Materials for Strengthening and Sealing in Water-Rich Environments Resisting Alternating Loads and Their Preparation Methods
By designing a multi-layered synergistic protection network using polyurethane rigid main chain modified materials, the problem of easy damage to tunnel and roadbed structures under high-frequency alternating loads and water scouring was solved, achieving efficient and long-lasting water-blocking reinforcement and self-repair effects.
Patent Information
- Application Number
- CN202611588047.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing water-blocking and reinforcement materials are difficult to adapt to the coupled effects of high-frequency alternating loads and water flow scouring, which makes tunnel and roadbed structures prone to damage and has low construction efficiency, failing to meet the requirements for long-term stable operation.
By using polyurethane rigid main chain modified material, a multi-level synergistic protection network is formed through covalent grafting design of fluorosilicone modified segments, dynamic disulfide bonds, rigid aromatic ring reinforcing segments and tertiary amine molecular segments, which enhances the hydrophobicity, self-healing ability and mechanical strength of the material, making it suitable for high-frequency alternating load environments.
It achieves long-term water-blocking reinforcement under high-frequency alternating loads and water scouring conditions. The material does not collapse underwater, has low expansion, high strength, and room temperature self-healing capability, which significantly improves the durability and construction efficiency of tunnels and roadbeds.
Smart Images

Figure CN123107028A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polyurethane materials technology, and specifically relates to a reinforcing and sealing material for water-rich environments that resists alternating loads and its preparation method. Background Technology
[0002] With the rapid development of my country's rail transit (subway, high-speed railway) and underground tunnel engineering, the long-term stability and safe operation of tunnel lining, subway subgrade and railway subgrade are facing severe challenges. Especially under the coupled conditions of complex geology and dynamic load, related engineering defects occur frequently, which seriously affect the durability of the project and the safety of train operation.
[0003] During subway and train operation, the starting, braking, and high-speed travel of trains generate continuous high-frequency alternating loads. These loads act on the subgrade and surrounding soil and lining structure of tunnels over a long period of time, which can easily lead to loosening of roadbed gravel and a decrease in soil compaction, thereby causing roadbed settlement and tunnel lining cracking. At the same time, underground engineering projects generally suffer from groundwater seepage problems, with sudden water inrush and seepage occurring frequently. The scouring effect of water flow will further aggravate the loss of gravel and softening of soil, damaging the integrity of the subgrade and lining, forming a dual destructive effect of "high-frequency load + water scouring", which significantly shortens the service life of the project.
[0004] Currently, materials used for tunnel water plugging and roadbed reinforcement mainly include traditional polyurethane water plugging agents, epoxy resin binders, and cement-based composite materials. However, these materials all have obvious defects and are difficult to adapt to the complex working conditions of high-frequency alternating loads and water-containing environments: Traditional polyurethane materials have certain water plugging performance, but their mechanical strength is insufficient. They are prone to fatigue cracking under high-frequency alternating loads and do not have self-healing capabilities. Once damaged, water seepage and structural damage will continue to intensify. Epoxy resin binders have high strength, but they are brittle, have poor flexibility, weak resistance to alternating loads, and poor hydrophobic properties. Their bonding strength drops significantly in water-containing environments, making it impossible to achieve long-term effective soil bonding and water plugging. Cement-based materials have weak erosion resistance, high shrinkage rate, and poor interfacial bonding with soil. They are difficult to adapt to the loose characteristics of roadbed gravel and do not have self-healing functions. After damage, they require frequent maintenance, resulting in high maintenance costs and low efficiency.
[0005] In addition, most existing water-blocking and reinforcement materials are multi-component systems that require on-site mixing during construction. The proportioning accuracy is difficult to control, resulting in low construction efficiency. Furthermore, uneven mixing can easily lead to unstable material performance. At the same time, there is a lack of self-healing water-blocking and reinforcement materials designed for high-frequency alternating load environments. Existing self-healing materials mostly focus on repair performance under static conditions. Under the coupled action of dynamic loads and water flow scouring, their self-healing efficiency is low and their durability is poor, which cannot meet the long-term stable use requirements of tunnels and subway / railway subgrades.
[0006] Therefore, developing a single-component water-blocking and reinforcement material that can adapt to high-frequency alternating load environments and possesses self-healing function, high strength, strong adhesion, excellent hydrophobicity, and resistance to water erosion is crucial to solving engineering pain points such as tunnel water inrush, loosening of roadbed gravel, and material fatigue damage under high-frequency loads. This would enable long-term water blocking and reinforcement of engineering projects, reduce maintenance costs, and ensure the safe and stable operation of rail transit and underground tunnel projects, becoming a pressing technical problem in this field. Summary of the Invention
[0007] The purpose of this invention is to overcome the common problems of traditional polyurethane grouting and consolidation materials, such as poor resistance to chemical erosion, easy damage propagation under alternating loads, loosening upon contact with water, and weak adaptability to curing construction. This invention provides a reinforcing and sealing material for water-rich environments that resists alternating loads and its preparation method.
[0008] In a first aspect, the present invention provides a water-rich environment-resistant alternating load-strengthening and sealing material, the material comprising a rigid polyurethane backbone, wherein the rigid polyurethane backbone is grafted with the following four functional side groups or block structures via urethane bonds: Fluorosilicone modified segments, wherein the fluorosilicone modified segments are derived from hydroxyl-terminated fluorosilicone diols, and have the general structural formula as follows: HO-R f -Si(CH3)2-[O-Si(CH3)2] m -O-Si(CH3)2-R f -OH, where R f The expression is -(CH2)2-(CF2)5-, and m is 1-16; A chain extension segment containing dynamic disulfide bonds, wherein the chain extension segment containing dynamic disulfide bonds is derived from 2-hydroxyethyl disulfide, and its structural formula is: HO-CH2-CH2-SS-CH2-CH2-OH; The rigid aromatic ring reinforcing segment is derived from 2,2-bis(4-hydroxyphenyl)propane, i.e., bisphenol A; The tertiary amine molecular chain segment, derived from N-ethyldiethanolamine, has the following structural formula: HO-CH2-CH2-N(C2H5)-CH2-CH2-OH.
[0009] In this invention, the water-rich environment refers to the construction environment of underground engineering where the aquifer is well-developed, the seepage flow is large, or the dynamic water flow velocity is ≥0.5m / s.
[0010] Specifically, the fluorosilicone modified segment is derived from a hydroxyl-terminated fluorosilicone diol, which is a perfluoropolysiloxane diol with hydroxyl-terminated ends.
[0011] Specifically, the fluorosilicone modified segments are perfluoropolyether segments or perfluoroalkylene segments, and the fluorosilicone modified segments are connected to the rigid polyurethane backbone through urethane bonds to impart low surface energy hydrophobic properties to the material. The dynamic disulfide bond contains at least one disulfide bond: -SS-, and the dynamic disulfide bond segment is connected to the rigid polyurethane backbone via urethane bonds to impart room temperature self-healing properties to the material. The rigid aromatic ring reinforcing segment contains at least one benzene ring structure, and the rigid aromatic ring reinforcing segment is connected to the rigid polyurethane main chain through urethane bonds to improve the mechanical strength and modulus of the material. A tertiary amine molecular chain segment, wherein the tertiary amine molecular chain segment contains at least one tertiary amine group, and the tertiary amine molecular chain segment is linked to the rigid polyurethane backbone by a urethane bond, for controlling the wet curing reaction rate of the material. The end groups of the polyurethane prepolymer main chain contain active isocyanate groups (-NCO).
[0012] Preferably, the rigid polyurethane backbone is provided by an aromatic diisocyanate, wherein the aromatic diisocyanate is 4,4'-diphenylmethane diisocyanate; the rigid polyurethane backbone contains diphenylmethane structural units introduced by the 4,4'-diphenylmethane diisocyanate.
[0013] Preferably, the mass ratio of each raw material component used to prepare the material is as follows: 100 parts of 4,4'-diphenylmethane diisocyanate, 12-18 parts of hydroxyl-terminated fluorosilicone modified diol, 4-6 parts of 2-hydroxyethyl disulfide, 8-12 parts of 2,2-di(4-hydroxyphenyl)propane, and 4-7 parts of N-ethyldiethanolamine.
[0014] Preferably, the NCO content of the material is 14.0%-20.0%.
[0015] Secondly, this invention discloses a method for preparing a water-rich environment-resistant alternating load-strengthening and sealing material, comprising the following steps: Step 1: 4,4'-diphenylmethane diisocyanate is subjected to a first prepolymerization reaction with a hydroxyl-terminated fluorosilicone modified diol to obtain a first prepolymer containing fluorosilicone modified segments. Step 2: The first prepolymer is subjected to a second prepolymerization reaction with 2-hydroxyethyl disulfide to obtain a second prepolymer, which contains fluorosilicone modified segments and dynamic disulfide bonds; Step 3: The second prepolymer is subjected to a third prepolymerization reaction with 2,2-bis(4-hydroxyphenyl)propane to obtain a third prepolymer, wherein the third prepolymer contains fluorosilicone modified segments, dynamic disulfide bonds and rigid aromatic ring structures; Step 4: The third prepolymer is subjected to a fourth prepolymerization reaction with N-ethyldiethanolamine to obtain a water-rich environment-resistant alternating load reinforcement and sealing material. The end groups of the water-rich environment-resistant alternating load reinforcement and sealing material contain active isocyanate groups: -NCO.
[0016] Preferably, in step 1, the prepolymerization reaction temperature is 75-85℃, the reaction time is 1.5-2.5h, and the reaction is stopped when the NCO content in the system drops to 26.5%-30.5%. In step 2, the prepolymerization reaction temperature is 80-90℃, the reaction time is 1-2h, and the reaction is stopped when the NCO content in the system drops to 22.5%-27.5%. In step 3, the second prepolymer and the dihydroxy compound containing a rigid aromatic ring structure are first stirred at 40-50°C until completely dissolved, and then the temperature is raised to 75-85°C for prepolymerization for 1.5-2.5 hours. The reaction is stopped when the NCO content in the system drops to 17.5%-22.5%. In step 4, a polyol compound containing a tertiary amine structure is added dropwise to the third prepolymer. The temperature is controlled not to exceed 20°C during the addition, and the addition time is 60-90 minutes. After the addition is completed, the temperature is raised to 75-85°C and the reaction continues for 1-2 hours. The reaction is stopped when the NCO content in the system drops to 14.0%-20.0%.
[0017] Preferably, before the prepolymerization reaction, the raw materials containing active hydrogen are subjected to vacuum dehydration treatment to ensure that the water content of each active hydrogen-containing raw material is less than 0.1%; the dihydroxy compound containing a rigid aromatic ring structure is ground to a particle size of less than 80 mesh before dehydration and then vacuum dried at 100°C for 3 hours; each prepolymerization reaction is carried out under inert gas protection, and the inert gas is replaced 2-4 times; in step 4, when the polyol compound containing a tertiary amine structure is added dropwise, the circulating condensation system is turned on to ensure that the temperature control accuracy is ±1°C; the stirring speed in each step is 200-300 r / min.
[0018] Among them, raw materials containing active hydrogen refer to raw materials containing hydroxyl groups (-OH) and capable of reacting with isocyanate groups, including hydroxyl-terminated fluorosilicone modified diols, dihydroxy compounds containing dynamic disulfide bonds, dihydroxy compounds containing rigid aromatic ring structures, and polyol compounds containing tertiary amine structures.
[0019] Preferably, the molecular weight and degree of branching of the products are controlled by stepwise control of the NCO content of each prepolymerization product, specifically as follows: The NCO content of the first prepolymer obtained in step 1 is controlled to be 26.5%-30.5%. The NCO content of the second prepolymer obtained in step 2 is controlled to be 22.5%-27.5%. The NCO content of the third prepolymer obtained in step 3 is controlled to be 17.5%-22.5%. The NCO content of the final product obtained in step 4 is controlled to be 14.0%-20.0%.
[0020] Preferably, the above-mentioned water-rich environment-resistant alternating load reinforcement and sealing material is used in water-blocking reinforcement of tunnels, rail transit subgrades or underground engineering projects under conditions of water and high-frequency alternating loads.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention modifies the polyurethane backbone by modifying the fluorosilicone segments, which significantly reduces the surface polarity and interfacial tension of the material. This prevents the material from being washed away, diluted, or emulsified and lost in a water flow environment. At the same time, it inhibits excessive water intrusion and achieves controllable low expansion, thus solving the technical problems of easy collapse and excessive foaming of traditional polyurethane during underwater grouting.
[0022] This invention introduces chain extension segments containing dynamic disulfide bonds, enabling the material to automatically trigger a dynamic covalent reaction of disulfide bond breakage and recombination at room temperature, thereby achieving autonomous healing of microcracks without the need for external stimulation or artificial repair. This significantly improves the fatigue durability and service life of the material under high-frequency alternating loads.
[0023] This invention utilizes the synergistic effect of rigid aromatic ring reinforcing segments and fluorosilicone modified segments to form a molecular mechanism of rigid load-bearing and flexible buffering, enabling the material to possess both high compressive strength and high bonding strength as well as impact toughness. At the same time, the tertiary amine molecular segments endow the material with self-catalytic function, taking into account both sufficient construction operation time and rapid early strength establishment, perfectly adapting to the emergency rapid repair needs of tunnels, rail transit subgrades and other projects. Attached Figure Description
[0024] Figure 1 This is a reaction diagram for the preparation of the first prepolymer of the present invention.
[0025] Figure 2 This is a reaction diagram for the preparation of the second prepolymer of the present invention.
[0026] Figure 3 This is a reaction diagram for the preparation of the third prepolymer of the present invention.
[0027] Figure 4 The reaction diagram for the preparation of the water-rich environment-resistant alternating load-strengthening and sealing material of the present invention is shown.
[0028] Figure 5 The diagram illustrates the main repair problems of the water-rich environment-resistant alternating load reinforcing and sealing material of the present invention in engineering sites. Detailed Implementation
[0029] The present invention will now be described in further detail with reference to specific embodiments. However, this should not be construed as limiting the scope of the present invention to the following embodiments; all technologies implemented based on the content of the present invention fall within the scope of the present invention.
[0030] Unless otherwise specified, all raw materials used in the specific embodiments of this invention are commercially available industrial-grade products with a purity of not less than 98%; the 4,4'-diphenylmethane diisocyanate used is WANNATE® MDI-100 produced by Wanhua Chemical Group Co., Ltd.; the hydroxyl-terminated fluorosilicone diol used is TD-FS2001 produced by Fuzhou Taipuda New Materials Co., Ltd.; the 2-hydroxyethyl disulfide used is produced by Langfang Zhaoqin Energy Technology Co., Ltd.; the 2,2-di(4-hydroxyphenyl)propane used is an industrial-grade superior product produced by Baling Petrochemical Branch of China Petroleum & Chemical Corporation; and the N-ethyldiethanolamine used is produced by BASF (China) Co., Ltd. The above raw materials are for illustrative purposes only and do not constitute a limitation on the source of the raw materials used in this invention.
[0031] Example 1 This embodiment provides a method for preparing a reinforcing and sealing material resistant to alternating loads for water-rich environments, specifically including the following steps: (1) Raw material pretreatment The hydroxyl-terminated fluorosilane diol, 2-hydroxyethyl disulfide, 2,2-di(4-hydroxyphenyl)propane, and N-ethyldiethanolamine were subjected to vacuum dehydration treatment to control the moisture content of each raw material to below 0.1%. The 2,2-di(4-hydroxyphenyl)propane was ground to a particle size of less than 80 mesh, vacuum dried at 100℃ for 3 hours, and then sealed and stored in a moisture-proof environment. The reaction vessel was purged with nitrogen three times to ensure that the reaction system was free of water, oxygen, and mechanical impurities.
[0032] The hydroxyl-terminated fluorosilicone diol used in this invention is TD-FS2001 produced by Fuzhou Taipuda New Materials Co., Ltd., with a hydroxyl value of approximately 56 mgKOH / g. This raw material is a perfluoropolysiloxane diol with hydroxyl-terminated ends. The terminal hydroxyl groups are linked to perfluoroalkyl segments via -Si(CH3)2-, which can react with isocyanate groups to form urethane bonds, thereby introducing the fluorosilicone segments into the polyurethane backbone in the form of covalent bonds.
[0033] The chemical name of the hydroxyl-terminated fluorosiloxane diol (TD-FS2001) used in this invention is: a perfluoropolysiloxane diol with hydroxyl-terminated ends, and its molecular structure is as follows: HO-Rf-Si(CH3)2-[O-Si(CH3)2]mO-Si(CH3)2-Rf-OH, Rf is -(CH2)2-(CF2)5-, m is 1~16, and the hydroxyl value is approximately 56 mgKOH / g.
[0034] (2) Synthesis of the first prepolymer Add 1000g of 4,4'-diphenylmethane diisocyanate to the reactor, purge with nitrogen, and stir at 200-300 rpm. Add 150g of terminal hydroxyl fluorosilane diol, and mix at 25°C for 30 minutes until homogeneous. Slowly raise the temperature to 80°C and maintain the temperature for 2 hours for prepolymerization. Monitor the NCO content until it reaches 27.5%-29.0%, then stop the reaction. Cool to 25°C to obtain the first prepolymer: functional isocyanate prepolymer 1. See the specific reaction formula below. Figure 1 : Figure 1 In the middle, R f It is -(CH2)2-(CF2)5-; (3) Synthesis of the second prepolymer Slowly add 50g of 2-hydroxyethyl disulfide to the first prepolymer and stir at 25°C for 20min. Increase the temperature to 85°C and prepolymerize for 1.5h, controlling the NCO content at 23.5%-26.5%. Cool to 25°C to obtain the second prepolymer: functional isocyanate prepolymer 2. See the specific reaction formula below. Figure 2 : Figure 2 middle,
[0035]
[0036] (4) Synthesis of the third prepolymer Add 100g of pretreated 2,2-bis(4-hydroxyphenyl)propane to the second prepolymer and stir at 45℃ for 3 hours until completely dissolved, forming a transparent, homogeneous liquid. Gradually increase the temperature to 80℃ and stir for 2 hours to prepolymerize, stopping when the NCO content reaches 18.5%-21.5%. Cool down to 25℃ to obtain the third prepolymer: functional isocyanate prepolymer 3. See the specific reaction formula below. Figure 3 , Figure 3 middle,
[0037] (5) Synthesis of reinforcement and sealing materials resistant to alternating loads for water-rich environments Turn on the reactor's circulating condensation cooling system to ensure temperature control accuracy of ±1℃.
[0038] 50 g of N-ethyldiethanolamine was slowly added dropwise to the third prepolymer using a metering pump, with the temperature controlled to not exceed 20 °C throughout the process, and the addition time being 60-90 min. After the addition was complete, the temperature was raised to 80 °C, and the reaction was continued for 1.5 h.
[0039] When the NCO content reaches 15.5%-18.5%, the reaction should be stopped immediately. The material should be cooled to below 30°C, sealed in nitrogen-filled packaging, and stored away from light to obtain a water-rich environment-resistant alternating load reinforcing and sealing material.
[0040] The reaction equation is as follows Figure 4 .
[0041] In this embodiment, the mass proportions of each raw material component are shown in Table 1 below: Table 1 shows the raw material composition of Example 1.
[0042] The NCO content of the obtained material is 15.5%-18.5%.
[0043] This embodiment employs a four-step prepolymerization reaction to sequentially introduce fluorosilicone-modified segments, dynamic disulfide bonds, rigid aromatic ring-reinforced segments, and tertiary amine molecular segments into the polyurethane backbone. Each functional segment is stably linked to the backbone via covalent bonds, avoiding the phase separation and performance degradation issues inherent in physical blending. The NCO content is used as the endpoint control index for each reaction step, precisely regulating the molecular weight and branching degree of the product, thus providing a structural basis for achieving subsequent performance characteristics.
[0044] Example 2 This embodiment provides a method for preparing a reinforcing and sealing material resistant to alternating loads for use in water-rich environments. The difference between this method and Embodiment 1 lies in the different raw material ratios.
[0045] Specifically, the mass proportions of each raw material component are shown in Table 2 below: Table 2 shows the raw material composition of Example 2.
[0046] The preparation method is the same as in Example 1, and the NCO content of the obtained material is 18.0%-20.0%.
[0047] In this embodiment, the proportion of rigid aromatic ring reinforcing segments is relatively low, and the proportion of tertiary amine molecular segments is also reduced accordingly. The resulting material tends to be weakly rigid and has a slower curing rate, making it suitable for underwater reinforcement scenarios with a long construction window.
[0048] Example 3 This embodiment provides a method for preparing a reinforcing and sealing material resistant to alternating loads for use in water-rich environments. The difference between this method and Embodiment 1 lies in the different raw material proportions. Specifically, the mass proportions of each raw material component are shown in Table 3 below: Table 3 shows the raw material composition of Example 3.
[0049] The preparation method is the same as in Example 1, and the NCO content of the obtained material is 14.5%-18.5%.
[0050] In this embodiment, the proportion of fluorosilicone modified segments and dynamic disulfide bonds is relatively high, and the resulting material has both excellent hydrophobicity and higher self-healing efficiency, making it suitable for rapid water plugging and self-healing reinforcement projects in high-flow-rate water environments.
[0051] Example 4 This embodiment provides a method for preparing a reinforcing and sealing material resistant to alternating loads for use in water-rich environments. The difference between this method and Embodiment 1 lies in the different raw material proportions. Specifically, the mass proportions of each raw material component are shown in Table 4 below: Table 4 shows the raw material composition of Example 4.
[0052] The preparation method is the same as in Example 1, and the NCO content of the obtained material is 14.0%-16.5%.
[0053] In this embodiment, the ratio of rigid aromatic ring reinforcing segments and tertiary amine molecular segments is relatively high, and the resulting material has high strength, rapid curing and good self-healing properties, making it suitable for engineering scenarios with high early strength requirements such as emergency repairs and rapid traffic opening.
[0054] Laboratory performance testing The performance of the materials obtained in each embodiment was tested according to the following standards and methods, and the results are shown in Table 5.
[0055] Table 5. Performance test results of materials obtained in each embodiment.
[0056] As can be seen from the data in Table 5: (1) The material has excellent hydrophobic and anti-erosion properties and low expansion properties, making it suitable for water-rich environments: All examples showed no emulsification after being stirred and dispersed in water, indicating that the slurry will not be diluted or washed away by the water flow when it enters the flowing groundwater environment; the underwater expansion ratio of the four groups of samples was only 1.01-1.07, without the problem of excessive foaming and loosening when exposed to water. Among them, the expansion ratio of Example 3 was as low as 1.01, with the best hydrophobic and water-blocking effect, which is suitable for high-velocity flowing water blocking scenarios; the expansion ratio of Example 2 increased slightly to 1.07, which is still far superior to traditional polyurethane grouting materials.
[0057] (2) The material combines rigidity and flexibility and has excellent mechanical properties: the compressive strength range of the material is 43-62MPa, and the maximum compressive deformation is 79%-87%, achieving a balance between high strength and high toughness.
[0058] (3) The material has excellent resistance to alternating loads, fatigue resistance and durability: After millions of high-frequency alternating fatigue loading, the strength retention rate of the four groups of samples is maintained at more than 89%, of which the fatigue strength retention rate of Example 3 is 91.5%, which is the best performance.
[0059] (4) The material has excellent resistance to acid and alkali and damp heat aging: After 500h of double 85 damp heat aging, the compressive strength retention rate of all samples is higher than 97%; after long-term immersion in 5% sulfuric acid and 5% strong alkali, the strength retention rate is generally higher than 92%, and the resistance to media erosion is excellent.
[0060] (5) Adaptation dimension of construction curing kinetics: The material curing time can be flexibly adjusted from 26 to 65 minutes, and the core of the adjustment is the amount of tertiary amine polyol added: The curing time of Example 4 is only 26 minutes, and the curing speed is fast, which is suitable for emergency tunnel repair and rapid traffic conditions; the curing time of Example 2 is extended to 65 minutes, with a sufficient construction operation window, which is suitable for slow grouting reinforcement of fine cracks and complex strata. The hydrophobic and water-slowing effect of fluorosilicone segments combined with the gradient catalysis of tertiary amine achieves the ideal construction characteristics of slow infiltration in the early stage and fast curing in the later stage.
[0061] In summary, the material possesses four core properties: hydrophobicity and water blocking, mechanical strength, fatigue resistance and durability, and curing speed. All embodiments simultaneously exhibit comprehensive advantages such as non-collapse underwater, low expansion, high strength and toughness, strong fatigue resistance, acid and alkali aging resistance, and adjustable construction window, perfectly matching the engineering repair needs of water-rich roadbeds and tunnel linings under high-frequency alternating load coupled with water environment.
[0062] Example 5 This example is a comparative example, differing from Example 4 in that: Sample 1 uses DL1000, which has a similar hydroxyl value to the terminal hydroxyl fluorosilane diol, for equivalent substitution; Samples 2-4 use PEG-200 to replace the missing monomer components (2-hydroxyethyl disulfide, 2,2-di(4-hydroxyphenyl)propane, and N-ethyldiethanolamine) according to the principle of equivalent hydroxyl content, to maintain the total number of hydroxyl groups in the system consistent with Example 4, so that the final NCO content of each comparative sample is similar to that of Example 4 (14.0%-16.5%). DL1000 has a similar hydroxyl value to the terminal hydroxyl fluorosilane diol, and the amount of PEG-200 added is determined based on the hydroxyl value (the hydroxyl values of 2-hydroxyethyl disulfide, 2,2-di(4-hydroxyphenyl)propane, N-ethyldiethanolamine, and PEG-200 are 727.5, 491.6, 842.1, and 561.0 mgKOH / g, respectively).
[0063] The specific configuration examples are shown in Table 6 below: Table 6 shows the raw material composition of various materials in Example 5.
[0064] Note: In each comparative sample, the number of hydroxyl moles of missing components was supplemented by PEG-200 according to the principle of equal overall hydroxyl equivalent. The hydroxyl values of 2-hydroxyethyl disulfide, 2,2-di(4-hydroxyphenyl)propane, N-ethyldiethanolamine, and PEG-200 are 727.5, 491.6, 842.1, and 561.0 mgKOH / g, respectively. After conversion based on equal overall hydroxyl equivalent, 5.95 parts, 10.9 parts, and 9.6 parts of PEG-200 were used to replace 5 parts of 2-hydroxyethyl disulfide, 12 parts of 2,2-di(4-hydroxyphenyl)propane, and 7 parts of N-ethyldiethanolamine, respectively.
[0065] The calculation formula is as follows:
[0066] The letters above represent (see table below for details), where N is the NCO content of the alternating load-resistant sealing material used in water-rich environments, and M is the total mass of raw materials used (see Table 7 below). Table 7 is a summary table of the raw material composition used.
[0067] The main performance of each sample is summarized in the table below: Table 8 is a summary table of the performance of multiple material samples in Example 5.
[0068] Example 5 is a single-factor deletion control experiment: fluorosilicone segments (sample 1), dynamic disulfide bonds (sample 2), rigid aromatic ring bisphenol A (sample 3), and tertiary amine catalytic segments (sample 4) were removed to verify the irreplaceability and partial synergistic effect of the four functional components. Based on the table above, the core conclusions are as follows: (1) Rigid aromatic ring + tertiary amine crosslinking is the core support for strength. The compressive strength of sample 3, which lacks bisphenol A, drops sharply to 32 MPa (62 MPa in complete example 4); the crosslinking density of sample 4, which lacks tertiary amine, is insufficient, with a compressive strength of only 27 MPa and a deformation drop to 56%, resulting in a significant increase in material brittleness. This proves that the rigid aromatic ring provides the cohesive framework and the tertiary amine promotes dense crosslinking, and the synergy between the two is a necessary basis for high strength and toughness.
[0069] (2) The synergistic effect of disulfide bonds and fluorosilicone hydrophobicity on fatigue life, with samples lacking dynamic disulfide bonds, 2, 3 × 10 6 After fatigue testing, the strength retention rate was only 65.12%; sample 1, lacking fluorine and silicon, had a fatigue retention rate of only 79.31% due to weakened dynamic bond interactions caused by moisture erosion; sample 4, lacking tertiary amine, had the lowest fatigue retention rate of only 56.45% due to loose cross-linking. This indicates that the synergistic mechanism of "fluorine and silicon water-proof protection, disulfide bond stability, and self-repair" is indispensable.
[0070] (3) Regarding the resistance to aging of multiple protective chains, the performance of sample 1, which lacks the hydrophobic barrier of fluorosilicone, is the most significantly reduced: after immersion in 5% sulfuric acid for 30 days, the strength retention rate is only 58.32% and the alkali resistance is only 59.59%, almost losing the ability to resist chemical corrosion; the other three groups of samples lacking a single component also saw their wet heat and acid-base aging retention rates drop to below 85%, far lower than the level of over 94% of the complete formula, proving that only the synergy of the four-layer protective network can achieve long-term weather resistance.
[0071] (4) The synergistic effect of fluorine and silicon and tertiary amine on the performance of water-rich conditions: Sample 1, which lacks fluorine and silicon, is in a semi-emulsion state when stirred in water, and the underwater expansion ratio increases to 1.27. It is easily dispersed by moving water and foams loosely; Sample 4, which lacks tertiary amine, has a solidification time of up to 120 minutes and a very slow solidification speed, which cannot meet the requirements of emergency rescue and construction efficiency.
[0072] In summary, the absence of any one of the four functional segments results in a precipitous decline in the corresponding core properties of the material, with overall performance far below that of the complete formulation. This demonstrates that the multi-component covalent bonding of this invention is not a simple superposition of functions, but rather forms a synergistic system that supports each other, producing unexpected comprehensive technical effects that cannot be achieved by single-component or two-component combinations, thus strongly supporting the inventiveness of the invention.
[0073] Engineering application verification The modified polyurethane bonding material prepared in Example 4 for reinforcing and sealing roadbeds under alternating loads in water-rich environments was applied to a section of a subway tunnel that passes under a highly water-rich sand layer. The lining structure had multiple through cracks, the dynamic water flow velocity was 0.8-1.2 m / s, and the long-term operation of the train caused continuous high-frequency vibrations.
[0074] Construction process: A single-component direct grouting process is adopted, eliminating the need for on-site mixing. The grouting pressure is 0.4-1.0 MPa, and a low-pressure slow grouting method is used for areas with high-speed flowing water. The on-site measured solidification time is approximately 25 minutes. After entering the water body, the grout maintains a continuous form without dispersing, emulsifying, or significant overflow or loss.
[0075] Seven days after construction, core drilling tests were conducted on the grouting solidified body: the solidified body was intact and dense, without honeycomb pores, and the measured compressive strength was 52 MPa. The bond interface was firm and there was no debonding. During the continuous monitoring period of 6 months, there were no new cracks, no debonding or loosening, and no recurrence of water seepage in the reinforced area, and the self-healing effect was stable.
[0076] Engineering verification results show that the material of this invention can achieve underwater non-collapse, low expansion, high-strength curing, and room-temperature self-healing under the coupled conditions of high-velocity water and high-frequency alternating loads, effectively solving the engineering problems of traditional materials being easily washed away, fatigued, and damaged under such conditions. Figure 5 As shown.
[0077] Explanation of the mechanism and synergistic effects of this invention: This invention integrates fluorosilicone-modified segments, dynamic disulfide bonds, rigid aromatic ring-reinforced segments, and tertiary amine molecular segments onto a single polyurethane molecular backbone through molecular design. These functional segments do not exist in isolation but rather achieve comprehensive properties that cannot be achieved by a single component or any combination of two through a synergistic mechanism. The segments influence and cooperate with each other at the molecular scale, forming an organic unity in four dimensions: hydrophobicity and erosion resistance, durability, high load-bearing capacity, and controllable rapid curing. This effectively solves common problems of traditional polyurethane grouting and consolidation materials, such as poor chemical resistance, susceptibility to damage propagation under alternating loads, easy erosion upon contact with water, loose foaming, and poor adaptability to curing and construction. This comprehensive performance cannot be expected by simply introducing and superimposing individual functional components, demonstrating the non-obviousness of this invention.
[0078] This invention is based on a rigid-flexible and superior anti-alternating load bearing system with quaternary functional chain segment covalent integrated molecular synergistic design. Through integrated molecular covalent grafting design, rigid aromatic ring reinforcing segments, fluorosilicone modified flexible segments, chain extension segments containing dynamic disulfide bonds, and tertiary amine molecular catalytic segments are integrated into the same rigid polyurethane backbone. Relying on the molecular-scale coupling and synergy of the four types of segments, a unified comprehensive performance of ultra-high structural strength, high toughness deformation, and fatigue resistance to millions of alternating loads is achieved.
[0079] In terms of structural design, the main chain diphenylmethane unit and the rigid aromatic ring segments of bisphenol A rely on π-π stacking of benzene rings and hydrogen bonding of urethane esters to construct high-density rigid hard-segment nanocrystalline domains, serving as the core strong load-bearing skeleton of the material and significantly improving the intermolecular cohesive energy and structural modulus. Complementing this, low surface energy fluorosilicone modified segments are uniformly dispersed in the gaps between the rigid skeleton, forming ordered nanophase-separated flexible buffer microregions. These, together with dynamic disulfide bonds penetrating the molecular chain, construct stress dynamic dissipation channels, achieving a molecular-level rigid-flexible synergistic mechanism of concentrated load bearing in hard segments, buffer energy absorption in soft segments, and real-time repair of micro-damage by dynamic bonds. In terms of performance, the material exhibits outstanding ultimate mechanical properties: compressive strength can reach 43-62 MPa; it also possesses excellent deformation toughness, with the maximum compressive deformation stably maintained at 79%-87%, overcoming the inherent contradiction of traditional rigid grouting materials being high-strength but brittle, and pure fluorosilicone modified materials having sufficient toughness but insufficient load bearing.
[0080] A multi-layered synergistic protection system, comprising hydrophobic shielding, rigid dense barrier, and dynamic self-healing bonds, provides ultra-long service durability under water-rich acid-alkali alternating conditions. This invention constructs a triple-progressive synergistic protection network, enabling the material to achieve long-term stable durability far exceeding that of single-modified polyurethane under harsh conditions such as flowing groundwater, acid-alkali corrosion, and millions of train alternating vibrations.
[0081] In terms of resistance to water, acid, alkali, and chemical corrosion: the rigid aromatic ring of bisphenol A and its aromatic hard segments form a dense cross-linked bulk barrier, and the dense hydrogen bonds and benzene ring stacking significantly reduce the gaps between molecular chains, hindering the diffusion and penetration of acid and alkali ions and water molecules into the material; the fluorosilicone modified segments spontaneously accumulate at the material's internal and external interfaces, constructing a molecular-level hydrophobic shielding layer, blocking the capillary penetration channels of aqueous solutions, and forming a dual anti-corrosion structure of "dense internal physical barrier + surface hydrophobic chemical shielding". Tests show that the material retains ≥92.5% compressive strength after 30 days of immersion in 5% sulfuric acid, ≥93.5% after 30 days of immersion in 5% sodium hydroxide, and at least 97% mechanical strength after 500 hours of humid heat aging at 85℃ / 85RH. It does not pulverize or de-adhere at the interface under long-term exposure to strata acids, alkalis, and groundwater.
[0082] In terms of fatigue durability under high-frequency alternating loads: the aforementioned dual dense hydrophobic barrier significantly reduces the initiation of early microcracks induced by water, and the dynamic disulfide bonds uniformly distributed in the molecular chains form a second dynamic self-healing protection mechanism. Conventional disulfide-modified polyurethanes without fluorosilicone shielding suffer from significantly reduced self-healing efficiency due to competitive inhibition of reversible disulfide bond breakage and recombination reactions by water molecules in an aqueous environment. In contrast, the fluorosilicone hydrophobic microenvironment of this invention isolates moisture interference, ensuring continuous and stable dynamic exchange of disulfide bonds in humid and underwater environments. When microcracks are generated under alternating loads, the molecular chains can be autonomously reconstructed, preventing crack propagation into macroscopic damage. 3×10 6 After high-frequency fatigue loading, the material strength retention rate remains stable at 89.3%-91.5%, eliminating the need for frequent repairs in long-term vibration subgrade scenarios such as subways and high-speed railways.
[0083] This invention leverages the synergistic regulation of molecular hydrophobic shielding and tertiary amine gradient catalysis to address the industry pain points of traditional polyurethane grouting at the molecular reaction mechanism level, such as water-induced collapse, over-foaming, and difficulty in adapting curing speeds to the dual needs of emergency and conventional grouting. The dual regulation of fluorosilicone water barrier and tertiary amine gradient catalysis achieves a low expansion ratio in water-rich environments and wide-window controllable construction adaptability. In terms of low expansion ratio and anti-dispersion performance in water-rich and fractured formations: the low surface energy of the fluorosilicone modified segments forms a continuous hydrophobic barrier, physically preventing external groundwater from intruding into the isocyanate reaction system; at the same time, the tertiary amine segments bonded to the main chain have selective catalytic characteristics, and the dual mechanism of "physical water blocking + chemical selective catalysis" works synergistically, resulting in an expansion ratio of only 1.01-1.07, which is far lower than the expansion level of conventional grouting polyurethane; in the stirring test in the flowing water environment, the grout completely settles to the bottom without emulsification and dispersion, and will not be passively dispersed and diluted by the water flow during grouting. The solidified body is dense inside without honeycomb-like loose pores, completely solving the problem of loose foaming and sealing failure in grouting of water-rich and fractured formations.
[0084] In terms of compatibility with construction operations and curing kinetics: the tertiary amine groups covalently grafted onto the molecular chain form a gradient catalytic synergistic effect with the hydrophobic segments of fluorosilicone. Fluorosilicone slows down the penetration of water, while the catalytic activity of the tertiary amine is gradually activated as water penetrates, creating an ideal curing curve of "low viscosity and slow reaction in the early stage, and rapid cross-linking and strong curing in the later stage." The viscosity increases slowly in the early stage, and the setting time can be flexibly controlled in the range of 26-65 minutes, providing ample grouting operation window to fully penetrate the gaps in the roadbed gravel and the fine cracks in the lining. The cross-linking rate increases rapidly in the later stage, establishing high consolidation strength in a short time, and is suitable for both conventional long-term reinforcement and rapid opening of tunnels after emergency repairs.
[0085] In terms of crack penetration grouting performance: the low viscosity characteristics in the early stage of curing, combined with the low surface tension of fluorosilicone segments, result in excellent grout penetration and leveling performance. It can autonomously fill micron-level fine cracks, closely adhere to the soil and concrete interface, and avoid voids and stratification, which greatly improves the overall reinforcement and seepage prevention of the roadbed and reduces the probability of leakage recurrence in the later stage.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A water-rich environment-resistant alternating load-strengthening and sealing material, characterized in that, The material comprises a rigid polyurethane backbone, on which the following four functional side groups or block structures are grafted via urethane bonds: Fluorosilicone modified segments, wherein the fluorosilicone modified segments are derived from hydroxyl-terminated fluorosilicone diols, and have the general structural formula as follows: HO-R f -Si(CH3)2-[O-Si(CH3)2] m -O-Si(CH3)2-R f -OH, where R f The expression is -(CH2)2-(CF2)5-, and m is 1-16; A chain extension segment containing dynamic disulfide bonds, wherein the chain extension segment containing dynamic disulfide bonds is derived from 2-hydroxyethyl disulfide, and its structural formula is: HO-CH2-CH2-SS-CH2-CH2-OH; The rigid aromatic ring reinforcing segment is derived from 2,2-bis(4-hydroxyphenyl)propane, i.e., bisphenol A; The tertiary amine molecular chain segment, derived from N-ethyldiethanolamine, has the following structural formula: HO-CH2-CH2-N(C2H5)-CH2-CH2-OH.
2. The water-rich environment-resistant alternating load reinforcing and sealing material according to claim 1, characterized in that, The end groups of the rigid polyurethane backbone contain active isocyanate groups: -NCO.
3. The water-rich environment-resistant alternating load reinforcing and sealing material according to claim 1, characterized in that, The rigid polyurethane backbone is provided by an aromatic diisocyanate, specifically 4,4'-diphenylmethane diisocyanate; the rigid polyurethane backbone contains diphenylmethane structural units introduced by the 4,4'-diphenylmethane diisocyanate.
4. The water-rich environment-resistant alternating load reinforcing and sealing material according to claim 1, characterized in that, The mass ratio of each raw material component used to prepare the material is as follows: 100 parts aromatic diisocyanate, 12-18 parts hydroxyl-terminated fluorosilicone modified diol, 4-6 parts dihydroxy compound containing dynamic disulfide bonds, 8-12 parts dihydroxy compound containing rigid aromatic ring structure, and 4-7 parts polyol compound containing tertiary amine structure.
5. The water-rich environment-resistant alternating load reinforcing and sealing material according to claim 1, characterized in that, The NCO content of the material is 14.0%-20.0%.
6. A method for preparing a water-rich environment-resistant alternating load-strengthening and sealing material according to any one of claims 1-5, characterized in that, Includes the following steps: Step 1: 4,4'-diphenylmethane diisocyanate is subjected to a first prepolymerization reaction with a hydroxyl-terminated fluorosilicone modified diol to obtain a first prepolymer containing fluorosilicone modified segments. Step 2: The first prepolymer is subjected to a second prepolymerization reaction with 2-hydroxyethyl disulfide to obtain a second prepolymer, which contains fluorosilicone modified segments and dynamic disulfide bonds; Step 3: The second prepolymer is subjected to a third prepolymerization reaction with 2,2-bis(4-hydroxyphenyl)propane to obtain a third prepolymer, wherein the third prepolymer contains fluorosilicone modified segments, dynamic disulfide bonds and rigid aromatic ring structures; Step 4: The third prepolymer is subjected to a fourth prepolymerization reaction with N-ethyldiethanolamine to obtain a water-rich environment-resistant alternating load reinforcement and sealing material. The end groups of the water-rich environment-resistant alternating load reinforcement and sealing material contain active isocyanate groups: -NCO.
7. The method for preparing the water-rich environment-resistant alternating load-strengthening and sealing material according to claim 6, characterized in that, In step 1, the prepolymerization reaction temperature is 75-85℃, the reaction time is 1.5-2.5h, and the reaction is stopped when the NCO content in the system drops to 26.5%-30.5%. In step 2, the prepolymerization reaction temperature is 80-90℃, the reaction time is 1-2h, and the reaction is stopped when the NCO content in the system drops to 22.5%-27.5%. In step 3, the second prepolymer and the dihydroxy compound containing a rigid aromatic ring structure are first stirred at 40-50°C until completely dissolved, and then the temperature is raised to 75-85°C for prepolymerization for 1.5-2.5 hours. The reaction is stopped when the NCO content in the system drops to 17.5%-22.5%. In step 4, a polyol compound containing a tertiary amine structure is added dropwise to the third prepolymer. The temperature is controlled not to exceed 20°C during the addition, and the addition time is 60-90 minutes. After the addition is completed, the temperature is raised to 75-85°C and the reaction continues for 1-2 hours. The reaction is stopped when the NCO content in the system drops to 14.0%-20.0%.
8. The preparation method according to claim 6, characterized in that, Before the prepolymerization reaction, the raw materials containing active hydrogen are subjected to vacuum dehydration treatment to ensure that the moisture content of each active hydrogen-containing raw material is less than 0.1%; the dihydroxy compound containing a rigid aromatic ring structure is ground to a particle size of less than 80 mesh before dehydration and then vacuum dried at 100℃ for 3 hours; each prepolymerization reaction is carried out under inert gas protection, and the inert gas is replaced 2-4 times; in step 4, when the polyol compound containing a tertiary amine structure is added dropwise, the circulating condensation system is turned on to ensure that the temperature control accuracy is ±1℃; the stirring speed in each step is 200-300 r / min.
9. The preparation method according to claim 6, characterized in that, The molecular weight and degree of branching of the products are controlled by stepwise control of the NCO content of each prepolymerization product, specifically as follows: The NCO content of the first prepolymer obtained in step 1 is controlled to be 26.5%-30.5%. The NCO content of the second prepolymer obtained in step 2 is controlled to be 22.5%-27.5%. The NCO content of the third prepolymer obtained in step 3 is controlled to be 17.5%-22.5%. The NCO content of the final product obtained in step 4 is controlled to be 14.0%-20.0%.