A method for producing thermally synergistic, durable, high-strength intermediate-heat silicate cement
By optimizing the mixing ratio of raw materials and using high-temperature rapid cooling and calcination technology, combined with the use of modified composite materials and granulated blast furnace slag and fly ash, the problems of insufficient early strength and poor durability of medium-heat silicate cement have been solved, and the performance of high strength, low heat of hydration and resistance to sulfate attack has been improved.
Patent Information
- Application Number
- CN202611420370.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing medium-heat silicate cements suffer from insufficient early strength and generally poor durability during the process of reducing heat of hydration. They also require high activity of admixtures, have poor stability, and are difficult to control in terms of process.
By optimizing the proportions and pretreatment processes of the mixed raw materials, using short-time high-temperature rapid cooling calcination technology to freeze the active mineral phase, introducing modified composite materials with nano-reinforcement and crystal nucleation effects, and combining the use of granulated blast furnace slag and fly ash, the heat of hydration is reduced and the resistance to sulfate attack is improved.
It significantly improves the early strength and durability of cement, reduces the heat of hydration, enhances resistance to sulfate attack, and meets the comprehensive performance requirements of medium-heat silicate cement.
Smart Images

Figure CN123106035A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cement production technology, specifically to a method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement. Background Technology
[0002] Thermal silicate cement is a type of cement specifically designed for large-volume concrete projects. Its main components include silicate cement clinker, appropriate amounts of gypsum, and finely ground granulated blast furnace slag or volcanic ash mixtures. It is a hydraulic cementitious material with moderate heat of hydration, slow heat release rate, good volume stability, strong resistance to sulfate attack, and high later-stage strength. It is widely used in hydropower dams, large foundations, nuclear power plants, and other projects. It can effectively reduce the excessive temperature difference between the inside and outside of concrete caused by the heat of cement hydration, thereby preventing concrete cracking caused by temperature stress.
[0003] However, in actual production, conventional intermediate-heat silicate cement often reduces the content of high-exothermic minerals to lower the heat of hydration, resulting in insufficient early strength and generally poor durability. Chinese patent application CN102276179A discloses a high-performance dam silicate cement, whose main raw materials are homogenized ground general-purpose silicate cement clinker and admixtures. The admixtures account for 30-75% of the total cement weight and include fly ash and granulated blast furnace slag. Increasing the admixture content reduces the proportion of clinker in the cement, lowering the heat of hydration and enabling effective recycling of industrial waste. However, high admixture content leads to lower early strength and generally poor durability, which is not conducive to long-term use. It also requires high activity of the admixtures and exhibits poor stability. Chinese patent application CN104761166A discloses a medium-heat composite cement and its preparation method, comprising silicate cement clinker, aluminate cement clinker, nano-tin oxide, glass fiber, silica fume, struvite, and gypsum, prepared through material preparation, grinding, premixing, and pulverizing. This medium-heat composite cement utilizes aluminate cement to improve early strength and uses nanomaterials and fibers to enhance toughness, with multi-component composites improving the overall performance of the cement. However, aluminate cement has a high heat of hydration, nano-tin oxide is prone to agglomeration, the cement has poor stability and durability, and the process control is extremely difficult.
[0004] Therefore, there is an urgent need to develop a high-strength, durable, and low-heat-of-hydration intermediate-heat silicate cement to improve its overall performance. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement. This method enhances the reactivity of raw materials by optimizing the proportions and pretreatment processes of the mixed raw materials; employs short-time high-temperature rapid cooling calcination technology to freeze the high-temperature active mineral phases, preventing the formation of low-activity minerals, thereby improving the chemical potential and cementitious properties of the clinker; and compensates for early strength loss caused by the addition of blended materials by introducing modified composite materials and utilizing their nano-reinforcing and nucleation effects. Simultaneously, the synergistic effect of the multi-component blends significantly reduces the heat of hydration of the cement and improves its resistance to sulfate attack.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for producing thermally synergistic durable high-strength medium-heat silicate cement, the cement comprising: 100 parts of clinker, 5-6 parts of retarder, and 18-25 parts of admixtures; The mixture consists of 100 parts granulated blast furnace slag, 30-50 parts fly ash, and 5-10 parts modified composite material; The modified composite material is prepared by modifying HA@SiO2 composite material; The clinker is obtained by calcining mixed raw materials; The mixed raw material consists of 100 parts limestone, 10-12 parts rock sand, 11-16 parts clay, and 2.5-4 parts refined iron ore; The retarder includes one or more of dihydrate gypsum, anhydrite, and desulfurized gypsum.
[0007] Furthermore, the production method includes: S1: After pretreatment of limestone, rock sand, clay, and refined iron ore, they are mixed evenly in proportion to obtain mixed raw materials; at the same time, modified composite materials are prepared. S2: Preheat the mixed raw materials, send them into a rotary kiln for calcination for 15-25 minutes, and cool them rapidly after calcination to obtain clinker; S3: Mix clinker, retarder and admixtures evenly according to the proportion to obtain thermally synergistic, durable, high-strength, medium-heat silicate cement; S4: The uniformly mixed cement product is transported to the homogenization silo for aeration and chemical stabilization.
[0008] Furthermore, in step S1: The limestone is selected as high-calcium and low-magnesium type, with a calcium oxide content of not less than 52% and a magnesium oxide content of not more than 2.0%. It is ground by a roller mill to a particle size of not more than 2 mm and then dried. The rock sand is selected from high silica quartz sand, with a silica content of not less than 92%, and is crushed to a particle size of not more than 100 micrometers by a high-pressure roller mill; The clay used is kaolin with an aluminum oxide content of not less than 35%, which is calcined at 550℃ to transform it into metakaolin. The refined iron ore is magnetite with a ferric oxide content of not less than 5%, and is ground to a specific surface area of not less than 400 square meters per kilogram.
[0009] Furthermore, the preparation steps of the modified composite material in step S1 are as follows: Short rod-shaped nano-hydroxyapatite was calcined in a muffle furnace at 550-650℃ for 2-4 hours and then ultrasonically dispersed in anhydrous ethanol to obtain an activated hydroxyapatite dispersion with a concentration of 24 mg / mL. The activated hydroxyapatite dispersion, ethanol solution, ammonia, and hexadecyltrimethylammonium bromide were mixed evenly according to the mass ratio, and then tetraethyl orthosilicate was added. The mixture was reacted at 25-35℃ for 12-24 hours. After centrifugation, washing, and drying at 80℃ for 12 hours, HA@SiO2 composite material was obtained. The ethanol solution was composed of anhydrous ethanol and deionized water in a volume ratio of 1:1. N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material are mixed in a certain mass ratio and reacted at 30-40℃ for 8-10 hours. After washing and drying, the modified composite material is obtained.
[0010] Furthermore, in step S1, the mass ratio of activated hydroxyapatite dispersion, ethanol solution, ammonia, hexadecyltrimethylammonium bromide, and tetraethyl orthosilicate is 100:180-240:14-18:1.2-1.8:5-8.
[0011] Furthermore, in step S1, the mass ratio of N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material is 950-1200:18-24:10-12:100.
[0012] Furthermore, in step S2, the mixed raw materials are preheated to 800-850°C and then fed into a rotary kiln. They are calcined at a speed of 3-4 revolutions per minute and a temperature of 1450-1480°C for 15-25 minutes. These calcination parameters can suppress the excessive growth of alite crystals, resulting in a fine and uniform crystal structure, which is beneficial to the early strength of cement. After calcination, the mixture is immediately and rapidly cooled to freeze the high-temperature active mineral phase, preventing the decomposition of C3S and the transformation of β-C2S into the less active γ-C2S. At the same time, the glass content is increased, further enhancing the chemical potential and cementitious properties of the clinker, ultimately yielding a highly active clinker.
[0013] Furthermore, the specific steps of step S3 are as follows: Add the clinker and retarder into a twin-shaft zero-gravity mixer according to the ratio, and mix for 3-5 minutes to ensure that the retarder is evenly dispersed. Add the admixture to the above mixture and continue mixing for 5-7 minutes to obtain a uniformly mixed cement product; The granulated blast furnace slag has a specific surface area of not less than 450 square meters per kilogram, a fly ash water requirement ratio of not more than 95%, and a 45-micron sieve residue of not more than 12%. As a type of solid waste, slag contains abundant silicon and aluminum elements. The calcium and aluminum minerals and expanded silicate substances contained in slag can promote the reaction of cement in the matrix, generate hardening products, and increase the strength, durability and impermeability of the matrix.
[0014] Furthermore, in step S4, the finished cement product is transported to the homogenization silo, the aeration system is turned on, the relative humidity inside the silo is controlled to not exceed 60%, and aeration homogenization and chemical stabilization are carried out for no less than 24 hours.
[0015] Compared with existing technologies, this method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement has the following advantages: This invention, through the synergistic effect of highly active clinker and modified composite materials, not only lays a solid foundation for the high strength of cement, but also accelerates the hydration reaction through nano-reinforcement and crystal nucleation effects, effectively compensating for the early strength loss that may be caused by the addition of admixtures. Furthermore, the introduction of granulated blast furnace slag and fly ash, combined with a short-time high-temperature rapid cooling calcination process, significantly reduces the heat of hydration of cement while maintaining performance stability, meeting the stringent requirements of medium-heat silicate cement. In addition, the design of the modified composite materials, with the insoluble composite film formed by the carboxyl groups on the surface, effectively blocks the penetration of corrosive ions, greatly improving the cement's resistance to sulfate attack and reducing durability degradation caused by long-term service.
[0016] Other advantages, objectives and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination or study, or may be learned from the practice of the invention. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.
[0018] Figure 1 This is a flowchart of a production method for thermally synergistic, durable, high-strength, medium-heat silicate cement. Detailed Implementation
[0019] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.
[0020] Example 1
[0021] A method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement includes the following steps: Limestone, rock sand, clay, and refined iron ore are processed separately. The limestone is selected as high-calcium, low-magnesium type, with a calcium oxide content of not less than 52% and a magnesium oxide content of not more than 2.0%. It is ground in a roller mill to a particle size of not more than 2 mm and then dried. The rock sand is selected as high-silica quartz sand, with a silica content of not less than 92%, and is crushed in a high-pressure roller mill to a particle size of not more than 100 micrometers. The clay is selected as kaolin, with an aluminum oxide content of not less than 35%, and is calcined at 550℃ to transform it into metakaolin. The refined iron ore is selected as magnetite with an ferric oxide content of not less than 5%, and is ground to a specific surface area of not less than 400 square meters per kilogram. The limestone, rock sand, clay, and refined iron ore are mixed evenly in a mass ratio of 100:10:11:2.5 to obtain a mixed raw material. The preparation method of the modified composite material includes the following steps: Nano-hydroxyapatite was pretreated by calcination in a muffle furnace at a temperature of 550℃ for 4 hours. After treatment, it was ultrasonically dispersed in anhydrous ethanol to obtain an activated hydroxyapatite dispersion with a concentration of 24 mg / mL. The activated hydroxyapatite dispersion, ethanol solution, ammonia, and hexadecyltrimethylammonium bromide were mixed evenly, and then tetraethyl orthosilicate was added. The mass ratio of the activated hydroxyapatite dispersion, ethanol solution, ammonia, hexadecyltrimethylammonium bromide, and tetraethyl orthosilicate was 100:180:14:1.2:5. The mixture was stirred and mixed to allow the reaction to proceed. The reaction temperature was 25℃ and the reaction time was 24h. After the reaction was completed, the mixture was centrifuged at a speed of 8000r / min for 8min. The mixture was then washed with anhydrous ethanol and deionized water and dried at 80℃ for 12h to obtain the HA@SiO2 composite material. N,N-Dimethylformamide, γ-aminopropyltriethoxysilane, and pyromellitic anhydride were mixed evenly, and then HA@SiO2 composite material was added. The mass ratio of N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material was 950:18:10:100. The mixture was stirred and mixed to allow the reaction to proceed. The reaction temperature was 30℃ and the reaction time was 10 hours. After the reaction was completed, the mixture was washed with anhydrous ethanol and deionized water and dried to obtain the modified composite material.
[0022] The mixed raw materials are preheated to 800℃, and then calcined in a rotary kiln at 1450℃ for 25 minutes at a rotation speed of 4 r / min. After calcination, the materials are rapidly cooled to obtain clinker. Clinker, dihydrate gypsum, and admixtures in a mass ratio of 100:5:18 are mixed evenly. The admixtures consist of granulated blast furnace slag, fly ash, and modified composite materials in a mass ratio of 100:30:5, resulting in thermally synergistic, durable, high-strength, medium-heat silicate cement.
[0023] Example 2
[0024] Limestone, rock sand, clay, and refined iron ore are processed separately. The limestone is selected as high-calcium, low-magnesium type, with a calcium oxide content of not less than 52% and a magnesium oxide content of not more than 2.0%. It is ground in a roller mill to a particle size of not more than 2 mm and then dried. The rock sand is selected as high-silica quartz sand, with a silica content of not less than 92%, and is crushed in a high-pressure roller mill to a particle size of not more than 100 micrometers. The clay is selected as kaolin, with an aluminum oxide content of not less than 35%, and is calcined at 550℃ to transform it into metakaolin. The refined iron ore is selected as magnetite with an ferric oxide content of not less than 5%, and is ground to a specific surface area of not less than 400 square meters per kilogram. The limestone, rock sand, clay, and refined iron ore are mixed evenly in a mass ratio of 100:11:14:3.5 to obtain a mixed raw material. The preparation method of the modified composite material includes the following steps: Nano-hydroxyapatite was pretreated by calcination in a muffle furnace at a temperature of 600℃ for 3 hours. After treatment, it was ultrasonically dispersed in anhydrous ethanol to obtain an activated hydroxyapatite dispersion with a concentration of 24 mg / mL. The activated hydroxyapatite dispersion, ethanol solution, ammonia, and hexadecyltrimethylammonium bromide were mixed evenly, and then tetraethyl orthosilicate was added. The mass ratio of the activated hydroxyapatite dispersion, ethanol solution, ammonia, hexadecyltrimethylammonium bromide, and tetraethyl orthosilicate was 100:210:16:1.5:6. The mixture was stirred and mixed to allow the reaction to proceed. The reaction temperature was 30℃ and the reaction time was 18h. After the reaction was completed, the mixture was centrifuged at a speed of 8000r / min for 8min. The mixture was then washed with anhydrous ethanol and deionized water and dried at 80℃ for 12h to obtain the HA@SiO2 composite material. N,N-Dimethylformamide, γ-aminopropyltriethoxysilane, and pyromellitic anhydride were mixed evenly, and then HA@SiO2 composite material was added. The mass ratio of N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material was 1100:21:11:100. The mixture was stirred and mixed to allow the reaction to proceed. The reaction temperature was 35℃ and the reaction time was 9 hours. After the reaction was completed, the mixture was washed with anhydrous ethanol and deionized water and dried to obtain the modified composite material.
[0025] The mixed raw materials are preheated to 820℃, and then calcined in a rotary kiln at 1460℃ for 20 minutes at a rotation speed of 3.5 r / min. After calcination, the materials are rapidly cooled to obtain clinker. Clinker, dihydrate gypsum, and admixtures in a mass ratio of 100:5.5:20 are mixed evenly. The admixtures consist of granulated blast furnace slag, fly ash, and modified composite materials in a mass ratio of 100:38:7, resulting in thermally synergistic, durable, high-strength, medium-heat silicate cement.
[0026] Example 3
[0027] A method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement includes the following steps: Limestone, rock sand, clay, and refined iron ore are processed separately. The limestone is selected as high-calcium, low-magnesium type, with a calcium oxide content of not less than 52% and a magnesium oxide content of not more than 2.0%. It is ground in a roller mill to a particle size of not more than 2 mm and then dried. The rock sand is selected as high-silica quartz sand, with a silica content of not less than 92%, and is crushed in a high-pressure roller mill to a particle size of not more than 100 micrometers. The clay is selected as kaolin, with an aluminum oxide content of not less than 35%, and is calcined at 550℃ to transform it into metakaolin. The refined iron ore is selected as magnetite with an ferric oxide content of not less than 5%, and is ground to a specific surface area of not less than 400 square meters per kilogram. The limestone, rock sand, clay, and refined iron ore are mixed evenly in a mass ratio of 100:11:14:3.5 to obtain a mixed raw material. The preparation method of the modified composite material includes the following steps: Nano-hydroxyapatite was pretreated by calcination in a muffle furnace at a temperature of 600℃ for 3 hours. After treatment, it was ultrasonically dispersed in anhydrous ethanol to obtain an activated hydroxyapatite dispersion with a concentration of 24 mg / mL. The activated hydroxyapatite dispersion, ethanol solution, ammonia, and hexadecyltrimethylammonium bromide were mixed evenly, and then tetraethyl orthosilicate was added. The mass ratio of the activated hydroxyapatite dispersion, ethanol solution, ammonia, hexadecyltrimethylammonium bromide, and tetraethyl orthosilicate was 100:210:16:1.5:6. The mixture was stirred and mixed to allow the reaction to proceed. The reaction temperature was 30℃ and the reaction time was 18h. After the reaction was completed, the mixture was centrifuged at a speed of 8000r / min for 8min. The mixture was then washed with anhydrous ethanol and deionized water and dried at 80℃ for 12h to obtain the HA@SiO2 composite material. N,N-Dimethylformamide, γ-aminopropyltriethoxysilane, and pyromellitic anhydride were mixed evenly, and then HA@SiO2 composite material was added. The mass ratio of N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material was 1100:21:11:100. The mixture was stirred and stirred to allow the reaction to proceed. The reaction temperature was 35℃, and the reaction time was 9 hours. After the reaction was completed, the mixture was washed with anhydrous ethanol and deionized water, and then dried to obtain the modified composite material. The mixed raw materials are preheated to 820℃, and then calcined in a rotary kiln at 1460℃ for 20 minutes at a rotation speed of 3.5 r / min. After calcination, the materials are rapidly cooled to obtain clinker. Clinker, dihydrate gypsum, and admixtures in a mass ratio of 100:5.5:24 are mixed evenly. The admixtures consist of granulated blast furnace slag, fly ash, and modified composite materials in a mass ratio of 100:38:9, resulting in thermally synergistic, durable, high-strength, medium-heat silicate cement.
[0028] Example 4
[0029] A method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement includes the following steps: Limestone, rock sand, clay, and refined iron ore are processed separately. The limestone is selected as high-calcium, low-magnesium type, with a calcium oxide content of not less than 52% and a magnesium oxide content of not more than 2.0%. It is ground in a roller mill to a particle size of not more than 2 mm and then dried. The rock sand is selected as high-silica quartz sand, with a silica content of not less than 92%, and is crushed in a high-pressure roller mill to a particle size of not more than 100 micrometers. The clay is selected as kaolin, with an aluminum oxide content of not less than 35%, and is calcined at 550℃ to transform it into metakaolin. The refined iron ore is selected as magnetite with an ferric oxide content of not less than 5%, and is ground to a specific surface area of not less than 400 square meters per kilogram. The limestone, rock sand, clay, and refined iron ore are mixed evenly in a mass ratio of 100:12:16:4 to obtain a mixed raw material. The preparation method of the modified composite material includes the following steps: Nano-hydroxyapatite was pretreated by calcination in a muffle furnace at a temperature of 650°C for 2 hours. After treatment, it was ultrasonically dispersed in anhydrous ethanol to obtain an activated hydroxyapatite dispersion with a concentration of 24 mg / mL. The activated hydroxyapatite dispersion, ethanol solution, ammonia, and hexadecyltrimethylammonium bromide were mixed evenly, and then tetraethyl orthosilicate was added. The mass ratio of the activated hydroxyapatite dispersion, ethanol solution, ammonia, hexadecyltrimethylammonium bromide, and tetraethyl orthosilicate was 100:240:18:1.8:8. The mixture was stirred and mixed to allow the reaction to proceed. The reaction temperature was 35℃ and the reaction time was 12h. After the reaction was completed, the mixture was centrifuged at a speed of 8000r / min for 8min. The mixture was then washed with anhydrous ethanol and deionized water and dried at 80℃ for 12h to obtain the HA@SiO2 composite material. N,N-Dimethylformamide, γ-aminopropyltriethoxysilane, and pyromellitic anhydride were mixed evenly, and then HA@SiO2 composite material was added. The mass ratio of N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material was 1200:24:12:100. The mixture was stirred and mixed to allow the reaction to proceed. The reaction temperature was 40℃ and the reaction time was 8 hours. After the reaction was completed, the mixture was washed with anhydrous ethanol and deionized water and dried to obtain the modified composite material.
[0030] The mixed raw materials are preheated to 850℃, and then calcined in a rotary kiln at 1480℃ for 15 minutes at a rotation speed of 4 r / min. After calcination, the mixture is rapidly cooled to obtain clinker. Clinker, dihydrate gypsum, and admixtures in a mass ratio of 100:6:25 are mixed evenly. The admixtures consist of granulated blast furnace slag, fly ash, and modified composite materials in a mass ratio of 100:50:10, resulting in thermally synergistic, durable, high-strength, medium-heat silicate cement.
[0031] Comparative Example 1 A method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement, compared with Example 3, involves replacing the modified composite material in Example 3 with an equal amount of nano-hydroxyapatite and nano-silica in a mass ratio of 1.8:1. The other components and preparation methods are completely consistent with Example 3.
[0032] Comparative Example 2 A method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement includes the following steps: Clinker, gypsum dihydrate, and modified composite material in a mass ratio of 100:5.5:24 were mixed evenly to obtain thermally synergistic, durable, high-strength, medium-heat silicate cement.
[0033] The clinker preparation method in this comparative example is completely consistent with the clinker preparation method in Example 3.
[0034] The preparation method of the modified composite material in this comparative example is completely consistent with the preparation method of the modified composite material in Example 2.
[0035] Comparative Example 3 A method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement, compared with Example 3, does not involve processing the raw materials of the mixed raw materials, but directly mixing them, while the other components and preparation methods are completely consistent with Example 3.
[0036] The silicate cements prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were ground to a specific surface area of approximately 300 m². 2 / kg, relevant tests were conducted, and the tests are as follows: Strength Test: Cement mortar specimens measuring 40mm × 40mm × 160mm were prepared according to standard specifications (cement: standard sand: water = 1:3:0.5). After curing under standard conditions for 7 days and 28 days respectively, their flexural and compressive strengths were determined using a universal testing machine. The compressive and flexural strengths at 7 days and 28 days were recorded. The test results are shown in the table below:
[0037] The test results in the table above show that the silicate cements corresponding to Examples 1 to 4 have excellent compressive and flexural strengths, with a 28-day compressive strength ≥ 52.5 MPa, meeting the high-strength cement standard and significantly higher than the comparative examples. In Comparative Example 1, the direct addition of nano-hydroxyapatite and nano-silica resulted in poorer mechanical properties. Comparative Example 2, which did not add granulated blast furnace slag and fly ash, had the worst mechanical properties, with 28-day compressive and 28-day flexural strengths of 42.1 MPa and 6.2 MPa, respectively. This indicates that the synergistic effect of the modified composite material with granulated blast furnace slag and fly ash can improve cement strength. In Comparative Example 3, the raw materials were not pretreated, resulting in a decrease in overall performance.
[0038] Hydration heat performance test: According to relevant test standards, the hydration heat of Examples 1 to 4 was recorded at 3 days and 7 days. Durability Test: Cement mortar specimens (40mm×40mm×160mm) were prepared according to standard specifications (cement:standard sand:water = 1:3:0.5). One set was immersed in clean water as a baseline. After 28 days, the initial compressive strength was measured as F0. The prepared cement mortar specimens were then immersed in a 5% Na2SO4 solution for an extended period, with the solution changed every 7 days. After 28 days, the compressive strength was measured as F0. n Strength loss rate (%) = (F0 - F nThe smaller the strength loss rate (F0×100%), the stronger the resistance to sulfate attack. The test results are shown in the table below.
[0039] The test results in the table above show that the silicate cement corresponding to Examples 1 to 4 has a 3-day heat of hydration of ≤251kJ / kg and a 7-day heat of hydration of ≤293kJ / kg, which meets the standard for medium-heat silicate cement. Furthermore, the 28-day strength loss rate is relatively small, indicating good durability. In contrast, the 28-day strength loss rate in Comparative Examples 1 to 3 is significantly increased, reaching 6.7%.
[0040] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement, characterized in that, The cement comprises: 100 parts clinker, 5-6 parts retarder, and 18-25 parts admixtures; The mixture consists of 100 parts granulated blast furnace slag, 30-50 parts fly ash, and 5-10 parts modified composite material; The modified composite material is prepared by modifying HA@SiO2 composite material; The clinker is obtained by calcining mixed raw materials; The mixed raw material consists of 100 parts limestone, 10-12 parts rock sand, 11-16 parts clay, and 2.5-4 parts refined iron ore; The retarder includes one or more of dihydrate gypsum, anhydrite, and desulfurized gypsum.
2. The production method of thermally synergistic durable high-strength medium-heat silicate cement according to claim 1, characterized in that, The method includes: S1: After pretreatment of limestone, rock sand, clay, and refined iron ore, they are mixed evenly in proportion to obtain mixed raw materials; at the same time, modified composite materials are prepared. S2: Preheat the mixed raw materials, send them into a rotary kiln for calcination for 15-25 minutes, and cool them rapidly after calcination to obtain clinker; S3: Mix clinker, retarder and admixtures evenly according to the proportion to obtain thermally synergistic, durable, high-strength, medium-heat silicate cement; S4: The uniformly mixed cement product is transported to the homogenization silo for aeration and chemical stabilization.
3. The production method of thermally synergistic durable high-strength medium-heat silicate cement according to claim 2, characterized in that, In step S1: The limestone is selected as high-calcium and low-magnesium type, with a calcium oxide content of not less than 52% and a magnesium oxide content of not more than 2.0%. It is ground by a roller mill to a particle size of not more than 2 mm and then dried. The rock sand is selected from high silica quartz sand, with a silica content of not less than 92%, and is crushed to a particle size of not more than 100 micrometers by a high-pressure roller mill; The clay used is kaolin with an aluminum oxide content of not less than 35%, which is calcined at 550℃ to transform it into metakaolin. The refined iron ore is magnetite with a ferric oxide content of not less than 5%, and is ground to a specific surface area of not less than 400 square meters per kilogram.
4. The method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement according to claim 2, characterized in that, The preparation steps of the modified composite material in step S1 are as follows: Short rod-shaped nano-hydroxyapatite was calcined in a muffle furnace at 550-650℃ for 2-4 hours and then ultrasonically dispersed in anhydrous ethanol to obtain an activated hydroxyapatite dispersion with a concentration of 24 mg / mL. The activated hydroxyapatite dispersion, ethanol solution, ammonia, and hexadecyltrimethylammonium bromide were mixed evenly according to the mass ratio, and then tetraethyl orthosilicate was added. The mixture was reacted at 25-35℃ for 12-24 hours, centrifuged, washed, and dried at 80℃ for 12 hours to obtain HA@SiO2 composite material. N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material are mixed in a certain mass ratio and reacted at 30-40℃ for 8-10 hours. After washing and drying, the modified composite material is obtained.
5. The method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement according to claim 4, characterized in that, In step S1, the mass ratio of activated hydroxyapatite dispersion, ethanol solution, ammonia, hexadecyltrimethylammonium bromide, and tetraethyl orthosilicate is 100:180-240:14-18:1.2-1.8:5-8.
6. The method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement according to claim 4, characterized in that, In step S1, the mass ratio of N,N-dimethylformamide, γ-aminopropyltriethoxysilane, pyromellitic anhydride, and HA@SiO2 composite material is 950-1200:18-24:10-12:
100.
7. The method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement according to claim 2, characterized in that, In step S2, the mixed raw materials are preheated to 800-850°C and then fed into a rotary kiln. They are calcined at a speed of 3-4 revolutions per minute and a temperature of 1450-1480°C for 15-25 minutes. After calcination, they are immediately and rapidly cooled.
8. The method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement according to claim 2, characterized in that, The specific steps of step S3 are as follows: Add the clinker and retarder into a twin-shaft zero-gravity mixer according to the ratio, and mix for 3-5 minutes to ensure that the retarder is evenly dispersed. Add the admixture to the mixture and continue mixing for 5-7 minutes to obtain a uniformly mixed cement product.
9. The method for producing thermally synergistic, durable, high-strength, medium-heat silicate cement according to claim 1, characterized in that, In step S4, the finished cement product is transported to the homogenization silo, the aeration system is turned on, the relative humidity inside the silo is controlled to not exceed 60%, and aeration homogenization and chemical stabilization are carried out for no less than 24 hours.
Citation Information
Patent Citations
A phenol-modified aliphatic water-reducing agent and its preparation method
CN102276179A
Intermediate-hydration-heat composite cement and preparation method thereof
CN104761166A