Integrated two-step steam-based system and method for preparing building gypsum powder with simultaneous dechlorination

By integrating a two-step steam dechlorination system, and utilizing technologies such as zoned spraying, negative pressure dehydration, and low-temperature steam calcination, the problem of high chloride ion content in desulfurized gypsum from coal-fired power plants has been solved, achieving efficient and low-energy-consumption preparation of building gypsum powder and ensuring product quality and economy.

CN123106040APending Publication Date: 2026-11-17SUZHOU XIRE ENERGY SAVING ENVIRONMENTAL PROTECTION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611362135.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing two-step steam heating process for preparing building gypsum powder, the high chloride ion content in the desulfurized gypsum from coal-fired power plants leads to quality problems such as corrosion of steel bars and yellow spots on the gypsum products. Furthermore, the modification of conventional dehydration equipment increases energy consumption and reduces economic efficiency.

Method used

An integrated synchronous dechlorination steam two-step system is adopted, including a pre-dechlorination pretreatment unit, a deep dehydration and dechlorination unit, a calcination-co-dechlorination unit, and a dechlorination co-control unit. Through zoned spraying, negative pressure dehydration, low-temperature steam calcination, and synergistic catalysis of trace dechlorination additives, high-efficiency removal of chloride ions is achieved.

Benefits of technology

Without increasing steam energy consumption, the chloride ion content in building gypsum powder is effectively reduced to ≤400ppm, ensuring that the gypsum strength and setting time meet the standards and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106040A_ABST
    Figure CN123106040A_ABST
Patent Text Reader

Abstract

This invention discloses a two-step steam-based system and method for preparing building gypsum powder with integrated synchronous dechlorination. The system comprises a pre-dechlorination pretreatment unit, a deep dehydration and dechlorination unit, a calcination-co-dechlorination unit, and a dechlorination co-control unit arranged in series. The pre-dechlorination pretreatment unit is connected to the discharge end of an existing gypsum hydrocyclone in a power plant. The deep dehydration and dechlorination unit is a partitioned, modified disc dehydrator. The calcination-co-dechlorination unit includes a primary steam rotary low-temperature dryer, a secondary steam paddle dryer, a steam tubular fluidized bed calciner, an online additive dosing device, a stratified gas phase collection hood, and a waste gas scrubbing and adsorption device. The dechlorination co-control unit includes three online chloride ion rapid detectors, a DCS control system, an electrically controlled steam flow regulating valve, a calcination temperature sensor, and an additive dosing actuator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of industrial solid waste resource utilization, building gypsum preparation and environmental dechlorination equipment technology, specifically to a two-step steam method for preparing building gypsum powder with integrated simultaneous dechlorination. Background Technology

[0002] The current method for preparing building gypsum powder from desulfurized gypsum generally employs a two-step steam-heated drying and calcination process. However, desulfurized gypsum from coal-fired power plants typically has a high chloride ion content (1000~2200ppm), and conventional gypsum drying and calcination processes do not reduce the chloride ion content. This results in a series of quality problems in the produced building gypsum powder. - It is difficult to consistently reduce the gypsum content to the building material standard (≤400ppm), resulting in gypsum products corroding steel bars, yellow spots on the slab surface, and rust on the keel.

[0003] Typically, coal-fired power plants dilute chloride ions by increasing the flushing water volume of the disc dewatering machine at the front end. This leads to a problem of high moisture content in gypsum. Higher moisture content increases energy consumption in gypsum preparation, reduces economic efficiency, and increases production costs for enterprises.

[0004] In some factories and power plants, the chloride ion content of the original desulfurization gypsum is generally 1000~2200ppm. Relying solely on the original disc dewatering machine for a single surface rinse can only remove a portion of the free chlorine on the surface, while the bound chlorine cannot be removed at all. The chloride ion content of the finished product often exceeds the standard, resulting in yellow spots on the surface of gypsum board and corrosion of the internal steel bars when it is used for gypsum board and self-leveling. Downstream customers refuse to accept it.

[0005] The current market practice of retrofitting disc dewatering machines by simply increasing the number of nozzles or adjusting their size, merely increasing the amount of rinsing water, is insufficient. It only washes the machine without removing the excess water, thus increasing the drying load and causing a surge in subsequent steam consumption. It can also easily lead to material blockage and sticking to the walls of the drying equipment.

[0006] In summary, existing gypsum preparation technologies lack dechlorination capabilities, while the existing power plant equipment for dechlorination has significant side effects. Summary of the Invention

[0007] This invention provides a two-step steam-based system and method for preparing building gypsum powder with integrated simultaneous dechlorination, in order to solve the technical problems existing in the prior art.

[0008] To achieve the above objectives, the present invention provides a steam two-step system for preparing building gypsum powder with integrated synchronous dechlorination, which includes a pre-dechlorination pretreatment unit, a deep dehydration and dechlorination unit, a calcination-co-dechlorination unit, and a dechlorination co-control unit arranged in series. The pre-dechlorination pretreatment unit is connected to the discharge end of the power plant's existing gypsum hydrocyclone and includes a sealed spray chamber, a multi-stage condensate spray device, an online turbidity monitor, a solid-liquid separation sieve plate, and a filtrate collection tank. The multi-stage condensate spray device uses power plant condensate atomized spray to wash away free chloride ions from gypsum particles, and the waste liquid collected in the filtrate collection tank is returned to the desulfurization wastewater system. The deep dehydration and dechlorination unit is a partitioned disc dehydrator. The disc surface of the partitioned disc dehydrator is divided into two independent front washing zone and rear dehydration zone along the material travel direction. The front washing zone and the rear dehydration zone are equipped with independent spray pipes and independent negative pressure vacuum pumps. The front washing zone is equipped with a low-pressure condensate spray pipe to maintain only the basic negative pressure to achieve secondary dechlorination of surface chloride ions. The rear dehydration zone has no spray pipes, but is equipped with an adjustable vacuum pump to forcibly remove the free water inside the gypsum after washing. The calcination-co-dechlorination unit includes a primary steam rotary low-temperature dryer, a secondary steam paddle dryer, a steam tubular fluidized bed calciner, an online addition device for trace additives, a stratified gas phase collection hood, and a waste gas scrubbing and adsorption device. The online addition device for trace additives is located on the feed screw of the steam tubular fluidized bed calciner and is used to add dechlorination additives. The stratified gas phase collection hood collects chlorine-containing waste gas in sections and transports it to the waste gas scrubbing and adsorption device. The low-temperature waste heat pipeline discharged from the steam tubular fluidized bed calciner is connected to the sealed spray chamber of the pre-dechlorination pretreatment unit for preheating the spray soft water. The dechlorination co-control unit includes three online rapid chloride ion detectors, a DCS control system, an electrically controlled steam flow regulating valve, a calcination temperature sensor, and an additive dosing actuator. The three online rapid chloride ion detectors are respectively located before the pre-dechlorination chamber discharge, after the disc dehydrator, and at the calcined finished product discharge end. Based on the real-time chloride ion detection data from the three locations, the DCS control system coordinates and regulates the pre-dechlorination spray flow, the zoned negative pressure of the disc dehydrator, the dosage of calcination additives, and the steam heating temperature to achieve adaptive closed-loop control of raw material chloride ion fluctuations.

[0009] In one embodiment of the present invention, preferably, the control logic of the DCS control system in the dechlorination co-control unit is as follows: (1) When the detected chloride ion value satisfies 400ppm < Cl - When the concentration is <1200ppm, increase the pre-dechlorination spray flow rate and adjust the negative pressure at the rear of the disc dewatering machine to complete the dechlorination. If the chloride ion concentration at the rear of the disc dewatering machine is still too high, start the online addition device for trace additives to add dechlorination additives, and complete the final index verification through the detector at the end of the steam tube fluidized bed calcining furnace. (2) When the detected chloride ion value satisfies 1200ppm < Cl -When the concentration is <1800ppm, the pre-dechlorination spray water volume is increased simultaneously and the dechlorination aid is added. Relying on the synergistic effect of water washing dechlorination and calcination gas phase dechlorination, the final index verification is completed by the detector at the end of the steam tube fluidized bed calciner.

[0010] In one embodiment of the present invention, preferably, the dechlorination aid is a low-alumina fly ash composite dechlorination aid.

[0011] In one embodiment of the present invention, preferably, the steam tube fluidized bed calcining furnace is used for low-temperature indirect heating at a temperature of 170~190°C.

[0012] In one embodiment of the present invention, preferably, the dechlorination aid reacts directionally with the bound chloride ions in the gypsum lattice, significantly reducing the activation energy for hydrogen chloride precipitation, and achieving the precipitation of bound chlorine gas phase at a low temperature of 170~190℃.

[0013] In one embodiment of the present invention, preferably, the sealed spray chamber of the pre-dechlorination pretreatment unit is equipped with a soft water preheating heat exchange pipeline, which is connected to the low-temperature flue gas waste heat outlet of the primary steam rotary low-temperature dryer and the steam tubular fluidized bed calciner respectively; the DCS control system adjusts the flow rate of low-temperature flue gas in conjunction with the inlet water temperature of the sealed spray chamber and the chloride ion concentration of the raw material: when the chloride ion content of the incoming material increases and the spray washing intensity needs to be increased, the low-temperature flue gas supply is automatically increased to increase the temperature of the spray condensate, and the warm water is used to enhance the dissolution and elution efficiency of free chloride and adsorbed chloride ions on the surface of gypsum particles, while simultaneously reducing the overall steam heating energy consumption, and realizing the coupled and coordinated control of waste heat recovery and segmented dechlorination process.

[0014] This invention also provides a two-step steam method for preparing building gypsum powder based on the above-mentioned integrated simultaneous dechlorination system, comprising the following steps: S1: Pre-dechlorination and zoned deep dehydration After solid-liquid separation by a hydrocyclone in the plant area, the desulfurization gypsum slurry from the power plant is sent to a closed spray chamber, where multi-layer atomized spraying with soft water from the power plant's condensate washes away free chloride ions from the gypsum. The material is then conveyed to a modified disc dewatering machine. In the initial water washing zone, low-pressure spraying removes adsorbed chloride ions, while in the subsequent dewatering zone, the spraying is shut off and the vacuum negative pressure is increased to 0.07 MPa, stabilizing the material's moisture content at 17%–19%. S2: Two-stage low-temperature drying and waste heat recovery After dehydration, the gypsum is sequentially fed into a primary steam rotary low-temperature dryer and a secondary steam paddle dryer to remove free water step by step; the low-temperature waste heat generated during drying and calcination is transported to a closed spray chamber to preheat the spray condensate. S3: Calcination-synergistic gas-phase dechlorination Before the dried gypsum enters the calcination furnace, a dechlorination aid is quantitatively added through an online micro-additive dosing device. After mixing, the mixture is sent to a steam tube fluidized bed calcination furnace at 170~190℃ for low-temperature calcination. The dechlorination aid reacts with the chlorine bound in the crystal lattice to generate hydrogen chloride gas. The chlorine-containing waste gas is collected by a stratified gas phase collection hood and sent to a waste gas washing and adsorption device for purification. The gypsum is then converted into qualified β-hemihydrate gypsum. S4: Intelligent Closed-Loop Control and Finished Product Homogenization The system collects data in real time from three online chloride ion detectors: one before pre-dewatering, one after the disc dewatering machine, and one at the calcined finished product discharge end. The data is then uploaded to the DCS control system. The DCS control system automatically matches the pre-dewatering spray flow rate, the negative pressure of the disc dewatering machine, the dosage of calcining additives, and the steam heating temperature based on the chloride ion content. After the calcined material is cooled by the waste heat of the tail gas, modified and ground, and homogenized and aged in the silo for a long time, the resulting calcined material produces building gypsum powder with chloride ion indicators that meet the standards of the construction industry.

[0015] In one embodiment of the present invention, preferably, the initial chloride ion content of the raw material desulfurized gypsum is 1000~2200ppm. After the synergistic dechlorination treatment in steps S1~S4, the chloride ion content of the finished product is stably controlled within the range of ≤400ppm, and the gypsum strength and setting time indicators meet the standards.

[0016] In one embodiment of the present invention, preferably, when the average chloride ion content of the raw material is 1650 ppm, a low-alumina fly ash composite dechlorination aid is added at a dosage of 1.2 kg / ton of gypsum.

[0017] In one embodiment of the present invention, preferably, in step S1, the opening degree of the spray valve in the front washing zone and the negative pressure value in the rear section of the partitioned modified disc dewatering machine are adjusted by the DCS control system according to the online moisture content at the pre-dewatering outlet; when the chloride ion content of the incoming material is too high and the moisture content is too low, the spray flow rate is increased and the negative pressure in the rear section is increased to compensate for the moisture; when the moisture content of the incoming material exceeds the standard after washing, the spray flow rate is reduced and the vacuum negative pressure is increased to control the drying of the material.

[0018] The present invention has the following beneficial technical effects: (1) The unique disc dehydration segmented spray reduces the moisture content after pre-washing and dechlorination through negative pressure synergy, without increasing the load on the downstream steam drying. (2) Low-temperature steam calcination and trace amounts of dechlorination aid are used to catalyze precipitation, combined with in-furnace layered gas phase capture, which greatly improves the chlorine removal rate without damaging the performance of gypsum products.

[0019] (3) Three-stage online chloride ion detection and real-time control can stably control the chloride ion content of the finished product even if the chloride content of the raw material fluctuates greatly. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 This is a flowchart of a two-step steam method for preparing building gypsum powder with integrated simultaneous dechlorination, according to an embodiment of the present invention. Detailed Implementation

[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] The purpose of this invention is to provide a two-step steam dechlorination system and method for preparing building gypsum powder with integrated synchronous dechlorination. This system achieves front-end dechlorination by adding a pre-washing dechlorination device combined with a deep negative pressure dehydration device; it also achieves calcination dechlorination through synergistic calcination gas-phase dechlorination using additives; and it incorporates online chlorine detection and intelligent closed-loop control to implement a precise dechlorination control strategy, reducing operating costs. Without significantly increasing steam energy consumption, the system stably reduces the maximum chloride ion concentration in the raw materials to within the standards required by the construction industry, while simultaneously ensuring that the strength and setting time of the building gypsum meet the required standards.

[0024] First embodiment: This invention provides a steam two-step system for preparing building gypsum powder with integrated synchronous dechlorination, which includes a pre-dechlorination pretreatment unit, a deep dehydration and dechlorination unit, a calcination-co-dechlorination unit, and a dechlorination co-control unit arranged in series. The pre-dechlorination pretreatment unit is connected to the discharge end of the power plant's existing gypsum hydrocyclone and includes a sealed spray chamber, a multi-stage condensate spray device, an online turbidity monitor, a solid-liquid separation sieve plate, and a filtrate collection tank. The multi-stage condensate spray device uses power plant condensate atomized spray to wash away free chloride ions from gypsum particles, and the waste liquid collected in the filtrate collection tank is returned to the desulfurization wastewater system. In this embodiment, the pre-dechlorination pretreatment unit of the present invention is connected after the hydrocyclone discharges, so as not to disrupt the original desulfurization and dehydration main line. After the free chloride ions of gypsum particles are washed away by the atomized spray of power plant condensate, the water content of the gypsum will rise to 21%~23%. In this invention, the gypsum is directly connected to the modified disc dewatering machine after the pre-dechlorination silo discharges, and the gypsum enters the modified disc dewatering machine.

[0025] The deep dehydration and dechlorination unit is a partitioned disc dehydrator. The disc surface of the partitioned disc dehydrator is divided into two independent front washing zone and rear dehydration zone along the material travel direction. The front washing zone and the rear dehydration zone are equipped with independent spray pipes and independent negative pressure vacuum pumps. The front washing zone is equipped with a low-pressure condensate spray pipe to maintain only the basic negative pressure to achieve secondary dechlorination of surface chloride ions. The rear dehydration zone has no spray pipes, but is equipped with an adjustable vacuum pump to forcibly remove the free water inside the gypsum after washing. Most existing modified disc dewatering machines only arrange spray pipes to cover the entire disc surface, spraying water uniformly without different areas. After washing, the overall moisture content of the gypsum soars, which is the biggest drawback of the existing washing process. The vacuum pump maintains a uniform negative pressure throughout the process, making it impossible to control the drying of materials in a targeted manner. This invention has made a front and rear partitioned solid structure modification. The pipelines and negative pressure systems of the front washing area and the rear dewatering area are completely separated, so that they do not interfere with each other.

[0026] Unlike conventional solutions that simply modify nozzles, this invention divides the disc dehydrator into two sections with separately arranged differentiated spray pipelines. The first section continues shallow rinsing with condensed soft water to further remove adsorbed chlorine, while the second section does not spray water but separately increases the vacuum negative pressure to the -0.07MPa range. Through negative pressure vacuum, the moisture content of 21%~23% after washing is stably compressed back to the process standard range of 17%~19%, solving the problems of excessive moisture after washing and soaring drying energy consumption. This segmented spray + dynamic negative pressure synergistic humidity control structure is a unique modification solution of this invention, different from ordinary single-assembly rinsing devices. Specifically: (1) Front washing zone: A set of low-pressure condensate spray pipes are laid along the rotating feed side of the disc. The nozzles are evenly facing the gypsum filter cake on the disc. The water flow gently washes the chloride ions attached to the surface of the gypsum particles. The vacuum pump in this section only maintains the basic negative pressure to ensure that the material does not fall off and does not perform strong dehydration. The focus is on completing the secondary dechlorination. (2) Post-dehydration zone: The spray pipe is completely eliminated in the rear half of the tray. An independent vacuum negative pressure pipe is laid separately and equipped with an adjustable vacuum pump. After the material enters this zone through the water washing zone, the system automatically raises the vacuum to 0.07MPa. The strong negative pressure quickly removes the free water inside the gypsum. (3) Control logic: The DCS control system adjusts the zone synchronously according to the online moisture content value at the pre-dehydration outlet. When the incoming material has high chlorine and low moisture, the flow rate of the front spray is increased, and the negative pressure of the rear section is increased to compensate for moisture. When the moisture content of the incoming material exceeds the standard after washing, the front spray is reduced and the vacuum of the rear section is increased. The two zones are linked in real time to achieve "washing chlorine while controlling water" to solve the problem that simple spraying only increases water and does not dehydrate.

[0027] The calcination-co-dechlorination unit includes a primary steam rotary low-temperature dryer, a secondary steam paddle dryer, a steam tubular fluidized bed calciner, an online addition device for trace additives, a stratified gas phase collection hood, and a waste gas scrubbing and adsorption device. The online addition device for trace additives is located on the feed screw of the steam tubular fluidized bed calciner and is used to add dechlorination additives (in this embodiment, the dechlorination additive is a low-alumina fly ash composite dechlorination additive). The stratified gas phase collection hood collects chlorine-containing waste gas in sections and transports it to the waste gas scrubbing and adsorption device. The low-temperature waste heat pipeline discharged from the steam tubular fluidized bed calciner is connected to the sealed spray chamber of the pre-dechlorination pretreatment unit for preheating the spray soft water. After dehydration and moisture control, the high-chlorinated gypsum is sent to the mature two-step steam drying section. In the existing technology, the conventional process is as follows: the first-stage drying adopts low-temperature steam rotary drying (no wall adhesion and no clogging), and the temperature is strictly controlled within 75℃, only evaporating the surface free water without damaging the dihydrate crystal structure of gypsum; the second-stage steam paddle dryer continues to deeply dry the material, reducing the moisture content to below 1%.

[0028] This invention incorporates a synergistic dechlorination system in the downstream calcination stage, specifically at the steam-tube fluidized bed calciner: (1) Add a trace amount of additive online dosing device to the feed screw of the calcining furnace, add low-alumina fly ash composite dechlorination additive, and the additive enters the steam tube fluidized bed calcining furnace evenly with the gypsum. Under the low temperature steam indirect heating atmosphere of 170~190℃, the additive reacts with the chloride ions bound in the gypsum lattice in a directional reaction, which greatly reduces the activation energy of hydrogen chloride precipitation. The bound chlorine can be stablely precipitated in the gas phase without significantly increasing the calcination temperature. This method can precipitate chlorine and avoid high temperature overburning that damages the quality of gypsum. (2) A layered gas phase collection and capture hood is set in the furnace body to collect chlorine-containing waste gas in sections and send it to the matching washing and adsorption device. Ordinary steam calcination has no auxiliary catalyst and no layered gas collection, so the chlorine precipitation efficiency is very low. This invention improves the removal rate by using auxiliary agents.

[0029] (3) The low-temperature waste heat discharged from the two-stage drying and calcining furnace is transported to the sealed spray chamber to preheat the soft water for rinsing and reduce the overall steam consumption.

[0030] The dechlorination co-control unit includes three online rapid chloride ion detectors, a DCS control system, an electrically controlled steam flow regulating valve, a calcination temperature sensor, and an additive dosing actuator. The three online rapid chloride ion detectors are respectively located before the pre-dechlorination chamber discharge, after the disc dehydrator, and at the calcined finished product discharge end. Based on the real-time chloride ion detection data from the three locations, the DCS control system coordinates and regulates the pre-dechlorination spray flow, the zoned negative pressure of the disc dehydrator, the dosage of calcination additives, and the steam heating temperature to achieve adaptive closed-loop control of raw material chloride ion fluctuations.

[0031] In the dechlorination co-control unit of this embodiment, the control logic of the DCS control system is as follows: (1) When the detected chloride ion value satisfies 400ppm < Cl - When the concentration is <1200ppm, increase the pre-dechlorination spray flow rate and adjust the negative pressure at the rear of the disc dewatering machine to complete the dechlorination. If the chloride ion concentration at the rear of the disc dewatering machine is still too high, start the online addition device for trace additives to add dechlorination additives, and complete the final index verification through the detector at the end of the steam tube fluidized bed calcining furnace. (2) When the detected chloride ion value satisfies 1200ppm < Cl - When the concentration is <1800ppm, the pre-dechlorination spray water volume is increased simultaneously and the dechlorination aid is added. Relying on the synergistic effect of water washing dechlorination and calcination gas phase dechlorination, the final index verification is completed by the detector at the end of the steam tube fluidized bed calciner.

[0032] In this embodiment, the dechlorination aid reacts directionally with the bound chloride ions in the gypsum lattice, significantly reducing the activation energy for hydrogen chloride precipitation, and achieving the precipitation of bound chlorine gas phase at a low temperature of 170~190℃.

[0033] In this embodiment, the sealed spray chamber of the pre-dechlorination pretreatment unit is equipped with a soft water preheating heat exchange pipeline, which is connected to the low-temperature flue gas waste heat outlet of the primary steam rotary low-temperature dryer and the steam tubular fluidized bed calciner. The DCS control system adjusts the flow rate of low-temperature flue gas in conjunction with the inlet water temperature and raw material chloride ion concentration of the sealed spray chamber. When the chloride ion content of the incoming material increases and the spray washing intensity needs to be increased, the low-temperature flue gas supply is automatically increased to raise the temperature of the spray condensate. The warm water enhances the dissolution and elution efficiency of free and adsorbed chloride ions on the surface of gypsum particles, and simultaneously reduces the overall steam heating energy consumption, realizing the coupled and coordinated control of waste heat recovery and segmented dechlorination process.

[0034] Figure 1 This is a flowchart of a two-step steam method for preparing building gypsum powder with integrated simultaneous dechlorination according to an embodiment of the present invention, as shown below. Figure 1 As shown, the present invention provides a two-step steam method for preparing building gypsum powder based on the above-mentioned integrated simultaneous dechlorination system, which includes the following steps: S1: Pre-dechlorination and zoned deep dehydration After solid-liquid separation by a hydrocyclone in the plant area, the desulfurization gypsum slurry from the power plant is sent to a closed spray chamber, where multi-layer atomized spraying with soft water from the power plant's condensate washes away free chloride ions from the gypsum. The material is then conveyed to a modified disc dewatering machine. In the initial water washing zone, low-pressure spraying removes adsorbed chloride ions, while in the subsequent dewatering zone, the spraying is shut off and the vacuum negative pressure is increased to 0.07 MPa, stabilizing the material's moisture content at 17%–19%. S2: Two-stage low-temperature drying and waste heat recovery After dehydration, the gypsum is sequentially fed into a primary steam rotary low-temperature dryer and a secondary steam paddle dryer to remove free water step by step; the low-temperature waste heat generated during drying and calcination is transported to a closed spray chamber to preheat the spray condensate. S3: Calcination-synergistic gas-phase dechlorination Before the dried gypsum enters the calcination furnace, a dechlorination aid is quantitatively added through an online micro-additive dosing device. After mixing, the mixture is sent to a steam tube fluidized bed calcination furnace at 170~190℃ for low-temperature calcination. The dechlorination aid reacts with the chlorine bound in the crystal lattice to generate hydrogen chloride gas. The chlorine-containing waste gas is collected by a stratified gas phase collection hood and sent to a waste gas washing and adsorption device for purification. The gypsum is then converted into qualified β-hemihydrate gypsum. S4: Intelligent Closed-Loop Control and Finished Product Homogenization The system collects data in real time from three online chloride ion detectors: one before pre-dewatering, one after the disc dewatering machine, and one at the calcined finished product discharge end. The data is then uploaded to the DCS control system. The DCS control system automatically matches the pre-dewatering spray flow rate, the negative pressure of the disc dewatering machine, the dosage of calcining additives, and the steam heating temperature based on the chloride ion content. After the calcined material is cooled by the waste heat of the tail gas, modified and ground, and homogenized and aged in the silo for a long time, the resulting calcined material produces building gypsum powder with chloride ion indicators that meet the standards of the construction industry.

[0035] In this embodiment, the initial chloride ion content of the raw material desulfurized gypsum is 1000~2200ppm. After the synergistic dechlorination treatment in steps S1~S4, the chloride ion content of the finished product is stably controlled within the range of ≤400ppm, and the gypsum strength and setting time meet the standards.

[0036] In this embodiment, under the condition that the average chloride ion content of the raw material is 1650 ppm, a low-alumina fly ash composite dechlorination aid is added at a dosage of 1.2 kg / ton of gypsum.

[0037] In this embodiment, in step S1, the opening degree of the spray valve in the front washing zone and the negative pressure value in the rear section of the partitioned modified disc dewatering machine are adjusted by the DCS control system according to the online moisture content at the pre-dewatering outlet. When the chloride ion content of the incoming material is too high and the moisture content is too low, the spray flow rate is increased and the negative pressure in the rear section is increased to compensate for the moisture. When the moisture content of the incoming material exceeds the standard after washing, the spray flow rate is reduced and the vacuum negative pressure is increased to control the drying of the material.

[0038] Second embodiment: Taking a certain factory's raw desulfurized gypsum with an average chloride ion content of 1650 ppm and 13.2% as an example: Front-end pretreatment section: The gypsum hydrocyclone discharge is fed into a closed spray chamber, where multi-layer spraying with unit condensed soft water is used. After spraying, the water content of the gypsum rises to 22.4%, and the chloride ion concentration at the pre-dehydration chamber outlet is 1080 ppm. The material enters the modified disc dewatering machine. The spray valve opening in the front washing zone is 65%, and the vacuum negative pressure in the rear dewatering zone is maintained at a stable level of about 0.07 MPa. After dewatering, the moisture content of the material drops back to 19.1%. The chloride ion concentration at the mid-stage drying detection point is 620 ppm, which is only slightly above the standard. The system then starts the addition of calcination aids.

[0039] Drying and calcination section: The material first enters the primary steam rotary low-temperature dryer to remove surface water, and then is sent to the secondary steam paddle dryer for deep drying; after that, it is sent to the steam tube fluidized bed calcination furnace, where the calcination temperature is controlled at 182℃. Because the chloride ion concentration after drying is 620ppm, the system automatically adds a low-alumina fly ash composite dechlorination aid at a dosage of 1.2kg / ton of gypsum; the layered gas phase collection and capture hood in the furnace continuously collects hydrogen chloride waste gas and sends it to the scrubbing tower for treatment.

[0040] Finished product testing and output: After calcination and cooling, the finished product was tested online and found to have 380 ppm chloride ions, 5.2% water of crystallization, and a 2-hour compressive strength of 6.9 MPa, all of which meet the national standards.

[0041] This invention features a unique segmented spray dehydration process using a disc, which reduces the moisture content after pre-washing and dechlorination through negative pressure without increasing the load on the subsequent steam drying. It employs low-temperature steam calcination combined with trace amounts of dechlorination aids for synergistic catalytic precipitation, along with in-furnace stratified gas phase capture, significantly improving the chlorine removal rate without compromising the performance of the gypsum product. Real-time online detection and control of chloride ions in three stages ensures stable control of the chloride ion content in the finished product even with significant fluctuations in the chlorine content of the raw materials.

[0042] Those skilled in the art will understand that the accompanying drawings are merely schematic diagrams of one embodiment, and the modules or processes shown in the drawings are not necessarily essential for implementing the present invention.

[0043] Those skilled in the art will understand that the modules in the apparatus of the embodiments can be distributed in the apparatus of the embodiments as described in the embodiments, or they can be located in one or more devices different from this embodiment with corresponding changes. The modules of the above embodiments can be combined into one module, or they can be further divided into multiple sub-modules.

[0044] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A two-step steam-based system for preparing building gypsum powder with integrated simultaneous dechlorination, characterized in that, It includes a pre-dechlorination pretreatment unit, a deep dehydration and dechlorination unit, a calcination-co-dechlorination unit, and a dechlorination co-control unit arranged in series; The pre-dechlorination pretreatment unit is connected to the discharge end of the power plant's existing gypsum hydrocyclone and includes a sealed spray chamber, a multi-stage condensate spray device, an online turbidity monitor, a solid-liquid separation sieve plate, and a filtrate collection tank. The multi-stage condensate spray device uses power plant condensate atomized spray to wash away free chloride ions from gypsum particles, and the waste liquid collected in the filtrate collection tank is returned to the desulfurization wastewater system. The deep dehydration and dechlorination unit is a partitioned disc dehydrator. The disc surface of the partitioned disc dehydrator is divided into two independent front washing zone and rear dehydration zone along the material travel direction. The front washing zone and the rear dehydration zone are equipped with independent spray pipes and independent negative pressure vacuum pumps. The front washing zone is equipped with a low-pressure condensate spray pipe to maintain only the basic negative pressure to achieve secondary dechlorination of surface chloride ions. The rear dehydration zone has no spray pipes, but is equipped with an adjustable vacuum pump to forcibly remove the free water inside the gypsum after washing. The calcination-co-dechlorination unit includes a primary steam rotary low-temperature dryer, a secondary steam paddle dryer, a steam tube fluidized bed calciner, an online addition device for trace additives, a stratified gas phase collection hood, and a waste gas scrubbing and adsorption device. The online addition device for trace additives is located on the feed screw of the steam tube fluidized bed calciner and is used to add dechlorination additives. The stratified gas phase collection hood collects chlorine-containing waste gas in sections and transports it to the waste gas scrubbing and adsorption device. The low-temperature waste heat pipeline discharged from the steam tube fluidized bed calciner is connected to the sealed spray chamber of the pre-dechlorination pretreatment unit for preheating the spray soft water. The dechlorination co-control unit includes three online rapid chloride ion detectors, a DCS control system, an electrically controlled steam flow regulating valve, a calcination temperature sensor, and an additive dosing actuator. The three online rapid chloride ion detectors are respectively located before the pre-dechlorination chamber discharge, after the disc dehydrator, and at the calcined finished product discharge end. Based on the real-time chloride ion detection data from the three locations, the DCS control system coordinates and regulates the pre-dechlorination spray flow, the zoned negative pressure of the disc dehydrator, the dosage of calcination additives, and the steam heating temperature to achieve adaptive closed-loop control of raw material chloride ion fluctuations.

2. The integrated synchronous dechlorination steam two-step method for preparing building gypsum powder according to claim 1, characterized in that, In the dechlorination co-control unit, the control logic of the DCS control system is as follows: (1) When the chloride ion value meets 400 ppm < Cl - < 1200 ppm, increase the pre-deionization spray flow and adjust the negative pressure at the rear of the disc dewaterer to complete the dechlorination; if the chloride ion at the rear of the disc dewaterer is still over the standard, start the trace amount of online additive dosing device to add dechlorination additives, and complete the final index verification through the detector at the end of the steam tubular boiling calcination furnace. (2) When the detected chloride ion value satisfies 1200ppm < Cl - When the concentration is <1800ppm, the pre-dechlorination spray water volume is increased simultaneously and the dechlorination aid is added. Relying on the synergistic effect of water washing dechlorination and calcination gas phase dechlorination, the final index verification is completed by the detector at the end of the steam tube fluidized bed calciner.

3. The integrated synchronous dechlorination steam two-step method for preparing building gypsum powder according to claim 1, characterized in that, The dechlorination aid is a low-alumina fly ash composite dechlorination aid.

4. The integrated synchronous dechlorination steam two-step method for preparing building gypsum powder according to claim 1, characterized in that, The steam tube type fluidized bed calcining furnace is used for low-temperature indirect heating at 170~190℃.

5. The integrated synchronous dechlorination steam two-step method for preparing building gypsum powder according to claim 4, characterized in that, The dechlorination aid reacts directionally with the bound chloride ions in the gypsum lattice, significantly reducing the activation energy for hydrogen chloride evolution, and achieving the gaseous evolution of bound chlorine at a low temperature of 170~190℃.

6. The integrated synchronous dechlorination steam two-step method for preparing building gypsum powder according to claim 1, characterized in that, The sealed spray chamber of the pre-dechlorination pretreatment unit is equipped with a soft water preheating heat exchange pipeline, which is connected to the low-temperature flue gas waste heat outlet of the primary steam rotary low-temperature dryer and the steam tubular fluidized bed calciner. The DCS control system adjusts the flow rate of low-temperature flue gas in conjunction with the inlet water temperature of the sealed spray chamber and the chloride ion concentration of the raw material. When the chloride ion content of the incoming material increases and the spray washing intensity needs to be increased, the low-temperature flue gas supply is automatically increased to raise the temperature of the spray condensate. The warm water enhances the dissolution and elution efficiency of free and adsorbed chloride ions on the surface of gypsum particles, and simultaneously reduces the overall steam heating energy consumption, realizing the coupled and coordinated control of waste heat recovery and segmented dechlorination process.

7. A two-step steam method for preparing building gypsum powder based on the integrated simultaneous dechlorination system according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1: Pre-dechlorination and zoned deep dehydration After solid-liquid separation by a hydrocyclone in the plant area, the desulfurization gypsum slurry from the power plant is sent to a closed spray chamber, where multi-layer atomized spraying with soft water from the power plant's condensate washes away free chloride ions from the gypsum. The material is then conveyed to a modified disc dewatering machine. In the initial water washing zone, low-pressure spraying removes adsorbed chloride ions, while in the subsequent dewatering zone, the spraying is shut off and the vacuum negative pressure is increased to 0.07 MPa, stabilizing the material's moisture content at 17%–19%. S2: Two-stage low-temperature drying and waste heat recovery After dehydration, the gypsum is sequentially fed into a primary steam rotary low-temperature dryer and a secondary steam paddle dryer to remove free water step by step; the low-temperature waste heat generated during drying and calcination is transported to a closed spray chamber to preheat the spray condensate. S3: Calcination-synergistic gas-phase dechlorination Before the dried gypsum enters the calcination furnace, a dechlorination aid is quantitatively added through an online micro-additive dosing device. After mixing, the mixture is sent to a steam tube fluidized bed calcination furnace at 170~190℃ for low-temperature calcination. The dechlorination aid reacts with the chlorine bound in the crystal lattice to generate hydrogen chloride gas. The chlorine-containing waste gas is collected by a stratified gas phase collection hood and sent to a waste gas washing and adsorption device for purification. The gypsum is then converted into qualified β-hemihydrate gypsum. S4: Intelligent Closed-Loop Control and Finished Product Homogenization The system collects data in real time from three online chloride ion detectors: one before pre-dewatering, one after the disc dewatering machine, and one at the calcined finished product discharge end. The data is then uploaded to the DCS control system. The DCS control system automatically matches the pre-dewatering spray flow rate, the negative pressure of the disc dewatering machine, the dosage of calcining additives, and the steam heating temperature based on the chloride ion content. After the calcined material is cooled by the waste heat of the tail gas, modified and ground, and homogenized and aged in the silo for a long time, the resulting calcined material produces building gypsum powder with chloride ion indicators that meet the standards of the construction industry.

8. The method for preparing building gypsum powder using a two-step steam method with integrated simultaneous dechlorination according to claim 7, characterized in that, The initial chloride ion content of the raw desulfurized gypsum is 1000~2200ppm. After the synergistic dechlorination treatment in steps S1~S4, the chloride ion content of the finished product is stably controlled within the range of ≤400ppm, and the gypsum strength and setting time meet the standards.

9. The method for preparing building gypsum powder using a two-step steam method with integrated simultaneous dechlorination according to claim 7, characterized in that, Under the condition that the average chloride ion concentration of the raw material is 1650 ppm, a low-alumina fly ash composite dechlorination aid is added at a dosage of 1.2 kg / ton of gypsum.

10. The method for preparing building gypsum powder using a two-step steam method with integrated simultaneous dechlorination according to claim 7, characterized in that, In step S1, the opening of the spray valve in the front washing zone and the negative pressure value in the rear section of the partitioned disc dewatering machine are adjusted by the DCS control system according to the online moisture content at the pre-dewatering outlet. When the chloride ion content of the incoming material is too high and the moisture content is too low, the spray flow rate is increased and the negative pressure in the rear section is increased to compensate for the moisture. When the moisture content of the incoming material exceeds the standard after washing, the spray flow rate is reduced and the vacuum negative pressure is increased to control the drying of the material.