A method for preparing float glass

By using tantalum-niobium tailings and zirconium acetate solution for pre-calcination, the float glass manufacturing process was optimized, solving the problems of insufficient light transmittance and bending strength of tantalum-niobium tailings in float glass production, and realizing the resource utilization and performance improvement of solid waste.

CN123105984APending Publication Date: 2026-11-17PINGXIANG ANYUAN GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611448788.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing float glass production, the high iron content of tantalum-niobium tailings affects light transmittance and color, and has low bending strength, making it difficult to achieve high-value utilization of solid waste.

Method used

Using tantalum-niobium tailings as part of the raw material, combined with pre-calcination treatment with zirconium acetate solution, and through magnetic separation to remove iron and homogenization treatment, highly dispersed active zirconium oxide is prepared to improve the glass network structure. By adding raw materials such as dolomite and limestone, the melting and annealing processes are optimized to improve flexural strength while maintaining light transmittance and color.

Benefits of technology

This method enables the resource utilization of tantalum-niobium tailings, improves the bending strength of float glass, and maintains good light transmittance and color, thus solving the application problem of tantalum-niobium tailings in float glass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to the field of inorganic materials technology, specifically to a method for preparing float glass, comprising the following steps: crushing and screening tantalum-niobium tailings, removing iron through magnetic separation, homogenizing, and dehydrating to obtain pretreated tantalum-niobium tailings; the formula consists of 37-57 parts quartz sand, 12-15 parts soda ash, 3.7-5.5 parts pretreated tantalum-niobium tailings, 11.2-16.8 parts dolomite, 2.1-3.1 parts limestone, 0.6-0.9 parts mirabilite, 0.01-0.03 parts carbon powder, 11.9-17.9 parts crushed glass, 0.40-0.63 parts zirconium acetate, and 0.05-0.15 parts cerium oxide, which are then mixed, melted, shaped, and annealed to obtain the finished float glass. The prepared float glass utilizes tantalum-niobium tailings as a partial raw material, achieving high-value utilization of solid waste. The prepared float glass has high strength and maintains good light transmittance and color.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of inorganic materials technology, specifically to a method for preparing float glass. Background Technology

[0002] Float glass is the mainstream production process for flat glass. Its conventional production process uses quartz sand, soda ash, dolomite, limestone, mirabilite, and carbon powder as basic raw materials. These materials undergo high-temperature melting, clarification, homogenization, and cooling in a glass melting furnace before being formed and annealed in a tin bath. The beneficiation process of tantalum and niobium ore generates a large amount of tantalum and niobium tailings, whose chemical composition is mainly SiO2, while also containing certain amounts of Al2O3, K2O, Na2O, and a small amount of Li2O. Li2O helps to lower the melting temperature, but these tailings usually have a high iron content, affecting light transmittance and color. Furthermore, existing float glass has relatively low flexural strength. This application aims to study the raw materials and preparation process of float glass, providing a method that allows tantalum and niobium tailings to be used as part of the raw material in the float glass production process, improving the flexural strength of float glass while maintaining good light transmittance and color. Summary of the Invention

[0003] In view of the shortcomings of the prior art, the purpose of this invention is to provide a method for preparing float glass. The float glass prepared by this invention can utilize tantalum and niobium tailings as part of the raw materials to achieve high-value utilization of solid waste. While improving the bending strength of the float glass, it also maintains good light transmittance and color.

[0004] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a method for preparing float glass, comprising the following steps: S1. The tantalum-niobium tailings raw material is crushed, screened, magnetically separated to remove iron, homogenized and dehydrated to obtain pretreated tantalum-niobium tailings. The above treatment can convert the tantalum-niobium tailings into usable glass preparation raw materials. S2. Take the following raw materials in the following weight proportions: 37-57 parts quartz sand, 12-15 parts soda ash, 3.7-5.5 parts pretreated tantalum-niobium tailings, 11.2-16.8 parts dolomite, 2.1-3.1 parts limestone, 0.6-0.9 parts mirabilite, 0.01-0.03 parts carbon powder, 11.9-17.9 parts crushed glass, 0.40-0.63 parts zirconium acetate, and 0.05-0.15 parts cerium oxide; wherein, quartz sand is used to introduce silica as a glass network forming body, soda ash is used to introduce sodium oxide as a fluxing agent, tantalum-niobium tailings replace feldspar to introduce alumina, silica, and lithium oxide as fluxing agents, dolomite introduces magnesium oxide as fluxing agents, limestone introduces calcium oxide for stabilization, carbon powder is used as a reducing agent, crushed glass is used as clinker, cerium oxide is used as a clarifying and decolorizing agent, and zirconium acetate introduces highly dispersed active zirconium oxide for reinforcement.

[0005] S3. Add zirconium acetate to water to prepare a 5-15 wt% zirconium acetate solution. Mix the raw materials in the above formula except for zirconium acetate, and then add the zirconium acetate solution and continue mixing to obtain a mixture. S4. After pre-firing the mixture at 450-550℃, it is put into a glass melting furnace for melting to obtain molten glass. Pre-firing at 450-550℃ can make the moisture in the raw materials evaporate and cause zirconium acetate to decompose in situ into highly dispersed zirconium oxide. S5. The molten glass is poured into a tin bath for shaping to obtain a glass ribbon; S6. Anneal the glass strip according to the set annealing regime, cool it to room temperature, and then cut and package it to obtain the finished float glass.

[0006] Further, in step S1, the crushing and screening process involves passing the crushed material through a 40-80 mesh sieve and collecting the undersize material. The magnetic separation for iron removal employs a wet high-intensity magnetic separator with a two-stage magnetic separation process, achieving a magnetic field strength ≥1.5T, thereby controlling the Fe2O3 content in the tantalum-niobium tailings to ≤0.2%. The homogenization process involves sending the magnetically separated tailings into a homogenization tank for mechanical stirring. The dewatering process involves pressure filtration followed by natural dewatering in a closed tailings tank until the moisture content is ≤10%. Through these specific pretreatment processes, the particle size of the tantalum-niobium tailings can be matched with other raw materials, preventing the formation of large, unmelted particles in the molten glass. The two-stage magnetic separation further reduces the iron content in the tailings, and the homogenization process ensures the uniformity of the raw materials.

[0007] Further, in step S1, the pretreated tantalum-niobium tailings mainly consist of 70-78% silicon dioxide, 10-18% aluminum oxide, 3-5% potassium oxide, 3-5% sodium oxide, 0.1-0.3% lithium oxide, and 0-0.2% iron oxide, with the balance being unavoidable impurities. Tantalum-niobium tailings can replace some of the silica sand. The aluminum oxide in the tailings can synergistically improve the flexural strength of the glass with the highly dispersed and active zirconium oxide decomposed from zirconium acetate. Sodium oxide and potassium oxide can promote melting and bubble removal, while lithium oxide has a strong fluxing effect, which is beneficial for improving the melting effect.

[0008] Further, in step S4, the pre-fired mixture is fed into a glass melting furnace, and the thermocouple temperatures of each small furnace zone along the length of the furnace are set to 1410-1420℃, 1450-1460℃, 1480-1490℃, 1500-1510℃, 1510-1520℃, 1470-1480℃, 1430-1440℃, and 1390-1400℃, respectively.

[0009] In the preparation of molten glass, the pre-fired mixture is fed into the melting zone of the glass melting furnace, where it melts on the surface of the molten glass. When it reaches the hot spot temperature (the highest temperature point in the entire furnace, 1510-1520℃), the melting is basically completed. Then it enters the hot spot temperature zone for clarification and subsequent homogenization to reduce the glass viscosity and suppress backflow to achieve glass homogenization. Finally, it is cooled to a suitable tin bath forming temperature and enters the next process. Furthermore, the pre-calcination method involves placing the mixture into a calcining furnace and pre-calcining it at 450-550℃ for 1-2 hours under a nitrogen atmosphere at a heating rate of 3-5℃ / min. This pre-calcination process allows moisture in the raw materials to evaporate and enables zirconium acetate to decompose in situ into highly dispersed, active zirconium oxide, which readily dissolves into the glass network during the heating process.

[0010] Furthermore, in S5, the protective atmosphere in the tin bath is N2:H2 = 95:5, and the pressure is a slight positive pressure of 10-20 Pa; the spreading temperature of the glass melt on the tin melt surface is 1060-1100℃, and the outlet temperature is controlled at 600-640℃; the drawing speed is 300-350 m / h.

[0011] Further, in step S6, the annealing process specifically involves feeding the glass ribbon into an annealing furnace and sequentially annealing it in zones A1, B1, B2, C, E1, D1, D2, E2, F1, F2, and F3. The annealing rate in zone A1 is 22-28°C / min, in zones B1 and B2 it is 6.17-18.33°C / min, in zone C it is 22.93-45.83°C / min, in zones E1, D1, D2, and E2 it is 7.51-54.99°C / min, in zone F1 it is 27.51-54.99°C / min, and in zones F2 and F3 it is 13.75-36.66°C / min.

[0012] Zone A1 rapidly cools the glass after it leaves the tin bath, passing the strain point to prevent thermal deformation. Zones B1 and B2 slowly pass the glass through the critical temperature range from the strain point to the annealing point at a lower rate, ensuring a uniform temperature field inside the glass and eliminating overall thermal stress. Zone C allows for a faster cooling rate since the glass has already passed the annealing point. Zones E1 / D1 / D2 / E2 undergo multi-stage cooling to prevent new temporary stresses caused by excessive temperature differences between the glass surface and interior. Zones F1 / F2 / F3 allow for rapid cooling as the glass is almost hardened, increasing production efficiency and ultimately resulting in finished glass with high flatness, satisfactory optical deformation, and fully released internal stress.

[0013] Further, in step S3, the mixing method is as follows: All raw materials of the above formulation, except for zirconium acetate, are fed into a mixer and dry-mixed for 30-60 seconds. Then, a zirconium acetate solution is sprayed in and mixing continues for 120-150 seconds. By first performing dry mixing to achieve uniform mixing of the powdered raw materials, and then spraying in the zirconium acetate solution to continue mixing, the adhesion between the components can be improved, and the zirconium acetate solution can coat the surface of the raw material particles, achieving uniform dispersion.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention utilizes tantalum-niobium tailings as a composite raw material containing SiO2, Al2O3, Li2O, K2O, and Na2O to partially replace quartz sand and soda ash, thereby realizing the resource utilization of industrial solid waste. The formula adds zirconium acetate, which is easily soluble in water. During the pre-calcination stage, zirconium acetate decomposes to produce highly dispersed active zirconium oxide, which can dissolve into the glass network in the heating stage. Together with the al2O3 introduced by the tailings in the glass network, it plays a synergistic role in improving the bending strength. The method provided by this application improves the bending strength of float glass while maintaining good light transmittance and color. Detailed Implementation

[0015] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. The described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0016] The preparation method of pretreated tantalum-niobium tailings in the embodiments and comparative examples of this invention is as follows: Tantalum-niobium tailings are taken, first coarsely crushed by a jaw crusher, then finely crushed by a double-roll crusher, and then screened by a vibrating screen. The 60-mesh undersize material is then sent to a wet high-intensity magnetic separator for two-stage magnetic separation. The magnetic field strength of the separator is 1.5T, until the Fe2O3 content drops below 0.2%. The magnetically separated tailings are sent to a homogenization tank and homogenized for 4 hours by mechanical stirring. Then, they are dewatered using a plate and frame filter press and transferred to a closed tailings tank for natural dewatering until the moisture content reaches 9.70%, thus obtaining pretreated tantalum-niobium tailings. Analysis shows that the main chemical composition of the pretreated tantalum-niobium tailings is: SiO2 76.72%, Al2O3 12.25%, Fe2O3 0.07%, CaO 0.23%, Na2O 3.22%, K2O 4.15%, and Li2O 0.15%.

[0017] Quartz sand, soda ash, dolomite, limestone, mirabilite, and charcoal powder were subjected to iron removal and sieving processes, and the raw materials selected for the following examples and comparative examples in this application are as follows: Quartz sand: SiO2 99.04%, Al2O3 0.32%, Fe2O3 0.06%, loss on ignition 0.38%, fineness 80 mesh; Soda ash: Na₂CO₃ 99.27%, NaCl 0.62%; Dolomite: SiO2 0.48%, Al2O3 0.14%, Fe2O3 0.05%, CaO 30.82%, MgO 21.01%, fineness 80 mesh.

[0018] Glauber's salt: Na₂SO₄ 98.25%, NaCl 0.65%; Limestone: SiO2 0.95%, Al2O3 0.13%, Fe2O3 0.07%, CaO 53.70%, MgO 1.18%, fineness 80 mesh.

[0019] Requirements for cullet: 20-50 mm cullet should account for more than 90% of the total volume, and the composition should be 72.2% SiO2, 1.10% Al2O3, 8.55% CaO, 4% MgO, 13.9% R2O, 0.08% Fe2O3, and 0.17% SO3.

[0020] Unless otherwise specified, all methods described herein are conventional methods, and all raw materials described herein are available from publicly available commercial sources.

[0021] Example 1 This embodiment provides a method for preparing float glass, including the following steps: 1. Weigh the following raw materials according to the following weight parts: 47.24 parts of quartz sand, 13.72 parts of soda ash, 4.61 parts of pretreated tantalum-niobium tailings (dry basis), 14.01 parts of dolomite, 2.66 parts of limestone, 0.77 parts of mirabilite, 0.02 parts of carbon powder, 14.98 parts of crushed glass, 0.51 parts of zirconium acetate, and 0.14 parts of cerium oxide.

[0022] 2. Mixing: Zirconium acetate is added to water to prepare a 10% zirconium acetate solution. All raw materials except zirconium acetate are fed into a mixer. The mixture is first dry-mixed at 300 rpm for 45 seconds. Then, while stirring, the atomized zirconium acetate solution is sprayed in and the mixture is continued for 135 seconds.

[0023] 3. Melting: The mixture is fed into a calcining furnace and pre-calcined at 500℃ for 1.5 hours in a nitrogen atmosphere at a heating rate of 4℃ / min. The mixture is then directly fed into a glass melting furnace. The melting regime is shown in Table 1 below. Table 1: Melting Process

[0024] 4. Forming: The molten glass is poured into a tin bath. The protective atmosphere in the tin bath is N2:H2=95:5, and the bath pressure is maintained at 15Pa. The temperature of the molten glass spreading on the tin surface is controlled at 1080℃, the temperature at the tin bath outlet is 620℃, and the drawing speed is 320.51m / h, resulting in a glass ribbon with a thickness of 6mm.

[0025] 5. Annealing: The glass ribbon enters the annealing furnace and is annealed according to the annealing temperature curve in Table 2 below. The drawing speed is 320.51 m / h, and the outlet temperature of zone F3 is 70℃. After annealing, the glass ribbon is cut and packaged to obtain the finished float glass product.

[0026] Table 2: Annealing Temperature Curve

[0027] The prepared float glass products were subjected to performance tests. The visible light transmittance was tested using GB / T 2680, the Lab value was determined using GB / T 36142, the bending strength was tested using the three-point bending method, the number of bubbles per unit area was counted using an optical microscope, and the appearance quality was tested using GB11614. Testing showed that the visible light transmittance of the float glass obtained in this embodiment was 90.2%, L The value is 95.5, a Value -0.2, b Value 0.8, number of bubbles 5 / m², bending strength 64MPa, appearance quality shows no point defects, no lines, no cracks, optical distortion 54°.

[0028] Example 2 This embodiment provides a method for preparing float glass, including the following steps: 1. Weigh the following raw materials according to the following weight parts: 47.24 parts of quartz sand, 13.72 parts of soda ash, 3.7 parts of pretreated tantalum-niobium tailings, 14.01 parts of dolomite, 2.66 parts of limestone, 0.77 parts of mirabilite, 0.02 parts of carbon powder, 14.98 parts of crushed glass, 0.4 parts of zirconium acetate, and 0.14 parts of cerium oxide.

[0029] 2. Mixing: Zirconium acetate is added to water to prepare a 10% zirconium acetate solution. Except for zirconium acetate, the above raw materials are fed into a mixer and dry-mixed for 30 seconds at a stirring speed of 400 rpm. Then, while stirring, the atomized zirconium acetate solution is sprayed in and the mixing continues for 120 seconds.

[0030] 3. Melting: The mixture is put into a calcining furnace and pre-calcined at 550°C for 1 hour in a nitrogen atmosphere at a heating rate of 5°C / min. The mixture is then sent to a glass melting furnace, and the melting process is the same as in Example 1.

[0031] 4. Forming: The above molten glass is poured into a tin bath. The protective atmosphere of the tin bath is N2:H2=95:5, the bath pressure is maintained at 10Pa, the temperature of the glass liquid spreading on the surface of the tin liquid is controlled at 1060℃, the temperature of the tin bath outlet is 620℃, and the drawing speed is 320.51m / h to obtain a glass ribbon with a thickness of 6mm.

[0032] 5. Annealing: The glass strip is put into the annealing furnace for annealing. The annealing process is the same as in Example 1. After annealing, it is cut and packaged to obtain the finished float glass.

[0033] The prepared float glass was subjected to performance testing using the same methods as in Example 1. The visible light transmittance of the obtained float glass was 90.5%. The value is 95.7, a Value -0.1, b Value 0.7, number of bubbles 4 / m², flexural strength 62MPa. Appearance quality shows no point defects, no lines, no cracks, and optical distortion 52°.

[0034] Example 3 This embodiment provides a method for preparing float glass, including the following steps: 1. Weigh the following raw materials according to the following weight parts: 47.24 parts of quartz sand, 13.72 parts of soda ash, 5.5 parts of pretreated tantalum-niobium tailings, 14.01 parts of dolomite, 2.66 parts of limestone, 0.77 parts of mirabilite, 0.02 parts of carbon powder, 14.98 parts of crushed glass, 0.63 parts of zirconium acetate, and 0.14 parts of cerium oxide.

[0035] 2. Mixing: Zirconium acetate is added to water to prepare a 10% zirconium acetate solution. All raw materials except zirconium acetate are fed into a mixer. The mixture is first dry-mixed for 30 seconds at a stirring speed of 400 rpm. Then, while stirring, the atomized zirconium acetate solution is sprayed in and the mixture is continued for 120 seconds.

[0036] 3. Melting: The mixture is put into a calcining furnace and pre-calcined at 450°C for 2 hours in a nitrogen atmosphere at a heating rate of 3°C / min. The mixture is then sent into a glass melting furnace, and the melting process is the same as in Example 1.

[0037] 4. Forming: The above molten glass is poured into a tin bath. The protective atmosphere of the tin bath is N2:H2=95:5, the bath pressure is maintained at 10Pa, the temperature of the glass liquid spreading on the surface of the tin liquid is controlled at 1060℃, the temperature of the tin bath outlet is 620℃, and the drawing speed is 320.51m / h to obtain a glass ribbon with a thickness of 6mm.

[0038] 5. Annealing: The glass strip is put into the annealing furnace for annealing. The annealing process is the same as in Example 1. After annealing, it is cut and packaged to obtain the finished float glass.

[0039] The prepared float glass was subjected to performance testing using the same methods as in Example 1. The visible light transmittance of the obtained float glass was 90.1%. The value is 95.3, a Value -0.1, b Value 1.2, number of bubbles 6 / m², flexural strength 66MPa. Appearance quality shows no point defects, no lines, no cracks, and optical distortion 53°.

[0040] The following comparative examples 1-3 examine the effect of adding tantalum-niobium tailings on the properties of float glass: Comparative Example 1 The only difference between this comparative example and Example 1 is that pretreated tantalum-niobium tailings are not used; instead, the 4.61 parts of pretreated tantalum-niobium tailings in Example 1 are replaced with an equal amount of quartz sand.

[0041] The resulting glass has a visible light transmittance of 91.0%, L The value is 95.9, a Value -0.1, b Value 0.5, number of bubbles 5 / m², bending strength 51MPa. Appearance quality shows no point defects, no lines, no cracks, and optical distortion 53°.

[0042] Comparative Example 2 The only difference between this comparative example and Example 1 is that the amount of pretreated tantalum-niobium tailings is reduced from 4.61 parts to 2.0 parts, and the amount of quartz sand is increased by 2.61 parts accordingly.

[0043] The resulting glass has a visible light transmittance of 90.8%, L The value is 95.7, a Value -0.1, b Value 0.6, number of bubbles 5 / m², bending strength 57MPa. Appearance quality shows no point defects, no lines, no cracks, and optical distortion 52°.

[0044] Comparative Example 3 The only difference between this comparative example and Example 1 is that the amount of pretreated tantalum-niobium tailings increased from 4.61 parts to 8.0 parts, and the amount of quartz sand decreased by 3.39 parts.

[0045] The resulting glass had a visible light transmittance of 89.4%, L The value is 94.2, a Value -0.2, b Value 2.0, number of bubbles 6 / m², flexural strength 59MPa. Appearance quality shows no point defects, no lines, no cracks, and optical distortion 53°.

[0046] As can be seen from the above, in Comparative Example 1, the flexural strength was reduced because no pretreated tantalum-niobium tailings were used compared to Example 1. In Comparative Example 2, the amount of tailings used was relatively low, and the flexural strength was still reduced compared to Example 1. In Comparative Example 3, the amount of tailings added was relatively high, and the light transmittance decreased and the glass coloring was heavier compared to Example 1. This shows that the amount of tailings added has a significant impact on the performance of float glass.

[0047] The following comparative examples 4-7 examine the effect of zirconium acetate addition on the properties of float glass: Comparative Example 4 The only difference between this comparative example and Example 1 is that zirconium acetate is not used, and the 0.51 parts of zirconium acetate in Example 1 are replaced with an equal amount of quartz sand. The mixing method in step 2 is as follows: the raw materials are fed into a mixer and dry-mixed at 300 rpm for 45 seconds. Then, under stirring, 4.6 parts of atomized water are sprayed in and the mixing continues for 135 seconds.

[0048] The resulting glass has a visible light transmittance of 90.3%, L The value is 95.6, a Value -0.2, b Value 0.8, number of bubbles 4 / m², bending strength 47MPa, appearance quality shows no point defects, no lines, no cracks, optical distortion 53°.

[0049] Comparative Example 5 The only difference between this comparative example and Example 1 is that zirconium acetate is replaced with an equimolar amount of zirconium oxide (D). 50 The material was replaced with 0.5 μm (i.e., 0.19 parts). The mixing method in step 2 was as follows: the raw material was fed into a mixer and dry-mixed at 300 rpm for 45 seconds. Then, 4.6 parts of water were sprayed in while stirring and the mixture was continued for 135 seconds.

[0050] The resulting glass had a visible light transmittance of 89.3%, L The value is 94.8, a Value -0.1, b Value 0.9, number of bubbles 7 / m², bending strength 54MPa. Appearance quality shows one 0.64mm point defect and two 0.32mm point defects, no lines, no cracks, and optical distortion 52°.

[0051] Comparative Example 6 The only difference between this comparative example and Example 1 is that the amount of zirconium acetate is reduced from 0.51 parts to 0.1 parts, and the amount of quartz sand is increased by 0.41 parts accordingly.

[0052] The resulting glass has a visible light transmittance of 90.4%, L The value is 95.6, a Value -0.2, b Value 0.8, number of bubbles 5 / m², flexural strength 52MPa. Appearance quality shows no point defects, no lines, no cracks, and optical distortion 51°.

[0053] Comparative Example 7 The only difference between this comparative example and Example 1 is that the amount of zirconium acetate is increased from 0.51 parts to 1.0 parts, and the amount of quartz sand is reduced by 0.49 parts.

[0054] The resulting glass had a visible light transmittance of 87.6%, L The value is 94.3, a Value -0.3, b Value 1.1, number of bubbles 10 / m², bending strength 61MPa. Appearance quality shows 3 0.2mm point defects, no lines, no cracks, and optical distortion 54°.

[0055] As shown above, Comparative Example 4, without the addition of zirconium acetate, exhibited a significantly lower flexural strength compared to Example 1. Comparative Example 5, with the direct addition of zirconium oxide, showed an improvement in flexural strength compared to Comparative Example 4, but it remained lower than Example 1, with a significantly reduced light transmittance, an increased number of bubbles, and the presence of dot-like defects. This may be due to the difficulty of fully diffusing ordinary zirconium oxide in the glass melt, leading to a decrease in glass uniformity. Comparative Example 6, with a zirconium acetate addition of 0.1 parts, showed a significant decrease in the flexural strength of the prepared float glass compared to Example 1, indicating that insufficient zirconium acetate had an insignificant strengthening effect on the glass network structure. Comparative Example 7, compared to Example 1, showed a decrease in flexural strength and an increase in dot-like defects and bubbles. This indicates that excessive zirconium acetate can lead to appearance degradation, and the presence of excessive unintegrated zirconium oxide in the glass network may also affect the uniformity of the glass network, resulting in a decrease in flexural strength.

[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and not to limit them; although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications can still be made to the specific implementation of this application or equivalent substitutions can be made to some technical features, all of which should be covered within the scope of the technical solutions claimed in this application.

Claims

1. A method of making a float glass, characterized in that, Includes the following steps: S1. The tantalum-niobium tailings raw material is crushed, screened, magnetically separated to remove iron, homogenized and dehydrated to obtain pretreated tantalum-niobium tailings. S2. Take the following raw materials in the following weight proportions: 37-57 parts quartz sand, 12-15 parts soda ash, 3.7-5.5 parts pretreated tantalum-niobium tailings, 11.2-16.8 parts dolomite, 2.1-3.1 parts limestone, 0.6-0.9 parts mirabilite, 0.01-0.03 parts carbon powder, 11.9-17.9 parts crushed glass, 0.40-0.63 parts zirconium acetate, and 0.05-0.15 parts cerium oxide; S3. Add zirconium acetate to water to prepare a 5-15 wt% zirconium acetate solution. Mix the raw materials in the above formula except for zirconium acetate, and then add the zirconium acetate solution and continue mixing to obtain a mixture. S4. After pre-firing the mixture at 450-550℃, it is put into a glass melting furnace for melting to obtain molten glass. S5. The molten glass is poured into a tin bath for shaping to obtain a glass ribbon; S6. Anneal the glass strip according to the set annealing regime, cool it to room temperature, and then cut and package it to obtain the finished float glass.

2. The method of making float glass according to claim 1, wherein, In step S1, the crushing and screening process involves passing the crushed material through a 40-80 mesh sieve and collecting the undersize material. The magnetic separation for iron removal employs a wet high-intensity magnetic separator for two-stage magnetic separation with a magnetic field strength ≥1.5T, controlling the Fe2O3 content in the tantalum-niobium tailings to ≤0.2%. The homogenization process involves sending the magnetically separated tailings into a homogenization tank for mechanical stirring. The dewatering process involves dewatering the tailings by pressure filtration and then allowing them to naturally dewater in a closed tailings tank until the moisture content is ≤10%.

3. The method of making float glass according to claim 1, wherein, In step S1, the pretreated tantalum-niobium tailings mainly consist of 70-78% silicon dioxide, 10-18% aluminum oxide, 3-5% potassium oxide, 3-5% sodium oxide, 0.1-0.3% lithium oxide, and 0-0.2% iron oxide, with the remainder being unavoidable impurities.

4. The method of making float glass according to claim 1, wherein, In step S4, the pre-calcined mixture is fed into a glass melting furnace. The thermocouple temperatures of each small furnace zone in the glass melting furnace are set to 1410-1420℃, 1450-1460℃, 1480-1490℃, 1500-1510℃, 1510-1520℃, 1470-1480℃, 1430-1440℃, and 1390-1400℃ respectively along the length of the furnace.

5. The method of making float glass according to claim 1, wherein, In step S4, the pre-calcination treatment method is to put the mixture into a calcination furnace and pre-calcine it at 450-550°C for 1-2 hours in a nitrogen atmosphere at a heating rate of 3-5°C / min.

6. The method of making float glass according to claim 1, wherein, In S5, the protective atmosphere in the tin bath is N2:H2 = 95:5, and the pressure is a slight positive pressure of 10-20 Pa; the spreading temperature of the glass melt on the tin melt surface is 1060-1100℃, and the outlet temperature is controlled at 600-640℃; the drawing speed is 300-350 m / h.

7. The method of making float glass according to claim 1, wherein, In S6, the annealing process specifically involves sending the glass strip into an annealing furnace and annealing it sequentially through zones A1, B1, B2, C, E1, D1, D2, E2, F1, F2, and F3. The annealing rates are as follows: A1 zone: 22-28℃ / min; B1 and B2 zone: 6.17-18.33℃ / min; C zone: 22.93-45.83℃ / min; E1, D1, D2, and E2 zone: 7.51-54.99℃ / min; F1 zone: 27.51-54.99℃ / min; and F2 and F3 zone: 13.75-36.66℃ / min.

8. The method of making float glass according to claim 1, wherein, In step S3, the mixing method is as follows: except for zirconium acetate, the raw materials of the above formula are fed into a mixer, dry-mixed for 30-60 seconds, and then a zirconium acetate solution is sprayed in and the mixing continues for 120-150 seconds.