Preparation method of antibacterial water-soluble betaine modified chitosan and film thereof

Through the preparation of betaine modified chitosan, the problem of insufficient water solubility and antibacterial properties of chitosan is solved, efficient modification of chitosan is achieved, the scope of application is broadened, and the preparation difficulty and cost are reduced.

CN118955761AActive Publication Date: 2024-11-15GUANGDONG ANDAO TECHNOLOGY CO LTD +1

Patent Information

Application Number
CN202411275991.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-15
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

No research on the modification of chitosan by betaine in the prior art has been found, which limits the water solubility and antibacteriality of chitosan in natural polymer materials applications and cannot effectively broaden its application range.

Method used

By modifying betaine on chitosan, reacting chloropropyl betaine with chitosan in aqueous alkali/urea solution, combined with desalination, extraction, drying, stirring and dialysis treatment, antibacterial water-soluble betaine modification was prepared. Chitosan and its membranes.

Benefits of technology

It enhances the water solubility and antibacterial properties of chitosan, reduces the difficulty and cost of preparation, provides biosafety, degradability and bactericidality, and broadens its application value in the field of natural polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955761A_ABST
    Figure CN118955761A_ABST
Patent Text Reader

Abstract

The invention relates to the field of preparation of natural polymer materials, and discloses a preparation method of antibacterial water-soluble betaine modified chitosan and a film thereof, which comprises the following steps: S1, preparation of chloropropyl betaine: desalting an aqueous solution of N, N-dimethylaminochloropropane hydrochloride, then reacting with tert-butyl bromoacetate, after the reaction is finished, adding dichloromethane for dissolving, and filtering to obtain a filtrate; and reacting with trifluoroacetic acid, pumping out dichloromethane after the reaction is finished, dropwise adding the reaction product into ethyl acetate for settling separation, and carrying out vacuum suction filtration to obtain chloropropyl betaine. S2, modifying chitosan with betaine, dispersing chitosan powder in an alkali / urea aqueous solution to obtain a clear and transparent chitosan solution, adding chloropropyl betaine into the chitosan solution for reaction, and after the reaction is finished, performing dialysis and freeze-drying treatment to obtain the betaine modified chitosan. After the betaine modified chitosan prepared by the invention is prepared into a film, the film has biological safety, degradability, bactericidal property and washability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of natural polymer material preparation, and in particular to a method for preparing antibacterial water-soluble betaine-modified chitosan and a film thereof. Background Art

[0002] Betaine, whose chemical name is N,N,N-trimethylglycine, has a chemical structure similar to that of amino acids and is a quaternary ammonium alkaloid. It is widely present in animals and plants. Lycium barbarum and leguminous plants contain betaine, of which beet molasses is the main source of betaine; mollusks (such as octopus, cuttlefish, shrimp, etc.) and the liver, spleen and amniotic fluid of vertebrates (including humans) also contain betaine. Betaine is stable in a wide pH range and is not easily destroyed by acids and alkalis. It has zwitterionic characteristics and can react with acids and alkalis. It is widely used in biochemistry, nutritional supplements, food additives, corrosion protection and other fields.

[0003] Chitosan is a cationic polysaccharide, which is a random copolymer composed of N-acetyl-D-glucosamine and D-glucosamine units connected by β-1,4 glycosidic bonds. In the industrial field, it can be obtained by removing some acetyl groups from the natural polysaccharide chitin. Chitosan has been widely used in many fields such as biomedicine, cosmetics, pharmaceuticals, agriculture, textiles, and food due to its biocompatibility, biodegradability, film-forming properties, and antibacterial activity. However, chitosan can only be dissolved in acidic aqueous solutions or alkaline / urea aqueous solutions, which limits its application range to a certain extent.

[0004] In recent years, a large number of researchers have published articles on the chemical modification of chitosan through its N-amino function. For example, a Chinese invention patent application with a publication number of CN109485747A discloses a water-soluble chitosan antibacterial derivative and a preparation method thereof, wherein the water-soluble chitosan antibacterial derivative comprises a chitosan skeleton and a bifunctional group for modifying the amino group on the chitosan skeleton, wherein the bifunctional group is a guanidine group and a carbonyl polyethylene glycol monomethyl ether. The invention gives chitosan good antibacterial properties and higher biosafety by simultaneously modifying the side chain of chitosan with a guanidine group and a short-chain polyethylene glycol. The preparation method thereof is as follows: chitosan is first reacted with carboxyl polyethylene glycol monomethyl ether; and then reacted with thiourea trioxide.

[0005] Another example is a Chinese invention patent application with publication number CN117343214A, which discloses a method for preparing a water-soluble and antibacterial chitosan derivative and its application in fruit and vegetable preservation, comprising the following steps: (1) reacting chitosan with phthalic anhydride to generate N-phthaloyl chitosan, protecting the amino group on C2 of chitosan; (2) reacting with N-bromosuccinimide (NBS) and triphenylphosphine (PPh3) to obtain 6-bromo-6-deoxy-N-phthaloyl chitosan; (3) then reacting with aminoglycoside antibiotics, removing the phthalic anhydride on C2 with hydrazine hydrate, and obtaining a water-soluble and antibacterial chitosan derivative. The chitosan derivative is grafted with a large number of amino groups at the C6 position, which improves the water solubility and antibacterial properties of chitosan while taking into account its biological safety and reducing drug resistance. The chitosan derivative can be compounded with polymers such as pullulan, gelatin, starch, cellulose or alginate, and sprayed or coated on the surface of food or fruits and vegetables to form a transparent coating, which can effectively inhibit the infection of pathogenic microorganisms.

[0006] However, there is no related research on modifying chitosan with betaine in the prior art. In view of this, the present invention proposes for the first time to chemically modify chitosan with betaine, aiming to enhance its water solubility and antibacterial properties, so as to broaden its application value in natural polymer materials. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing antibacterial water-soluble betaine-modified chitosan and a film thereof, and to prepare betaine-modified chitosan by substitution reaction between organic compounds, thereby providing a new way for the modification of chitosan; and further providing at least a beneficial choice or creating conditions for solving one or more technical problems existing in the prior art.

[0008] To achieve the above objectives, the present invention adopts the following technical solutions.

[0009] A method for preparing antibacterial water-soluble betaine-modified chitosan comprises the following steps: 1) preparing chloropropyl betaine, adding sodium hydroxide solution to an aqueous solution of N,N-dimethylaminochloropropane hydrochloride under ice bath conditions for desalting; after the desalting is completed, adding ethyl acetate for extraction, and using anhydrous magnesium sulfate to dry the extract; after the drying is completed, vacuum filtration is performed to obtain a solution, and then tert-butyl bromoacetate is added to the solution for stirring reaction; after the reaction is completed, dichloromethane is added to dissolve, and trifluoroacetic acid is added for stirring reaction; after the reaction is completed, the dichloromethane is drained, and the extract is dried. The reaction product is added to ethyl acetate for sedimentation separation and vacuum filtration to obtain chloropropyl betaine; 2) betaine-modified chitosan, chitosan powder is dispersed in an alkali / urea aqueous solution to form a suspension; then, the suspension is placed in a refrigerator until it is completely frozen, then stirred and thawed at room temperature, and centrifuged to obtain a clear and transparent chitosan solution; chloropropyl betaine is added to the chitosan solution, first reacted at low temperature for a period of time, and then reacted at room temperature for a period of time; after the reaction is completed, the pH value is adjusted to 7 with a hydrochloric acid solution, and then dialyzed and freeze-dried to obtain betaine-modified chitosan.

[0010] More preferably, in step 1), the desalting time is 30±10 min.

[0011] More preferably, in step 1), the stirring reaction time of adding tert-butyl bromoacetate is 6-8 hours.

[0012] More preferably, in step 1), the temperature for adding trifluoroacetic acid and stirring the reaction is 50±5° C., and the reaction time is 3-5 hours.

[0013] More preferably, in step 1), the usage ratio of N,N-dimethylaminochloropropane hydrochloride, sodium hydroxide and tert-butyl bromoacetate is 12-18:3-5:25-35.

[0014] More preferably, in step 2), the alkali / urea aqueous solution is an aqueous solution of KOH, LiOH and urea, and in the alkali / urea aqueous solution, the content of KOH is 5-8wt%, the content of LiOH is 8-10wt%, and the content of urea is 8-10wt%.

[0015] More preferably, in step 2), the reaction time at low temperature is 12-18 hours, and the reaction time at room temperature is 12-18 hours.

[0016] More preferably, in step 2), the molar ratio of chitosan to chloropropyl betaine is 1:3-1:9.

[0017] On the other hand, the present invention also provides a method for preparing an antibacterial water-soluble betaine-modified chitosan film, wherein the betaine-modified chitosan prepared as above is dissolved in pure water to prepare a film-forming liquid, the film-forming liquid is centrifugally degassed and then poured into a culture dish for drying, and finally the film is peeled off to obtain the betaine-modified chitosan film.

[0018] More preferably, the concentration of the film-forming solution is 1-5wt%, the drying temperature is 40-60°C, and the drying time is 20-30 hours.

[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects.

[0020] 1. The present invention provides a betaine modified chitosan process, and the reaction conditions do not require strict anhydrous and anaerobic conditions, and there is no involvement of oxidants and catalysts. The operating conditions are relatively mild, which reduces the difficulty and cost of preparation; the water-soluble and antibacterial properties of the modified chitosan are enhanced.

[0021] 2. After the betaine-modified chitosan prepared by the present invention is prepared into a film, it has biological safety, degradability, bactericidal property, and water washability. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Shown is the synthetic route of betaine-modified chitosan.

[0023] Figure 2 Shown is the H NMR spectrum of betaine-modified chitosan.

[0024] Figure 3 Infrared image of betaine-modified chitosan.

[0025] Figure 4 Aqueous solubility graph of betaine-modified chitosan.

[0026] Figure 5 Fig. Adhesion and film-forming properties of betaine-modified chitosan.

[0027] Figure 6 Coating simulated washability plot of betaine-modified chitosan.

[0028] Figure 7 Macroscopic image and electron microscope (SME) image of betaine modified chitosan film.

[0029] Figure 8 In vitro antibacterial test diagram of betaine modified chitosan. DETAILED DESCRIPTION

[0030] The specific implementation of the present invention is further described below to make the technical solution and beneficial effects of the present invention clearer and more specific. The following embodiments are exemplary and intended to explain the present invention, but cannot be construed as limiting the present invention.

[0031] Additional aspects and advantages of the present invention will become apparent from the following description or may be learned by practice of the present invention.

[0032] Reference Figure 1 As shown, in the present invention, the preparation method of antibacterial water-soluble betaine-modified chitosan includes: 1) Preparation of chloropropyl betaine, N, N-dimethylamino chloropropane hydrochloride aqueous solution is reacted with tert-butyl bromoacetate after desalting, dichloromethane is added to dissolve, and then reacted with trifluoroacetic acid, dichloromethane is drained after the reaction, and the reaction product is added dropwise to ethyl acetate for sedimentation separation and vacuum filtration to obtain chloropropyl betaine. 2) Betaine-modified chitosan, chitosan powder is dispersed in an alkali / urea aqueous solution to obtain a clear and transparent chitosan solution, chloropropyl betaine is added to the chitosan solution for reaction, and after the reaction, dialysis and freeze-drying are performed to obtain betaine-modified chitosan.

[0033] Specifically, the process of preparing chloropropyl betaine in step 1) is as follows: adding sodium hydroxide solution to an aqueous solution of N,N-dimethylaminochloropropane hydrochloride under ice bath conditions for desalting; then adding ethyl acetate to complete extraction, and using anhydrous magnesium sulfate for drying; after drying, vacuum filtration is performed to obtain a solution; then tert-butyl bromoacetate is added to the solution for magnetic stirring reaction; after the reaction is completed, dichloromethane is added to dissolve, and then trifluoroacetic acid is added for magnetic stirring reaction; after the reaction is completed, the dichloromethane is drained, and the reaction product is added dropwise to ethyl acetate for sedimentation separation and vacuum filtration, thereby obtaining chloropropyl betaine.

[0034] Step 2) The process of betaine-modified chitosan is as follows: chitosan powder is dispersed in an alkali / urea aqueous solution to form a suspension; then, the suspension is placed in a refrigerator until it is completely frozen, then stirred and thawed at room temperature, and centrifuged to obtain a clear and transparent chitosan solution, after which chloropropyl betaine is added to the chitosan solution, first reacted at low temperature and then reacted at room temperature; after the reaction is completed, the pH value is adjusted to 7 with a hydrochloric acid solution, dialyzed and freeze-dried to obtain betaine-modified chitosan.

[0035] When preparing the betaine modified chitosan film, the betaine modified chitosan prepared as above is dissolved in pure water to prepare a film-forming solution, the film-forming solution is centrifugally degassed and then poured into a culture dish to dry, and finally the film is peeled off to obtain the betaine modified chitosan film. Example

[0036] A method for preparing antibacterial water-soluble betaine modified chitosan comprises the following preparation steps.

[0037] Step 1 S1: Preparation of chloropropyl betaine. 15.8g of N,N-dimethylaminochloropropane hydrochloride was dissolved in water to form an aqueous solution. Under ice bath conditions, 4.0g of sodium hydroxide solution was added to the aqueous solution of N,N-dimethylaminochloropropane hydrochloride for 30min of desalination. Ethyl acetate was then added to complete the extraction, and anhydrous magnesium sulfate was used for 12h of drying. After drying, vacuum filtration was performed to obtain the solution. Then 29.26g of tert-butyl bromoacetate was added dropwise to the solution, and a 6h magnetic stirring reaction was performed. After the reaction was completed, dichloromethane was added to dissolve, and trifluoroacetic acid was slowly added dropwise, and the reaction was magnetically stirred at 50°C for 3h. Finally, after the reaction was completed, dichloromethane was drained, and the reaction product was added dropwise to ethyl acetate for sedimentation separation and vacuum filtration to obtain chloropropyl betaine.

[0038] Step 2 S2: Betaine modified chitosan. First, 0.58g chitosan powder was dispersed in an alkali / urea aqueous solution containing 7wt% KOH, 8wt% LiOH, and 8wt% urea to form a suspension. Then, the suspension was placed in a -30°C refrigerator until completely frozen, then stirred and thawed at room temperature, and centrifuged for 15min (3000rpm) to obtain a clear and transparent chitosan solution. After that, 4.18g chloropropyl betaine was added to the chitosan solution, first reacted at low temperature for 12h, and then reacted at room temperature for 12h. After the reaction, the pH value was adjusted to 7 with 1mol / L hydrochloric acid solution, and dialyzed and freeze-dried to obtain betaine modified chitosan LBM-CS. Example

[0039] A method for preparing antibacterial water-soluble betaine modified chitosan comprises the following preparation steps.

[0040] Step 1 S1: Preparation of chloropropyl betaine. 15.8g of N,N-dimethylaminochloropropane hydrochloride was dissolved in water to form an aqueous solution. Under ice bath conditions, 4.0g of sodium hydroxide solution was added to the aqueous solution of N,N-dimethylaminochloropropane hydrochloride for 30min of desalination. Ethyl acetate was then added to complete the extraction, and anhydrous magnesium sulfate was used for 12h of drying. After drying, vacuum filtration was performed to obtain the solution. Then 29.26g of tert-butyl bromoacetate was added dropwise to the solution, and a 6h magnetic stirring reaction was performed. After the reaction was completed, dichloromethane was added to dissolve, and trifluoroacetic acid was slowly added dropwise, and the reaction was magnetically stirred at 50°C for 3h. Finally, after the reaction was completed, dichloromethane was drained, and the reaction product was added dropwise to ethyl acetate for sedimentation separation and vacuum filtration to obtain chloropropyl betaine.

[0041] Step 2 S2: Betaine modified chitosan. First, 0.58g chitosan powder was dispersed in an alkali / urea aqueous solution containing 7wt% KOH, 8wt% LiOH, and 8wt% urea to form a suspension. Then, the suspension was placed in a -30°C refrigerator until completely frozen, then stirred and thawed at room temperature, and centrifuged for 15min (3000rpm) to obtain a clear and transparent chitosan solution. After that, 8.37g chloropropyl betaine was added to the chitosan solution, first reacted at low temperature for 12h, and then reacted at room temperature for 12h. After the reaction, the pH value was adjusted to 7 with 1mol / L hydrochloric acid solution, and dialyzed and freeze-dried to obtain betaine modified chitosan MBM-CS. Example

[0042] A method for preparing antibacterial water-soluble betaine modified chitosan comprises the following preparation steps.

[0043] Step 1 S1: Preparation of chloropropyl betaine. 15.8g of N,N-dimethylaminochloropropane hydrochloride was dissolved in water to form an aqueous solution. Under ice bath conditions, 4.0g of sodium hydroxide solution was added to the aqueous solution of N,N-dimethylaminochloropropane hydrochloride for 30min of desalination. Ethyl acetate was then added to complete the extraction, and anhydrous magnesium sulfate was used for 12h of drying. After drying, vacuum filtration was performed to obtain the solution. Then 29.26g of tert-butyl bromoacetate was added dropwise to the solution, and a 6h magnetic stirring reaction was performed. After the reaction was completed, dichloromethane was added to dissolve, and trifluoroacetic acid was slowly added dropwise, and the reaction was magnetically stirred at 50°C for 3h. Finally, after the reaction was completed, dichloromethane was drained, and the reaction product was added dropwise to ethyl acetate for sedimentation separation and vacuum filtration to obtain chloropropyl betaine.

[0044] Step 2 S2: Betaine modified chitosan. First, 0.58g chitosan powder was dispersed in an alkali / urea aqueous solution containing 7wt% KOH, 8wt% LiOH, and 8wt% urea to form a suspension. Then, the suspension was placed in a -30°C refrigerator until completely frozen, then stirred and thawed at room temperature, and centrifuged for 15min (3000rpm) to obtain a clear and transparent chitosan solution. After that, 12.56g chloropropyl betaine was added to the chitosan solution, first reacted at low temperature for 12h, and then reacted at room temperature for 12h. After the reaction, the pH value was adjusted to 7 with 1mol / L hydrochloric acid solution, and dialyzed and freeze-dried to obtain betaine modified chitosan HBM-CS. Example

[0045] A method for preparing a betaine-modified chitosan film, wherein the preparation steps are as follows: the betaine-modified chitosan prepared in step 2 S2 of embodiment 1 is dissolved in pure water to prepare a film-forming liquid with a mass fraction of 2%. The film-forming liquid is centrifuged and degassed, and then poured into a plastic culture dish. The film is then placed in an oven and dried at a temperature of 45° C. Finally, the film is peeled off to obtain a betaine-modified chitosan film.

[0046] Among them, the culture dish is a plastic culture dish with a diameter of 90 mm, 25 mL of film-forming liquid is poured in, and the drying time is 24 h.

[0047] In order to verify the structure of betaine-modified chitosan, the present invention conducted nuclear magnetic 1H NMR characterization on LBM-CS, MBM-CS, and HBM-CS. The results are as follows Figure 2 As shown. Figure 2 It can be seen that 1.97-2.08 ppm is the chemical shift of CONH-, and 3.10-3.30 is the chemical shift of methyl on quaternary ammonium salt and methylene on quaternary ammonium salt. The DS of betaine-modified chitosan was calculated by peak area, and the DS of LBM-CS was 40.29%, the DS of MBM-CS was 45.65%, and the DS of HBM-CS was 50.43%. The 1H NMR graph showed that betaine-modified chitosan was successfully synthesized in each embodiment.

[0048] In order to further verify the structure of betaine-modified chitosan, the present invention also characterized the infrared spectrum of betaine-modified chitosan by infrared method, such as Figure 3 As shown, for chitosan, at 3400 cm -1 The absorption peak at 1629cm is attributed to the stretching vibration peaks of hydroxyl (-OH) and amino (-NH2). -1 The absorption peak at 1000-1300cm is attributed to the stretching vibration peak of the amide bond (-CONH-) in the chitosan molecule. -1 The absorption peak near 1523cm -1 The absorption peak at is the stretching vibration peak of the methyl group (-CH3) in the introduced chloropropyl betaine molecule. The infrared results show that the substitution reaction between chitosan and chloropropyl betaine is completed, and the product is betaine modified chitosan.

[0049] In order to determine the water solubility of betaine-modified chitosan, 0.1 g of chitosan, 0.1 g of LBM-CS, 0.1 g of MBM-CS and 0.1 g of HBM-CS were added to the corresponding glass bottles, and 2 mL of pure water was added to each glass bottle to observe its dissolution in 10 minutes. The results are shown in Figure 4As shown, at 10 min, chitosan was not dissolved in 2 mL of pure water, while LBM-CS, MBM-CS and HBM-CS were completely dissolved in 2 mL of pure water, indicating that chitosan is not water-soluble, and the synthesized LBM-CS, MBM-CS and HBM-CS are water-soluble.

[0050] In order to determine the adhesion and film-forming ability of betaine-modified chitosan on hydrophobic surfaces, 1 mL of 1 wt% LBM-CS, MBM-CS and HBM-CS solutions were dropped onto 75 mm × 25 mm hydrophobic surfaces (glass and plastic), and their adhesion and film-forming properties were observed after drying at room temperature for 24 h. Figure 5 As shown. Figure 5 It can be seen that LBM-CS, MBM-CS and HBM-CS solutions can be easily spread on the hydrophobic surface and form a uniform film after drying. The obtained coating can be easily peeled off from the plastic substrate, but not easily peeled off from the glass substrate. This shows that LBM-CS, MBM-CS and HBM-CS have the ability to form a film on the hydrophobic surface, and betaine-modified chitosan can adhere better to the glass substrate than the plastic substrate.

[0051] In order to verify the washability of betaine-modified chitosan coating, the coating was immersed in tap water for friction washing in a way that simulated washing fruits, and the coating was observed to fall off from the substrate into the water. Figure 6 As shown, after the LBM-CS, MBM-CS and HBM-CS coatings were rubbed and washed in tap water for 4 minutes, the entire coating fell off the substrate into the water. This shows that the LBM-CS, MBM-CS and HBM-CS coatings prepared by the present invention are washable, and betaine-modified chitosan can be prepared into an antibacterial coating, which can be applied to the field of fruit and vegetable preservation and ensure that the fruit and vegetable can be easily removed from the surface before eating.

[0052] Figure 7 The macroscopic image and electron microscope (SME) image of the betaine-modified chitosan film prepared in Example 4 are shown; Figure 7 It can be seen intuitively that the surfaces of LBM-CS, MBM-CS and HBM-CS films are flat, smooth and transparent, without obvious cracks and holes, with dense cross-sections and no voids, and have good air tightness and light transmittance.

[0053] In order to verify the antibacterial property of betaine-modified chitosan, the present invention also conducted an in vitro antibacterial test: S. aureus (Staphylococcus aureus) and E. coli (Gram-negative bacteria) were used as antibacterial objects to test the in vitro antibacterial performance of betaine-modified chitosan film. LBM-CS, MBM-CS, HBM-CS and blank control groups with mass concentrations of 1×1%, 1 / 2×1%, 1 / 4×1%, 1 / 8×1%, 1 / 16×1%, 1 / 32×1% and 1 / 64×1% were respectively compared with 1x10 6 CFU / mL of S. aureus and E. coli bacteria were co-cultured for 3 hours, and 100 μL of the co-culture solution was spread on agar for 24 hours to observe the colony growth. Figure 8 As shown. Figure 8 It can be seen that LBM-CS, MBM-CS and HBM-CSQ-CS have strong antibacterial activity, and their antibacterial activity is mainly generated by the electrostatic interaction between cationic quaternary ammonium salts and negatively charged cell or bacterial membranes. These results show that betaine-modified chitosan can effectively inhibit or delay the growth of microorganisms and has good application prospects in antibacterial applications.

[0054] It should be noted that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0055] The above embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. The parts not described in the specific embodiments are all prior art or common knowledge.

[0056] It should be noted that, in the description of the present invention, the content of the present invention can be more easily understood by referring to the detailed description of the preferred implementation method of the present invention above and the embodiments included. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definitions in this specification shall prevail.

[0057] In the present invention, the term "prepared from..." is used synonymously with "comprising". The terms "comprising", "including", "having", "containing" or any other variation thereof, as used in the present invention, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0058] In the present invention, when an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range limited by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including a range of "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When a numerical range is described in the present invention, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0059] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.

Claims

1. A method for preparing antibacterial water-soluble betaine-modified chitosan, It is characterized in that Here are the steps: 1) preparing chloropropyl betaine, adding sodium hydroxide solution to an aqueous solution of N,N-dimethylaminochloropropane hydrochloride under ice bath conditions for desalting; after the desalting is completed, adding ethyl acetate for extraction, and using anhydrous magnesium sulfate to dry the extract; after the drying is completed, vacuum filtration is performed to obtain a solution, and then tert-butyl bromoacetate is added to the solution for stirring reaction; after the reaction is completed, dichloromethane is added to dissolve, and then trifluoroacetic acid is added for stirring reaction; after the reaction is completed, the dichloromethane is drained, and the reaction product is added to ethyl acetate for sedimentation separation and vacuum filtration, thereby obtaining chloropropyl betaine; 2) Betaine-modified chitosan, dispersing chitosan powder in an alkali / urea aqueous solution to form a suspension; then, placing the suspension in a refrigerator until completely frozen, stirring and thawing at room temperature, and centrifuging to obtain a clear and transparent chitosan solution; adding chloropropyl betaine to the chitosan solution, first reacting at low temperature for a period of time, and then reacting at room temperature for a period of time; After the reaction, the pH value was adjusted to 7 with hydrochloric acid solution, and then dialyzed and freeze-dried to obtain betaine-modified chitosan.

2. A method for preparing an antibacterial water-soluble betaine-modified chitosan according to claim 1, It is characterized in that In step 1), the desalting time is 30±10 min.

3. A method for preparing an antibacterial water-soluble betaine-modified chitosan according to claim 1, It is characterized in that In step 1), tert-butyl bromoacetate is added and stirred for reaction for 6-8 hours.

4. The method for preparing an antibacterial water-soluble betaine-modified chitosan according to claim 1, It is characterized in that In step 1), the temperature for adding trifluoroacetic acid and stirring the reaction is 50±5° C., and the reaction time is 3-5 hours.

5. The method for preparing an antibacterial water-soluble betaine-modified chitosan according to claim 1, It is characterized in that In step 1), the usage ratio of N,N-dimethylaminochloropropane hydrochloride, sodium hydroxide and tert-butyl bromoacetate is 12-18:3-5:25-35.

6. The method for preparing an antibacterial water-soluble betaine-modified chitosan according to claim 1, It is characterized in that In step 2), the alkali / urea aqueous solution is an aqueous solution of KOH, LiOH and urea, and in the alkali / urea aqueous solution, the content of KOH is 5-8wt%, the content of LiOH is 8-10wt%, and the content of urea is 8-10wt%.

7. The method for preparing an antibacterial water-soluble betaine-modified chitosan according to claim 1, It is characterized in that In step 2), the reaction time at low temperature is 12-18 hours, and the reaction time at room temperature is 12-18 hours.

8. The method for preparing an antibacterial water-soluble betaine-modified chitosan according to claim 1, It is characterized in that In step 2), the molar ratio of chitosan to chloropropyl betaine is 1:3-1:

9.

9. A method for preparing an antibacterial water-soluble betaine-modified chitosan film, It is characterized in that The betaine-modified chitosan prepared by the method for preparing an antibacterial water-soluble betaine-modified chitosan as claimed in any one of claims 1 to 8 is dissolved in pure water to prepare a film-forming solution, the film-forming solution is centrifugally degassed and then poured into a culture dish for drying, and finally the film is peeled off to obtain a betaine-modified chitosan film.

10. The method for preparing an antibacterial water-soluble betaine-modified chitosan film according to claim 9, It is characterized in that The concentration of the film-forming solution is 1-5wt%, the drying temperature is 40-60°C, and the drying time is 20-30 hours.

Citation Information

Patent Citations

  • A betaine-based amphoteric thickener based on guar gum derivatives and its preparation method

    CN102277141A

  • Polysaccharide hydrogel containing betaine-modified chitosan and preparation method thereof

    CN108014376A

  • Enhanced relaxivity monomeric and multimeric compounds

    CN1128534A

  • Method for synthesizing 5-substituted oxazolidinone by using bipyridine ionic liquid catalyst

    CN116332867A

  • Betaine group-containing polysaccharides with recurring anhydroglucose units, their synthesis and their use in cosmetic preparations

    US5124446A

Cited By

  • Biological preparation containing arbuscular mycorrhizal fungi and preparation method thereof

    CN119867087A

  • A biological preparation containing arbuscular mycorrhizal fungi and its preparation method

    CN119867087B