A fiber-reinforced acid-resistant geopolymer castable and its preparation method

By using a multi-layered protection mechanism of fiber-reinforced acid-resistant geopolymer castable, the problem of insufficient corrosion resistance of existing acid-resistant concrete in strong acid and high-temperature acid mist environments has been solved. It achieves high compressive strength, flexural strength and impact toughness, reduces construction costs and realizes the resource utilization of industrial solid waste.

CN123106080APending Publication Date: 2026-11-17NANJING ALLIED RONGDA ENG MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611364904.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing acid-resistant concrete materials have insufficient corrosion resistance in strong acid, high-temperature acid mist and acidic flowing media environments, making them prone to structural damage. Moreover, the construction process is complex and costly, making it difficult to meet the long-term safe operation requirements of industrial plants.

Method used

Fiber-reinforced acid-resistant geopolymer castable is composed of cementitious materials, activators, additives, acid-resistant aggregates, acid-resistant powders, nanoparticles, abrasives, carbonaceous raw materials, and basalt fibers. Through a three-dimensional network polyaluminosilicate gel structure and multi-level particle size distribution, it forms a multi-layer acid-resistant protection mechanism, enhancing the material's impermeability, impact toughness, and compressive strength.

Benefits of technology

It significantly improves the corrosion resistance of materials in strong acid and high-temperature acid mist environments, reduces the drying shrinkage rate and thermal expansion coefficient, reduces microcracks, achieves high compressive strength, flexural strength and impact toughness, reduces construction costs and realizes the resource utilization of industrial solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106080A_ABST
    Figure CN123106080A_ABST
Patent Text Reader

Abstract

This invention discloses a fiber-reinforced acid-resistant geopolymer castable and its preparation method, belonging to the technical field of functional building materials. The castable comprises the following raw materials in parts by weight: 52-68 parts acid-resistant aggregate, 5-12 parts acid-resistant powder, 4-11 parts abrasion-resistant material, 11-36 parts precursor powder, 2-5 parts nanoparticles, 0-0.75 parts carbonaceous raw material, 0-0.75 parts fiber-reinforcing material, 0.02-0.05 parts admixture, and 13-20 parts activator. The precursor powder is one or more of slag powder, fly ash, and metakaolin, which are excited by sodium silicate solution to generate a three-dimensional network polyaluminosilicate gel. This invention constructs a three-dimensional acid-resistant protection mechanism by using acid-resistant aggregate and powder to form a macroscopic inert skeleton, geopolymer gel to form a dense interfacial transition zone, and carbonaceous raw material to provide a hydrophobic protective barrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of castable technology, specifically to a fiber-reinforced acid-resistant geopolymer castable and its preparation method. Background Technology

[0002] Geopolymers are produced primarily from aluminosilicate materials. Under alkali activation, they undergo depolymerization and condensation to form a three-dimensional network of polyaluminosilicate gels composed of silicon-oxygen tetrahedra and aluminum-oxygen tetrahedra. The reaction process and product structure characteristics differ from ordinary silicate cement and water glass acid-resistant concrete. As a green building cementitious material, geopolymers can facilitate the disposal and resource utilization of industrial solid waste, reducing solid waste pollution. Furthermore, due to their unique structure and properties, they have enormous application potential in the field of civil engineering.

[0003] Depending on the type of cementing material, acid-resistant concrete mainly includes water glass acid-resistant concrete, resin-based acid-resistant concrete, asphalt-based acid-resistant concrete, and sulfur-based acid-resistant concrete.

[0004] Water glass acid-resistant concrete is an acid-resistant material made from water glass, a hardener, acid-resistant powder, and coarse and fine aggregates. Its hardening process relies on the silica gel formed by the reaction of water glass and the hardener, which binds the powder and aggregates together. Water glass acid-resistant concrete possesses good physical properties and chemical corrosion resistance, and can withstand most inorganic and organic acids. However, the hardener, sodium fluorosilicate, contains fluorine, which is highly toxic, and therefore cannot be used in the food industry. Due to the influence of its curing mechanism, the construction process of water glass concrete is relatively complex. Construction is more suitable when the ambient temperature is above 25℃, resulting in a shorter initial setting time and faster hardening speed. Construction is not advisable when the ambient temperature is below 10℃. Its impermeability and water resistance are relatively poor.

[0005] Furan resin acid-resistant concrete is a type of acid-resistant concrete made by mixing furan resin, furan powder, acid-resistant fine aggregate, and acid-resistant coarse aggregate in a certain proportion. It has good acid corrosion resistance, impermeability, and water resistance. However, organic materials have poor heat resistance, and the raw materials are highly toxic and expensive, which limits its use due to the limitations of construction site conditions and project costs.

[0006] Acid-resistant asphalt concrete is made by encapsulating acid-resistant powders such as quartz powder and acid-resistant aggregates with asphalt. Its raw materials are widely available, the manufacturing process is simple, and construction is convenient. However, due to its high toxicity during construction, it is generally used in open areas and requires adequate protective equipment.

[0007] Sulfur-based acid-resistant concrete uses sulfur as a binder, adding acid-resistant powder and toughening agents, then heating and boiling the mixture before pouring the semi-fluid material into a layer of coarse aggregate to form a type of concrete. This type of concrete has a dense structure, hardens quickly, has high strength, good acid resistance, is easy to construct, requires no curing, and is especially suitable for emergency repair projects.

[0008] In modern industrial sectors such as chemical, metallurgical, pharmaceutical, power, and pickling / electroplating industries, numerous production processes involve the storage, transportation, and handling of highly acidic media such as sulfuric acid, hydrochloric acid, and nitric acid. These corrosive fluids, under both normal and high-temperature conditions, cause severe chemical corrosion to metals, cement-based materials, and ordinary anti-corrosion coatings, leading to frequent problems such as equipment corrosion and perforation, concrete structure crumbling and spalling, and floor sanding and cracking. Taking the hydrometallurgical industry as an example, critical facilities such as electrolytic cells and leaching tanks are constantly exposed to acidic environments with a pH < 2. While traditional granite masonry offers some acid resistance, leaks are prone to occur at the joints; stainless steel equipment also faces the risk of pitting and stress corrosion in acidic media containing chloride ions. In the field of chemical wastewater treatment, structures such as equalization tanks and neutralization tanks must withstand both immersion in acidic wastewater and wear during mechanical cleaning processes. Statistics show that losses due to industrial shutdowns, equipment replacements, and safety accidents caused by acid corrosion amount to tens of billions of yuan annually. In addition, some high-temperature acid mist environments (such as the sulfuric acid concentration process in titanium dioxide production) place more stringent requirements on the heat resistance and acid resistance synergistic performance of materials.

[0009] Therefore, developing new building materials with excellent acid resistance, good impermeability, and resistance to erosion and wear from solid particles is of great engineering significance and economic benefit for ensuring the long-term safe operation of industrial plants, reducing maintenance costs, and achieving green manufacturing. Summary of the Invention

[0010] The purpose of this invention is to overcome the aforementioned deficiencies of the prior art and provide a fiber-reinforced acid-resistant geopolymer castable and its preparation method, so as to significantly improve the long-term acid corrosion resistance of geopolymers under the coupled environment of strong acid, high-temperature acid mist, and acidic flowing media; achieve ultra-low porosity and extremely low permeability coefficient; while ensuring excellent acid resistance, the fiber toughening forms a non-brittle failure mode, reduces the drying shrinkage rate and thermal expansion coefficient, reduces the generation of microcracks, and obtains high compressive strength, flexural strength and impact toughness to meet the requirements of load-bearing and dynamic loads; realize the high-value utilization of industrial solid waste, reduce costs and reduce carbon emissions.

[0011] This invention utilizes a mixture of cementitious materials, activators, additives, acid-resistant aggregates, acid-resistant powders, nanoparticles, abrasives, carbonaceous raw materials, and basalt fibers to create an acid-resistant geopolymer material, achieving excellent technical results. The cementitious component is primarily industrial solid waste, realizing solid waste resource utilization while conserving resources and energy, reducing carbon emissions, and promoting environmental friendliness. Furthermore, the construction process is simple and convenient. The alkaline activator used activates the potential activity of the ground industrial solid waste, forming a three-dimensional network of polyaluminosilicate gel with excellent mechanical properties, acid solution corrosion resistance, and heat resistance. The acid-resistant aggregates, acting as the material skeleton, bear the main load, effectively reducing shrinkage and improving volume stability. Their excellent acid resistance allows them to remain stable in acidic environments, preventing corrosion and structural damage. The acid-resistant powders fill the micropores between the aggregates, optimizing particle size distribution and making the material denser. Simultaneously, they participate in the geopolymerization reaction, improving the interface. Bonding strength further enhances resistance to acid penetration and corrosion; nanoparticles can significantly improve material density by utilizing nanoscale filling effect and surface activity, accelerating the dissolution and condensation reaction of silicon-aluminum raw materials in alkaline environments, refining pore structure, and improving early strength, acid resistance, and impermeability; abrasion-resistant materials are used to enhance the surface hardness and wear resistance of materials, suitable for working conditions subject to erosion and wear (such as acid flow environments), preventing premature surface deterioration, thereby maintaining long-term acid resistance; basalt fibers play a reinforcing and toughening role, utilizing their high tensile strength and acid resistance to effectively inhibit the propagation of microcracks in materials under drying shrinkage or stress, improve bending and impact resistance, and improve brittleness without sacrificing acid resistance.

[0012] Based on the above findings, the present invention provides the following technical solution:

[0013] This invention provides a fiber-reinforced acid-resistant geopolymer castable, comprising the following raw materials in parts by weight: 52-68 parts of acid-resistant aggregate, 5-12 parts of acid-resistant powder, 4-11 parts of abrasion-resistant material, 11-36 parts of precursor powder, 2-5 parts of nano-powder, 0-0.75 parts of carbonaceous raw material, 0-0.75 parts of fiber reinforcing material, 0.02-0.05 parts of additives, and 13-20 parts of activator.

[0014] In some embodiments of the present invention, the acid-resistant aggregate is one or more of fused quartz, quartzite, granite, diabase, and basalt. By weight, there are 12-18 parts of acid-resistant aggregate with a particle size of 5-3 mm, 18-25 parts of acid-resistant aggregate with a particle size of 3-1 mm, and 22-25 parts of acid-resistant aggregate with a particle size of 1-0 mm.

[0015] In some embodiments of the present invention, the acid-resistant aggregate shall meet the following technical requirements: acid resistance (by weight) not less than 98%; moisture content not greater than 0.5%; and shall not contain impurities that are not acid-resistant, such as soil, limestone, dolomite, and iron filings.

[0016] In some embodiments of the present invention, the acid-resistant powder is one or more of fused silica powder, cast stone powder, and quartz powder. By weight, 3-5 parts are acid-resistant powder with a particle size of 200 mesh, and 2-7 parts are acid-resistant powder with a particle size of 325 mesh.

[0017] In some embodiments of the present invention, the acid-resistant powder shall meet the following technical requirements: acid resistance (by weight) not less than 98%; moisture content not greater than 0.5%; and shall not contain impurities that are not acid-resistant, such as soil, limestone, dolomite, and iron filings.

[0018] In some embodiments of the present invention, the wear-resistant material is brown fused alumina. By weight, 2-5 parts of brown fused alumina with a particle size of 1-0 mm, 1-3 parts of brown fused alumina with a particle size of 200 mesh, and 1-3 parts of brown fused alumina with a particle size of 325 mesh.

[0019] In some embodiments of the present invention, the geopolymer precursor powder is selected from one or more of slag powder, fly ash, and metakaolin. By weight, the amounts are 1-10 parts slag powder, 10-20 parts fly ash, and 0-6 parts metakaolin powder.

[0020] In some embodiments of the present invention, the slag powder meets the S95 slag grade in the national standard GB / T 18046-2017 "Granulated Blast Furnace Slag Powder for Cement, Mortar and Concrete".

[0021] In some embodiments of the present invention, the fly ash meets the Class I F fly ash standard of the national standard GB / T 1596-2017 "Fly Ash for Cement and Concrete".

[0022] In some embodiments of the present invention, the metakaolin powder meets the Class I metakaolin powder requirements of the national standard GB / T 46064-2025 "Metakaolin Powder for Concrete and Mortar".

[0023] In some embodiments of the present invention, the activator is a sodium silicate solution, in which 13-20 parts by weight are used.

[0024] In some embodiments of the present invention, the sodium silicate solution shall meet the following technical requirements: the water glass modulus is 2.05 (±0.1), and the Baumé degree is 35~38.

[0025] In some embodiments of the present invention, the active micro powder is selected as active alumina micro powder or zirconium-containing silicon micro powder. By weight, 0.5-1 parts are active alumina micro powder with a particle size of 0-1 μm, 0.5-1 parts are active alumina micro powder with a particle size of 2-5 μm, and 1-3 parts are zirconium-containing silicon micro powder with a particle size of 0-1 μm.

[0026] In some embodiments of the present invention, the zirconium-containing silicon micropowder shall meet the following technical requirements: the sum of the contents of SiO2 and ZrO2 in the zirconium-containing silicon micropowder shall be ≥95%.

[0027] In some embodiments of the present invention, the carbonaceous raw material is spherical pitch and carbon black powder. By weight, 0-0.5 parts of spherical pitch with a particle size of 0-1 mm and 0-0.25 parts of N990 carbon black are used.

[0028] In some embodiments of the present invention, the fiber reinforcing material is one or more of basalt fiber, heat-treated carbon fiber, and acid-resistant glass fiber. The fiber reinforcing material with a length of 2-4 mm is 0-0.75 parts by weight. Preferably, it is 3 mm.

[0029] In some embodiments of the present invention, the admixture is a polycarboxylate-based or naphthalene-based high-efficiency water-reducing agent, with 0.02-0.05 parts by weight.

[0030] The present invention also provides a method for preparing the above-mentioned acid-resistant geopolymer castable, comprising the following steps:

[0031] S1. Weigh out the acid-resistant aggregate, acid-resistant powder, abrasive, precursor powder, nano-powder, carbonaceous raw material, fiber reinforcing material, additives and water glass solution according to the weight ratio.

[0032] S2. Dry mix the precursor powder, nano-powder, carbonaceous raw material, fiber reinforcement material and additives in a mixer for 85-95 seconds, then add water glass solution and stir for 110-130 seconds to obtain a gelling material.

[0033] S3. Add wear-resistant material, acid-resistant powder and acid-resistant aggregate to the cementitious material in sequence, stir for 120 seconds to obtain acid-resistant geopolymer castable;

[0034] S4. Pour the acid-resistant geopolymer castable into the mold to form a shape;

[0035] S5, obtained after maintenance.

[0036] In some embodiments of the present invention, the curing is either room temperature curing or high temperature steam curing; the room temperature curing is to cover the casting with a plastic film immediately after casting and keep it moist at room temperature for 26-30 days; the high temperature steam curing is to cure the casting under 75-85℃ water steam conditions for 46-50 hours 10-14 hours after casting.

[0037] The beneficial effects of this invention are as follows:

[0038] First, this invention is the first to systematically integrate a geopolymer cementitious system, an acid-resistant aggregate / powder system, and a carbonaceous hydrophobic protective system, constructing a three-dimensional acid-resistant protection mechanism of "macroscopic inert barrier – mesoscopic stable network – microscopic physical shielding." Existing research shows that geopolymers, with their unique three-dimensional network gel structure, exhibit significantly better acid resistance than ordinary silicate cement (OPC). The mechanism can be attributed to the initial low permeability forming a physical barrier, and the dense layer remaining after acid etching of the low calcium-to-silica ratio gel preventing the penetration of acidic media. This invention further strengthens this: First, the acid-resistant aggregate and acid-resistant powder (acid resistance not less than 98%) constitute a macroscopic inert skeleton, fundamentally avoiding material collapse caused by the neutralization reaction between alkaline components and acid in ordinary castables; second, the [SiO4] in the polyaluminosilicate gel... 4- [AlO4] 5- The oxygen bridges connect to form a zeolite-like three-dimensional cage-like network structure, which is stable and does not undergo significant ion leaching or structural collapse in acidic media. The gel tightly coats the aggregate surface, forming a dense interfacial transition zone, eliminating the "loose interfacial layer" common in ordinary castables and preventing acid from penetrating along the aggregate edges. Furthermore, the spherical asphalt in the carbonaceous raw material has excellent chemical stability and significant hydrophobic properties, effectively repelling the wetting and penetration of water and acidic aqueous solutions, forming a waterproof barrier within the material. The acid resistance of asphalt-based materials has been widely used in various anti-corrosion projects, exhibiting good resistance to various inorganic and organic acids. The synergistic effect of these three factors allows the castable of this invention to maintain structural integrity and mechanical properties even after long-term service in acidic media of different types and concentrations, with acid resistance significantly superior to existing similar products.

[0039] Secondly, this invention achieves a comprehensive improvement in mechanical properties through multi-component synergistic design. Firstly, fly ash, slag powder, and metakaolin, three precursor powders, are excited by a water glass solution to form a dense three-dimensional network of polyaluminosilicate gel. This gel firmly binds the aggregates and powders into a cohesive whole, filling the micron- and submicron-sized pores remaining after aggregate and powder accumulation, complementing the particle size distribution and giving the material high strength and high density. With scientific proportioning, the compressive strength of industrial solid waste precursor powders such as slag powder and fly ash can be increased by approximately 30% to 40% compared to traditional cement-based materials. Secondly, activated alumina micropowder can dissolve and release ions in the strongly alkaline environment of water glass, supplementing the active aluminum source in the system to optimize the Si / Al molar ratio of the gel. Studies have shown that by adding activated alumina micropowder to change the Si / Al ratio, the compressive strength of the geopolymer first increases and then decreases, with a significant improvement under the optimal active Si / Al ratio conditions. This promotes the formation of polyaluminosilicate gels with higher cross-linking degree and more stable structure, further improving the compressive and flexural strength of the material. Thirdly, brown fused alumina has high hardness (Mohs hardness of approximately 9) and high wear resistance. After uniform distribution, it can significantly improve the surface wear resistance of the castable and resist the erosion of acidic fluids containing solid particles. Fourthly, basalt fiber, heat-treated carbon fiber, and acid-resistant glass fiber, through three-dimensional random distribution, form a bridging effect when microcracks occur, preventing crack propagation and improving the flexural strength, impact toughness, and fracture energy of the material. The combined effect of these components gives the castable of this invention excellent mechanical properties of high strength, high wear resistance, and high toughness.

[0040] Third, this invention follows modern particle close packing theory, establishing a multi-level particle size distribution system from millimeter-scale aggregates to submicron-scale active micropowders. In this invention, acid-resistant aggregates are distributed in three grades: 5-3mm, 3-1mm, and 1-0mm; acid-resistant powders are distributed in two grades: 200 mesh and 325 mesh; brown corundum is distributed in three grades: 1-0mm, 200 mesh, and 325 mesh; activated alumina micropowders are distributed in two grades: 0-1μm and 2-5μm; zirconium-containing silicon micropowder is in the 0-1μm grade; and carbon black N990 further fills the submicron-scale pores, forming a multi-scale continuous dense packing from millimeters to submicrons. The spherical particle morphology of the zirconium-containing silicon micropowder improves the flowability of the powder packing, and its ultrafine particle size and high chemical inertness of ZrO2 can fill nanoscale pores, improving the interfacial transition zone. Carbon black, with its ultrafine particle size, fully fills the submicron-scale pores, further reducing the material's porosity. The multi-stage particle size distribution enables the castable of this invention to achieve extremely low porosity and permeability, effectively blocking the penetration channels of acid, water and harmful ions, thereby greatly improving the impermeability and durability of the material.

[0041] Fourth, this invention addresses the problems of shrinkage cracks caused by moisture evaporation during the drying process and thermal stress cracking due to mismatched thermal expansion coefficients of components in ordinary castables from multiple perspectives. First, the acid-resistant aggregate and acid-resistant powder form a rigid skeleton, bearing the main load and effectively reducing the overall drying shrinkage and thermal expansion coefficient of the material. Second, the polyaluminosilicate gel tightly wraps the aggregate surface, forming a dense interfacial transition zone, eliminating the hidden danger of microcracks easily generated due to weak interfacial bonding in ordinary castables. Third, the fiber-reinforced material is three-dimensionally randomly distributed in the matrix, constraining the matrix's drying shrinkage, reducing early microcracks, and consuming energy through fiber pull-out and breakage during crack propagation, significantly improving the material's crack resistance. The three-dimensional network gel structure formed by slag powder, fly ash, and metakaolin as precursor powders possesses excellent volume stability, greatly reducing the risk of cracking during construction and use, which is beneficial for large-area casting and complex structural applications.

[0042] Fifth, this invention innovatively introduces spherical asphalt and carbon black powder as carbonaceous functional fillers, achieving multiple synergistic effects. Spherical asphalt possesses excellent chemical stability and hydrophobic properties. As a micro-filler, it is uniformly dispersed in the castable matrix, significantly reducing the capillary water absorption rate of the material and effectively repelling the wetting and penetration of water and acidic aqueous solutions. Carbon black N990, with its ultrafine particle size, fully fills submicron-level pores, reducing the porosity of the material and providing chemically inert carbonaceous protection at the microscopic level. Together with acid-resistant aggregates, acid-resistant powders, and geopolymer gels, they jointly construct a multi-level, comprehensive acid-resistant protection system from macroscopic to microscopic levels.

[0043] Sixth, this invention extensively utilizes industrial solid waste as its main raw material, resulting in significant energy conservation, emission reduction, and environmental benefits. Fly ash and slag powder are both industrial solid wastes, and their high-volume use in geopolymers can effectively utilize large quantities of solid waste. Studies show that carbon emissions during geopolymer preparation are approximately 1 / 15 to 1 / 10 of those of traditional cement, and energy consumption is approximately 1 / 6 to 1 / 4. Slag powder and fly ash are both industrial solid wastes, and their high-volume use (up to 30% or more) can not only significantly reduce the use of high-energy-consuming materials such as cement and lower carbon emissions, but also effectively reduce raw material costs. Metakaolin, as a natural mineral raw material, is widely available and inexpensive.

[0044] Seventh, this invention significantly improves the flowability of castables through the synergistic effect of polycarboxylate superplasticizer and the spherical particle morphology of reactive micropowder, enabling the material to achieve good workability with relatively low water consumption. The polycarboxylate superplasticizer effectively improves the flowability and workability of the castable, increasing the bulk density and impermeability of the material. The spherical particle morphology of zirconium silicate powder improves the flowability of powder packing, further enhancing the flowability of the castable. The synergistic effect of the polycarboxylate superplasticizer and reactive micropowder allows the castable of this invention to be applied under both vibration casting and self-leveling conditions, adapting to different engineering needs. The preparation process is simple, curing at room temperature, suitable for on-site preparation and application, reducing construction energy consumption and costs. Simultaneously, the components exhibit good compatibility, preventing agglomeration and stratification during mixing, ensuring the consistency and reliability of the castable quality. Attached Figure Description

[0045] Figure 1 A photograph of the surface morphology of the acid-resistant geopolymer castable sample block prepared in Example 1 of the present invention after being soaked in 50% sulfuric acid solution at 80°C for 3 days;

[0046] Figure 2 This is a photograph of the surface morphology of a sample block of ordinary cement-based castable prepared in Comparative Example 1 of the present invention after being soaked in 50% sulfuric acid solution at 80°C for 3 days. Detailed Implementation

[0047] The present invention will be further described in detail below with reference to embodiments and comparative examples. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in this field. Reagents or instruments used, unless otherwise specified, are all commercially available conventional reagent products.

[0048] In the various embodiments and comparative examples, acid-resistant geopolymer castables were prepared according to the following method: acid-resistant aggregates, acid-resistant powders, abrasive materials, precursor powders, nanoparticles, carbonaceous raw materials, fiber reinforcing materials, additives, and water glass solution were weighed according to the weight ratio; the precursor powders, nanoparticles, carbonaceous raw materials, fiber reinforcing materials, and additives were dry-mixed in a mixer for 90 seconds, and then water glass solution was added and stirred for 120 seconds to obtain cementitious material 1; the weighed abrasive materials, acid-resistant powders, and acid-resistant aggregates were added to cementitious material 1 in sequence and stirred for 120 seconds; the acid-resistant geopolymer castable was poured into a mold for molding; the curing method was room temperature curing (immediately after casting, the mold was covered with a plastic film and kept moist at room temperature for 28 days).

[0049] Example 1

[0050] Weigh each raw material according to the following proportions by weight:

[0051] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0052] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0053] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0054] Precursor powder: 1 part slag powder; 20 parts fly ash.

[0055] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0056] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0057] Water-reducing agent: 0.05 parts of FDN-A.

[0058] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0059] After molding and curing according to the above preparation method, the mechanical properties and acid resistance of the castable are tested.

[0060] Example 2

[0061] Weigh each raw material according to the following proportions by weight:

[0062] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0063] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0064] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0065] Precursor powder: 6 parts slag powder; 15 parts fly ash.

[0066] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0067] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0068] Water-reducing agent: 0.05 parts of FDN-A.

[0069] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0070] After molding and curing according to the above preparation method, the mechanical properties and acid resistance of the castable are tested.

[0071] Example 3

[0072] Weigh each raw material according to the following proportions by weight:

[0073] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0074] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0075] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0076] Precursor powder: 11 parts slag powder; 10 parts fly ash.

[0077] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0078] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0079] Water-reducing agent: 0.05 parts of FDN-A.

[0080] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0081] After molding and curing according to the above preparation method, the mechanical properties and acid resistance of the castable are tested.

[0082] Example 4

[0083] Weigh each raw material according to the following proportions by weight:

[0084] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0085] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0086] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0087] Precursor powder: 1 part slag powder; 20 parts fly ash.

[0088] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0089] Carbonaceous raw materials: 0.5 parts of spherical pitch (0-1mm); 0.25 parts of carbon black N990.

[0090] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0091] Water-reducing agent: 0.05 parts of FDN-A.

[0092] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0093] After molding and curing according to the above preparation method, the mechanical properties and acid resistance of the castable are tested.

[0094] Example 5

[0095] Weigh each raw material according to the following proportions by weight:

[0096] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0097] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0098] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0099] Precursor powder: 6 parts slag powder; 15 parts fly ash.

[0100] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0101] Carbonaceous raw materials: 0.5 parts of spherical pitch (0-1mm); 0.25 parts of carbon black N990.

[0102] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0103] Water-reducing agent: 0.05 parts of FDN-A.

[0104] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0105] After molding and curing according to the above preparation method, the mechanical properties and acid resistance of the castable are tested.

[0106] Example 6

[0107] Weigh each raw material according to the following proportions by weight:

[0108] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0109] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0110] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0111] Precursor powder: 11 parts slag powder; 10 parts fly ash.

[0112] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0113] Carbonaceous raw materials: 0.5 parts of spherical pitch (0-1mm); 0.25 parts of carbon black N990.

[0114] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0115] Water-reducing agent: 0.05 parts of FDN-A.

[0116] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0117] After molding and curing according to the above preparation method, the mechanical properties and acid resistance of the castable are tested.

[0118] Example 7

[0119] Weigh each raw material according to the following proportions by weight:

[0120] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0121] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0122] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0123] Precursor powder: 1 part slag powder; 14 parts fly ash; 6 parts metakaolin.

[0124] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0125] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0126] Water-reducing agent: 0.05 parts of FDN-A.

[0127] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0128] The acid-resistant geopolymer castable was poured into a mold and shaped; the curing method was adjusted to high-temperature steam curing (cured for 48 hours under 80℃ water steam conditions 12 hours after casting). After curing, the mechanical properties and acid resistance of the castable were tested.

[0129] Example 8

[0130] Weigh each raw material according to the following proportions by weight:

[0131] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0132] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0133] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0134] Precursor powder: 6 parts slag powder; 10.5 parts fly ash; 4.5 parts metakaolin.

[0135] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0136] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0137] Water-reducing agent: 0.05 parts of FDN-A.

[0138] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0139] Acid-resistant geopolymer castable was poured into a mold and shaped; the curing method was high-temperature steam curing (cured for 48 hours under 80℃ water steam conditions 12 hours after casting). After curing, the mechanical properties and acid resistance of the castable were tested.

[0140] Example 9

[0141] Weigh each raw material according to the following proportions by weight:

[0142] Acid-resistant aggregates: 15 parts of fused silica, 5-3 mm; 23 parts of fused silica, 3-1 mm; and 22 parts of fused silica, 1-0 mm.

[0143] Acid-resistant powder: 3 parts of fused silica powder, 200 mesh; 3 parts of fused silica powder, 325 mesh.

[0144] Abrasion-resistant materials: 5 parts of brown fused alumina, 1-0 mm; 1 part of brown fused alumina, 200 mesh; 3 parts of brown fused alumina, 325 mesh.

[0145] Precursor powder: 11 parts slag powder; 7 parts fly ash; 3 parts metakaolin.

[0146] Nanoparticles: 0.5 parts of activated alumina microparticles (1μm); 0.5 parts of activated alumina microparticles (2-5μm); 3 parts of zirconium-containing silicon microparticles (1μm).

[0147] Fiber reinforcement material: basalt fiber, 3mm, 0.5 parts.

[0148] Water-reducing agent: 0.05 parts of FDN-A.

[0149] Activator: 13 parts of water glass solution (modulus 2.05±0.05).

[0150] The acid-resistant geopolymer castable was poured into a mold and shaped; the curing method was adjusted to high-temperature steam curing (cured for 48 hours under 80℃ water steam conditions 12 hours after casting). After curing, the mechanical properties and acid resistance of the castable were tested.

[0151] Comparative Example 1

[0152] Weigh each raw material according to the following proportions by weight:

[0153] Acid-resistant aggregates: 12 parts of fused silica, 5-3 mm; 24 parts of fused silica, 3-1 mm; 18 parts of fused silica, 1-0 mm.

[0154] Acid-resistant powder: 12 parts of quartz powder, 180 mesh; 10 parts of cast stone powder, 325 mesh.

[0155] Cementitious material: PⅡ42.5 cement, 24 parts.

[0156] Additive: Polycarboxylate superplasticizer, 0.02 parts.

[0157] Water: 6.2 parts.

[0158] After molding and curing according to the above preparation method, the mechanical properties and acid resistance of the castable are tested.

[0159] Performance testing

[0160] The comprehensive performance of the castables prepared in Examples 1-9 and Comparative Example 1 was tested respectively.

[0161] Compressive strength and flexural strength: The 28-day compressive strength and 28-day flexural strength were tested in accordance with GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete".

[0162] Acid solution corrosion resistance: The weight loss rate and surface morphology were tested after immersion in 10% citric acid solution for 7 days, 10% lactic acid solution for 7 days, 10% acetic acid solution for 7 days, 20% sulfuric acid solution at 80℃ for 3 days, 50% sulfuric acid solution at 80℃ for 3 days, 20% hydrochloric acid solution for 3 days, 20% nitric acid solution for 3 days, and 20% phosphoric acid solution for 3 days.

[0163] The test results are shown in Table 1.

[0164] Table 1: Overall performance test results of each embodiment and comparative example

[0165] Test Project 28-day compressive strength (MPa) 28-day flexural strength (MPa) 10% Citric Acid (7 days) 10% lactic acid (7 days) 10% acetic acid (7 days) 20% sulfuric acid at 80℃ (3 days) 50% sulfuric acid at 80℃ (3 days) 20% hydrochloric acid (3 days) 20% nitric acid (3 days) 20% phosphoric acid (3 days) Example 1 35.7 3.4 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 0.42% / No peeling or cracking 0.61% / No peeling or cracking 0.22% / No peeling or cracking 0.29% / No peeling or cracking 0.31% / No peeling or cracking Example 2 52.9 4 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 0.52% / No peeling or cracking 0.83% / No peeling or cracking 0.37% / No peeling or cracking 0.31% / No peeling or cracking 0.44% / No peeling or cracking Example 3 58.1 4.9 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 1.11% / No cracks 1.27% / No cracks 0.35% / No cracks 0.29% / No cracks 0.37% / No cracks Example 4 33.9 3.2 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 0.43% / No peeling or cracking 0.55% / No peeling or cracking 0.21% / No peeling or cracking 0.25% / No peeling or cracking 0.30% / No peeling or cracking Example 5 53.9 3.9 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 0.51% / No peeling or cracking 0.72% / No peeling or cracking 0.35% / No peeling or cracking 0.29% / No peeling or cracking 0.41% / No peeling or cracking Example 6 55.6 4.9 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 1.08% / No cracks 1.12% / No cracks 0.29% / No cracks 0.29% / No cracks 0.36% / No cracks Example 7 41.3 3.6 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 0.41% / No peeling or cracking 0.60% / No peeling or cracking 0.21% / No peeling or cracking 0.25% / No peeling or cracking 0.28% / No peeling or cracking Example 8 55.6 4.1 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 0.49% / No peeling or cracking 0.81% / No peeling or cracking 0.35% / No peeling or cracking 0.30% / No peeling or cracking 0.41% / No peeling or cracking Example 9 60.8 5 <0.2% / No peeling or cracking <0.2% / No peeling or cracking <0.2% / No peeling or cracking 1.05% / No cracks 1.21% / No cracks 0.32% / No cracks 0.29% / No cracks 0.33% / No cracks Comparative Example 1 61.3 6.5 8.1% / aggregate leakage <0.2% / No peeling or cracking 13.2% / aggregate leakage 24.9% / aggregate leakage >30% / test block fracture 8.7% / Surface peeling 3.1% / Surface peeling 0.5% / surface dissolution

[0166] As shown in Table 1, the weight loss rate of the acid-resistant geopolymer castables prepared in Examples 1-9 of this invention in various acidic media is significantly lower than that of Comparative Example 1. The surface morphology of these castables is characterized by no peeling, no cracks, or only cracks without peeling. In contrast, Comparative Example 1 exhibits severe corrosion phenomena such as aggregate leakage, specimen breakage, surface peeling, and surface dissolution in various acid solutions. This demonstrates that the present invention achieves excellent acid corrosion resistance in castables through the systematic synergy of acid-resistant aggregates, acid-resistant powders, abrasive materials, cementitious components, activators, nanoparticles, carbonaceous raw materials, fiber reinforcement materials, and additives.

[0167] The acid-resistant geopolymer castable described in this invention is suitable for a variety of harsh working conditions. In the chemical industry, it can be used for acid-resistant and corrosion-resistant engineering projects such as various pickling tanks, electrolytic cells, acid storage tank linings, and acid liquid conveying channels; in the hydrometallurgical field, it is suitable for acid-resistant and corrosion-resistant facilities such as acid leaching tanks, acidolysis reactors, and slurry conveying pipeline linings; in the environmental protection field, it can be used for corrosion-resistant structures such as flue gas desulfurization unit linings, acidic wastewater treatment ponds, and acid-base neutralization ponds; in the power industry, it is suitable for flue gas linings of wet desulfurization systems and acid liquid drainage ditches; in the defense and military industry, it can be used for the protection of various acidic media storage and transportation facilities. In addition, this castable is also suitable for complex working conditions that require simultaneous performance of multiple requirements such as acid resistance, wear resistance, and impact resistance, such as the lining protection of equipment such as acidic fluid conveying pipelines and mixing tanks containing solid particles.

[0168] In summary, this invention, through the systematic synergy of acid-resistant aggregates, acid-resistant powders, abrasive materials, cementitious components, activators, nanoparticles, carbonaceous raw materials, fiber reinforcing materials, and additives, has successfully prepared a geopolymer castable that possesses excellent acid resistance, high mechanical strength, high density, high toughness, good workability, and green environmental protection characteristics. The various technical features support each other and synergistically enhance each other, achieving technical effects that cannot be achieved by a single component or simple combination, demonstrating significant technological progress and broad application prospects.

[0169] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A fiber-reinforced acid-resistant geopolymer castable, characterized in that, The raw materials include the following parts by weight: 52-68 parts acid-resistant aggregate, 5-12 parts acid-resistant powder, 4-11 parts wear-resistant material, 11-36 parts precursor powder, 2-5 parts nano-powder, 0-0.75 parts carbonaceous raw material, 0-0.75 parts fiber reinforcing material, 0.02-0.05 parts additives, and 13-20 parts activator.

2. The fiber-reinforced acid-resistant geopolymer castable according to claim 1, characterized in that, The acid-resistant aggregate is one or more of fused quartz, quartzite, granite, diabase, and basalt. By weight, it comprises 12-18 parts of acid-resistant aggregate with a particle size of 5-3 mm, 18-25 parts of acid-resistant aggregate with a particle size of 3-1 mm, and 22-25 parts of acid-resistant aggregate with a particle size of 1-0 mm.

3. The fiber-reinforced acid-resistant geopolymer castable according to claim 1, characterized in that, The acid-resistant powder is one or more of fused silica powder, cast stone powder, and quartz powder. By weight, there are 3-5 parts of acid-resistant powder with a particle size of 200 mesh and 2-7 parts of acid-resistant powder with a particle size of 325 mesh.

4. The fiber-reinforced acid-resistant geopolymer castable according to claim 1, characterized in that, The wear-resistant material is brown fused alumina, comprising, by weight, 2-5 parts of brown fused alumina with a particle size of 1-0 mm, 1-3 parts of brown fused alumina with a particle size of 200 mesh, and 1-3 parts of brown fused alumina with a particle size of 325 mesh.

5. The fiber-reinforced acid-resistant geopolymer castable according to claim 1, characterized in that, The precursor powder is one or more of slag powder, fly ash, and metakaolin; when the precursor powder includes slag powder, fly ash, and metakaolin, the proportions by weight are 1-10 parts slag powder, 10-20 parts fly ash, and 0-6 parts metakaolin powder.

6. The fiber-reinforced acid-resistant geopolymer castable according to claim 1, characterized in that, The nanoparticles are activated alumina microparticles and zirconium-containing silicon microparticles. By weight, the activated alumina microparticles with a particle size of 0-1 μm are 0.5-1 parts, the activated alumina microparticles with a particle size of 2-5 μm are 0.5-1 parts, and the zirconium-containing silicon microparticles with a particle size of 0-1 μm are 1-3 parts.

7. The fiber-reinforced acid-resistant geopolymer castable according to claim 1, characterized in that, The carbonaceous raw materials are spherical pitch and carbon black powder, with 0-0.5 parts of spherical pitch with a particle size of 0-1 mm and 0-0.25 parts of N990 carbon black by weight.

8. The fiber-reinforced acid-resistant geopolymer castable according to claim 1, characterized in that, The fiber reinforcement material is one or more of basalt fiber, heat-treated carbon fiber, and acid-resistant glass fiber; the length of the fiber reinforcement material is 2-4 mm.

9. The method for preparing the acid-resistant geopolymer castable according to any one of claims 1-8, characterized in that, Includes the following steps: S1. Weigh out the acid-resistant aggregate, acid-resistant powder, abrasive, precursor powder, nano-powder, carbonaceous raw material, fiber reinforcing material, additives and water glass solution according to the weight ratio. S2. Dry mix the precursor powder, nano-powder, carbonaceous raw material, fiber reinforcement material and additives in a mixer for 85-95 seconds, then add water glass solution and stir for 110-130 seconds to obtain a gelling material. S3. Add wear-resistant material, acid-resistant powder and acid-resistant aggregate to the cementitious material in sequence, stir for 120 seconds to obtain acid-resistant geopolymer castable; S4. Pour the acid-resistant geopolymer castable into the mold to form a shape; S5, obtained after maintenance.

10. The method for preparing the acid-resistant geopolymer castable according to claim 9, characterized in that, The curing process is either room temperature curing or high temperature steam curing. The room temperature curing process involves immediately covering the casting with a plastic film after casting and maintaining moisture at room temperature for 26-30 days. The high temperature steam curing process involves curing the casting under 75-85℃ steam conditions for 46-50 hours 10-14 hours after casting.