A high-temperature resistant aniline-based organosilicon Mannich base quaternary ammonium salt corrosion inhibitor and its preparation method
By introducing aniline and siloxane segments into the Mannich base molecule, and utilizing the synergistic effect of strong adsorption by phenyl π bonds and coordination film formation by siloxane bonds, the problem of easy desorption of Mannich base corrosion inhibitors in high-temperature CO2 environments was solved, achieving highly efficient metal corrosion protection.
Patent Information
- Application Number
- CN202611275377.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing Mannich base corrosion inhibitors are prone to desorption from the adsorption membrane in high-temperature CO2 environments, have limited phenyl content, and poor silicate compounding effect, making it difficult to achieve long-term protection at high temperatures.
By introducing aniline groups (increasing phenyl density) and siloxane segments into the Mannich base molecule, a dense adsorption layer is formed by utilizing the synergistic effect of strong adsorption of phenyl π bonds and coordination film formation of siloxane bonds, thereby enhancing the adsorption strength and film density of the corrosion inhibitor at high temperatures.
It achieves efficient corrosion protection for metals in a wide temperature range of 140℃~200℃ and under high pressure CO2 environment, with a corrosion inhibition efficiency of over 96%, significantly improving the chemical adsorption stability and film density at high temperatures.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to a high-temperature resistant aniline-based organosilicon Mannich base quaternary ammonium salt corrosion inhibitor and its preparation method, belonging to the technical field of high-temperature corrosion inhibitors, and applied to the field of high-temperature and high-pressure CO2 corrosion protection technology in the oil and gas development process. Background Technology
[0002] The development of high-temperature, high-pressure oil and gas resources has exacerbated corrosion in oil and gas fields, making corrosion inhibitors a crucial technology for corrosion control and attracting widespread attention. Mannich base corrosion inhibitors, with their excellent high-temperature resistance, are currently the most commonly used type of high-temperature corrosion inhibitor. However, as oil and gas development temperatures continue to rise, the adsorption films formed solely by the chemical and electrostatic adsorption of polar groups (such as C / C double bonds, large π bonds in benzene rings, N, O, etc.) are insufficient to resist desorption caused by enhanced molecular thermal motion under high-temperature conditions. This makes it difficult for existing Mannich base corrosion inhibitors to meet industrial requirements under ultra-high temperature conditions.
[0003] Sodium silicate, an inorganic salt, hydrolyzes into silicic acid when dissolved in water. The oxygen atoms on the silanol groups (Si-OH) and silicon-oxygen bonds (Si-O-Si) in the silicic acid molecule carry lone pairs of electrons, making them typical Lewis base sites. These sites can act as ligands to form coordinate bonds with metal ions (Lewis acids). Silicic acid has four coordinateable oxygen atoms, classifying it as a polydentate ligand. It can simultaneously coordinate with one or more metal centers, ultimately forming a dense, water- and acid-insoluble silica-oxygen network phase film on the metal surface, providing more effective protection for the base metal.
[0004] To leverage the properties of silicon-oxygen network phase-forming films, a common practice in the prior art is to combine corrosion inhibitors with silicates. For example, Chinese patent application CN 119265568 A uses polyetheramine as the main corrosion inhibitor and sodium silicate or potassium silicate as an auxiliary agent, giving the corrosion inhibitor excellent temperature and salt resistance. Chinese patent application CN107620069 A combines Mannich base with sodium silicate to form an adsorption layer and a hydrophobic film on the metal surface. Chinese patent application CN 118755462 B uses linoleic acid imidazoline quaternary ammonium salt as the main agent and potassium chromate, sodium silicate, and potassium iodide as auxiliary agents to form an insoluble oxide film through physical adsorption. However, silicates themselves are not surfactants and are difficult to form a strong, oriented adsorption layer on the metal surface. To this end, Chinese patent application CN 113214309 B attempted to introduce organosiloxanes into Mannich base molecules, using γ-aminopropyltrimethoxysilane or γ-aminopropylmethyldiethoxysilane with aldehydes and ketones to synthesize organosilicon Mannich bases, in order to achieve the synergistic effect of silicon-oxygen bonds and Mannich bases.
[0005] However, the phenyl content in existing organosilicon Mannich base molecules is limited, relying mainly on coordination adsorption provided by siloxane segments. The directional adsorption generated by the interaction of the large π-electron cloud of the phenyl group with empty orbitals on the metal surface can significantly enhance the adsorption strength of the corrosion inhibitor molecules on the metal surface and alter the interfacial electrochemical behavior, making it a key group for improving high-temperature corrosion inhibition performance. Currently, there is a lack of a technical solution to introduce high-density phenyl groups (especially aniline groups) into the molecular framework of organosilicon Mannich bases, while simultaneously utilizing the strong phenyl π-bond adsorption and silicon-oxygen bond coordination to achieve synergistic effects in film formation. Therefore, how to further increase the phenyl content in the molecule based on existing organosilicon Mannich bases to synergistically enhance the chemical adsorption stability and film density at high temperatures, in order to achieve long-term protection in CO2 corrosion environments at 180℃ or even higher, remains a pressing technical challenge in this field. Summary of the Invention
[0006] The purpose of this invention is to provide an aniline-based organosilicon Mannich base and its quaternary ammonium salt, and a corrosion inhibitor composition containing this compound. Addressing the problems of existing Mannich base corrosion inhibitors such as easy desorption of the adsorbed film in high-temperature CO2 environments, limited phenyl content, and poor silicate compounding effects, this invention, through molecular structure design, simultaneously introduces aniline groups (increasing phenyl density and utilizing strong adsorption through large π bonds) and siloxane segments (forming a silicon-oxygen network coordination film) into the Mannich base framework. Utilizing the synergistic effect of phenyl π-bond adsorption and silicon-oxygen bond coordination film formation, the adsorption strength and film density of the corrosion inhibitor on the metal surface are significantly enhanced at high temperatures. This achieves highly efficient corrosion protection for metals (including low-alloy steel and martensitic stainless steel) in a wide temperature range of 140℃ to 200℃ and under high-pressure CO2 environments, with a corrosion inhibition efficiency of over 96%.
[0007] The aniline-based organosilicon Mannich base provided by this invention has the structure shown in Formula I:
[0008] In Formula 1, R1 is selected from C1-C10 alkyl groups.
[0009] The aniline-based organosilicon Mannich base can be prepared by a method including the following steps: Using cinnamaldehyde and aniline organosiloxane as reactants, a condensation reaction is first carried out under acidic conditions to form an imine-onium intermediate, and then acetophenone is added to obtain the aniline organosilane Mannich base through the Mannich reaction.
[0010] Preferably, the condensation reaction is carried out at a temperature of 90°C to 130°C for 2 to 4 hours. Preferably, the reaction temperature of the Mannich reaction is 90°C to 130°C, and the reaction time is 2 to 4 hours. Preferably, the molar ratio of cinnamaldehyde to aniline organosiloxane is 1:1.05-1.2, and the molar ratio of acetophenone to cinnamaldehyde is 1.05-1.2:1; Preferably, the acidic condition is achieved by adjusting the pH value to 3-4 using hydrochloric acid or acetic acid.
[0011] The aniline-based organosilicon Mannich base quaternary ammonium salt provided by this invention has the structure shown in Formula II:
[0012] In Formula II, R1 is selected from C1-C10 alkyl groups, and R2 is selected from C12-C18 alkyl or benzyl groups.
[0013] The aniline-based organosilicon Mannich base quaternary ammonium salt can be prepared by a method including the following steps: Using the aniline-based organosilicon Mannich base and a haloalkanes as reactants, the quaternary ammonium salt of the aniline-based organosilicon Mannich base is prepared by a quaternization reaction. Preferably, the haloalkane is a chlorinated C12-C18 alkane or benzyl chloride; Preferably, the molar ratio of the aniline-based organosilicon Mannich base to the haloalkane is 1:1.05 to 1.2; Preferably, the quaternization reaction is carried out at a temperature of 90°C to 130°C for 2 to 4 hours.
[0014] Furthermore, the present invention provides a high-temperature corrosion inhibitor composition comprising the following components in weight percentages: 20%–30% of aniline-based organosilicon Mannich base or quaternary ammonium salt of aniline-based organosilicon Mannich base; 20%–30% of surfactant; 5%–10% of alkynyl alcohol; 30%–40% of solvent. Preferably, the composition of the high-temperature corrosion inhibitor composition is as follows: The mass percentage of the aniline-based organosilicon Mannich base or the quaternary ammonium salt of the aniline-based organosilicon Mannich base is 22% to 30%, the mass percentage of the surfactant is 22% to 28%, the mass percentage of the alkynol is 5% to 8%, and the mass percentage of the solvent is 35% to 42%.
[0015] Preferably, the surfactant is selected from cationic surfactants and / or nonionic surfactants; Preferably, the cationic surfactant is selected from one or more of alkyl quaternary ammonium salts, benzyl quaternary ammonium salts, and alkyl imidazoline quaternary ammonium salts; Preferably, the nonionic surfactant is selected from Tween surfactants and / or OP surfactants; More preferably, the surfactant is OP-10 and / or Tween T-80; Preferably, the alkynol is selected from one or more of propynol, butynol, pentynol, and their derivatives; Preferably, the alkynol is selected from one or more of propynol, butynol, pentynol, and 3-phenylpropynol.
[0016] Preferably, the solvent is selected from one or more of ethanol, ethylene glycol, N,N-dimethylformamide (DMF), and N-ethylmorpholine.
[0017] The corrosion inhibitor composition of the present invention can be used in metal corrosion protection, specifically for metal corrosion protection in high temperature and / or high pressure CO2 corrosion environments, and the application temperature can be 140℃~200℃.
[0018] Furthermore, the present invention also provides a method for metal corrosion prevention, comprising the step of adding the corrosion inhibitor composition to a corrosive medium in contact with the metal; Preferably, the amount of the corrosion inhibitor composition added is 1% to 3% of the mass of the corrosive medium; Preferably, the corrosive medium is produced water from oil and gas fields or a formate solution; Preferably, the corrosive medium contains CO2; More preferably, the temperature of the corrosive medium is 140℃~200℃, and the partial pressure of CO2 is 1MPa~15MPa.
[0019] The metal is low alloy steel, martensitic stainless steel or super martensitic stainless steel. Preferably, the low alloy steel is P110S steel, the martensitic stainless steel is 13Cr stainless steel, and the super martensitic stainless steel is S13Cr stainless steel.
[0020] In this invention, the N / O atoms in the Mannich base framework provide chemisorption, anchoring the molecule to the metal surface; the large π electron clouds of the three benzene rings in the molecule overlap with the empty d orbitals of the Fe atoms, resulting in strong directional adsorption and significantly improving the high-temperature resistance to desorption; the siloxane groups undergo hydrolysis and condensation in an aqueous medium, forming a dense silicon-oxygen network inorganic protective film in situ on the metal surface through Si-O-Fe coordination bonds. These three elements achieve spatial coupling through the same molecular framework, forming an integrated composite protective layer of organic adsorption layer and inorganic phase-forming film. The addition of alkynyl alcohol further fills the microscopic defects in the adsorption layer. Therefore, this invention achieves highly efficient protection of metals over a wide temperature range of 140℃ to 200℃ and under high-pressure CO2 conditions, with a corrosion inhibition efficiency exceeding 96%.
[0021] This invention combines the adsorption of high-density phenyl π bonds with aniline groups with in-situ coordination film formation of siloxanes, achieving intramolecular synergistic effects. This effectively solves the technical problem of easy desorption of existing Mannich base corrosion inhibitors at high temperatures, yielding significant beneficial results. In a harsh corrosive environment of 180℃ and a CO2 partial pressure of 10MPa, the corrosion inhibitor of this invention achieves a corrosion inhibition efficiency of over 96% for three commonly used oil and gas field pipe materials: P110S, 13Cr, and S13Cr. In contrast, the commercially available high-temperature CO2 corrosion inhibitor in Comparative Example 1 only achieves 57%–69%, and the aniline-free organosilicon Mannich base in Comparative Example 2 only achieves 70%–79%, indicating that the introduction of aniline groups increases the corrosion inhibition efficiency by approximately 18–27 percentage points. Within a wide temperature range of 140℃–200℃, the corrosion inhibition efficiency of this invention remains consistently above 96%, while the commercially available product continuously decreases from 77.7% to 66.5%, demonstrating a significant advantage in high-temperature stability. In addition, the corrosion inhibitor of the present invention is a homogeneous liquid, which is convenient to add and only requires 2% of the amount to achieve efficient corrosion protection; the synthesis process is simple (90℃~130℃, normal pressure), the raw materials are widely available, and it is suitable for industrial production. Detailed Implementation
[0022] In order to provide a clearer understanding of the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention will now be described in detail below, but it should not be construed as limiting the scope of implementation of the present invention.
[0023] Example 1: Preparation of High-Temperature Resistant Aniline-Based Organosilicon Mannich Base Corrosion Inhibitor (1) Synthesis of aniline-based organosilicon Mannich bases 13.2 g (0.1 mol) of cinnamaldehyde and 32.7 g (0.11 mol) of N-phenyl-γ-aminopropyltriethoxysilane were added to a reactor equipped with a condenser and a water separator. 40 g of ethylene glycol was added as a solvent, and the pH of the solution was adjusted to 3.2 with acetic acid. The mixture was stirred and heated to 110 °C. The reaction was continued with stirring for 3 hours. Then, 13.2 g (0.11 mol) of acetophenone was added, and the temperature was maintained at 110 °C. The reaction was continued with stirring for another 3 hours, yielding a brownish-red viscous liquid, which is the aniline-based organosilicon Mannich base. The reaction equation is shown below (R1 is ethyl):
[0024] (2) Compound formulation of corrosion inhibitors Take 25g of the above-mentioned aniline-based organosilicon Mannich base, add 25g of surfactant OP-10, then add 8g of propargyl alcohol and 42g of ethylene glycol, heat to 50℃ and stir for 30min to ensure that all components are fully miscible. After cooling, a homogeneous reddish-brown liquid is obtained, which is the compound corrosion inhibitor. The composition is: aniline-based organosilicon Mannich base 25wt%, surfactant 25wt%, propargyl alcohol 8wt%, and solvent 42wt%.
[0025] Example 2: Preparation of high-temperature resistant aniline-based organosilicon Mannich base corrosion inhibitor The difference between this embodiment and Embodiment 1 lies in the synthesis temperature and the formulation.
[0026] (1) Synthesis of aniline-based organosilicon Mannich bases 13.2 g (0.1 mol) of cinnamaldehyde and 28.1 g (0.11 mol) of N-phenyl-γ-aminopropyltrimethoxysilane (R1=CH3) were added to a reactor equipped with a condenser and a water separator. 40 g of ethylene glycol was added as a solvent, and the pH of the solution was adjusted to 3.0 with hydrochloric acid. The mixture was stirred and heated to 100 °C. The reaction was continued with stirring for 3.5 h. Then, 13.2 g (0.11 mol) of acetophenone was added, and the temperature was maintained at 100 °C. The reaction was continued with stirring for another 3.5 h, yielding a brownish-red viscous liquid, which is the aniline-based organosilicon Mannich base.
[0027] (2) Compound formulation of corrosion inhibitors Take 28g of the above-mentioned aniline-based organosilicon Mannich base, add 20g of Tween T-80, then add 5g of butynol and 47g of N,N-dimethylformamide (DMF), heat to 50℃ and stir for 30min, and after cooling, obtain a homogeneous reddish-brown liquid, which is the compound corrosion inhibitor.
[0028] Example 3: Preparation of aniline-based organosilicon Mannich base quaternary ammonium salt corrosion inhibitor (1) Synthesis of aniline-based organosilicon Mannich bases The aniline-based organosilicon Mannich base was synthesized according to step (1) of Example 1.
[0029] (2) Mannich base quaternization reaction Take 100g of the aniline-based organosilicon Mannich base prepared in step (1), add it to the reactor, then add 45g (0.22mol) of dodecane chloride, stir and heat to 110℃, react for 3h to obtain the aniline-based organosilicon Mannich base quaternary ammonium salt, which is a dark red viscous liquid. The reaction equation is as follows (R1 is ethyl):
[0030] (3) Compound formulation of corrosion inhibitors Take 30g of the above-mentioned aniline-based organosilicon Mannich base quaternary ammonium salt, add 25g of surfactant OP-10, then add 10g of propynyl alcohol and 35g of ethylene glycol, heat to 50℃ and stir for 30min, and after cooling, obtain a homogeneous dark red liquid, which is the compound corrosion inhibitor.
[0031] Example 4 The difference between this embodiment and Example 3 lies in the different quaternizing reagents and compound compositions.
[0032] (1) Synthesis of aniline-based organosilicon Mannich bases The aniline organosilicon Mannich base was synthesized according to the method of step (1) in Example 2 (using trimethoxysiloxane, R1=CH3).
[0033] (2) Mannich base quaternization reaction Take 100g of the aniline-based organosilicon Mannich base prepared in step (1), add it to the reactor, then add 28g (0.22mol) of benzyl chloride, stir and heat to 100℃, react for 3h to obtain the aniline-based organosilicon Mannich base benzyl quaternary ammonium salt.
[0034] (3) Compound formulation of corrosion inhibitors Take 25g of the above-mentioned aniline-based organosilicon Mannich base benzyl quaternary ammonium salt, add 30g of Tween T-80, then add 8g of propynyl alcohol and 37g of N,N-dimethylformamide (DMF), heat to 50℃ and stir for 30min, and after cooling, obtain a homogeneous liquid, which is the compound corrosion inhibitor.
[0035] Example 5 The difference between this embodiment and Embodiment 3 is that a composite surfactant is used.
[0036] (1) Synthesis of aniline organosilicon Mannich base quaternary ammonium salt: The aniline organosilicon Mannich base quaternary ammonium salt was synthesized according to the steps (1) and (2) of Example 3.
[0037] (2) Formulation of corrosion inhibitor: Take 22g of the above-mentioned aniline organosilicon Mannich base quaternary ammonium salt, add 15g of cetyltrimethylammonium bromide (CTAB) and 5g of OP-10 as a composite surfactant, then add 7g of pentyne alcohol and 51g of ethylene glycol, heat to 50℃ and stir for 30min, and after cooling, obtain a homogeneous liquid, which is the compound corrosion inhibitor.
[0038] Example 6: The difference between this example and Example 1 is the synthesis temperature and the type of alkynol.
[0039] (1) Synthesis of aniline-based organosilicon Mannich bases 13.2 g (0.1 mol) of cinnamaldehyde and 32.7 g (0.11 mol) of N-phenyl-γ-aminopropyltriethoxysilane were added to a reactor, followed by 40 g of ethylene glycol. The pH was adjusted to 3.5 with acetic acid, and the mixture was stirred and heated to 120 °C. The first reaction time was 2.5 h. Subsequently, 13.2 g (0.11 mol) of acetophenone was added, and the reaction was continued at 120 °C for another 2.5 h to obtain an aniline-based organosilicon Mannich base.
[0040] (2) Compound formulation of corrosion inhibitors Take 30g of the above-mentioned aniline-based organosilicon Mannich base, add 22g of Tween T-80, then add 6g of 3-phenylpropynol and 42g of N-ethylmorpholine, heat to 50℃ and stir for 30min, and after cooling, obtain a homogeneous liquid, which is the compound corrosion inhibitor A6.
[0041] Comparative Example 1 The corrosion inhibitor used in this comparative example is an existing high-temperature CO2 corrosion inhibitor, with the following composition: 35% imidazoline quaternary ammonium salt main agent (structure shown in the following formula), 30% isopropanol, 10% OP-10, and 25% deionized water.
[0042]
[0043] Comparative Example 2 In this comparative example, conventional aminosiloxanes (γ-aminopropyltriethoxysilane, without aniline groups) were used to replace aniline-based organosiloxanes. An aniline-free organosilicone Mannich base was synthesized according to the method of Example 1, and then compounded according to the formulation of Example 1 to obtain a corrosion inhibitor, which was used to compare the effect of the introduction of aniline groups on the improvement of corrosion inhibition performance.
[0044] Specific steps: 13.2g (0.1mol) cinnamaldehyde and 24.4g (0.11mol) γ-aminopropyltriethoxysilane were added to the reactor, 40g ethylene glycol was added as a solvent, the pH was adjusted to 3.2 with acetic acid, and the temperature was raised to 110℃ for 3h; then 13.2g (0.11mol) acetophenone was added, and the reaction was continued at 110℃ for 3h to obtain an organosilicon Mannich base without aniline groups. The corrosion inhibitor was compounded according to the formula (2) of Example 1 (25g Mannich base, 25g OP-10, 8g propynyl alcohol, 42g ethylene glycol).
[0045] Performance characterization: To verify the performance of the corrosion inhibitor of the present invention, the corrosion inhibitors of Examples 1-6 and Comparative Examples 1-2 were subjected to high-temperature CO2 corrosion performance tests.
[0046] Formate high-temperature and high-pressure CO2 corrosion performance test: Standards followed: NACE TM0169-2020 "Standard Guide for Laboratory Immersion Corrosion Testing of Metals", with reference to SY / T 5273-2019 "Performance Evaluation Method for Corrosion Inhibitors Used in Oilfield Produced Water".
[0047] Experimental conditions: temperature 180℃, CO2 partial pressure 10MPa, and the test solution had a density of 1.25 g / cm³. 3 Potassium formate solution.
[0048] Test materials: low alloy steel P110S, martensitic stainless steel 13Cr and super martensitic stainless steel S13Cr, sample size 50×10×3mm.
[0049] Test period: 72 hours. Corrosion inhibitor dosage: 2% (mass percentage based on 100% of the test solution mass).
[0050] The experimental results are shown in the table below: Table 1. High-temperature CO2 corrosion performance test results of different embodiments and comparative examples.
[0051] The results above show that in a formate high-temperature and high-pressure corrosion environment of 180℃ and CO2 partial pressure of 10MPa, the uniform corrosion rate of all three materials without the addition of corrosion inhibitors is greater than 0.25 mm / a, indicating extremely severe corrosion. After adding the corrosion inhibitors of Examples 1-6 of this invention, the corrosion rate of P110SS decreased to 0.118~0.142 mm / a, with a corrosion inhibition efficiency exceeding 97%; the corrosion rate of 13Cr decreased to 0.081~0.105 mm / a, with a corrosion inhibition efficiency exceeding 96%; and the corrosion rate of S13Cr decreased to 0.063~0.088 mm / a, with a corrosion inhibition efficiency exceeding 96%. Among them, Example 2 showed high corrosion inhibition efficiency for all three materials. The corrosion inhibition efficiency of Comparative Example 1 at a 2% addition amount was only 57%~69%, far lower than that of this invention. The corrosion inhibition efficiency of Comparative Example 2 (organosilicon Mannich base without aniline group) was only 70%~79%, indicating that the introduction of aniline group plays a key role in improving corrosion inhibition performance.
[0052] Comparison of corrosion inhibition performance at different temperatures: To further evaluate the high-temperature resistance of the corrosion inhibitor of this invention, Example 2 (quaternary ammonium salt type) and Comparative Example 1 were selected, and CO2 corrosion tests were conducted at four temperatures: 140℃, 160℃, 180℃, and 200℃. The test conditions were the same as in Test (I), the material was P110SS, the amount of corrosion inhibitor added was 2%, and the test period was 72 hours. The test results are shown in the table below: Table 2. Results of CO2 corrosion performance tests on different embodiments and comparative products at different temperatures. (Table 1)
[0053] As shown in the table above, the blank corrosion rate decreased from 18.36 mm / a to 2.968 mm / a as the temperature increased from 140℃ to 200℃. The corrosion inhibitor in Example 2 maintained a stable corrosion inhibition efficiency of over 97% within the temperature range of 140~180℃, and still reached 96.5% at 200℃, demonstrating excellent high-temperature resistance. In contrast, the corrosion inhibition efficiency of Comparative Example 1 decreased from 77.7% to 66.5%, showing a significant performance decline at high temperatures. These results indicate that the synergistic mechanism of phenyl π-bond adsorption and silicon-oxygen bond coordination film formation in the corrosion inhibitor of this invention exhibits significant stability and superiority under high-temperature conditions.
Claims
1. An aniline-based organosilicon Mannich base having the structure shown in Formula I: In Formula 1, R1 is selected from C1-C10 alkyl groups.
2. An aniline-based organosilicon Mannich base quaternary ammonium salt having the structure shown in Formula II: In Formula II, R1 is selected from C1-C10 alkyl groups, and R2 is selected from C12-C18 alkyl or benzyl groups.
3. The method for preparing the aniline-based organosilicon Mannich base according to claim 1, comprising the following steps: Using cinnamaldehyde and aniline organosiloxane as reactants, a condensation reaction is first carried out under acidic conditions to form an imine-onium intermediate, and then acetophenone is added to obtain the aniline organosilane Mannich base through the Mannich reaction.
4. The preparation method of the aniline-based organosilicon Mannich base quaternary ammonium salt according to claim 2, comprising the following steps: Using the aniline-based organosilicon Mannich base and haloalkanes as reactants, the aniline-based organosilicon Mannich base quaternary ammonium salt is prepared by a quaternization reaction.
5. A high-temperature corrosion inhibitor composition comprising the following components by weight percentage: 20%–30% of aniline-based organosilicon Mannich base or quaternary ammonium salt of aniline-based organosilicon Mannich base; 20%–30% of surfactant; 5%–10% of alkynyl alcohol; 30%–40% of solvent. in, The aniline-based organosilicon Mannich base is the aniline-based organosilicon Mannich base according to claim 1, and the aniline-based organosilicon Mannich base quaternary ammonium salt is the aniline-based organosilicon Mannich base quaternary ammonium salt according to claim 2.
6. The corrosion inhibitor composition according to claim 5, characterized in that: The surfactant is selected from cationic surfactants and / or nonionic surfactants; The cationic surfactant is selected from one or more of alkyl quaternary ammonium salts, benzyl quaternary ammonium salts, and alkyl imidazoline quaternary ammonium salts; The nonionic surfactant is selected from Tween surfactants and / or OP surfactants; The alkynol is selected from one or more of propynol, butynol, pentynol and their derivatives; The solvent is selected from one or more of ethanol, ethylene glycol, N,N-dimethylformamide, and N-ethylmorpholine.
7. The corrosion inhibitor composition according to claim 5 or 6, characterized in that: The mass percentage of the aniline-based organosilicon Mannich base or the quaternary ammonium salt of the aniline-based organosilicon Mannich base is 22% to 30%, the mass percentage of the surfactant is 22% to 28%, the mass percentage of the alkynol is 5% to 8%, and the mass percentage of the solvent is 35% to 42%.
8. The application of the aniline-based organosilicon Mannich base of claim 1, the aniline-based organosilicon Mannich base quaternary ammonium salt of claim 2, or the corrosion inhibitor composition of any one of claims 5-7 in metal corrosion protection; Preferably, the application is a metal corrosion protection application in a high-temperature and / or high-pressure CO2 corrosive environment; More preferably, the application temperature is 140°C to 200°C.
9. A method for preventing metal corrosion, comprising the step of adding the corrosion inhibitor composition of any one of claims 5-7 to a corrosive medium in contact with the metal; Preferably, the amount of the corrosion inhibitor composition added is 1% to 3% of the mass of the corrosive medium; Preferably, the corrosive medium is produced water from oil and gas fields or a formate solution; Preferably, the corrosive medium contains CO2; More preferably, the temperature of the corrosive medium is 140℃~200℃, and the partial pressure of CO2 is 1MPa~15MPa.
10. The metal corrosion prevention method according to claim 9, characterized in that: The metal is low alloy steel, martensitic stainless steel or super martensitic stainless steel. Preferably, the low alloy steel is P110S steel, the martensitic stainless steel is 13Cr stainless steel, and the super martensitic stainless steel is S13Cr stainless steel.
Citation Information
Patent Citations
Preparation method for acidizing corrosion inhibitor
CN107620069A
A Mannich base, a Mannich base quaternary ammonium salt, its preparation method and application
CN113214309B
A low-temperature acidification corrosion inhibitor for petroleum and preparation method thereof
CN118755462B
High-performance carbon dioxide corrosion inhibitor and preparation method thereof
CN119265568A