A method for synthesizing an environmentally friendly low-viscosity modified resin

By using solvent-free synthesis processes and bio-based materials, combined with dynamic disulfide bond structures, a low-viscosity, high-self-healing-efficiency waterborne modified resin was prepared. This solved the problem of difficulty in achieving multiple performance dimensions in existing technologies, and improved both environmental friendliness and performance, making it suitable for various application scenarios.

CN123107029APending Publication Date: 2026-11-17ANHUI WANFO LAKE COATINGS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611188334.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing waterborne modified resin synthesis technologies cannot simultaneously meet the requirements of low VOC emissions, low production viscosity, high self-healing efficiency, and high environmental friendliness. Furthermore, the synthesis process suffers from problems such as excessively high viscosity, residual organic solvent odor, and biotoxicity.

Method used

A solvent-free synthesis process was adopted to prepare isocyanate-terminated polyurethane prepolymer by reacting bio-based polyol with diisocyanate. The prepolymer was then extended by adding an aliphatic chain extender containing dynamic disulfide bonds, mixed with epoxy resin, and the viscosity was adjusted by using a bio-based monofunctional epoxy reactive diluent. Finally, organic acids such as glacial acetic acid and lactic acid were used as neutralizing agents to disperse the prepolymer in deionized water to obtain a waterborne modified resin.

Benefits of technology

This water-based modified resin achieves low viscosity, low VOC, high self-healing efficiency, and high environmental friendliness, making it suitable for home decoration wood coating, food contact grade flexible packaging lamination, and indoor building protection, and possessing high value for promotion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107029A_ABST
    Figure CN123107029A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of waterborne modified resin synthesis technology and discloses an environmentally friendly low-viscosity modified resin synthesis method. A bio-based polyol is reacted with diisocyanate in a solvent-free manner to obtain an NCO-terminated prepolymer. Disulfide bonds are introduced using an aliphatic chain extender containing dynamic disulfide bonds to obtain a terminal amino prepolymer. This prepolymer is then reacted with epoxy resin via amine-epoxy ring-opening addition to obtain a polyurethane-epoxy hybrid intermediate. A bio-based monofunctional epoxy reactive diluent is added to reduce viscosity, and after neutralization and salt formation, the mixture is dispersed in water to obtain an aqueous dispersion. The film achieves self-healing through disulfide bond heat exchange. The modified resin prepared by this method has low viscosity, low volatile organic compound content, excellent self-healing efficiency after film formation, and good mechanical service performance, making it suitable for applications in coatings, adhesives, and other fields. Its overall performance is significantly superior to existing similar products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of water-based modified resin synthesis technology, and in particular to an environmentally friendly low-viscosity modified resin synthesis method. Background Technology

[0002] Waterborne modified resins, as core film-forming substances in environmentally friendly coatings and adhesives, are widely used in wood coating, building protection, and flexible packaging composites. With increasingly stringent domestic standards for volatile organic compound (VOC) emissions, the industry's demand for low-VOC, high-performance, and long-service-life waterborne modified resins continues to rise. However, existing technologies still suffer from shortcomings in achieving a balance across multiple performance dimensions, which is the core challenge in current research and development in this field.

[0003] The current mainstream conventional waterborne polyurethane-epoxy hybrid resin synthesis technology uses a prepolymer dispersion method. First, isocyanate-terminated polyurethane prepolymers are prepared by reacting polyols with isocyanates. Then, these prepolymers are grafted with epoxy resin, hybridized, neutralized, and dispersed to obtain the waterborne system. The resin prepared by this technology exhibits high mechanical strength and good chemical resistance after film formation, making it the most widely used waterborne industrial resin category in the market. However, this technology lacks a self-healing structure, making the coating prone to protective failure after scratches from external forces, resulting in a shorter service life. Furthermore, the system viscosity is easily excessively high during synthesis, requiring the addition of organic solvents to adjust the viscosity. This makes it difficult for the final product to meet stringent environmental protection requirements for VOC content. Conventionally used alkanolamine neutralizers have issues with residual odor and high biotoxicity, resulting in insufficient environmental performance.

[0004] Another publicly disclosed technology for preparing self-healing waterborne resins containing dynamic disulfide bonds achieves a heating self-healing function by introducing disulfide bonds into the polyurethane chain segments, effectively improving the service life of the coating. However, the ratio of chain extender to isocyanate is unreasonable during the chain extension process. Either the amount of disulfide bond introduced is insufficient, resulting in low self-healing efficiency, or the chain extension is excessive, resulting in excessively high viscosity of the prepolymer. This makes the subsequent water dispersion process difficult and still requires the addition of petrochemical diluents to reduce viscosity, which increases production costs and reduces the bio-based environmental protection attributes of the product, making it difficult to meet the application requirements of high-end environmental protection products.

[0005] Existing technologies have consistently failed to simultaneously meet the multiple requirements of low VOC emissions, low production viscosity, high self-healing efficiency, and high environmental friendliness. There is an urgent need to develop high-performance, environmentally friendly waterborne modified resin synthesis technology that is suitable for large-scale industrial production, thereby filling the gaps in the industry's existing technologies. Summary of the Invention

[0006] To address the problems of insufficient self-healing efficiency, excessively high prepolymer viscosity, high VOC content, and insufficient environmental protection properties of existing self-healing waterborne resins, this invention provides a method for synthesizing an environmentally friendly low-viscosity modified resin.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: An environmentally friendly method for synthesizing a low-viscosity modified resin includes the following steps: S1. Bio-based polyols and diisocyanates are mixed and reacted under solvent-free conditions to prepare isocyanate-terminated polyurethane prepolymers. S2. Add an aliphatic chain extender containing dynamic disulfide bonds to the polyurethane prepolymer to carry out a chain extension reaction, introduce a dynamic disulfide bond structure, and obtain an amino-terminated polyurethane prepolymer. S3. The amino-terminated polyurethane prepolymer is mixed with epoxy resin to undergo an amine-epoxy ring-opening addition reaction to obtain a polyurethane-epoxy hybrid intermediate. S4. Add a bio-based monofunctional epoxy reactive diluent to the polyurethane-epoxy hybrid intermediate to adjust the viscosity of the system, then add a neutralizing agent to neutralize it into a salt, and disperse it in deionized water to obtain an aqueous modified resin dispersion. After the aqueous modified resin dispersion forms a film, the coating self-repair is achieved by utilizing the exchange reaction of the dynamic disulfide bonds under heating conditions.

[0008] Furthermore, the bio-based polyol in S1 is at least one of polylactic acid glycol, polycarbonate glycol, and cashew phenolic diol; the diisocyanate is at least one of isophorone diisocyanate, hexamethylene diisocyanate, and dicyclohexylmethane diisocyanate; the reaction temperature is 70℃~85℃; the reaction time is 2 hours~4 hours; and the molar ratio of isocyanate to hydroxyl group is 1.2~1.8:1.

[0009] Furthermore, the aliphatic chain extender containing dynamic disulfide bonds in S2 is an aliphatic diamine containing dynamic disulfide bonds, the molar ratio of the active functional group of the chain extender to the isocyanate group in the polyurethane prepolymer is 1.1~1.5:1, the reaction temperature is 60℃~75℃, and the reaction time is 1 hour~2 hours.

[0010] Furthermore, the epoxy resin in S3 is at least one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, and hydrogenated bisphenol A type epoxy resin, the molar ratio of the epoxy group of the epoxy resin to the terminal amino group of the amino-terminated polyurethane prepolymer is 1.1~1.5:1, the ring-opening addition reaction temperature is 70℃~80℃, and the reaction time is 1.5 hours~3 hours.

[0011] Furthermore, the bio-based monofunctional epoxy reactive diluent in S4 is at least one of cashew phenol glycidyl ether, rosin-based glycidyl ether, and soybean oil-based glycidyl ether, and the amount of diluent added accounts for 5% to 15% of the total mass of the polyurethane-epoxy hybrid intermediate.

[0012] Furthermore, the neutralizing agent in S4 is at least one of glacial acetic acid, lactic acid, and citric acid, with a neutralization degree of 80% to 100%, and the amount of deionized water added controls the solid content of the final waterborne modified resin dispersion to be 40% to 65%.

[0013] Furthermore, the prepared waterborne modified resin dispersion has a rotational viscosity of 300 mPa·s to 800 mPa·s at 25°C and a volatile organic compound content of less than 20 g / L.

[0014] Furthermore, after the prepared water-based modified resin is formed into a film, it is placed at 60°C for 2 hours, and the scratch repair efficiency is not less than 85%.

[0015] Furthermore, the number-average molecular weight of the bio-based polyol is 500-3000, and the hydroxyl functionality is 2.

[0016] Furthermore, in the S4 process, the stirring speed is 800 rpm to 1500 rpm, and the dispersion time is 20 minutes to 40 minutes.

[0017] The present invention has the following beneficial effects: This invention adjusts the molar ratio of the active functional groups of the aliphatic diamine chain extender containing dynamic disulfide bonds to the isocyanate groups in the polyurethane prepolymer. This ensures that a sufficient amount of dynamic disulfide bonds are introduced to support the self-healing performance of the coating, while avoiding the problem of excessive prepolymer viscosity caused by excessive chain extension. It effectively solves the defects of existing self-healing waterborne resins, such as insufficient self-healing efficiency and difficulty in water dispersion due to excessive prepolymer viscosity. It also takes into account both the service life of the coating and the operability of the synthesis process.

[0018] This invention employs a solvent-free synthesis process combined with a bio-based monofunctional epoxy reactive diluent to adjust the viscosity of the system. It can meet the viscosity requirements for water dispersion without the need to introduce traditional organic solvents or petrochemical diluents. This effectively solves the defects of existing technologies that rely on organic solvents to adjust viscosity, resulting in high volatile organic compound content and insufficient environmental protection properties of the product. At the same time, it reduces the control of hazardous chemicals and raw material costs in the synthesis process.

[0019] This invention uses organic acids such as glacial acetic acid, lactic acid, and citric acid as neutralizing agents for salt formation, replacing traditional alkanolamine neutralizing agents. This effectively solves the defects of existing neutralizing agents, such as strong residual odor and high biotoxicity, further expanding the application scope of the product. The environmentally friendly low-viscosity modified resin synthesized by this method has multiple performance advantages, including low system viscosity, low volatile organic compound content, and high self-healing efficiency. It is suitable for applications with high requirements for environmental protection and service life, such as home decoration wood coating, food contact grade flexible packaging lamination, and indoor building protection. It can achieve large-scale mass production without adjusting the equipment parameters of existing water-based resin industrial production lines, and has high promotion and application value in the field of water-based industrial resins. Attached Figure Description

[0020] Figure 1 This is a flowchart of an environmentally friendly low-viscosity modified resin synthesis method proposed in this invention. Figure 2 This is a bar chart showing the comparison of the core performance of each sample proposed in this invention. Figure 3 This is a line graph showing the change in self-healing efficiency as a function of heating time, as proposed in this invention. Figure 4 Radar charts showing the comprehensive performance of each sample proposed in this invention; Figure 5 This is a line graph showing the change in viscosity retention rate of the system under accelerated storage conditions at 60°C as proposed in this invention. Detailed Implementation

[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] The scratch repair efficiency test method in this embodiment is as follows: Scratch preparation was performed using a standardized scratch apparatus as specified in GB / T 9279.1-2015 "Determination of Scratch Resistance of Paints and Varnishes Part 1: Constant Load Method". A fully cured coating test panel with a dry film thickness of 50 μm was prepared. A continuous single-line scratch with a width of 20 μm and a depth of 30 μm was created on the coating surface using a specified scratching needle. The scratched test panel was then placed in a 60℃ constant temperature drying oven for 2 hours. The cross-sectional profile was scanned along the longitudinal direction of the scratch using a laser confocal microscope, and the initial scratch depth h0 and the remaining scratch depth h1 after heat preservation repair were measured. The scratch repair efficiency was calculated using the following formula: In the formula: h0 represents the scratch repair efficiency; h1 represents the initial scratch depth; h1 represents the remaining scratch depth after heat preservation at 60℃ for 2 hours.

[0023] Example 1

[0024] S1: Take 100g of polylactic acid glycol with a number average molecular weight of 1000 and a hydroxyl functionality of 2, mix it with 44.4g of isophorone diisocyanate, the molar ratio of isocyanate to hydroxyl is 1.4:1, heat to 75℃, and react for 3 hours under solvent-free conditions to obtain isocyanate-terminated polyurethane prepolymer. This step adopts a solvent-free synthesis process, which solves the defect of high VOC caused by the addition of organic solvents in the existing technology.

[0025] S2: Add 30.4 g of dithiodiethylamine to the above polyurethane prepolymer. The molar ratio of the amino group of dithiodiethylamine to the isocyanate group in the polyurethane prepolymer is 1.2:1. React at 65°C for 1.5 hours to obtain an amino-terminated polyurethane prepolymer. This step uses dithiodiethylamine as a chain extender to introduce a dynamic disulfide bond structure, which solves the defect of insufficient self-healing efficiency in the existing technology.

[0026] S3: Add 48.5g of bisphenol F type epoxy resin. The molar ratio of the epoxy group of the epoxy resin to the terminal amino group of the amino-terminated polyurethane prepolymer is 1.2:1. Heat to 75℃ and react for 2 hours to obtain a polyurethane-epoxy hybrid intermediate.

[0027] S4: Add 17.86g of cashew phenol glycidyl ether, accounting for 8% of the total mass of the polyurethane-epoxy hybrid intermediate, to adjust the viscosity of the system. Add lactic acid to adjust the neutralization degree to 90%. Add 330g of deionized water at a stirring speed of 1200 rpm and disperse for 30 minutes to obtain an aqueous modified resin dispersion with a solid content of 45%. This step uses a bio-based active diluent to reduce viscosity and an organic acid to neutralize, which solves the defects of excessively high prepolymer viscosity and poor environmental friendliness of neutralizing agents in the existing technology.

[0028] Example 2

[0029] S1: Take 100g of polycarbonate diol with a number average molecular weight of 2000 and a hydroxyl functionality of 2, mix it with 25.2g of hexamethylene diisocyanate, the molar ratio of isocyanate to hydroxyl is 1.8:1, heat to 85℃, and react for 2 hours under solvent-free conditions to obtain isocyanate-terminated polyurethane prepolymer.

[0030] S2: Add 21.2 g of dithiodiethylamine to the above polyurethane prepolymer. The molar ratio of the amino group of dithiodiethylamine to the isocyanate group in the polyurethane prepolymer is 1.5:1. React at 75°C for 1 hour to obtain an amino-terminated polyurethane prepolymer.

[0031] S3: Add 54.2g of hydrogenated bisphenol A type epoxy resin, the molar ratio of the epoxy group of the epoxy resin to the terminal amino group of the amino-terminated polyurethane prepolymer is 1.5:1, heat to 80℃ and react for 1.5 hours to obtain a polyurethane-epoxy hybrid intermediate.

[0032] S4: Add 30.06g of rosin-based glycidyl ether, accounting for 15% of the total mass of the polyurethane-epoxy hybrid intermediate, to adjust the viscosity of the system. Add glacial acetic acid to adjust the neutralization degree to 100%. Add 270g of deionized water at a stirring speed of 1500 rpm and disperse for 20 minutes to obtain an aqueous modified resin dispersion with a solid content of 60%.

[0033] Example 3

[0034] S1: Take 100g of cashew phenol diol with a number average molecular weight of 500 and a hydroxyl functionality of 2, mix it with 78.6g of dicyclohexylmethane diisocyanate, the molar ratio of isocyanate to hydroxyl is 1.2:1, heat to 70℃, and react for 4 hours under solvent-free conditions to obtain isocyanate-terminated polyurethane prepolymer.

[0035] S2: Add 30.8 g of dithiodiethylamine to the above polyurethane prepolymer. The molar ratio of the amino group of dithiodiethylamine to the isocyanate group in the polyurethane prepolymer is 1.1:1. React at 60°C for 2 hours to obtain an amino-terminated polyurethane prepolymer.

[0036] S3: Add 62.8g of bisphenol A type epoxy resin. The molar ratio of the epoxy group of the epoxy resin to the terminal amino group of the amino-terminated polyurethane prepolymer is 1.1:1. Heat to 70℃ and react for 3 hours to obtain a polyurethane-epoxy hybrid intermediate.

[0037] S4: Add 13.61g of soybean oil-based glycidyl ether, accounting for 5% of the total mass of the polyurethane-epoxy hybrid intermediate, to adjust the viscosity of the system. Add citric acid to adjust the neutralization degree to 80%. Add 410g of deionized water at a stirring speed of 800 rpm and disperse for 40 minutes to obtain an aqueous modified resin dispersion with a solid content of 40%.

[0038] Example 4

[0039] S1: Take 150g of polylactic acid glycol with a number average molecular weight of 1500 and a hydroxyl functionality of 2, mix it with 46.6g of isophorone diisocyanate, the molar ratio of isocyanate to hydroxyl is 1.3:1, heat to 80℃, and react for 2.5 hours under solvent-free conditions to obtain isocyanate-terminated polyurethane prepolymer.

[0040] S2: Add 30.7g of cystamine to the above polyurethane prepolymer. The molar ratio of the amino group of cystamine to the isocyanate group in the polyurethane prepolymer is 1.3:1. React at 70℃ for 1.2 hours to obtain an amino-terminated polyurethane prepolymer.

[0041] S3: Add 26g of bisphenol A epoxy resin and 24g of bisphenol F epoxy resin. The molar ratio of total epoxy groups to the terminal amino groups of the terminal amino polyurethane prepolymer is 1.3:1. Heat to 78℃ and react for 2.2 hours to obtain a polyurethane-epoxy hybrid intermediate.

[0042] S4: Add 13.8g of cashew phenol glycidyl ether and 13.8g of rosin-based glycidyl ether, accounting for 10% of the total mass of the polyurethane-epoxy hybrid intermediate, to adjust the viscosity of the system. Add a 1:1 mass ratio of glacial acetic acid and lactic acid mixed neutralizer to adjust the degree of neutralization to 85%. Add 352g of deionized water at a stirring speed of 1000 rpm and disperse for 35 minutes to obtain an aqueous modified resin dispersion with a solid content of 50%.

[0043] Comparative Example The comparative example uses an existing conventional self-healing waterborne polyurethane-epoxy hybrid resin synthesis process: S1: Take 100g of petroleum-based polyether diol with a number average molecular weight of 1000, mix it with 44.4g of isophorone diisocyanate, add 10g of acetone as solvent, heat to 75℃ and react for 3 hours to obtain isocyanate-terminated polyurethane prepolymer with a molar ratio of isocyanate to hydroxyl groups of 1.4:1.

[0044] S2: Add 8.8g of ethylenediamine as a chain extender, and react at 65℃ for 1.5 hours to obtain an amino-terminated polyurethane prepolymer. S3: Add 48.5g of bisphenol F epoxy resin, with a molar ratio of epoxy groups to amino-terminated groups of 1.2:1, and react at 75℃ for 2 hours to obtain a polyurethane-epoxy hybrid intermediate.

[0045] S4: Triethylamine was added to adjust the neutralization degree to 90%. 320g of deionized water was added while stirring at 1200 rpm. The mixture was dispersed for 30 minutes, and acetone was removed under reduced pressure to obtain an aqueous modified resin dispersion with a solid content of 45%.

[0046] Core reaction molecular formula The chain extension stage reaction formula is: OCNNCO+H2N-CH2CH2-SS-CH2CH2-NH2→ H2N-CH2CH2-SS-CH2CH2-HNNH-CH2CH2-SS-CH2CH2-NH2. This reaction introduces dynamic disulfide bonds into the polyurethane backbone in a directional manner. When heated, the disulfide bonds can undergo a reversible exchange reaction, which allows the broken molecular chains at the scratch to reconnect, thus solving the defects of existing technologies that lack self-healing structures or have insufficient repair efficiency.

[0047] Test data table and description Table 1 Comparison of core synthesis parameters for each sample

[0048] This table clarifies the differences in raw materials and processes between the embodiments and the comparative examples. The four embodiments conform to the core features of the technical solution of this invention, while the comparative examples adopt existing mainstream technical solutions, which can intuitively reflect the differences between the two types of technical paths.

[0049] Table 2 Test results of core performance of each sample

[0050] This table presents the measured performance data for each sample. The viscosity, VOC, and repair efficiency of the four examples all meet the specified ranges, demonstrating significantly better performance than the comparative examples. This verifies that the technical solution of this invention can solve the four core defects of existing technologies, and the technical effect is stable. The 32% repair efficiency of the comparative example originates from the physical healing caused by the thermal fluidity of the coating at 60°C, rather than from the dynamic exchange of chemical bonds. The repair efficiencies of the examples in this invention are all >85%, confirming the intrinsic self-healing effect of dynamic disulfide bonds.

[0051] refer to Figure 2 This figure visually illustrates the core performance differences between the four embodiments of the present invention and the prior art comparative examples. The rotational viscosity of the systems at 25°C in all four embodiments is in the range of 300-800 mPa·s, far lower than the 1280 mPa·s of the comparative example, verifying that the viscosity-reducing effect of the bio-based monofunctional epoxy diluent meets the requirements of water dispersion processes. The VOC content of all four embodiments is below 20 g / L, far lower than the 28 g / L of the comparative example, confirming the environmental advantages of the solvent-free synthesis process. The scratch repair efficiency of all four embodiments is higher than 85%, superior to the 32% of the comparative example, demonstrating the significant self-healing effect introduced by the aliphatic chain extender containing dynamic disulfide bonds. All three performance categories are superior to the prior art, fully supporting the advanced nature of the technical solution of the present invention.

[0052] refer to Figure 3 This figure illustrates the difference in self-healing kinetics between a representative embodiment of the present invention and a comparative example of the prior art. In Example 4 of the present invention, the repair efficiency increases rapidly with heating time, achieving nearly 30% repair rate after 30 minutes and reaching 90% after 120 minutes. Further extending the heating time does not significantly improve the repair efficiency, demonstrating that the dynamic disulfide bond exchange reaction can be completed in a short time, indicating a fast intrinsic self-healing reaction rate and high repair degree. In contrast, the repair efficiency of the comparative example increases slowly with heating time, reaching only 32% after 120 minutes, with minimal improvement after subsequent heating. This demonstrates that it relies solely on the thermal flow of the coating for physical healing, resulting in limited repair effectiveness. This further verifies the rationality and superior performance of the self-healing structure design of the present invention.

[0053] refer to Figure 4This figure covers three core evaluation dimensions: synthesis process performance, environmental performance, and coating service performance, and can intuitively present the differences in comprehensive performance among different samples. The system flowability score is calculated by inversely converting the viscosity at 25°C rotational viscosity; the lower the viscosity, the higher the score. The environmental performance score is calculated by inversely converting the VOC content; the lower the VOC, the higher the score. The radar chart coverage area of ​​the four embodiments is much larger than that of the comparative example, indicating that the comprehensive performance of the technical solution of this invention is superior to the prior art. The scores in self-healing efficiency, system flowability, and environmental performance are more than doubled compared to the comparative example, directly addressing the three core defects of the prior art: low repair efficiency, excessively high prepolymer viscosity, and excessive VOC content. Meanwhile, the film hardness and adhesion scores of the four embodiments are comparable to or even better than those of the comparative example, confirming that the polyurethane-epoxy hybrid structure and the directional introduction of dynamic disulfide bonds in this invention do not sacrifice the basic mechanical service performance of the coating. This solves the hidden problem of the difficulty in balancing self-healing performance and mechanical performance commonly found in self-healing resins, making it suitable for various application scenarios.

[0054] refer to Figure 5 This figure characterizes the storage stability of different samples. The test conditions are the industry-standard accelerated storage at 60°C, corresponding to a 12-month storage period at room temperature. In Example 1 of this invention, the viscosity retention rate decreases slowly with storage time, remaining above 90% after 28 days, indicating uniform dispersion, stable hybrid structure, and no significant particle agglomeration or sedimentation during storage. In contrast, the viscosity retention rate of the prior art comparative example decreases rapidly, reaching only 42% after 28 days. This indicates that its prepolymer has an excessively high initial viscosity, insufficient shear dispersion during water dispersion, uneven particle size, and is prone to phase separation during storage. The sedimentation of the effective components leads to a significant decrease in system viscosity. This figure directly verifies that the low-viscosity design of this invention can significantly improve the storage stability of waterborne resins, solving the core defect of short shelf life in existing technologies.

[0055] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. An environmentally friendly low viscosity modified resin synthesis method, characterized by, Includes the following steps: S1. Bio-based polyols and diisocyanates are mixed and reacted under solvent-free conditions to prepare isocyanate-terminated polyurethane prepolymers. S2. Add an aliphatic chain extender containing dynamic disulfide bonds to the polyurethane prepolymer to carry out a chain extension reaction, introduce a dynamic disulfide bond structure, and obtain an amino-terminated polyurethane prepolymer. S3. The terminal amino polyurethane prepolymer is mixed with epoxy resin to undergo an amine-epoxy ring-opening addition reaction to obtain a polyurethane-epoxy hybrid intermediate. S4. Add a bio-based monofunctional epoxy reactive diluent to the polyurethane-epoxy hybrid intermediate to adjust the viscosity of the system, then add a neutralizing agent to neutralize it into a salt, and disperse it in deionized water to obtain an aqueous modified resin dispersion. After the aqueous modified resin dispersion forms a film, the finished product is obtained.

2. The method for synthesizing an environmentally friendly low viscosity modified resin according to claim 1, characterized in that, The bio-based polyol in S1 is at least one of polylactic acid glycol, polycarbonate glycol, and cashew nut glycol; the diisocyanate is at least one of isophorone diisocyanate, hexamethylene diisocyanate, and dicyclohexylmethane diisocyanate; the reaction temperature is 70℃~85℃; the reaction time is 2 hours~4 hours; and the molar ratio of isocyanate to hydroxyl group is 1.2~1.8:

1.

3. The method for synthesizing an environmentally friendly low viscosity modified resin according to claim 1, characterized in that, The aliphatic chain extender containing dynamic disulfide bonds in S2 is an aliphatic diamine containing dynamic disulfide bonds. The molar ratio of the active functional group of the chain extender to the isocyanate group in the polyurethane prepolymer is 1.1~1.5:

1. The reaction temperature is 60℃~75℃ and the reaction time is 1 hour~2 hours.

4. The method for synthesizing an environmentally friendly low viscosity modified resin according to claim 1, characterized in that, The epoxy resin in S3 is at least one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, and hydrogenated bisphenol A type epoxy resin. The molar ratio of the epoxy group of the epoxy resin to the terminal amino group of the amino-terminated polyurethane prepolymer is 1.1~1.5:

1. The ring-opening addition reaction temperature is 70℃~80℃, and the reaction time is 1.5 hours~3 hours.

5. The method for synthesizing an environmentally friendly low viscosity modified resin according to claim 1, characterized in that, The bio-based monofunctional epoxy reactive diluent in S4 is at least one of cashew phenol glycidyl ether, rosin-based glycidyl ether, and soybean oil-based glycidyl ether, and the amount of diluent added accounts for 5% to 15% of the total mass of the polyurethane-epoxy hybrid intermediate.

6. The environmentally friendly low viscosity modified resin synthesis method according to claim 1, characterized by, The neutralizing agent in S4 is at least one of glacial acetic acid, lactic acid, and citric acid, with a neutralization degree of 80% to 100%. The amount of deionized water added controls the solid content of the final waterborne modified resin dispersion to be 40% to 65%.

7. The method for synthesizing the environmentally friendly low-viscosity modified resin according to claim 1, characterized in that, The prepared waterborne modified resin dispersion has a rotational viscosity of 300 mPa·s to 800 mPa·s at 25°C and a volatile organic compound content of less than 20 g / L.

8. The method for synthesizing the environmentally friendly low-viscosity modified resin according to claim 1, characterized in that, After the prepared water-based modified resin is formed into a film, it is placed at 60°C for 2 hours, and the scratch repair efficiency is not less than 85%.

9. The method for synthesizing the environmentally friendly low-viscosity modified resin according to claim 2, characterized in that, The bio-based polyol has a number-average molecular weight of 500-3000 and a hydroxyl functionality of 2.

10. The method for synthesizing the environmentally friendly low-viscosity modified resin according to claim 1, characterized in that, The stirring speed in the dispersion process of S4 is 800 rpm to 1500 rpm, and the dispersion time is 20 minutes to 40 minutes.