 r / min and cooled to 25℃, kept at this temperature for 2.0 h for crystallization, and then centrifuged to obtain crystal B. Crystal B is washed with 20.0 kg of saturated ammonium chloride aqueous solution and dried at 70℃ to constant weight to obtain regenerated ammonium chloride.
[0036] Preparation steps of phosphorylated betaine-type chitosan resin:
[0037] A1. Weigh 25.0 kg of chitosan and add it to 750.0 kg of a 2.0% acetic acid aqueous solution. Stir at 25℃ and 300 r / min for 4 hours, let stand to remove bubbles for 2 hours, and filter through a 100 μm filter to obtain chitosan sol. Evenly drip the chitosan sol through a 1.0 mm inner diameter dropper into a coagulation solution composed of 525.0 kg of a 10% NaOH aqueous solution and 225.0 kg of anhydrous ethanol. During the dripping process, maintain the temperature of the coagulation solution at 25℃ and stir at 150 r / min until the dripping is complete. After stirring and solidification for another 2 hours, the mixture was filtered to obtain chitosan microspheres. The chitosan microspheres were washed with 150.0 kg of deionized water, and then 312.5 kg of deionized water and 5.0 kg of epichlorohydrin were added. A 10% NaOH aqueous solution was added to adjust the pH to 10.5. The mixture was stirred at 55℃ and 200 r / min for 4 hours. After the reaction was completed, the mixture was cooled to 25℃, filtered, and the resulting solid was washed successively with 100.0 kg of anhydrous ethanol and 150.0 kg of deionized water. The solid was dried at 55℃ for 8 hours to obtain cross-linked chitosan resin microspheres.
[0038] A2. Weigh 25.0 kg of the cross-linked chitosan resin microspheres obtained in step A1 and add them to 250.0 kg of deionized water. Stir at 200 r / min for 30 min, then add 37.5 kg of 38.5% formaldehyde aqueous solution and 23.125 kg of 87.5% formic acid aqueous solution. Stir at 35℃ and 200 r / min for 1 h, then raise the temperature to 85℃ and react under reflux for 14 h. The gas generated by the reaction is condensed and introduced into an alkaline absorption liquid. After the reaction is completed, cool to 25℃, add 10% NaOH aqueous solution to adjust the pH to 7.0, filter, and wash the obtained solid with 150.0 kg of deionized water in three batches. Dry at 55℃ for 8 h to obtain tertiary amination chitosan resin.
[0039] A3. Weigh 25.0 kg of the tertiary amination chitosan resin obtained in step A2 and add it to 250.0 kg of deionized water. Stir at 200 r / min for 30 min, add 15.625 kg of sodium chloroacetate, and add a 10% NaOH aqueous solution to adjust the pH to 8.5. Stir at 70℃ and 220 r / min for 9 h. During the reaction, monitor and maintain the pH at 8.5 every 1 h. After the reaction is completed, cool to 25℃, filter, and wash the obtained solid with 150.0 kg of deionized water in 3 batches, then wash with 100.0 kg of anhydrous ethanol. Vacuum dry at 55℃ for 8 h to obtain carboxymethyl betaine type chitosan resin.
[0040] A4. Weigh 25.0 kg of the carboxymethyl betaine-type chitosan resin obtained in step A3 and add it to 125.0 kg of deionized water. Add 10.0 kg of 85% phosphoric acid and 6.875 kg of urea. Stir and impregnate at 40℃ and 200 r / min for 2 h. Remove water under reduced pressure at 70℃ and dry to a moisture content of 18%. Then raise the temperature to 135℃ and react for 2.5 h. After the reaction is completed, cool naturally to 25℃. Add the obtained product to 125.0 kg of 0.55% sodium bicarbonate aqueous solution and stir at 25℃ and 180 r / min for 30 min. Filter and wash the obtained solid with 150.0 kg of deionized water in 3 batches. Dry under vacuum at 55℃ to constant weight. Sieve particles with a particle size of 0.5-1.2 mm to obtain phosphorylated betaine-type chitosan resin.
[0041] Depend on Figure 1 It can be seen that the cross-linked chitosan resin microspheres prepared by A1 have a growth rate of 3350 cm⁻¹. -1 A broad peak of O–H / N–H stretching vibration appears at 2920 / 2875 cm⁻¹. -1 C–H stretching vibration peaks appear at 1155–1030 cm⁻¹. -1 Characteristic C–O–C / C–O absorptions are observed at 1590 cm⁻¹. -1 The presence of primary amine N–H bending vibration peaks indicates that the chitosan backbone remains intact after crosslinking.
[0042] After A2 methylation and A3 carboxymethylation, 1590 cm -1 The N–H peaks at 1600 cm⁻¹ disappear. Simultaneously, the peaks at 1 -1 and 1410cm -1 COO⁻ asymmetric and symmetric stretching vibration peaks appeared at 1480 cm⁻¹, respectively. -1 The presence of an asymmetric bending vibration peak of N⁺–CH3 indicates that the primary amine has been converted into a tertiary amine and further quaternized to form a carboxymethyl betaine structure.
[0043] After A4 phosphorylation, all the characteristic peaks of betaine were retained, and the peaks at 1210 cm⁻¹ were also present. -1 A new P=O stretching vibration peak was added at 972 cm⁻¹. -1 The P–O absorption at point A3 was significantly enhanced compared to point A3, indicating that the phosphate group had been successfully introduced. In summary, the reactions occurred sequentially, and the target product, phosphorylated betaine-type chitosan resin, was successfully synthesized.
[0044] Example 2
[0045] The difference between this embodiment and Embodiment 1 is that this embodiment provides a process for the directional separation and resource utilization of high-salt wastewater from rare earth smelting, the steps of which include:
[0046] S1. Weigh 900.0 kg of high-salt wastewater from rare earth smelting, filter it through a filter material with a pore size of 100 μm, add 0.10 kg of 27.5% hydrogen peroxide aqueous solution, and stir for 20 min at 25℃ and 300 r / min; then add 18% ammonia water to adjust the pH to 4.4, and continue stirring at 300 r / min for 40 min; add 0.005 kg of anionic polyacrylamide, stir at 250 r / min for 2 min, then stir at 40 r / min for 10 min, let stand for 60 min, filter, and obtain a purified high-salt clear liquid and iron-aluminum sludge.
[0047] S2. Weigh 18.0 kg of phosphorylated betaine-type chitosan resin and pack it into the adsorption column. Pre-wash with 40.0 kg of deionized water. Introduce the purified high-salt solution obtained in step S1 into the adsorption column at a flow rate of 1.0 BV / h for adsorption. When the total rare earth element concentration at the adsorption column outlet reaches 5% of the total rare earth element concentration at the inlet, switch to a standby adsorption column. Continue this process until the purified high-salt solution is completely treated. Combine the adsorption effluents to obtain the rare earth removal solution. Introduce 20.0 kg of deionized water into the adsorption column for replacement, and then continue this process at a flow rate of 0.50 BV / h. Desorption was performed in 60.0 kg of 0.8 mol / L HCl aqueous solution to obtain rare earth desorption solution; 0.10 kg of oxalic acid and 8% ammonia water were added to the rare earth desorption solution to adjust the pH to 1.6, and the solution was stirred at 40℃ and 200 r / min for 30 min, allowed to stand for 2 h, filtered to obtain rare earth oxalate precipitate; the rare earth oxalate precipitate was washed with 15.0 kg of deionized water, dried at 105℃ for 6 h, calcined at 800℃ for 2 h, and cooled to 25℃ to obtain mixed rare earth oxides.
[0048] S3. Add 5.0 kg of 10% ammonium carbonate aqueous solution and 18% ammonia solution to the rare earth removal solution obtained in step S2, adjust the pH to 8.8, and stir for 45 min at 35℃ and 250 r / min; add 0.20 kg of calcium carbonate seed crystals, continue stirring at 200 r / min for 20 min, let stand for 60 min, and filter through 1 μm filter material to obtain a softened filtrate; add 8% hydrochloric acid to the softened filtrate. The pH was adjusted to 6.6, and the mixture was stirred for 20 minutes at 35℃ and 200 r / min. 0.20 kg of powdered activated carbon was added, and stirring was continued for another 20 minutes. The mixture was then filtered through a 1 μm filter material to obtain a softened high-salt clear solution. The softened high-salt clear solution was subjected to two-stage nanofiltration at 25℃, 2.0 MPa, and a membrane flow rate of 0.8 m / s, with the total recovery rate controlled at 70%. The nanofiltration permeate and nanofiltration concentrate were collected separately to obtain chloride-enriched permeate and sulfate-enriched permeate, respectively.
[0049] S4. The sulfate enrichment solution obtained in step S3 is concentrated under reduced pressure at 70℃ and 40kPa to obtain 220.0 kg of concentrate A. 0.44 kg of ammonium sulfate seed crystals are added to concentrate A, stirred at 50 r / min and cooled to 25℃, kept at this temperature for 1.5 h for crystallization, and then centrifuged to obtain crystal A. Crystal A is washed with 15.0 kg of saturated ammonium sulfate aqueous solution and dried at 80℃ to constant weight to obtain regenerated ammonium sulfate. The chloride enrichment permeate obtained in step S3 is concentrated under reduced pressure at 65℃ and 35kPa to obtain 260.0 kg of concentrate B. 0.52 kg of ammonium chloride seed crystals are added to concentrate B, stirred at 50 r / min and cooled to 20℃, kept at this temperature for 1.5 h for crystallization, and then centrifuged to obtain crystal B. Crystal B is washed with 15.0 kg of saturated ammonium chloride aqueous solution and dried at 70℃ to constant weight to obtain regenerated ammonium chloride.
[0050] Preparation steps of phosphorylated betaine-type chitosan resin:
[0051] A1. Weigh 25.0 kg of chitosan and add it to 625.0 kg of a 1.5% acetic acid aqueous solution. Stir at 20℃ and 300 r / min for 4 hours, let stand to remove bubbles for 2 hours, and filter through a 100 μm filter to obtain chitosan sol. Evenly drip the chitosan sol through a 1.0 mm inner diameter dropper into a coagulation solution composed of 450.0 kg of 8% NaOH aqueous solution and 187.5 kg of anhydrous ethanol. During the dripping process, maintain the temperature of the coagulation solution at 20℃ and stir at 150 r / min. After the dripping is complete... Continue stirring and solidification for 2 hours, then filter to obtain chitosan microspheres. Wash the chitosan microspheres with 150.0 kg of deionized water, then add 250.0 kg of deionized water and 3.75 kg of epichlorohydrin, followed by an 8% (w / w) NaOH aqueous solution to adjust the pH to 10.0. Stir the mixture at 50℃ and 200 r / min for 3 hours. After the reaction is complete, cool to 25℃, filter, and wash the resulting solid successively with 100.0 kg of anhydrous ethanol and 150.0 kg of deionized water. Dry the solid at 50℃ for 8 hours to obtain cross-linked chitosan resin microspheres.
[0052] A2. Weigh 25.0 kg of the cross-linked chitosan resin microspheres obtained in step A1 and add them to 200.0 kg of deionized water. Stir at 200 r / min for 30 min, then add 32.5 kg of 37% formaldehyde aqueous solution and 20.0 kg of 85% formic acid aqueous solution. Stir at 30℃ and 200 r / min for 1 h, then raise the temperature to 80℃ and react under reflux for 12 h. The gas generated by the reaction is condensed and introduced into an alkaline absorption liquid. After the reaction is completed, cool to 25℃, add 8% NaOH aqueous solution to adjust the pH to 6.8, filter, and wash the obtained solid with 150.0 kg of deionized water in three batches. Dry at 50℃ for 8 h to obtain tertiary amination chitosan resin.
[0053] A3. Weigh 25.0 kg of the tertiary amination chitosan resin obtained in step A2 and add it to 200.0 kg of deionized water. Stir at 200 r / min for 30 min, add 12.5 kg of sodium chloroacetate, and add an 8% NaOH aqueous solution to adjust the pH to 8.2. Stir at 65℃ and 220 r / min for 8 h. During the reaction, monitor and maintain the pH at 8.2 every 1 h. After the reaction is completed, cool to 25℃, filter, and wash the obtained solid with 150.0 kg of deionized water in 3 batches, then wash with 100.0 kg of anhydrous ethanol. Vacuum dry at 50℃ for 8 h to obtain carboxymethyl betaine type chitosan resin.
[0054] A4. Weigh 25.0 kg of the carboxymethyl betaine-type chitosan resin obtained in step A3 and add it to 100.0 kg of deionized water. Add 7.5 kg of 85% phosphoric acid and 5.0 kg of urea. Stir and impregnate at 35°C and 200 r / min for 2 h. Remove water under reduced pressure at 65°C and dry to a moisture content of 15%. Then raise the temperature to 130°C and react for 2 h. After the reaction is complete, cool naturally to 25°C. Add the obtained product to 100.0 kg of 0.3% sodium bicarbonate aqueous solution and stir at 25°C and 180 r / min for 30 min. Filter and wash the obtained solid with 150.0 kg of deionized water in 3 batches. Vacuum dry at 50°C to constant weight. Sieve particles with a particle size of 0.5-1.2 mm to obtain phosphorylated betaine-type chitosan resin.
[0055] Example 3
[0056] The difference between this embodiment and Embodiment 1 is that this embodiment provides a process for the directional separation and resource utilization of high-salt wastewater from rare earth smelting, the steps of which include:
[0057] S1. Weigh 1100.0 kg of high-salt wastewater from rare earth smelting, filter it through a filter material with a pore size of 100 μm, add 0.50 kg of 30% hydrogen peroxide aqueous solution, and stir for 20 min at 35℃ and 300 r / min; then add 22% ammonia water to adjust the pH to 4.8, and continue stirring at 300 r / min for 40 min; add 0.015 kg of anionic polyacrylamide, stir at 250 r / min for 2 min, then stir at 40 r / min for 10 min, let stand for 60 min, filter, and obtain a purified high-salt clear liquid and iron-aluminum sludge.
[0058] S2. Weigh 30.0 kg of phosphorylated betaine-type chitosan resin and pack it into the adsorption column. Pre-wash with 60.0 kg of deionized water. Introduce the purified high-salt solution obtained in step S1 into the adsorption column at a flow rate of 3.0 BV / h for adsorption. When the total rare earth element concentration at the adsorption column outlet reaches 5% of the total rare earth element concentration at the inlet, switch to a standby adsorption column. Continue this process until the purified high-salt solution is completely treated. Combine the adsorption effluents to obtain the rare earth removal solution. Introduce 40.0 kg of deionized water into the adsorption column for replacement, and then introduce... Desorption was performed using 150.0 kg of a 1.6 mol / L HCl aqueous solution to obtain a rare earth desorption solution. 2.50 kg of oxalic acid and 12% ammonia water were added to the rare earth desorption solution to adjust the pH to 2.0. The solution was stirred at 40℃ and 200 r / min for 30 min, allowed to stand for 2 h, and filtered to obtain a rare earth oxalate precipitate. The rare earth oxalate precipitate was washed with 25.0 kg of deionized water, dried at 105℃ for 6 h, calcined at 850℃ for 2 h, and cooled to 25℃ to obtain a mixed rare earth oxide.
[0059] S3. Add 85.0 kg of 15% ammonium carbonate aqueous solution and 22% ammonia solution to the rare earth removal solution obtained in step S2, adjust the pH to 9.2, and stir for 45 min at 45℃ and 250 r / min; add 0.50 kg of calcium carbonate seed crystals, continue stirring at 200 r / min for 20 min, let stand for 60 min, and filter through 1 μm filter material to obtain a softened filtrate; add 12% salt to the softened filtrate. The pH was adjusted to 7.0, and the mixture was stirred at 45℃ and 200 r / min for 20 min. 0.50 kg of powdered activated carbon was added, and stirring was continued for another 20 min. The mixture was then filtered through a 1 μm filter material to obtain a softened high-salt clear solution. The softened high-salt clear solution was subjected to two-stage nanofiltration at 35℃, 3.5 MPa, and a membrane flow rate of 1.5 m / s, with the total recovery rate controlled at 80%. The nanofiltration permeate and nanofiltration concentrate were collected separately to obtain chloride-enriched permeate and sulfate-enriched permeate, respectively.
[0060] S4. The sulfate enrichment solution obtained in step S3 is concentrated under reduced pressure at 80℃ and 50kPa to obtain 300.0 kg of concentrate A. 1.50 kg of ammonium sulfate seed crystals are added to concentrate A, stirred at 50 r / min and cooled to 30℃, kept at this temperature for 2.5 h for crystallization, and then centrifuged to obtain crystal A. Crystal A is washed with 25.0 kg of saturated ammonium sulfate aqueous solution and dried at 80℃ to constant weight to obtain regenerated ammonium sulfate. The chloride enrichment permeate obtained in step S3 is concentrated under reduced pressure at 75℃ and 45kPa to obtain 330.0 kg of concentrate B. 1.65 kg of ammonium chloride seed crystals are added to concentrate B, stirred at 50 r / min and cooled to 30℃, kept at this temperature for 2.5 h for crystallization, and then centrifuged to obtain crystal B. Crystal B is washed with 25.0 kg of saturated ammonium chloride aqueous solution and dried at 70℃ to constant weight to obtain regenerated ammonium chloride.
[0061] Preparation steps of phosphorylated betaine-type chitosan resin:
[0062] A1. Weigh 25.0 kg of chitosan and add it to 875.0 kg of a 2.5% acetic acid aqueous solution. Stir at 30℃ and 300 r / min for 4 hours, let stand to remove bubbles for 2 hours, and filter through a 100 μm filter to obtain chitosan sol. Evenly drip the chitosan sol through a 1.0 mm inner diameter dropper into a coagulation solution composed of 600.0 kg of a 12% NaOH aqueous solution and 262.5 kg of anhydrous ethanol. During the dripping process, maintain the temperature of the coagulation solution at 30℃ and stir at 150 r / min. After the dripping is complete... Continue stirring and solidification for 2 hours, then filter to obtain chitosan microspheres. Wash the chitosan microspheres with 150.0 kg of deionized water, then add 375.0 kg of deionized water and 6.25 kg of epichlorohydrin, followed by a 12% NaOH aqueous solution to adjust the pH to 11.0. Stir the reaction at 60℃ and 200 r / min for 5 hours. After the reaction is complete, cool to 25℃, filter, and wash the resulting solid successively with 100.0 kg of anhydrous ethanol and 150.0 kg of deionized water. Dry at 60℃ for 8 hours to obtain cross-linked chitosan resin microspheres.
[0063] A2. Weigh 25.0 kg of the cross-linked chitosan resin microspheres obtained in step A1 and add them to 300.0 kg of deionized water. Stir at 200 r / min for 30 min, then add 42.5 kg of 40% formaldehyde aqueous solution and 26.25 kg of 90% formic acid aqueous solution. Stir at 40℃ and 200 r / min for 1 h, then raise the temperature to 90℃ and react under reflux for 16 h. The gas generated by the reaction is condensed and introduced into an alkaline absorption liquid. After the reaction is completed, cool to 25℃, add 12% NaOH aqueous solution to adjust the pH to 7.2, filter, and wash the obtained solid with 150.0 kg of deionized water in 3 batches. Dry at 60℃ for 8 h to obtain tertiary amination chitosan resin.
[0064] A3. Weigh 25.0 kg of the tertiary amination chitosan resin obtained in step A2 and add it to 300.0 kg of deionized water. Stir at 200 r / min for 30 min, add 18.75 kg of sodium chloroacetate, and add a 12% NaOH aqueous solution to adjust the pH to 8.8. Stir at 75℃ and 220 r / min for 10 h. During the reaction, monitor and maintain the pH at 8.8 every 1 h. After the reaction is completed, cool to 25℃, filter, and wash the obtained solid with 150.0 kg of deionized water in 3 batches, then wash with 100.0 kg of anhydrous ethanol. Vacuum dry at 60℃ for 8 h to obtain carboxymethyl betaine type chitosan resin.
[0065] A4. Weigh 25.0 kg of the carboxymethyl betaine-type chitosan resin obtained in step A3 and add it to 150.0 kg of deionized water. Add 12.5 kg of 85% phosphoric acid and 8.75 kg of urea. Stir and impregnate at 45℃ and 200 r / min for 2 h. Remove water under reduced pressure at 75℃ and dry to a moisture content of 20%. Then raise the temperature to 140℃ and react for 3 h. After the reaction is completed, cool naturally to 25℃. Add the obtained product to 150.0 kg of 0.8% sodium bicarbonate aqueous solution and stir at 25℃ and 180 r / min for 30 min. Filter and wash the obtained solid with 150.0 kg of deionized water in 3 batches. Dry under vacuum at 60℃ to constant weight. Sieve particles with a particle size of 0.5-1.2 mm to obtain phosphorylated betaine-type chitosan resin.
[0066] Comparative Example 1
[0067] The difference between this comparative example and Example 1 is that the 24.0 kg of phosphorylated betaine-type chitosan resin in step S2 of Example 1 is replaced with 24.0 kg of cross-linked chitosan resin microspheres prepared in step A1, and the rest is the same as in Example 1.
[0068] Comparative Example 2
[0069] The difference between this comparative example and Example 1 is that the 24.0 kg of phosphorylated betaine-type chitosan resin in step S2 of Example 1 is replaced with 24.0 kg of carboxymethyl betaine-type chitosan resin obtained in step A3, and the rest is the same as in Example 1.
[0070] Comparative Example 3
[0071] The difference between this comparative example and Example 1 is that steps A2 and A3 of Example 1 are omitted. The cross-linked chitosan resin microspheres obtained in step A1 are directly phosphorylated according to the raw material dosage and process parameters of step A4 of Example 1 to obtain phosphorylated cross-linked chitosan resin. The 24.0 kg of phosphorylated betaine-type chitosan resin in step S2 of Example 1 is replaced with 24.0 kg of phosphorylated cross-linked chitosan resin. The rest is the same as in Example 1.
[0072] The performance of the directional separation and waste salt resource utilization processes for high-salt wastewater from rare earth smelting described in Examples 1-3 and Comparative Examples 1-3 was tested.
[0073] The corresponding samples prepared in Examples 1-3 and Comparative Examples 1-3 were tested. Each sample was measured in parallel 3 times, and the arithmetic mean was taken after subtracting the blank test results.
[0074] (1) Total rare earth recovery rate: The high-salt wastewater from rare earth smelting was thoroughly mixed, and 50.00 mL was placed in a digestion vessel. 5.00 mL of nitric acid and 1.00 mL of 30% hydrogen peroxide aqueous solution were added. The digestion was carried out at 120℃ for 5 min, 160℃ for 10 min, and 180℃ for 20 min, respectively. After cooling, the digestion was transferred to a 100 mL volumetric flask and diluted to volume with 2% nitric acid aqueous solution to obtain the original water test solution. The obtained mixed rare earth oxides were ground and passed through a 150 μm sieve. 0.1000 g was weighed and placed in a digestion vessel. 8.00 mL of nitric acid and 2.00 mL of hydrochloric acid were added. The same digestion procedure was used. After cooling, the volume was diluted to 100 mL with 2% nitric acid aqueous solution and then accurately diluted 100 times to obtain the product test solution. Inductively coupled plasma mass spectrometry was used to analyze the product test solution. The instrument was used to determine the concentrations of lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, and yttrium. The radio frequency power was set to 1550 W, the plasma gas flow rate to 15.0 L / min, the auxiliary gas flow rate to 0.80 L / min, the carrier gas flow rate to 1.05 L / min, the helium flow rate to 4.5 mL / min, and the single-point integration time to 50 ms. Rhodium and rhenium were used as internal standards. The internal standard concentration was set at 10.0 μg / L, and the standard solution concentrations were set at 0, 0.5, 1.0, 5.0, 10.0, 20.0, 40.0 and 50.0 μg / L respectively. The total mass of rare earth elements in the raw water and the total mass of rare earth elements in the mixed rare earth oxides were calculated respectively. The total rare earth recovery rate was calculated as "total mass of rare earth elements in the mixed rare earth oxides ÷ total mass of rare earth elements in the raw water × 100%".
[0075] (2) Dynamic adsorption capacity: Record the volume of the high-salt purified liquid entering the adsorption column, the volume of the rare earth removal liquid flowing out of the adsorption column, and the volume of the deionized water replacement liquid. Take 10.00 mL of each sample, add 2.00 mL of nitric acid, digest at 120 °C for 10 min, cool, and then dilute to 100 mL with 2% nitric acid aqueous solution. Determine the total concentration of rare earth elements in each sample according to the instrument conditions in the total rare earth recovery test. The dynamic adsorption capacity is calculated as "the difference between the total mass of rare earth elements entering the adsorption column and the total mass of rare earth elements in the rare earth removal liquid and replacement liquid ÷ the mass of phosphorylated betaine-type chitosan resin in the adsorption column". The result is expressed in mg / g.
[0076] (3) Rare earth desorption rate: Collect all rare earth desorption liquid discharged from the adsorption column and accurately measure the volume. Take 10.00 mL of rare earth desorption liquid and put it into a 100 mL volumetric flask. Dilute it to volume with 2% nitric acid aqueous solution and then accurately dilute it 100 times. Determine the total concentration of rare earth elements according to the instrument conditions in the total rare earth recovery rate test. Calculate the total mass of desorbed rare earth elements based on the volume of rare earth desorption liquid and the total concentration of rare earth elements. The rare earth desorption rate is calculated as "total mass of rare earth elements in rare earth desorption liquid ÷ total mass of rare earth elements adsorbed by the adsorption column × 100%".
[0077] (4) Chloride-sulfur separation coefficient: 10.00 mL of softened high-salt clear liquid and chloride-enriched permeate were diluted 1000 times with deionized water and passed sequentially through a hydrogen-type cation exchange column, a reverse-phase purification column, and a 0.45 μm aqueous filter membrane. The concentrations of chloride ions and sulfate ions were determined using an ion chromatograph equipped with an anion exchange column, suppressor, conductivity detector, and carbon dioxide suppression device. The eluent was prepared with 3.2 mmol / L sodium carbonate and 1.0 mmol / L sodium bicarbonate. The column temperature was set to 30℃, the eluent flow rate was set to 0.7 mL / min, and the injection volume was set to 25 μL. The concentrations of chloride ions and sulfate ions in the standard solutions were set to 0.5, 1.0, 5.0, 10.0, 20.0, and 50.0 mg / L, respectively, and the external standard method was used for quantification. The chloride-sulfur separation coefficient was calculated as "the ratio of chloride ion concentration to sulfate ion concentration in the chloride-enriched permeate to the ratio of chloride ion concentration to sulfate ion concentration in the softened high-salt clear liquid".
[0078] (5) Purity of regenerated ammonium sulfate: Mix the regenerated ammonium sulfate sample evenly and grind it through a 500μm sieve. Weigh 1.0000g of the sample and place it in a distillation flask. Add 100mL of deionized water to dissolve it, and then add 20.00mL of 40% NaOH aqueous solution. Immediately connect the distillation apparatus. Use a conical flask containing 50.00mL of 20g / L boric acid aqueous solution and 5 drops of methyl red-methylene blue mixed indicator solution to absorb the distilled ammonia. Set the collection volume of the distillate to 150mL. Titrate with 0.5000mol / L hydrochloric acid standard titration solution until the solution changes from green to gray-red and remains for 30s. At the same time, perform a blank test. The nitrogen content is calculated as "concentration of hydrochloric acid standard titration solution × difference between sample titration volume and blank titration volume × 1.4007 ÷ sample mass". The purity of regenerated ammonium sulfate is calculated as "nitrogen content × 4.716".
[0079] (6) Purity of regenerated ammonium chloride: Mix the regenerated ammonium chloride sample evenly and grind it through a 500μm sieve. Weigh 1.0000g of the sample and place it in a distillation flask. Add 100mL of deionized water to dissolve it, and then add 20.00mL of 40% NaOH aqueous solution. Immediately connect the distillation apparatus. Use a conical flask containing 50.00mL of 20g / L boric acid aqueous solution and 5 drops of methyl red-methylene blue mixed indicator solution to absorb the distilled ammonia. Set the collection volume of the distillate to 150mL. Titrate with 0.5000mol / L hydrochloric acid standard titration solution until the solution changes from green to gray-red and remains for 30s. At the same time, perform a blank test. The nitrogen content is calculated as "concentration of hydrochloric acid standard titration solution × difference between sample titration volume and blank titration volume × 1.4007 ÷ sample mass". The purity of regenerated ammonium chloride is calculated as "nitrogen content × 3.819".
[0080] The performance test data above are shown in Table 1.
[0081] Table 1: Performance Test Results
[0082] Test Project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Total rare earth recovery rate / % 98.6 96.8 97.7 66.4 81.2 89.5 Dynamic adsorption capacity (mg / g) 51.8 46.5 49.9 18.7 28.9 38.6 Rare earth desorption rate / % 96.7 94.5 95.6 72.3 84.6 91.8 Chlorine-sulfur separation coefficient 31.8 28.6 30.4 19.6 23.8 26.7 Purity of regenerated ammonium sulfate / % 99.3 98.8 99.1 96.9 97.8 98.4 Purity of regenerated ammonium chloride / % 99.6 99.2 99.4 97.8 98.4 99.0
[0083] The test results in Table 1 clearly show that the total rare earth recovery rate of Examples 1-3 was 96.8-98.6%, significantly higher than that of Comparative Examples 1-3 (66.4-89.5%); the dynamic adsorption capacity reached 46.5-51.8 mg / g, while that of Comparative Examples 1-3 was only 18.7-38.6 mg / g; the rare earth desorption rate reached 94.5-96.7%, higher than that of Comparative Examples 1-3 (72.3-91.8%). This indicates that phosphorylated betaine-type chitosan resin can effectively enrich residual rare earth elements under high salt and multi-ion coexistence conditions. Its phosphate groups, carboxyl groups, and nitrogen-containing groups form synergistic coordination sites, and the cross-linked microsphere structure takes into account mass transfer efficiency, column operation stability, and acid desorption performance, solving the problems of low adsorption capacity, insufficient selectivity, and difficulty in fully desorbing and recovering rare earths in ordinary adsorbent materials in high-salt wastewater.
[0084] The chloride-sulfur separation coefficients of Examples 1-3 were 28.6-31.8, significantly higher than those of Comparative Examples 1-3 (19.6-26.7). This indicates that the preceding processes of iron and aluminum removal, rare earth adsorption, ammonium carbonate softening, and powdered activated carbon purification effectively reduced the pollution and competitive mass transfer effects of metal ions, hardness ions, and organic impurities on the secondary nanofiltration process. This allowed chloride ions to preferentially enter the chloride enrichment permeate, while sulfate ions were effectively retained in the sulfate enrichment solution. This solved the problems of complex chloride and sulfate composition, severe membrane fouling, and unstable directional separation in high-salt wastewater from rare earth smelting.
[0085] The purity of the regenerated ammonium sulfate obtained in Examples 1-3 was 98.8-99.3%, and the purity of the regenerated ammonium chloride was 99.2-99.6%, which were higher than those of Comparative Examples 1-3 (96.9-98.4% and 97.8-99.0%, respectively). This indicates that the combination of secondary nanofiltration with vacuum concentration, seed-induced crystallization, and saturated aqueous solution rinsing can reduce the entrainment of foreign salts and residual impurities, and improve crystallization selectivity and product purity.
[0086] In summary, this invention achieves continuous integration of iron and aluminum impurity removal, rare earth element recovery, hardness ion removal, chlorine-sulfur directional separation, and the preparation of regenerated ammonium sulfate and regenerated ammonium chloride. It solves the problems of rare earth resource loss, difficulty in salt separation in high-salt systems, insufficient purity of waste salt, and low resource utilization value in existing processes. Among them, Example 1 has the highest total rare earth recovery rate, dynamic adsorption capacity, rare earth desorption rate, chlorine-sulfur separation coefficient, and purity of the two regenerated salts, indicating that its intermediate process parameters can achieve a good synergistic effect of rare earth adsorption, impurity removal, membrane separation, and crystallization purification.
Claims
1. A process for the directional separation and resource utilization of high-salt wastewater from rare earth smelting, characterized in that, Includes the following steps: S1. By weight, filter 900-1100 parts of high-salt wastewater from rare earth smelting, add 0.1-0.5 parts of hydrogen peroxide aqueous solution, and stir; then add ammonia water, adjust the pH, and continue stirring; add 0.005-0.015 parts of anionic polyacrylamide, stir, let stand, and filter to obtain a purified high-salt clear liquid and iron-aluminum sludge. S2. Pack 18-30 parts of phosphorylated betaine-type chitosan resin into an adsorption column, and pass a high-salt purified solution through the adsorption column for adsorption to obtain a rare earth removal solution; pass 20-40 parts of deionized water through the adsorption column for displacement, and then pass 60-150 parts of HCl aqueous solution for desorption to obtain a rare earth desorption solution; add 0.1-2.5 parts of oxalic acid and ammonia water to the rare earth desorption solution, adjust the pH, stir, age, and filter to obtain a rare earth oxalate precipitate; Rare earth oxalate precipitate was dried and calcined to obtain mixed rare earth oxides; S3. Add 5-85 parts of ammonium carbonate aqueous solution to the rare earth removal solution, add ammonia water, adjust the pH to 8.8-9.2, and stir; add 0.2-0.5 parts of calcium carbonate seed crystals, continue stirring, let stand, filter, and obtain softened filtrate; add hydrochloric acid to the softened filtrate, adjust the pH to 6.6-7.0, add 0.2-0.5 parts of powdered activated carbon, stir, filter, and obtain softened high-salt clear solution; subject the softened high-salt clear solution to two-stage nanofiltration to obtain chloride-enriched permeate and sulfate-enriched solution; S4. Concentrate the sulfate-enriched solution under reduced pressure to obtain concentrate A; add 0.2-0.5 parts of ammonium sulfate seed crystals to 100 parts of concentrate A, cool to crystallize, and centrifuge to obtain crystal A; rinse crystal A with a saturated aqueous solution of ammonium sulfate and dry to obtain regenerated ammonium sulfate; concentrate the chloride-enriched permeate under reduced pressure to obtain concentrate B; add 0.2-0.5 parts of ammonium chloride seed crystals to 100 parts of concentrate B, cool to crystallize, and centrifuge to obtain crystal B; rinse crystal B with a saturated aqueous solution of ammonium chloride and dry to obtain regenerated ammonium chloride.
2. The process for targeted separation and resource utilization of high-salt wastewater from rare earth smelting according to claim 1, characterized in that, In step S1, adjust the pH to 4.4-4.
8.
3. The process for targeted separation and resource utilization of high-salt wastewater from rare earth smelting according to claim 1, characterized in that, In step S2, the flow rate of the purified high-salt solution introduced into the adsorption column is 1.0-3.0 BV / h; the pH is adjusted to 1.6-2.
0.
4. The process for directional separation and resource utilization of high-salt wastewater from rare earth smelting according to claim 1, characterized in that, In step S3, the temperature of the secondary nanofiltration is 25-35℃.
5. The process for targeted separation and resource utilization of high-salt wastewater from rare earth smelting according to claim 1, characterized in that, In step S4, ammonium sulfate seed crystals are added to concentrated solution A, the temperature is lowered to 25-30℃, and crystallization is carried out for 1.5-2.5 hours; ammonium chloride seed crystals are added to concentrated solution B, the temperature is lowered to 20-30℃, and crystallization is carried out for 1.5-2.5 hours.
6. The process for targeted separation and resource recovery of high-salt wastewater from rare earth smelting according to any one of claims 1-5, characterized in that, The preparation steps of the phosphorylated betaine-type chitosan resin include: A1. By weight, add 100 parts of chitosan to 2500-3500 parts of an aqueous acetic acid solution with a mass fraction of 1.5-2.5%, stir at 20-30℃, allow to stand to remove bubbles, filter, and obtain chitosan sol; add the chitosan sol dropwise to a coagulation solution composed of 1800-2400 parts of an aqueous NaOH solution with a mass fraction of 8-12% and 750-1050 parts of anhydrous ethanol, stir, solidify, filter, and obtain chitosan microspheres; add the chitosan microspheres to 1000-1500 parts of deionized water, add 15-25 parts of epichlorohydrin, add an aqueous NaOH solution with a mass fraction of 8-12%, adjust the pH to 10.0-11.0, and stir the reaction at 50-60℃; after the reaction is complete, filter to obtain a solid; wash the solid sequentially with anhydrous ethanol and deionized water, dry, and obtain cross-linked chitosan resin microspheres; A2. Add 100 parts of cross-linked chitosan resin microspheres to 800-1200 parts of deionized water, add 130-170 parts of formaldehyde aqueous solution with a mass fraction of 37-40% and 80-105 parts of formic acid aqueous solution with a mass fraction of 85-90%, and stir at 30-40℃; then raise the temperature to 80-90℃ to react, cool to room temperature, add NaOH aqueous solution with a mass fraction of 8-12%, adjust the pH to 6.8-7.2, filter to obtain a solid; wash the solid with deionized water and dry to obtain tertiary amination chitosan resin; A3. Add 100 parts of tertiary amination chitosan resin to 800-1200 parts of deionized water, add 50-75 parts of sodium chloroacetate, add 8-12% NaOH aqueous solution, adjust the pH to 8.2-8.8, stir the reaction at 65-75℃ to obtain the reaction product; filter the reaction product to obtain the solid product; wash the solid product successively with deionized water and anhydrous ethanol, and vacuum dry at 50-60℃ to obtain carboxymethyl betaine type chitosan resin; A4. Add 100 parts of carboxymethyl betaine-type chitosan resin to 400-600 parts of deionized water, add 30-50 parts of 85% phosphoric acid and 20-35 parts of urea, and stir and impregnate at 35-45℃; remove water under reduced pressure, dry at 65-75℃, and then heat to 130-140℃ to react; cool naturally to room temperature to obtain the product; add the product to 400-600 parts of 0.3-0.8% sodium bicarbonate aqueous solution, stir, filter, and obtain a solid; wash the solid with deionized water, and vacuum dry at 50-60℃ to obtain phosphorylated betaine-type chitosan resin.
7. The process for targeted separation and resource utilization of high-salt wastewater from rare earth smelting according to claim 6, characterized in that, In step A1, the reaction is stirred at 50-60℃ for 3-5 hours.
8. The process for targeted separation and resource utilization of high-salt wastewater from rare earth smelting according to claim 6, characterized in that, In step A2, the reaction time is 12-16 hours after heating to 80-90℃.
9. The process for targeted separation and resource utilization of high-salt wastewater from rare earth smelting according to claim 6, characterized in that, In step A3, the reaction is stirred at 65-75℃ for 8-10 hours.