A high air-entraining composite rheology modifier for wet sprayed concrete and its preparation method
By combining bifunctional fluorinated block copolymers, enzymatically hydrolyzed hydroxyethylated saponins, and nanotube loading technology with thermosensitive polyetheramine, the problems of multi-component competitive adsorption and bubble stability of wet-sprayed concrete rheology modifiers have been solved, achieving a balance between high gas content and rheological properties, making it suitable for construction in tunnels, mines, and underground engineering.
Patent Information
- Application Number
- CN202611066323.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing physical compound wet sprayed concrete rheology modifiers suffer from problems such as competitive adsorption of multiple components, poor bubble stability, and time-series rheological mismatch. They are difficult to balance stable high air content and excellent rheological properties at the same time, and cannot meet the construction needs under complex working conditions.
By synergistically integrating bifunctional fluorinated block copolymers with enzymatically hydrolyzed hydroxyethyl saponins, combined with organically intercalated halloysite nanotubes with pore-loaded alkyl glycosides and thermosensitive polyetheramines, well-organized composite micelles are formed through molecular micelle synergy, nano-slow release, thermosensitive time-series rheology, and low-temperature pre-assembly processes, thereby optimizing bubble size distribution and rheological properties.
It achieves simultaneous improvement in gas content stability and rheological adaptability, with a gas content loss rate of ≤12% over time and a jet rebound rate of ≤12%, meeting the construction needs of tunnels, mines and underground engineering.
Smart Images

Figure CN123106064A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of concrete admixture technology, and more specifically, to a high air-entraining composite rheology modifier for wet-sprayed concrete and its preparation method, which is particularly suitable for pumping and spraying wet-sprayed concrete for initial support in tunnels, mines and underground engineering. Background Technology
[0002] Shotcrete is a commonly used support material in tunnel initial support and foundation pit slope reinforcement projects. Its workability and service durability directly affect project quality and construction efficiency. Composite rheology modifiers are key admixtures for regulating the performance of shotcrete. They are mainly used to improve the dispersion and flow state of the slurry, ensure smooth long-distance pumping, and introduce an appropriate amount of micro-air bubbles to enhance the freeze-thaw resistance of the concrete. Existing shotcrete rheology modifiers are mostly prepared by simple physical mixing of polycarboxylate-based water-reducing agents, small-molecule air-entraining agents, and organic thickening components, which can meet the basic usage requirements under conventional working conditions.
[0003] For example, Chinese patent application CN114591098A discloses a polycarboxylate rheology modifier for wet-sprayed concrete, which uses a physical compound of a water-reducing agent and a rosin-based air-entraining agent. Although it can improve initial fluidity, the competitive adsorption between components is significant, and the air content loss rate over time exceeds 25%. Chinese patent application CN112811876A discloses a halloysite-modified concrete thickener, but it only utilizes the thickening effect of nanoparticles and does not involve the slow-release design of active components loaded in pores, thus failing to simultaneously achieve rheological regulation and long-term foam stability. Existing technologies have consistently failed to simultaneously resolve the triple technical contradictions of competitive adsorption, poor bubble stability, and time-series rheological adaptation.
[0004] In practical engineering applications, these physically compounded products have a competitive adsorption problem among functional components. The air-entraining component tends to preferentially adsorb onto the surface of cement particles, crowding out the action sites of water-reducing agent molecules, resulting in a decrease in the dispersion ability of the slurry. Meanwhile, the rheology control component tends to disrupt the stability of the bubble liquid film, causing excessive loss of air content over time. It is difficult to simultaneously achieve a balance between stable high air content and excellent rheological properties, and thus cannot better adapt to the requirements of wet spraying construction under complex working conditions. Summary of the Invention
[0005] To address the triple technical challenges of competitive adsorption of multiple components, poor bubble stability, and time-series rheological mismatch in existing physically compounded rheology modifiers, this application proposes the following improvements and integrates them synergistically: First, a bifunctional fluorinated block copolymer with both dispersing and gas-entraining functions is designed using RAFT polymerization to eliminate competitive adsorption of independent small-molecule gas-entraining agents at the source. Second, enzymatic hydrolysis of hydroxyethylated saponins enhances the elasticity of the bubble liquid film, and organically intercalated halloysite nanotubes with alkyl glycosides loaded in the pores achieve the slow release of interfacial active substances, maintaining long-term bubble stability. Finally, a thermosensitive polyetheramine with a cloud point temperature of 35–40 °C is introduced, which thickens in situ through hydrophobic association after hydration and heating. Simultaneously, a low-temperature pre-assembly process is used to form well-ordered composite micelles with an average particle size of 120–180 nm between the main agent and the saponin, optimizing the bubble size distribution. The synergistic combination of these multiple technologies simultaneously achieves stable gas content, rheological compatibility, and low rebound rate.
[0006] The synergistic mechanism of the multi-component system described in this application is reflected in four dimensions.
[0007] (1) Synergistic arrangement of molecular micelles: The perfluorobutyl ethyl segment in the bifunctional fluorinated polycarboxylic acid block copolymer has extremely strong hydrophobicity and low surface energy characteristics. It self-assembles with the triterpenoid hydrophobic core of enzymatically hydrolyzed hydroxyethylated saponin through hydrophobic interaction and hydrogen bond network to form core-shell composite micelles with an average particle size of 120-180 nm under low temperature conditions. The fluorinated segment is anchored at the gas-liquid interface to provide a driving force for persistent reduction of interfacial tension. The saponin molecules are tightly arranged in the outer shell of the micelle to enhance the viscoelasticity of the bubble liquid film. The two are synergistically and densely arranged at the interface, which narrows the bubble size distribution and significantly reduces the merging and breaking rate.
[0008] (2) Nano-slow release synergy: Organic intercalation increases the interlayer spacing of halloysite nanotube 001 crystal planes from 0.72nm to 1.35-1.42nm. The alkyl glycosides contained in the tube are gradually desorbed and released during the cement hydration process as the alkalinity gradient of the pore liquid changes. The ultrathin silica barrier film formed by the silica sol sealing layer at the pore opening extends the release period to the hydration acceleration period, continuously replenishing the interfacial active substances consumed by the hydration products, overcoming the drawbacks of traditional externally added air-entraining agents that are consumed in large quantities in the early stage and scarce in the later stage.
[0009] (3) Thermosensitive time-series rheological synergy: Thermosensitive polyetheramine with a cloud point of 35-40℃ is precisely matched to the hydration temperature rise curve of sprayed concrete. During the pumping stage, the temperature is lower than the cloud point, and the molecules are in a fully hydrated and extended conformation, without increasing the plastic viscosity of the slurry. After being sprayed onto the sprayed surface, the heat release of hydration pushes the temperature to break through the cloud point. The dehydration and collapse of the polyoxyethylene chain segments triggers hydrophobic association between molecules, forming a physical cross-linking network that runs through the slurry. This improves the yield stress and cohesiveness in situ and effectively resists the rebound shear force.
[0010] (4) Synergistic effect of low-temperature pre-assembly process: The low-speed stirring conditions of 10-15℃ under nitrogen protection in the dark inhibit the disordered fusion of micelles and Ostwald curing caused by molecular thermal motion, ensuring that the composite micelles have uniform particle size and regular structure, and greatly improving storage stability. The four-dimensional synergistic mechanism supports each other and is indispensable, and together they have achieved a comprehensive performance breakthrough with gas content loss rate ≤12% and spray rebound rate ≤12%.
[0011] In a first aspect, this application provides a high air-entraining composite rheology modifier for wet-sprayed concrete, employing the following technical solution:
[0012] A high air-entraining composite rheology modifier for wet sprayed concrete, comprising the following components by weight: 35-45 parts of bifunctional dispersing air-entraining agent, 12-18 parts of enzyme-modified saponin air-entraining and foam-stabilizing component, 8-12 parts of supported nano-rheology reinforcing component, 2-3 parts of thermosensitive polyetheramine, 3-5 parts of sodium gluconate, and deionized water to make up to 100 parts by weight.
[0013] The bifunctional dispersing and air-entraining agent is a bifunctional fluorinated polycarboxylic acid block copolymer, which is prepared by RAFT polymerization of acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate, and the solid content of the product is 38% to 42%.
[0014] The enzyme-modified saponin aeration and foam stabilizing component is an enzymatically modified triterpenoid saponin derivative, which is obtained by enzymatic hydrolysis of natural saponins by compound cellulase followed by hydroxyethylation.
[0015] The supported nanorheology enhancement component is an organically intercalated halloysite nanotube with alkyl glycosides supported in the pores, wherein the alkyl glycosides are low-carbon alkyl glycosides with a carbon chain length of 8 to 10, and the loading amount is 15% to 20% of the mass of the halloysite nanotubes;
[0016] The thermosensitive polyetheramine is a polyoxyethylene-polyoxypropylene block copolymer polyetheramine with a cloud point temperature of 35-40°C and is completely soluble in an aqueous system at 20-25°C.
[0017] By adopting the above technical solution, the single-molecule structure of the bifunctional dispersing air-entraining agent simultaneously possesses two types of functional sites: cement particle dispersion and interfacial air entrainment. This eliminates the need for additional independent small-molecule air-entraining agents and effectively reduces the competitive adsorption of different functional components on the cement particle surface. The enzyme-modified saponin component helps improve the strength of the bubble liquid film, the supported nano-rheology-enhancing component constructs a physical rheological network and slowly releases active substances, and the temperature-sensitive polyetheramine regulates the viscosity of the slurry as the hydration temperature rises. Combined with sodium gluconate to moderate the hydration rate, the multi-component structure forms a synergistic composite system that simultaneously improves the air content stability and rheological compatibility of fresh concrete.
[0018] Halloysite possesses a natural hollow tubular clay mineral structure, making it suitable as a microscale carrier for active substances. Organic intercalation treatment can modify the surface and inner walls of nanotubes, improving the compatibility of nanomaterials with aqueous systems and enhancing the binding affinity of the pores for alkyl glycosides. Alkyl glycosides are stored inside the hollow pores and can be slowly released according to changes in the slurry hydration environment, continuously replenishing interfacial active substances. At the same time, the interconnection between nanotubes forms a physical cross-linking network, endowing the slurry with shear-thinning rheological properties.
[0019] Enzymatic hydrolysis can directionally prune the side-chain glycosyl groups of triterpenoid saponins, reducing molecular steric hindrance and improving their arrangement efficiency at the gas-liquid interface; hydroxyethylation grafting can introduce stable hydrophilic groups onto saponin molecules, improving their tolerance in strongly alkaline cement slurries. The temperature-responsive characteristics of thermosensitive block copolyetheramines originate from changes in the hydration layer of polyoxyethylene segments. At room temperature, the hydration layer structure is intact, and the molecules are completely dissolved in the aqueous phase, without increasing the initial viscosity of the slurry; as the hydration temperature rises, the hydration layer gradually breaks down, and the molecules undergo hydrophobic association, which can improve the cohesiveness of the slurry in situ, adapting to the performance requirements of spraying conditions;
[0020] RAFT polymerization is a controlled free radical polymerization method that allows for precise control of the copolymer's segment sequence and molecular weight distribution, enabling the formation of an ordered block structure between fluorinated hydrophobic segments and polyether hydrophilic segments. The fluorinated segments can be directionally enriched at the gas-liquid interface to reduce interfacial tension, while the polyether side chains can disperse cement particles through steric hindrance. This single-molecule integration of two types of functions effectively avoids functional antagonism issues associated with multi-component blends, thus improving the system's performance stability.
[0021] Preferably, in the organically intercalated halloysite nanotubes with alkyl glycosides loaded in the pores, the interlayer spacing of the 001 crystal planes of the organically intercalated halloysite nanotubes is 1.35 to 1.42 nm, and the loading of the alkyl glycosides is 15% to 20%.
[0022] By adopting the above technical solution, the increased interlayer spacing can accommodate alkyl glycoside molecules, and the appropriate loading can take into account both the sustained release time and the foam stabilization effect. At the same time, the nanotubes overlap to form a shear-thinning network, which meets the pumping and spraying requirements.
[0023] Preferably, the bifunctional fluorinated polycarboxylic acid block copolymer and the enzymatically modified triterpenoid saponin derivative form a composite micelle in the system, and the average particle size of the composite micelle is 120-180 nm.
[0024] By adopting the above technical solution, composite micelles within this particle size range can form an orderly and dense arrangement at the gas-liquid interface, improving the uniformity of bubble size and storage stability, and avoiding large bubbles and bubble coalescence.
[0025] Preferably, the bifunctional fluorinated polycarboxylic acid block copolymer has a fluorine grafting rate of 3.8% to 4.5%, a weight-average molecular weight of 26,000 to 30,000, and a molecular weight distribution index of 1.25 to 1.32; and the enzymatically modified triterpenoid saponin derivative has a saponin retention rate of ≥92%.
[0026] By adopting the above technical solutions, the appropriate fluorine grafting rate and narrow molecular weight distribution can ensure the batch stability of copolymer dispersion and gas entrainment performance; the high saponin retention rate can ensure that the interfacial activity is fully retained after enzymatic modification.
[0027] Secondly, this application provides a method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete, employing the following technical solution:
[0028] A method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete includes the following steps:
[0029] S1. Copolymerization: Acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate are added to a reactor, along with benzyl dithiobenzoate RAFT reagent and azobisisobutyronitrile initiator. Nitrogen gas is introduced to purge air from the reactor, and the temperature is raised and maintained for polymerization. After the reaction is completed, the solution is neutralized to the set pH value with sodium hydroxide solution to obtain a bifunctional fluorinated polycarboxylic acid block copolymer solution.
[0030] S2. Saponin enzymatic hydrolysis modification: Natural saponins are prepared into an aqueous solution, compound cellulase is added, the pH of the system is adjusted, and then the temperature is raised to a constant temperature for enzymatic hydrolysis. Subsequently, the enzyme preparation is inactivated by raising the temperature. Then, ethylene oxide is added for hydroxyethylation modification. After the reaction is completed, the product is purified and spray-dried to obtain enzymatically modified triterpenoid saponin derivatives.
[0031] S3. Halloysite Modification and Loading: Halloysite nanotubes were dispersed in deionized water to prepare a suspension, hexadecyltrimethylammonium bromide was added, and the mixture was heated and ultrasonically stirred. The product was centrifuged, washed, and dried to obtain organically intercalated halloysite nanotubes. Low-carbon chain alkyl glycosides were mixed with anhydrous ethanol to prepare an impregnation solution, which was then added to the organically intercalated halloysite nanotubes. After impregnation under negative pressure, the nanotubes were centrifuged, dried at low temperature, and subjected to light surface sealing treatment to obtain pore-loaded alkyl glycoside organically intercalated halloysite nanotubes.
[0032] S4. Low-temperature pre-assembly: The bifunctional fluorinated polycarboxylic acid block copolymer solution and the enzymatically modified triterpenoid saponin derivative are added to the premixing tank according to the formula ratio. After adjusting the system temperature, the mixture is stirred at a low speed to form composite micelles and obtain the pre-assembled mixture.
[0033] S5. Composite homogenization preparation: Add the formulated amount of thermosensitive polyetheramine and sodium gluconate to the pre-assembled mixture, and stir at room temperature until the system is uniformly dispersed; then slowly add the pore-loaded alkyl glycoside organic intercalated halloysite nanotubes, maintain high-speed dispersion, and filter through a sieve to obtain the high-air-entraining composite rheology agent product.
[0034] By adopting the above technical solution and employing a stepwise preparation and recombinant molding process, each functional active component is first synthesized separately. Specific process conditions can be matched to the reaction characteristics of each component, ensuring that the structure and performance of each component meet the standards. Then, a low-temperature pre-assembly process promotes the formation of well-ordered composite micelles between the main agent and the saponin component. Finally, the remaining components are added stepwise to complete homogenization. The entire process is seamlessly integrated, preventing the deactivation or disordered aggregation of active components during preparation, thus ensuring the uniformity of the final product's performance and storage stability.
[0035] Preferably, in step S1, the molar ratio of acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate is 5.8–6.2:1.8–2.2:0.8–1.2:2.8–3.2; the amount of RAFT reagent added is 0.8%–1.2% of the total monomer mass; the amount of azobisisobutyronitrile added is 0.2%–0.4% of the total monomer mass; the nitrogen gas introduction time is 15–25 min; the polymerization temperature is 75–80 °C; the polymerization time is 4–5 h; and the pH value of the neutralized system is 6–7.
[0036] By adopting the above technical solutions, adjusting the monomer ratio can precisely control the proportion of hydrophobic and hydrophilic segments in the copolymer molecules, so that the dispersion and gas entrainment functions can be matched and balanced; adjusting the addition ratio of chain transfer agent and initiator can control the molecular weight and distribution width of polymer, and improve the performance stability of different batches of products; sufficient nitrogen replacement can fully remove oxygen in the reaction system, eliminate the inhibitory effect of oxygen molecules on free radical polymerization, and ensure that the polymerization reaction proceeds smoothly.
[0037] Preferably, in step S2, the mass fraction of the natural saponin aqueous solution is 13%–17%, the pH value of the system after adjustment is 4.6–5.0, the enzymatic hydrolysis temperature is 48–52°C, the enzymatic hydrolysis time is 2.5–3.5 h, and the inactivation temperature is 85–95°C; the reaction temperature of the hydroxyethylation modification is 65–75°C, the reaction pressure is 0.2–0.3 MPa, and the amount of ethylene oxide added is 15%–25% of the mass of the natural saponin.
[0038] By adopting the above technical solutions, the pH and temperature of the enzymatic hydrolysis system can be controlled within a suitable range, ensuring that the composite cellulase is in an optimal active state, achieving directional skewing of saponin sugar chains without destroying the saponin core structure; temperature inactivation can completely terminate the enzymatic hydrolysis reaction, avoiding residual enzyme activity in subsequent processes that could affect product performance; the hydroxyethylation reaction is carried out under appropriate temperature and pressure conditions, ensuring the ring-opening grafting efficiency of ethylene oxide and effectively improving the alkali resistance and interfacial stability of saponin molecules.
[0039] Preferably, in step S3, the halloysite suspension has a mass fraction of 8%–12%, the amount of hexadecyltrimethylammonium bromide added is 8%–12% of the mass of the halloysite nanotubes, the intercalation reaction temperature is 75–85°C, the ultrasonic stirring time is 1.5–2.5 h, the absolute pressure of the negative pressure environment is 0.03–0.05 MPa, the impregnation time is 33–42 min, the low-temperature drying temperature is 35–45°C, and the surface light sealing is performed using a silica sol solution with a silica sol mass fraction of 2%–4% for a treatment time of 10–15 min.
[0040] By adopting the above technical solutions and controlling the concentration of the suspension and the ratio of the modifier, the organic intercalation reaction can be fully carried out, and the surface of the nanotube and the inner wall of the pore can be hydrophobically modified. Impregnation under negative pressure can use the pressure difference to expel the residual air inside the nanotube, promote the full entry of alkyl glycosides into the hollow pores, and improve the uniformity of loading. The silica sol light sealing can form a thin barrier layer at the pore opening, delay the release rate of alkyl glycosides, and will not damage the loaded active material.
[0041] The negative pressure environment can expel residual air from the hollow channels of halloysite nanotubes, allowing the pressure difference to drive the alkyl glycoside solution to fully enter the cavity. Tests showed that under the same conditions, the loading rate of alkyl glycosides impregnated at normal pressure was only 8.2%, far lower than the 17.5% of impregnated under negative pressure, proving that the negative pressure process can significantly improve loading efficiency and uniformity. Mild pore sealing with silica sol can form an ultra-thin silica barrier layer at the pore openings, slowing down the release rate of alkyl glycosides during hydration, extending the foam stabilization time, and without completely blocking the pores and preventing the release of active materials.
[0042] The preferred silica sol modulus is 3.2–3.5, and the pH of the sealing solution is controlled at 9–10. After sealing, the specific surface area of halloysite nanotube pores decreases by 12%–18%, and the median pore size shrinks from 25 nm to 18 nm while maintaining a mesoporous structure. Alkyl glycosides can be continuously released within 24 hours of hydration. Thermogravimetric-differential scanning calorimetry (TGC) tests show that the cumulative release rate of alkyl glycosides in the silica sol-sealed samples in the hydration simulation solution is 65%–75% after 24 hours, while that of the unsealed samples reaches over 90% after 4 hours.
[0043] Preferably, in step S4, the temperature of the system after adjustment is 10-15°C, the speed of the low-speed stirring is 80-120 r / min, the stirring time is 25-30 min, the system is kept away from light and a trace amount of nitrogen is continuously introduced during the stirring process, and the average particle size of the composite micelles after pre-assembly is 120-180 nm.
[0044] In step S5, the stirring time at room temperature is 18-22 min, the high-speed dispersion rate is 800-1200 r / min, the high-speed dispersion time is 25-35 min, the filtration uses a 90-110 mesh sieve, and the pH value of the final product is controlled at 6.5-7.5.
[0045] By adopting the above technical solution, low-speed stirring under low-temperature conditions can reduce the intensity of molecular thermal motion, promoting the orderly aggregation of fluorinated copolymers and saponin molecules through hydrophobic association and hydrogen bonding to form a composite micelle structure with uniform size. Light protection and trace nitrogen protection can prevent the active components from oxidative degradation and ensure the stability of the micelle structure. The regular composite micelles can improve the size uniformity of subsequent gas-inducing bubbles and reduce the phenomenon of large bubbles and bubble coalescence.
[0046] First, the soluble functional components are stirred and mixed to form a homogeneous liquid system. Then, the nano-components are added. Using a stepped stirring rate from low to high reduces direct contact between nanoparticles and the formation of hard agglomerates. Simultaneously, shearing action breaks up soft agglomerates, ensuring uniform dispersion throughout the system. Filtering through a sieve of appropriate size removes residual trace agglomerates and insoluble impurities, improving the uniformity of the finished product's appearance and its stability in use. Maintaining the pH of the finished product within the neutral range accommodates the chemical stability requirements of each functional component, reducing the risk of active substance degradation and structural damage, and extending the product's shelf life.
[0047] Thirdly, this application provides an application of a high air-entraining composite rheology modifier for wet-sprayed concrete, employing the following technical solution:
[0048] A high-air-entraining composite rheology modifier for wet-sprayed concrete, applicable to wet-sprayed concrete in tunnels, mine roadways, foundation pit slopes, underground water conservancy caverns, or civil defense projects.
[0049] By adopting the above technical solution, the composite rheology modifier can simultaneously impart stable air content and suitable rheological properties to wet-sprayed concrete, effectively reducing the rebound rate of the spray and meeting the construction needs of tunnel support, slope reinforcement and other projects.
[0050] In summary, this application has the following beneficial effects:
[0051] 1. Since this application adopts a composite system of bifunctional dispersing and air-entraining main agent combined with enzyme-modified saponin air-entraining and foam-stabilizing components and supported nano-rheology-enhancing components, the main agent single molecule has both dispersing rheology regulation and air-entraining capabilities, which can reduce the competitive adsorption and functional antagonism between different functional components, thus achieving the effect of simultaneously improving the air content and rheological stability of fresh concrete.
[0052] 2. In this application, organic intercalated halloysite nanotubes with alkyl glycosides loaded in the pores are preferably used as the rheology enhancement component. Since the hollow pores of the nanotubes can store active components and release them slowly during the hydration process, and the nanoparticles can overlap to form a physical cross-linking network, the effect of long-term foam stabilization and shear thinning rheology regulation is achieved.
[0053] 3. In this application, a temperature-sensitive polyetheramine with a cloud point temperature matching the heating range of cement hydration is preferred. Since this component is completely soluble at room temperature and does not interfere with the initial pumping fluidity, it undergoes hydrophobic association after heating to form a secondary cross-linked structure, thereby achieving the effect of balancing pumping resistance and rebound control requirements after spraying.
[0054] 4. The method of this application, by setting a low-temperature pre-assembly process before compounding and homogenization, promotes the formation of structurally uniform composite micelles between the main agent and saponin component under light-proof and low-speed stirring conditions, optimizes the molecular arrangement at the interface, and thus achieves the effect of improving the uniformity of bubble size and the storage stability of the system. Attached Figure Description
[0055] Figure 1 This is a flowchart of a method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete, provided in this application;
[0056] Figure 2 This is a bar chart comparing the air content and time loss test results of freshly mixed concrete in the various embodiments and comparative examples provided in this application;
[0057] Figure 3 This is a bar chart comparing the test results of the rheological properties of freshly mixed concrete in the various embodiments provided in this application with those in the comparative examples;
[0058] Figure 4 This is a bar chart comparing the rebound rate test results of wet sprayed concrete in the various embodiments and comparative examples provided in this application. Detailed Implementation
[0059] The present application will be further described in detail below with reference to embodiments and comparative examples. Unless otherwise specified, the experimental methods used below are conventional methods. Unless otherwise specified, the materials, reagents, methods and instruments used are all conventional materials, reagents, methods and instruments in the art, which can be obtained by those skilled in the art through commercial channels or prepared according to literature methods.
[0060] Technical concept: Current wet sprayed concrete construction has high requirements for the pumping rheological properties of slurry and the stability of air bubbles. Conventional composite rheology modifiers are mostly made by physical mixing of polycarboxylate superplasticizers, small molecule air-entraining agents and organic thickening components. Various functional components exist in the system in the form of independent molecules, which are prone to competitive adsorption on the surface of cement particles. The air-entraining components occupy the dispersion sites, which weakens the flow properties of the slurry. The rheology modifiers are also prone to destroying the air bubble liquid film structure, which leads to the aggravated loss of air content over time. Overall, it is difficult to achieve both stable high air content and excellent rheological properties, and cannot fully meet the needs of wet spraying construction under complex working conditions.
[0061] This technical solution addresses the issue from three dimensions: molecular functional integration, nanocarrier modification, and synergistic process control. First, it prepares a bifunctional fluorinated polycarboxylic acid block copolymer that combines dispersion and gas entrainment, reducing the number of independent functional components and the risk of competitive adsorption. Second, it modifies halloysite nanotubes through organic intercalation, negative pressure loading, and mild pore sealing to encapsulate alkyl glycosides within the tubes for sustained release, simultaneously contributing to rheological network construction and long-term foam stabilization. Third, it combines thermosensitive polyetheramine to achieve temporal rheological control during the pumping and spraying stages, and uses a low-temperature pre-assembly process to promote the formation of well-defined composite micelles between the main agent and modified saponins. Through the synergistic use of multiple technologies, the system's gas content stability and rheological adaptability are simultaneously improved.
[0062] Microstructural characterization of raw materials was compared using gel permeation chromatography: the weight-average molecular weight of the bifunctional fluorinated polycarboxylic acid block copolymer in this application was 26,000–30,000, with a molecular weight distribution index of 1.25–1.32; the weight-average molecular weight of commercially available ordinary polycarboxylic acid water-reducing agent was approximately 15,000, with a distribution index >2.0. X-ray diffraction analysis showed that the interplanar spacing of the unmodified halloysite ore 001 was 0.72 nm, which increased to 1.35–1.42 nm after organic intercalation with hexadecyltrimethylammonium bromide in this application. Thermogravimetric analysis revealed that the alkyl glycoside loading in the organically intercalated halloysite nanotubes with pores was 15%–20%, significantly higher than the 8.2% in samples impregnated under normal pressure. ¹H NMR confirmed that the enzymatic hydrolysis of hydroxyethylated saponins retained the triterpenoid core structure, with a saponin retention rate ≥92%.
[0063] Hydration temperature rise-cloud point matching verification: Under the benchmark concrete mix proportion, after adding the rheology modifier from Example 1, the temperature change curve at the center of the slurry was recorded using a semi-adiabatic temperature rise test device. The test showed that the initial temperature of the slurry was 20℃, and the temperature rose to 35℃ 15-20 minutes after mixing, at which point the concrete had been pumped and spraying had begun; the temperature reached a peak of 42-45℃ 30-40 minutes after mixing, and the temperature-sensitive polyetheramine completed the hydrophobic association transformation in the 35-40℃ range. The hydration temperature rise curve closely matched the cloud point range, ensuring that the cohesiveness was promptly improved after spraying onto the sprayed surface.
[0064] Preparation example: The preparation method of thermosensitive polyetheramine is as follows:
[0065] The preparation process parameters for thermosensitive polyetheramine can be adjusted within the following ranges: the molecular weight of the double-terminated amino polyoxypropylene raw material can be selected within the range of 400–2000; the ethylene oxide feed rate is 120%–200% of the polyoxypropylene mass; the amount of potassium hydroxide catalyst is 0.3%–0.8% of the total raw material mass; the molecular distillation temperature is 130–140℃; and the absolute pressure is 0.01–0.03 MPa. By adjusting the ethylene oxide feed rate and block ratio, the cloud point can be controlled within 35–40℃ to precisely match the hydration temperature rise range of wet-sprayed concrete.
[0066] By mass, 100 parts of double-amino-terminated polyoxypropylene raw material with a molecular weight of 600 were added to a closed high-pressure reactor, and 0.5 parts of potassium hydroxide solid were added simultaneously as an epoxy addition catalyst. The reactor was purged three times with nitrogen gas to remove all air. The system was heated to 110°C, and 160 parts of ethylene oxide monomer were slowly introduced in multiple stages to carry out block addition polymerization. The reaction was carried out at a constant temperature for 6 hours. After polymerization, the temperature was lowered to 70°C, and 0.6 parts of glacial acetic acid were added in stages to stir and neutralize until the pH of the overall system reached 7 and was neutral. The negative pressure system was turned on to remove residual small molecule impurities of epoxy in the reactor. After natural cooling, crude polyether material was obtained. All crude product was sent to a molecular distillation apparatus and distilled at a constant temperature of 135°C and an absolute pressure of 0.02 MPa for 4 hours to separate and remove low molecular weight polyether fragment impurities. After distillation, the finished product, temperature-sensitive polyetheramine, was obtained. The finished product has a mass ratio of 3.2 parts to 6.8 parts of hydrophilic polyoxyethylene segments and hydrophobic polyoxypropylene segments. It can be completely dissolved in deionized water at room temperature (20 to 25°C), and the turbidity point of the aqueous solution is stable in the range of 35 to 40°C.
[0067] The obtained thermosensitive polyetheramine was tested by GPC and found to have a weight-average molecular weight of 1450–1650. The mass ratio of polyoxyethylene (PEO) to polyoxypropylene (PPO) segments was characterized by ¹H NMR and found to be 3.2:6.8. The turbidity point was determined by the 1wt% aqueous solution heating method, with the temperature at which the solution just became turbid being taken as the turbidity point, and the test value was 35–40℃.
[0068] Example 1: This example provides a high air-entraining composite rheology modifier for wet sprayed concrete, which contains the following components by weight: 40 parts of bifunctional dispersing air-entraining agent, 15 parts of enzyme-modified saponin air-entraining and foam-stabilizing component, 10 parts of supported nano-rheology reinforcing component, 2.5 parts of thermosensitive polyetheramine, 4 parts of sodium gluconate, and deionized water to make up to 100 parts by weight.
[0069] Among them, the supported nano-rheology enhancement component is a channel-loaded alkyl glycoside organic intercalated halloysite nanotube, and the loading of alkyl glycoside is 17.5% of the mass of halloysite nanotube; the alkyl glycoside is selected as a low carbon alkyl glycoside with a carbon chain length of 8 to 10, and the molecular size is matched with the inner diameter of the hollow pores of halloysite, resulting in better loading uniformity.
[0070] Among them, the enzyme-modified saponin aeration and foam stabilizing component is an enzymatically modified triterpenoid saponin derivative, which is prepared by enzymatic hydrolysis of natural saponins by composite cellulase followed by hydroxyethylation. The thermosensitive polyetheramine is a polyoxyethylene-polyoxypropylene block copolyetheramine prepared in the preparation example, with a cloud point temperature of 37.5℃ and can be completely dissolved in the aqueous phase system at room temperature of 20-25℃.
[0071] Among them, the bifunctional dispersing and air-entraining agent is a bifunctional fluorinated polycarboxylic acid block copolymer, which is prepared by RAFT polymerization of acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate and methoxy polyethylene glycol acrylate, with a solid content of 40%. The block structure can realize the orderly arrangement of fluorinated hydrophobic segments and polyether hydrophilic segments, and the performance fluctuation is smaller compared with random copolymer products.
[0072] The preparation method of the above-mentioned high air-entraining composite rheology modifier for wet-sprayed concrete includes the following steps:
[0073] S1. Copolymerization: Acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate are added to a reactor, along with benzyl dithiobenzoate RAFT reagent and azobisisobutyronitrile initiator. Nitrogen gas is introduced to purge air from the reactor, and the temperature is raised and maintained for polymerization. After the reaction is completed, the solution is neutralized to the set pH value with sodium hydroxide solution to obtain a bifunctional fluorinated polycarboxylic acid block copolymer solution.
[0074] The four monomers were used in a molar ratio of 6:2:1:3. The RAFT reagent was added at 1% of the total monomer mass, and the azobisisobutyronitrile was added at 0.3% of the total monomer mass. Nitrogen gas was continuously introduced for 20 minutes to completely replace the oxygen in the reactor. The polymerization temperature was kept constant at 77.5℃ for 4.5 hours. After neutralization, the pH of the system was stable at 6.5. The sodium hydroxide used for neutralization was a 10% aqueous solution. The stirring speed was 200 r / min and the stirring time was 15 minutes. Nitrogen gas was introduced from the bottom of the reactor by bubbling to effectively remove residual oxygen in the dead corners of the reactor and prevent premature deactivation of the initiator.
[0075] The obtained copolymers were tested by gel permeation chromatography (GPC), and the weight-average molecular weight (Mw) was 26,000–30,000, and the molecular weight distribution index (PDI) was 1.25–1.32. The fluorine grafting rate was tested by X-ray photoelectron spectroscopy (XPS), and the monomer conversion rate was determined to be ≥95% by bromination method.
[0076] S2. Saponin enzymatic hydrolysis modification: Natural saponins are prepared into an aqueous solution, compound cellulase is added, the pH of the system is adjusted, and then the temperature is raised to a constant temperature for enzymatic hydrolysis. Subsequently, the enzyme preparation is inactivated by raising the temperature. Then, ethylene oxide is added for hydroxyethylation modification. After the reaction is completed, the product is purified and spray-dried to obtain enzymatically modified triterpenoid saponin derivatives.
[0077] The system comprises 15% natural saponins in aqueous solution, with the pH adjusted to 4.8 before enzymatic hydrolysis. The composite cellulase is a 1:1 mixture of endoglucanase and exoglucanase, which can directionally cleave saponin sugar chains and optimize molecular surface activity. Enzymatic hydrolysis is carried out at a constant temperature of 50℃ for 3 hours, followed by inactivation at 90℃ for 20 minutes. The hydroxyethylation reaction is carried out at 70℃ and 0.25MPa, with ethylene oxide added at 20% of the natural saponins' mass. Purification involves washing three times with pure water, and spray drying is performed at an inlet temperature of 160℃ and an outlet temperature of 70℃. Hydroxyethylation modification can improve the alkali resistance of saponin molecules, making them suitable for the strongly alkaline slurry environment after cement hydration. Spray drying uses centrifugal atomization, resulting in uniform powder particle size and faster dispersion in subsequent compounding.
[0078] Before the hydroxyethylation reaction, 0.3% by weight of potassium hydroxide of natural saponins was added as a catalyst; the obtained enzymatically modified triterpenoid saponin derivatives were tested by a laser particle size analyzer, and the average particle size of the spray-dried powder was 20-30 μm; the saponin retention rate was determined by high performance liquid chromatography to be ≥92%.
[0079] S3. Halloysite Modification and Loading: Halloysite nanotubes were dispersed in deionized water to prepare a suspension, hexadecyltrimethylammonium bromide was added, and the mixture was heated and ultrasonically stirred. The product was centrifuged, washed, and dried to obtain organically intercalated halloysite nanotubes. Low-carbon chain alkyl glycosides were mixed with anhydrous ethanol to prepare an impregnation solution, which was then added to the organically intercalated halloysite nanotubes. After impregnation under negative pressure, the nanotubes were centrifuged, dried at low temperature, and subjected to light surface sealing treatment to obtain pore-loaded alkyl glycoside organically intercalated halloysite nanotubes.
[0080] The process involved a halloysite suspension with a mass fraction of 10%, and cetyltrimethylammonium bromide with a mass fraction of 10% of the halloysite. The intercalation reaction was carried out at a constant temperature of 80℃, followed by ultrasonic stirring for 2 hours at a power of 300W. The mixture was centrifuged at 4000 r / min, washed three times with pure water, and pre-dried in an oven at 60℃. The impregnation solution consisted of anhydrous ethanol to alkyl groups at a mass ratio of 5:1, with an absolute negative pressure of 0.04 MPa, and impregnated for 37.5 minutes. The mixture was then dried at low temperature at 40℃, and a silica sol sealing solution with a mass fraction of 3% was used for 12.5 minutes of soaking. Cetyltrimethylammonium bromide modifies the surface and pore walls of halloysite, enhancing the loading affinity of alkyl glycosides. Negative pressure impregnation removes air from the tube, ensuring loading depth and uniformity.
[0081] The organically intercalated halloysite was tested by XRD, and the interlayer spacing of the 001 crystal plane increased from 0.72 nm in the original ore to 1.35–1.42 nm. The pore volume was tested by BET method and found to be 0.16–0.19 cm³ / g, with an average pore size of 20–25 nm. The alkyl glycoside loading was determined by thermogravimetric analysis (TG) under a nitrogen atmosphere at 800 °C, and the loading rate was calculated by the weight loss difference between the intercalated and loaded samples.
[0082] S4. Low-temperature pre-assembly: The bifunctional fluorinated polycarboxylic acid block copolymer solution and the enzymatically modified triterpenoid saponin derivative are added to the premixing tank according to the formula ratio. After adjusting the system temperature, the mixture is stirred at a low speed to form composite micelles and obtain the pre-assembled mixture.
[0083] The system was kept at a constant temperature of 12.5℃, with a low stirring speed of 100r / min and a stirring time of 27.5min. The entire process was conducted in the dark with continuous protection from trace amounts of nitrogen. The average particle size of the composite micelles was 150nm, and the liquid level in the stirred tank was controlled at 70%. The low temperature and dark conditions can inhibit the disordered aggregation and growth of micelles, ensure uniform micelle size, and improve the uniformity of bubble distribution in subsequent gas induction.
[0084] S5. Composite homogenization preparation: Add the formulated amount of thermosensitive polyetheramine and sodium gluconate to the pre-assembled mixture, and stir at room temperature until the system is uniformly dispersed; then slowly add the pore-loaded alkyl glycoside organic intercalated halloysite nanotubes, maintain high-speed dispersion, and filter through a sieve to obtain the high air-entraining composite rheology agent product;
[0085] The process involved stirring at low speed for 20 minutes at room temperature (300 rpm), followed by high-speed dispersion at 1000 rpm for 30 minutes. Filtration was performed using a 100-mesh standard sieve, and the mixture was allowed to stand for 30 minutes to defoam, resulting in a stable pH of 7.0 for the final product. The feeding sequence of first mixing at low speed and then adding the nano-components prevented nanotube aggregation and ensured the stability of the system's rheological and gas-entraining properties. The defoaming process removed large air bubbles introduced during dispersion, improving the storage stability of the final product.
[0086] Example 2: This example provides a high air-entraining composite rheology modifier for wet sprayed concrete, which contains the following components by weight: 35 parts of bifunctional dispersing air-entraining agent, 12 parts of enzyme-modified saponin air-entraining and foam-stabilizing component, 8 parts of supported nano-rheology reinforcing component, 2 parts of thermosensitive polyetheramine, 3 parts of sodium gluconate, and deionized water to make up to 100 parts by weight.
[0087] Among them, the supported nano-rheology enhancement component is a channel-loaded alkyl glycoside organic intercalated halloysite nanotube, and the loading amount of alkyl glycoside is 15% of the mass of halloysite nanotube; the alkyl glycoside is selected as a low carbon alkyl glycoside with a carbon chain length of 8 to 10, and the molecular size is matched with the inner diameter of the hollow pores of halloysite, resulting in better loading uniformity.
[0088] Among them, the enzyme-modified saponin aeration and foam stabilizing component is an enzymatically modified triterpenoid saponin derivative, which is prepared by enzymatic hydrolysis of natural saponins by composite cellulase followed by hydroxyethylation. The thermosensitive polyetheramine is a polyoxyethylene-polyoxypropylene block copolyetheramine prepared in the preparation example, with a cloud point temperature of 35℃ and can be completely dissolved in the aqueous phase system at room temperature of 20-25℃.
[0089] Among them, the bifunctional dispersing and air-entraining agent is a bifunctional fluorinated polycarboxylic acid block copolymer, which is prepared by RAFT polymerization of acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate and methoxy polyethylene glycol acrylate, with a solid content of 38%. The block structure can realize the orderly arrangement of fluorinated hydrophobic segments and polyether hydrophilic segments, and the performance fluctuation is smaller compared with random copolymer products.
[0090] The preparation method of the above-mentioned high air-entraining composite rheology modifier for wet-sprayed concrete includes the following steps:
[0091] S1. Copolymerization: Acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate are added to a reactor, along with benzyl dithiobenzoate RAFT reagent and azobisisobutyronitrile initiator. Nitrogen gas is introduced to purge air from the reactor, and the temperature is raised and maintained for polymerization. After the reaction is completed, the solution is neutralized to the set pH value with sodium hydroxide solution to obtain a bifunctional fluorinated polycarboxylic acid block copolymer solution.
[0092] The four monomers were in a molar ratio of 5.8:1.8:0.8:2.8. The RAFT reagent was added at 0.8% of the total monomer mass, and the azobisisobutyronitrile was added at 0.2% of the total monomer mass. Nitrogen was continuously introduced for 15 minutes to completely replace the oxygen in the reactor. The polymerization temperature was kept constant at 75℃ for 4 hours. After neutralization, the pH of the system was stable at 6. The sodium hydroxide used for neutralization was a 10% aqueous solution. The stirring speed was 200 r / min and the stirring time was 10 minutes. Nitrogen was introduced from the bottom of the reactor by bubbling to effectively remove residual oxygen in the dead corners of the reactor and prevent premature deactivation of the initiator.
[0093] S2. Saponin enzymatic hydrolysis modification: Natural saponins are prepared into an aqueous solution, compound cellulase is added, the pH of the system is adjusted, and then the temperature is raised to a constant temperature for enzymatic hydrolysis. Subsequently, the enzyme preparation is inactivated by raising the temperature. Then, ethylene oxide is added for hydroxyethylation modification. After the reaction is completed, the product is purified and spray-dried to obtain enzymatically modified triterpenoid saponin derivatives.
[0094] The system comprises 13% natural saponins in aqueous solution, with the pH adjusted to 4.6 before enzymatic hydrolysis. The composite cellulase is a 1:1 mixture of endoglucanase and exoglucanase, which can directionally cleave saponin sugar chains and optimize molecular surface activity. Enzymatic hydrolysis is carried out at a constant temperature of 48℃ for 2.5 hours, followed by inactivation at 85℃ for 15 minutes. The hydroxyethylation reaction is carried out at 65℃ and 0.2 MPa, with ethylene oxide added at 15% of the natural saponins' mass. Purification involves washing twice with pure water, and spray drying is performed at an inlet temperature of 150℃ and an outlet temperature of 65℃. Hydroxyethylation modification can improve the alkali resistance of saponin molecules, making them suitable for the strongly alkaline slurry environment after cement hydration. Spray drying uses centrifugal atomization, resulting in uniform powder particle size and faster dispersion in subsequent compounding.
[0095] S3. Halloysite Modification and Loading: Halloysite nanotubes were dispersed in deionized water to prepare a suspension, hexadecyltrimethylammonium bromide was added, and the mixture was heated and ultrasonically stirred. The product was centrifuged, washed, and dried to obtain organically intercalated halloysite nanotubes. Low-carbon chain alkyl glycosides were mixed with anhydrous ethanol to prepare an impregnation solution, which was then added to the organically intercalated halloysite nanotubes. After impregnation under negative pressure, the nanotubes were centrifuged, dried at low temperature, and subjected to light surface sealing treatment to obtain pore-loaded alkyl glycoside organically intercalated halloysite nanotubes.
[0096] The process involved an halloysite suspension with a mass fraction of 8%, cetyltrimethylammonium bromide added at 8% of the halloysite mass, an intercalation reaction at a constant temperature of 75℃, ultrasonic stirring for 1.5 hours at an ultrasonic power of 300W, centrifugation at 3500 r / min, washing twice with pure water, and pre-drying in an oven at 55℃. The impregnation solution had an anhydrous ethanol to alkyl mass ratio of 5:1, a negative pressure of 0.03 MPa, and impregnation for 33 minutes. Low-temperature drying was performed at 35℃, and a silica sol sealing solution with a mass fraction of 2% was used for soaking for 10 minutes. Cetyltrimethylammonium bromide can modify the surface and pore walls of halloysite, enhancing the loading affinity of alkyl glycosides. Negative pressure impregnation can remove air from the tube, ensuring loading depth and uniformity.
[0097] S4. Low-temperature pre-assembly: The bifunctional fluorinated polycarboxylic acid block copolymer solution and the enzymatically modified triterpenoid saponin derivative are added to the premixing tank according to the formula ratio. After adjusting the system temperature, the mixture is stirred at a low speed to form composite micelles and obtain the pre-assembled mixture.
[0098] The system was kept at a constant temperature of 10℃, with a low stirring speed of 80r / min and a stirring time of 25min. The entire process was conducted in the dark with continuous protection from trace amounts of nitrogen. The average particle size of the composite micelles was 120nm, and the liquid level in the stirred tank was controlled at 65%. The low temperature and dark conditions can inhibit the disordered aggregation and growth of micelles, ensure uniform micelle size, and improve the uniformity of bubble distribution in subsequent gas induction.
[0099] S5. Composite homogenization preparation: Add the formulated amount of thermosensitive polyetheramine and sodium gluconate to the pre-assembled mixture, and stir at room temperature until the system is uniformly dispersed; then slowly add the pore-loaded alkyl glycoside organic intercalated halloysite nanotubes, maintain high-speed dispersion, and filter through a sieve to obtain the high air-entraining composite rheology agent product;
[0100] The process involved 18 minutes of low-speed stirring at room temperature (250 rpm), followed by 25 minutes of high-speed dispersion at 800 rpm. Filtration was performed using a 90-mesh standard sieve, and the mixture was allowed to stand for 20 minutes to defoam, resulting in a stable pH of 6.5 for the final product. The feeding sequence of first mixing at low speed and then adding the nano-components prevented nanotube aggregation and ensured the stability of the system's rheological and gas-entraining properties. The defoaming process removed large air bubbles introduced during dispersion, improving the storage stability of the final product.
[0101] Example 3: This example provides a high air-entraining composite rheology modifier for wet sprayed concrete, which contains the following components by weight: 45 parts of bifunctional dispersing air-entraining agent, 18 parts of enzyme-modified saponin air-entraining and foam-stabilizing component, 12 parts of supported nano-rheology reinforcing component, 3 parts of thermosensitive polyetheramine, 5 parts of sodium gluconate, and deionized water to make up to 100 parts by weight.
[0102] Among them, the supported nano-rheology enhancement component is a channel-supported alkyl glycoside organic intercalated halloysite nanotube, with the alkyl glycoside loading amount being 20% of the halloysite nanotube mass; the alkyl glycoside is selected as a low-carbon alkyl glycoside with a carbon chain length of 8 to 10, and the molecular size is adapted to the inner diameter of the hollow pores of halloysite, resulting in better loading uniformity.
[0103] Among them, the enzyme-modified saponin aeration and foam stabilizing component is an enzymatically modified triterpenoid saponin derivative, which is prepared by enzymatic hydrolysis of natural saponins by composite cellulase followed by hydroxyethylation. The thermosensitive polyetheramine is a polyoxyethylene-polyoxypropylene block copolyetheramine prepared in the preparation example, with a cloud point temperature of 40℃ and can be completely dissolved in the aqueous phase system at room temperature of 20-25℃.
[0104] Among them, the bifunctional dispersing and air-entraining agent is a bifunctional fluorinated polycarboxylic acid block copolymer, which is prepared by RAFT polymerization of acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate and methoxy polyethylene glycol acrylate, with a solid content of 42%. The block structure can realize the orderly arrangement of fluorinated hydrophobic segments and polyether hydrophilic segments, and the performance fluctuation is smaller compared with random copolymer products.
[0105] The preparation method of the above-mentioned high air-entraining composite rheology modifier for wet-sprayed concrete includes the following steps:
[0106] S1. Copolymerization: Acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate are added to a reactor, along with benzyl dithiobenzoate RAFT reagent and azobisisobutyronitrile initiator. Nitrogen gas is introduced to purge air from the reactor, and the temperature is raised and maintained for polymerization. After the reaction is completed, the solution is neutralized to the set pH value with sodium hydroxide solution to obtain a bifunctional fluorinated polycarboxylic acid block copolymer solution.
[0107] The molar ratio of the four monomers was 6.2:2.2:1.2:3.2. The amount of RAFT reagent added was 1.2% of the total monomer mass, and the amount of azobisisobutyronitrile added was 0.4% of the total monomer mass. Nitrogen gas was continuously introduced for 25 minutes to completely replace the oxygen in the reactor. The polymerization temperature was kept constant at 80℃ for 5 hours. After neutralization, the pH of the system was stable at 7. The sodium hydroxide used for neutralization was a 10% aqueous solution. The stirring speed for neutralization was 200 r / min, and the stirring time was 20 minutes. Nitrogen gas was introduced from the bottom of the reactor by bubbling, which could effectively remove residual oxygen in the dead corners of the reactor and avoid premature deactivation of the initiator.
[0108] S2. Saponin enzymatic hydrolysis modification: Natural saponins are prepared into an aqueous solution, compound cellulase is added, the pH of the system is adjusted, and then the temperature is raised to a constant temperature for enzymatic hydrolysis. Subsequently, the enzyme preparation is inactivated by raising the temperature. Then, ethylene oxide is added for hydroxyethylation modification. After the reaction is completed, the product is purified and spray-dried to obtain enzymatically modified triterpenoid saponin derivatives.
[0109] The system comprises 17% natural saponins in aqueous solution, with the pH adjusted to 5.0 before enzymatic hydrolysis. The composite cellulase is a 1:1 mixture of endoglucanase and exoglucanase, which can directionally cleave saponin sugar chains and optimize molecular surface activity. Enzymatic hydrolysis is carried out at a constant temperature of 52℃ for 3.5 hours, followed by inactivation at 95℃ for 25 minutes. The hydroxyethylation reaction is carried out at 75℃ and 0.3MPa, with ethylene oxide added at 25% of the natural saponins' mass. Purification involves washing with pure water four times, and spray drying is performed at an inlet temperature of 170℃ and an outlet temperature of 75℃. Hydroxyethylation modification can improve the alkali resistance of saponin molecules, making them suitable for the strongly alkaline slurry environment after cement hydration. Spray drying is performed using centrifugal atomization, resulting in uniform powder particle size and faster dispersion in subsequent compounding.
[0110] S3. Halloysite Modification and Loading: Halloysite nanotubes were dispersed in deionized water to prepare a suspension, hexadecyltrimethylammonium bromide was added, and the mixture was heated and ultrasonically stirred. The product was centrifuged, washed, and dried to obtain organically intercalated halloysite nanotubes. Low-carbon chain alkyl glycosides were mixed with anhydrous ethanol to prepare an impregnation solution, which was then added to the organically intercalated halloysite nanotubes. After impregnation under negative pressure, the nanotubes were centrifuged, dried at low temperature, and subjected to light surface sealing treatment to obtain pore-loaded alkyl glycoside organically intercalated halloysite nanotubes.
[0111] The halloysite suspension had a mass fraction of 12%, and the cetyltrimethylammonium bromide was added at 12% of the halloysite mass. The intercalation reaction was carried out at a constant temperature of 85℃, with ultrasonic stirring for 2.5 hours at an ultrasonic power of 300W. The centrifugation speed was 4500 r / min, and the mixture was washed four times with pure water and pre-dried in an oven at 65℃. The impregnation solution had an anhydrous ethanol to alkyl mass ratio of 5:1, a negative pressure of 0.05 MPa, and was impregnated for 42 minutes. The mixture was then dried at low temperature at 45℃, and the silica sol sealing solution had a mass fraction of 4% and was soaked for 15 minutes. The cetyltrimethylammonium bromide can modify the surface and pore walls of halloysite, improving the loading affinity of alkyl glycosides. The negative pressure impregnation can remove air from the tube, ensuring the loading depth and uniformity.
[0112] S4. Low-temperature pre-assembly: The bifunctional fluorinated polycarboxylic acid block copolymer solution and the enzymatically modified triterpenoid saponin derivative are added to the premixing tank according to the formula ratio. After adjusting the system temperature, the mixture is stirred at a low speed to form composite micelles and obtain the pre-assembled mixture.
[0113] The system was kept at a constant temperature of 15℃, with a low stirring speed of 120r / min and a stirring time of 30min. The entire process was kept in the dark and continuously protected with trace amounts of nitrogen. The average particle size of the composite micelles was 180nm, and the liquid level in the stirred tank was 75%. The low temperature and dark conditions can inhibit the disordered aggregation and growth of micelles, ensure the uniformity of micelle size, and improve the uniformity of bubble distribution in subsequent gas induction.
[0114] S5. Composite homogenization preparation: Add the formulated amount of thermosensitive polyetheramine and sodium gluconate to the pre-assembled mixture, and stir at room temperature until the system is uniformly dispersed; then slowly add the pore-loaded alkyl glycoside organic intercalated halloysite nanotubes, maintain high-speed dispersion, and filter through a sieve to obtain the high air-entraining composite rheology agent product;
[0115] The process involved stirring at low speed for 22 minutes at room temperature (350 rpm), followed by high-speed dispersion at 1200 rpm for 35 minutes. Filtration was performed using a 110-mesh standard sieve, and the mixture was allowed to stand for 40 minutes to defoam, resulting in a stable pH of 7.5 for the final product. The feeding sequence of first mixing at low speed and then adding the nano-components prevented nanotube aggregation and ensured the stability of the system's rheological and gas-entraining properties. The standing defoaming process removed large air bubbles introduced during dispersion, improving the storage stability of the final product.
[0116] Comparative Example 1: The only difference between this comparative example and Example 1 is that the bifunctional fluorinated polycarboxylic acid block copolymer is replaced with a commercially available ordinary polycarboxylic acid superplasticizer with equal solid content, and sodium dodecyl sulfonate small molecule air-entraining agent is added according to the same air-entraining effect. The total mass of the main agent remains unchanged at 40 parts, and the other components and preparation process are exactly the same as in Example 1.
[0117] Comparative Example 2: The only difference between this comparative example and Example 1 is that the pore-loaded alkyl glycoside organically intercalated halloysite nanotubes are replaced with an equal mass of halloysite nanotubes that have only undergone hexadecyltrimethylammonium bromide organic intercalation and have not been treated with alkyl glycoside loading. At the same time, an equal amount of low-carbon chain alkyl glycosides are directly added in the S5 composite homogenization step. The total mass of alkyl glycosides is exactly the same as the loading amount in Example 1. The other components and preparation process are exactly the same as in Example 1.
[0118] Comparative Example 3: The only difference between this comparative example and Example 1 is that the thermosensitive polyetheramine is replaced with an equal mass of hydroxypropyl methylcellulose conventional organic thickener, while the other components and preparation process are exactly the same as in Example 1.
[0119] Comparative Example 4: The only difference between this comparative example and Example 1 is that the S4 low-temperature pre-assembly step is omitted, and the bifunctional fluorinated polycarboxylic acid block copolymer solution and the enzymatically modified triterpenoid saponin derivative are added to the premixing tank at room temperature of 25°C and stirred at the same speed for the same duration. The remaining steps and parameters are exactly the same as in Example 1.
[0120] Comparative Example 5: This comparative example uses the conventional wet sprayed concrete composite rheology modifier formulation and preparation process in the field. The components are conventional polycarboxylate superplasticizer, rosin thermal polymer air-entraining agent, hydroxyethyl cellulose thickener, sodium gluconate and deionized water. The basic functional efficacy of each component is the same as that of Example 1. It is prepared by a room temperature physical mixing process, and the remaining test conditions are completely consistent with those of Example 1.
[0121] Comparative Example 6: Based on Example 1, the bifunctional fluorinated polycarboxylic acid block copolymer was replaced with a commercially available ordinary polycarboxylic acid superplasticizer with equal solid content and sodium dodecyl sulfonate with equal air-entraining effect. At the same time, the pore-loaded alkyl glycoside organically intercalated halloysite nanotubes were replaced with an equal mass of halloysite nanotubes that had only undergone hexadecyltrimethylammonium bromide organic intercalation and had not been treated with alkyl glycoside loading, and an equal amount of low-carbon chain alkyl glycosides was added in step S5. The remaining components and preparation process were exactly the same as in Example 1.
[0122] Comparative Example 7: Based on Example 1, the thermosensitive polyetheramine was replaced with an equal mass of hydroxypropyl methylcellulose, and the S4 low-temperature pre-assembly step was cancelled and replaced with mixing at room temperature of 25°C. The remaining components and preparation process were exactly the same as in Example 1.
[0123] Comparative Example 8: Based on Example 1, Comparative Example 2 and Comparative Example 3 were replaced, while the remaining components and preparation processes were exactly the same as in Example 1.
[0124] Comparative Example 9: Based on Example 1, Comparative Example 1 and Comparative Example 4 were replaced simultaneously, while the remaining components and preparation processes were exactly the same as in Example 1.
[0125] I. Air Content and Time-Related Air Loss Test of Freshly Mixed Concrete. This test references the standard GB / T50080-2016 "Standard for Test Methods of Performance of Ordinary Concrete Mixtures". C25 grade wet-sprayed reference concrete was prepared. The cementitious materials were P.O42.5 ordinary Portland cement and Grade II fly ash. The aggregates were medium sand with a fineness modulus of 2.7 and continuously graded crushed stone with a particle size of 5 to 16 mm. The water-cement ratio was set at 0.45, the sand ratio was set at 50%, and the rheology modulus dosage of each group was 1.0% of the total mass of cementitious materials. Rheology modulus samples from Examples 1-3 and Comparative Examples 1-9 were added respectively. After uniform mixing with a forced mixer, the initial air content was tested according to the air pressure method specified in the standard. After the test, the concrete mixture was placed in an environment with a temperature of 20℃ and a relative humidity of 95% for 2 hours, and the air content was tested again. The values of the two tests were recorded, and the air content loss rate over time was calculated.
[0126] II. Rheological Properties Testing of Freshly Mixed Concrete. This test follows the standard GB / T38143-2019 "Methods for Determination of Rheological Properties of Concrete". A benchmark concrete mix proportion identical to that used in the air content test was employed. The rheology modifier dosage for each group was 1.0% of the total mass of the cementitious materials. Rheology modifier samples from Examples 1-9 and Comparative Examples 1-5 were added, and after thorough mixing, tests were conducted using a coaxial cylindrical rheometer. The ambient temperature was controlled at 20℃, and the shear rate was measured at 10 s⁻¹. -1 With 100s -1 The plastic viscosity under the given conditions was measured, the shear thinning index of the system was calculated, and the yield stress 30 min after mixing was tested to evaluate the long-term stability of the rheological properties.
[0127] The shear thinning index is calculated based on a power-law fluid model, with the formula: τ=K⋅γ n In the formula, τ is the shear stress (Pa), K is the consistency coefficient (Pa·sⁿ), γ is the shear rate (s⁻¹), and n is the shear thinning exponent. When n < 1, the system exhibits shear thinning characteristics, and the smaller the value of n, the more significant the shear thinning characteristics. The value of n is obtained by fitting rheological data in the range of 10 to 100 s⁻¹ using the rheometer software.
[0128] III. Wet-sprayed concrete rebound rate test. The standard for this test is JGJ / T372-2016 "Technical Specification for Application of Shotcrete". The benchmark concrete mix proportion is completely consistent with the two tests mentioned above. The rheology modifier dosage of each group is 1.0% of the total mass of cementitious materials. Rheology modifier samples of Examples 1-9 and Comparative Examples 1-5 are added respectively. The spraying test is carried out using wet spraying equipment. The sprayed surface is a standard concrete slab with vertical setting. The spraying distance is controlled at 1.0m and the spraying working pressure is controlled at 0.5MPa. The concrete material falling during the spraying process is collected throughout. The total mass of the falling material and the total mass of the sprayed material are weighed to calculate the rebound rate of each group. At the same time, the adhesion state and sagging of the sprayed surface are observed.
[0129] IV. Hardened Concrete and Storage Stability Tests: In this test, compressive strength was performed according to GB / T50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete," and freeze-thaw resistance was performed according to GB / T50082-2009 "Standard for Test Methods of Long-Term Performance and Durability of Ordinary Concrete." A reference concrete mix proportion identical to the aforementioned three tests was used. The rheology modifier dosage for each group was 1.0% of the total mass of cementitious materials. Rheology modifier samples from Examples 1-3 and Comparative Examples 1-9 were added, while Comparative Example 6 served as a blank reference group without any admixtures. After mixing and molding, the samples were transferred to a standard curing room for curing to the corresponding age. The cubic compressive strength was tested at 3d, 7d, and 28d. A rapid freezing method was used to conduct freeze-thaw cycle tests, and the relative dynamic modulus of elasticity after 300 cycles was tested to evaluate the concrete's freeze-thaw resistance grade. The storage stability test of rheology modifiers involved sealing each group of rheology modifiers in a constant temperature environment of 25°C and letting them stand for 30 days. Then, they were added to the reference concrete at the same dosage to test the initial air content and calculate the retention rate of the air content after standing relative to the initial air content of the new rheology modifier.
[0130] Table 1: Performance Test Results of High Air-Entraining Composite Rheology Modifier for Wet-Shot Concrete
[0131] Group Initial gas content / % 2h gas content / % Gas content loss over time / % 10s⁻¹ Plastic viscosity / Pa・s 100s⁻¹ Plastic viscosity / Pa・s Shear thinning index 30min yield stress / Pa Rebound rate / % Example 1 5.9 5.4 8.5 2.35 0.41 0.42 132 10.2 Example 2 5.3 4.7 11.3 2.10 0.46 0.48 118 11.9 Example 3 5.7 5.1 10.5 2.48 0.44 0.45 141 11.0 Comparative Example 1 5.6 4.0 28.6 2.05 0.72 0.68 98 18.6 Comparative Example 2 5.5 4.2 23.6 2.18 0.58 0.55 125 15.3 Comparative Example 3 5.4 4.4 18.5 3.12 1.12 0.72 168 16.8 Comparative Example 4 5.6 4.6 17.9 2.22 0.53 0.51 120 14.1 Comparative Example 5 4.8 3.5 27.1 2.88 1.05 0.75 155 22.7 Comparative Example 6 5.2 2.9 44.2 2.38 0.88 0.78 82 24.8 Comparative Example 7 4.9 2.7 44.9 3.42 1.28 0.85 192 23.5 Comparative Example 8 5.0 2.8 44.0 3.05 1.18 0.82 178 25.6 Comparative Example 9 5.3 2.6 50.9 2.45 0.95 0.80 85 26.2
[0132] Note: All groups in this test used a uniform C25 grade wet-sprayed benchmark concrete mix proportion, with a water-cement ratio of 0.45, a sand ratio of 50%, and a rheology modifier dosage of 1.0% of the total mass of cementitious materials. The test environment temperature was kept constant at 20℃. Air content testing was performed using the pneumatic method. Rheological performance testing was conducted using a coaxial cylindrical rheometer. The rebound rate test had a spraying distance controlled at 1.0m and a spraying working pressure controlled at 0.5MPa. The shear thinning index was calculated based on a power-law fluid model; a smaller value indicates more significant shear thinning characteristics and better fluidity under high-shear pumping conditions. The air content loss over time rate is the ratio of the decrease in air content after 2 hours of settling to the initial air content; a smaller value indicates stronger bubble stability.
[0133] Table 2: Test Results of Hardened Concrete and Storage Stability
[0134] Group 3d compressive strength / MPa 7d compressive strength / MPa 28-day compressive strength / MPa Relative dynamic elastic modulus after 300 freeze-thaw cycles / % Freeze resistance rating 30-day gas content retention rate (%) Example 1 16.8 24.5 32.7 91.2 F300 92.5 Example 2 17.1 24.9 33.1 88.7 F300 90.3 Example 3 16.5 24.1 32.2 90.5 F300 91.8 Comparative Example 1 15.9 22.8 30.5 72.3 F200 75.6 Comparative Example 2 16.2 23.5 31.2 76.8 F200 78.2 Comparative Example 3 16.0 23.2 30.8 74.5 F200 80.1 Comparative Example 4 16.4 23.8 31.6 82.4 F250 83.7 Comparative Example 5 15.3 22.1 29.8 68.5 F150 70.2 Comparative Example 6 15.5 22.3 29.8 65.2 F150 68.5 Comparative Example 7 15.2 21.8 29.2 63.8 F150 66.3 Comparative Example 8 15.1 21.5 29.0 62.4 F150 65.8 Comparative Example 9 15.4 22.0 29.5 64.7 F150 67.2
[0135] As can be seen from Examples 1-3 and Comparative Example 1, and Table 1, the use of a bifunctional fluorinated polycarboxylate main agent that combines dispersion and air entrainment functions can avoid competitive adsorption and functional antagonism when traditional water-reducing agents are combined with independent air entraining agents, and simultaneously improve the air entrainment efficiency and rheological stability of the system. This molecular-level integrated design is one of the core factors for improving the overall performance. This is because without the fluorinated bifunctional main agent, the small molecule air entraining agent and water-reducing agent compete for adsorption, and the anchoring effect of the fluorinated segments on the gas-liquid interface disappears, resulting in bubble coalescence and increased resilience.
[0136] As can be seen from Examples 1-3 and Comparative Example 2, and Table 1, the design of loading alkyl glycosides into the pores of halloysite nanotubes can transform nanoclay from a consumable component of air-entraining material into a long-lasting, bubble-stabilizing, slow-release carrier, while retaining the reinforcing effect of nanomaterials on the rheological network, achieving a dual positive effect of rheological regulation and bubble stabilization. This is because directly added alkyl glycosides are consumed in the initial stage of mixing and cannot stabilize bubbles for a long time; unloaded halloysite nanotubes, on the contrary, damage the bubble liquid film and aggravate the loss of gas content.
[0137] As can be seen from Examples 1-3 and Comparative Example 3, and Table 1, the use of temperature-sensitive polyetheramine with cloud point response characteristics can trigger secondary cross-linking thickening by means of the exothermic reaction of cement hydration. This ensures low viscosity flowability during the pumping stage while improving cohesiveness after spraying, thus resolving the contradiction between the pumping and rebound performance of traditional constant viscosity thickeners. Conventional thickeners increase viscosity and pumping resistance during the pumping stage, while temperature-sensitive polyetheramine only thickens in situ after hydration and heating, successfully decoupling the contradictory viscosity requirements of pumping and spraying.
[0138] As can be seen from Examples 1-3 and Comparative Example 4, and Table 1, the low-temperature pre-assembly process can promote the formation of structurally uniform composite micelles between the main agent and the saponin component through intermolecular interactions, avoiding disordered dispersion and competitive arrangement of the two types of components in the system, effectively improving the uniformity of bubble size and the long-term stability of the system, which is a key process guarantee for achieving functional synergy. Mixing at room temperature leads to random distribution of the main agent and saponin, which cannot form regular composite micelles, resulting in uneven bubble size and low liquid film strength, thus deteriorating both gas content loss and rebound rate.
[0139] As can be seen from Examples 1-3 and Comparative Example 5, and Table 1, the composite rheology modifier of this application, through multi-dimensional synergistic cooperation of molecular design, nanocarrier modification, temperature-sensitive timing regulation and exclusive preparation process, can comprehensively outperform conventional physical compound products in core performance such as air entrainment stability, rheological adaptability and rebound control, and is more suitable for the complex construction conditions of wet sprayed concrete; the components of physical compound products act independently and interfere with each other, lacking the molecular integration, nano-slow release and temperature-sensitive regulation mechanism of this application, and therefore their performance is comprehensively inferior to the synergistic system of this application.
[0140] As can be seen from Examples 1-3 and Comparative Examples 6-9, and Table 1, when two core technical features are simultaneously missing, the gas content loss rate over time surges to over 44%, and the rebound rate climbs to over 23.5%, resulting in a precipitous deterioration in performance. Compared to the comparative examples with a single missing feature, the increase in rebound rate due to the absence of two missing features is far greater than the linear sum of the effects of each individual factor, demonstrating a non-linear synergistic coupling effect between multiple technical means. The absence of any core process or structure will lead to irreversible degradation of overall performance. The combined solution of this application has produced unexpected technical effects.
[0141] As can be seen from the test results in Table 2, the composite rheology modifier of this application can improve the workability of freshly mixed grout while ensuring that the compressive strength of hardened concrete meets the design requirements. Moreover, thanks to its stable and uniform microbubble structure, it significantly improves the freeze-thaw durability of concrete, with a freeze-thaw resistance grade of F300, which is far superior to conventional products. At the same time, after 30 days of static storage, the air content retention rate of the product still remains above 90%, demonstrating excellent storage stability and meeting the needs of on-site preparation and long-term storage in engineering projects.
[0142] High-cost perfluorobutyl ethyl acrylate can reduce the amount of fluorinated monomers by 15%~20% by improving the efficiency of fluorinated block polymerization without performance degradation; the whole process can be used to build a continuous modular production line; small and medium-sized admixture plants can simplify the negative pressure impregnation process to segmented atmospheric pressure long-term impregnation and low-temperature static setting to replace nitrogen-protected light-proof pre-assembly, with low equipment investment and product performance meeting engineering standards.
[0143] The production wastewater includes halloysite washing wastewater, saponin impregnation wastewater, and enzymatic hydrolysis wastewater; clay washing wastewater is recycled after flocculation sedimentation and activated carbon adsorption; natural saponin enzymatic hydrolysis wastewater is biomass organic wastewater that can be naturally biodegraded; the finished product leachate has free fluoride ions <0.1mg / L, no heavy metals or toxic organic precipitates, and meets the GB8076-2008 environmental protection standard for admixtures; the entire production process produces no volatile toxic waste gas, meeting the requirements of green chemical production.
[0144] In addition to tunnels and slopes, it can be used for shotcrete support in mine roadways, seepage prevention spraying in water conservancy tunnels, and shotcrete in underground shelters. Multiple field applications have verified that the rebound rate is consistently below 12%, saving 35-45 kg / m³ of cementitious materials. 3 Construction efficiency is improved by more than 20%.
[0145] Engineering Application Case: A highway tunnel support project used C25 wet-mixed shotcrete with a water-cement ratio of 0.45 and a sand ratio of 50%. High-air-entraining composite rheology modifier from Example 1 of this application was added at a dosage of 1.0% of the cementitious material mass. Field test results: Concrete slump 180mm, initial air content 5.8%, 2-hour air content loss rate 9.1%, no pipe blockage at a pumping distance of 120m, average rebound rate of 10.8%, lower than the rebound rate of conventional products by more than 20%, saving approximately 40kg of cementitious material per cubic meter of concrete, improving construction efficiency by 25%, and achieving a 28-day compressive strength of 33.2MPa for hardened concrete, with a frost resistance grade of F300, meeting the long-term service requirements of the tunnel project.
[0146] The perfluorobutyl ethyl acrylate used in this application is a short-chain fluorinated monomer, which accounts for a low proportion in the copolymer, and the fluorinated segments are directionally enriched at the gas-liquid interface of the slurry. Following the method specified in GB8076-2008 "Concrete Admixtures", the leachate of hardened concrete mixed with the composite rheology modifier of Example 1 was tested for free fluoride ions. The results showed no detectable free fluoride ions (<0.1 mg / L), indicating that the fluorine element is completely sealed in the concrete matrix in the form of a stable copolymer, with no risk of precipitation. The finished product meets the environmental protection requirements of GB8076 and can be safely used in various underground engineering and water conservancy projects.
[0147] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A high air-entraining composite rheology modifier for wet-sprayed concrete, characterized in that: By weight, it consists of the following components: 35-45 parts of bifunctional dispersing and air-entraining agent, 12-18 parts of enzyme-modified saponin air-entraining and foam-stabilizing component, 8-12 parts of supported nano-rheology enhancement component, 2-3 parts of thermosensitive polyetheramine, 3-5 parts of sodium gluconate, and deionized water to make up to 100 parts by weight. The bifunctional dispersing and air-entraining agent is a bifunctional fluorinated polycarboxylic acid block copolymer, which is prepared by RAFT polymerization of acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate, and the solid content of the product is 38% to 42%. The enzyme-modified saponin aeration and foam stabilizing component is an enzymatically modified triterpenoid saponin derivative, which is obtained by enzymatic hydrolysis of natural saponins by compound cellulase followed by hydroxyethylation. The supported nanorheology enhancement component is an organically intercalated halloysite nanotube with alkyl glycosides supported in the pores, wherein the alkyl glycosides are low-carbon alkyl glycosides with a carbon chain length of 8 to 10, and the loading amount is 15% to 20% of the mass of the halloysite nanotubes; The thermosensitive polyetheramine is a polyoxyethylene-polyoxypropylene block copolymer polyetheramine with a cloud point temperature of 35-40°C and is completely soluble in an aqueous system at 20-25°C.
2. The high air-entraining composite rheology modifier for wet-sprayed concrete according to claim 1, characterized in that: In the organically intercalated halloysite nanotubes with alkyl glycosides loaded in the pores, the interlayer spacing of the 001 crystal planes of the organically intercalated halloysite nanotubes is 1.35–1.42 nm, and the loading of the alkyl glycosides is 15%–20%.
3. The high air-entraining composite rheology modifier for wet-sprayed concrete according to claim 1, characterized in that: The bifunctional fluorinated polycarboxylic acid block copolymer and the enzymatically modified triterpenoid saponin derivative form composite micelles in the system, and the average particle size of the composite micelles is 120-180 nm.
4. The high air-entraining composite rheology modifier for wet-sprayed concrete according to claim 1, characterized in that: The bifunctional fluorinated polycarboxylic acid block copolymer has a fluorine grafting rate of 3.8% to 4.5%, a weight-average molecular weight of 26,000 to 30,000, and a molecular weight distribution index of 1.25 to 1.32; the enzymatically modified triterpenoid saponin derivative has a saponin retention rate of ≥92%.
5. A method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete, characterized in that, The preparation of a high air-entraining composite rheology modifier for wet-sprayed concrete according to any one of claims 1-4 includes the following steps: S1. Copolymerization: Acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate are added to a reactor. Benzyl dithiobenzoate RAFT reagent and azobisisobutyronitrile initiator are added. Nitrogen gas is introduced to purge air from the reactor, and the temperature is raised and maintained for polymerization. After the reaction is completed, the solution is neutralized to the set pH value with sodium hydroxide solution to obtain a bifunctional fluorinated polycarboxylic acid block copolymer solution. S2. Saponin enzymatic hydrolysis modification: Natural saponins are prepared into an aqueous solution, compound cellulase is added, the pH of the system is adjusted, and then the temperature is raised to a constant temperature for enzymatic hydrolysis. Subsequently, the enzyme preparation is inactivated by raising the temperature. Then, ethylene oxide is added for hydroxyethylation modification. After the reaction is completed, the product is purified and spray-dried to obtain enzymatically modified triterpenoid saponin derivatives. S3. Halloysite Modification and Loading: Halloysite nanotubes were dispersed in deionized water to prepare a suspension, hexadecyltrimethylammonium bromide was added, and the mixture was heated and ultrasonically stirred. The product was centrifuged, washed, and dried to obtain organically intercalated halloysite nanotubes. Low-carbon chain alkyl glycosides were mixed with anhydrous ethanol to prepare an impregnation solution, which was then added to the organically intercalated halloysite nanotubes. After impregnation under negative pressure, the nanotubes were centrifuged, dried at low temperature, and subjected to light surface sealing treatment to obtain pore-loaded alkyl glycoside organically intercalated halloysite nanotubes. S4. Low-temperature pre-assembly: The bifunctional fluorinated polycarboxylic acid block copolymer solution and the enzymatically modified triterpenoid saponin derivative are added to the premixing tank according to the formula ratio. After adjusting the system temperature, the mixture is stirred at a low speed to form composite micelles and obtain the pre-assembled mixture. S5. Composite homogenization preparation: Add the formulated amount of thermosensitive polyetheramine and sodium gluconate to the pre-assembled mixture, and stir at room temperature until the system is uniformly dispersed; then slowly add the pore-loaded alkyl glycoside organic intercalated halloysite nanotubes, maintain high-speed dispersion, and filter through a sieve to obtain the high-air-entraining composite rheology agent product.
6. The method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete according to claim 5, characterized in that: In step S1, the molar ratio of acrylic acid, methyl methacrylate, perfluorobutyl ethyl acrylate, and methoxy polyethylene glycol acrylate is 5.8–6.2:1.8–2.2:0.8–1.2:2.8–3.2; the amount of RAFT reagent added is 0.8%–1.2% of the total monomer mass; the amount of azobisisobutyronitrile added is 0.2%–0.4% of the total monomer mass; the nitrogen gas is introduced for 15–25 min; the polymerization temperature is 75–80 °C; the polymerization time is 4–5 h; and the pH value of the neutralized system is 6–7.
7. The method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete according to claim 5, characterized in that: In step S2, the mass fraction of the natural saponin aqueous solution is 13%–17%, the pH value of the system after adjustment is 4.6–5.0, the enzymatic hydrolysis temperature is 48–52℃, the enzymatic hydrolysis time is 2.5–3.5 h, and the inactivation temperature is 85–95℃; the reaction temperature of the hydroxyethylation modification is 65–75℃, the reaction pressure is 0.2–0.3 MPa, and the amount of ethylene oxide added is 15%–25% of the mass of the natural saponin.
8. The method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete according to claim 5, characterized in that: In step S3, the halloysite suspension has a mass fraction of 8%–12%, the amount of hexadecyltrimethylammonium bromide added is 8%–12% of the mass of the halloysite nanotubes, the intercalation reaction temperature is 75–85℃, the ultrasonic stirring time is 1.5–2.5 h, the absolute pressure of the negative pressure environment is 0.03–0.05 MPa, the impregnation time is 33–42 min, the low-temperature drying temperature is 35–45℃, and the surface light sealing is performed using a silica sol solution with a silica sol mass fraction of 2%–4% for a treatment time of 10–15 min.
9. The method for preparing a high air-entraining composite rheology modifier for wet-sprayed concrete according to claim 5, characterized in that: In step S4, the temperature of the system after adjustment is 10-15℃, the speed of the low-speed stirring is 80-120 r / min, the stirring time is 25-30 min, the system is kept away from light and a trace amount of nitrogen is continuously introduced during the stirring process, and the average particle size of the composite micelles after pre-assembly is 120-180 nm. In step S5, the stirring time at room temperature is 18-22 min, the high-speed dispersion rate is 800-1200 r / min, the high-speed dispersion time is 25-35 min, the filtration uses a 90-110 mesh sieve, and the pH value of the final product is controlled at 6.5-7.
5.
10. An application of a high air-entraining composite rheology modifier for wet-sprayed concrete, characterized in that, The high air-entraining composite rheology modifier for wet sprayed concrete as described in any one of claims 1-4 is applied to wet sprayed concrete in tunnels, mine roadways, foundation pit slopes, underground water conservancy caverns, or civil defense projects.
Citation Information
Patent Citations
Super early strength concrete and preparation method thereof
CN112811876A
Modified cancrinite ceramsite capable of efficiently removing ammonia nitrogen and preparation method of modified cancrinite ceramsite