A wear-resistant polyurethane elastomer material and its preparation method
By chemically bonding silicone oil to polyurethane elastomers and constructing a high-density hydrogen bond network, the problem of insufficient wear resistance of traditional polyurethane materials under harsh working conditions has been solved, thereby improving the wear resistance and extending the service life of the materials.
Patent Information
- Application Number
- CN202611580729.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional polyurethane materials have insufficient wear resistance under harsh working conditions, poor compatibility of blended components, easy migration and precipitation, resulting in unstable surface properties, weak interfacial bonding, and easy generation of microcracks during wear.
Hydroxy silicone oil is used to participate in the chemical construction of the polyurethane backbone, and a high-density hydrogen bond network is constructed through catechol derivatives to form a synergistic structure of chemically bonded silicone oil modification/high-density hydrogen bond network enhancement.
It significantly improves the wear resistance of polyurethane elastomers, avoids the migration and precipitation of silicone oil additives, inhibits the initiation and propagation of wear microcracks, and extends the service life of materials.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polyurethane elastomer preparation technology. Specifically, this invention relates to a wear-resistant polyurethane elastomer material and its preparation method. Background Technology
[0002] Polyurethane elastomers are widely used in mining equipment, industrial transmissions, seals, and wear-resistant components due to their excellent wear resistance, high strength, and good resilience. However, under harsh operating conditions, traditional polyurethane materials still have key performance bottlenecks, making it difficult to meet the extreme wear resistance requirements of high-end applications.
[0003] Existing modification techniques often improve wear resistance by physically blending low surface energy materials (such as silicone oil or fluorinated additives), but these techniques have significant drawbacks: poor compatibility between the blended components and the polyurethane matrix, leading to easy migration and precipitation, resulting in unstable surface properties; weak interfacial bonding, increased stress concentration points under stress, and easy generation of microcracks during wear, thus accelerating material wear. Therefore, developing novel polyurethane elastomers with excellent wear resistance has become an urgent breakthrough in this field. Summary of the Invention
[0004] One object of the present invention is to solve at least the above-mentioned problems and / or defects, and to provide at least the advantages described below.
[0005] To achieve these objectives and other advantages of the present invention, a wear-resistant polyurethane elastomer material is provided, comprising, by molar fraction, the following components in a total molar fraction of 100 parts: 5-20 parts of polyol, 0.1-2 parts of hydroxyl silicone oil, 10-60 parts of polyisocyanate, 5-40 parts of small molecule chain extender, and 0.1-2 parts of catechol derivative.
[0006] Preferably, the polyol is one or more of polyester polyol, polyether polyol, polycaprolactone polyol, and polycarbonate polyol, with a number average molecular weight of 500-5000 g / mol; and the hydroxyl silicone oil is dihydroxy polydimethylsiloxane with a number average molecular weight of 500-2000 g / mol.
[0007] Preferably, the polyether polyol is polytetrahydrofuran diol; and the polycaprolactone polyol is polycaprolactone diol.
[0008] Preferably, the polyisocyanate is one or more selected from 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, terephthalic diisocyanate, dimethylbenzene diisocyanate, and 3,3-dimethyl-4,4-diphenylmethane diisocyanate; and the small molecule chain extender is one or more selected from 4,4'-methylenebis(2-chloroaniline), ethanolamine, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, ethylenediamine, 2-methyl-1,5-pentanediamine, and diethyltoluenediamine.
[0009] Preferably, the catechol derivative is a catechol with a diol hydroxyl end cap, and its general structural formula is shown in Formula I: .
[0010] Preferably, the catechol containing diol hydroxyl-terminated end-capped hydroxyl group is one or more of N-(3,4-dihydroxyphenyl)diethanolamine, N-(3,4-dihydroxyphenyl)diisopropanolamine, and N-(3,4-dihydroxyphenyl)di-n-butanolamine; the structural formula of N-(3,4-dihydroxyphenyl)diethanolamine is shown in Formula II; the structural formula of N-(3,4-dihydroxyphenyl)diisopropanolamine is shown in Formula III; and the structural formula of N-(3,4-dihydroxyphenyl)di-n-butanolamine is shown in Formula IV.
[0011]
[0012] Preferably, one or more of stannous octoate, dibutyltin dilaurate, triethylenediamine, and diethylenediamine may be added to the wear-resistant polyurethane elastomer material as catalysts for the polymerization reaction; colorants, antioxidants, light stabilizers, and ultraviolet absorbers may also be added to the wear-resistant polyurethane elastomer material as additives.
[0013] A method for preparing the wear-resistant polyurethane elastomer material as described above includes the following steps: Step 1: Add polyol and hydroxyl silicone oil to the reactor and dehydrate them under high temperature and reduced pressure. Then cool down to the reaction temperature, add polyisocyanate and mix evenly. React under nitrogen atmosphere to obtain prepolymer. Step 2: Add the small molecule chain extender and catechol derivative to the prepolymer, stir and mix, and then pour it into a preheated mold for curing reaction. After curing, the material is aged to obtain wear-resistant polyurethane elastomer material.
[0014] Preferably, in step one, the temperature of the high-temperature decompression dehydration treatment is 110~130℃, the pressure of the high-temperature decompression dehydration treatment is 200~400Pa, and the time of the high-temperature decompression dehydration treatment is 1~3h; the reaction temperature is 70~80℃, and the reaction time is 1~4h.
[0015] Preferably, in step two, the stirring speed is 300~500 rpm, the stirring time is 1~5 min, the curing temperature is 120~140℃, the curing time is 1~3 h, the ripening temperature is 90~110℃, and the ripening time is 10~30 h.
[0016] More preferably, the number average molecular weight of the polyol is 1000~3000 g / mol.
[0017] In this invention, polyols, as the soft segments of polyurethane, significantly influence the material's flexibility, hydrolysis resistance, and other properties through their type and molecular weight. Hydroxyl silicone oil, as a modifier, with its dihydroxyl structure, participates in the construction of the polyurethane backbone, rather than through simple physical blending, thus avoiding the migration and precipitation problems common with traditional silicone oil additives. Polyisocyanates, as the main source of hard segments, react with polyols to form prepolymers. Small molecule chain extenders are used to further react with the prepolymers, increasing the proportion of hard segments in the molecular chain and improving the material's strength and modulus. Catechol derivatives, as modifiers, are composed of diol-terminated catechols; this component is used to construct a high-density hydrogen bond network, resisting microcrack propagation and maintaining material integrity.
[0018] The present invention has at least the following beneficial effects: This invention significantly improves the wear resistance of polyurethane elastomers through a unique dual-effect synergistic structural design of "chemically bonded silicone oil modification / high-density hydrogen bond network reinforcement". Its core advantages are: hydroxyl silicone oil, as a dihydroxyl-terminated active component, directly participates in the chemical construction of the polyurethane backbone, thereby overcoming the defects of poor compatibility and easy migration and precipitation of traditional physically blended silicone oils; catechol derivatives, with their diol hydroxyl-terminated structure, construct a high-density hydrogen bond network in the curing reaction. As a reversible physical crosslinking point, it can dissipate energy and restrict molecular chain slippage under frictional stress, inhibiting the initiation and propagation of wear microcracks.
[0019] Other advantages, objectives and features of the present invention will become apparent in part from the following description, and in part from those skilled in the art through study and practice of the invention. Detailed Implementation
[0020] The present invention will now be described in further detail so that those skilled in the art can implement it based on the description.
[0021] It should be understood that terms such as “having,” “comprising,” and “including” as used herein do not exclude the presence or addition of one or more other elements or combinations thereof.
[0022] Example 1 A wear-resistant polyurethane elastomer material, by molar proportion, comprises the following components: 15.67 parts of polyol (polycaprolactone diol, molecular weight 1000 g / mol), 1 part of hydroxyl silicone oil (dihydroxy polydimethylsiloxane, molecular weight 800 g / mol), 50 parts of polyisocyanate (toluene diisocyanate), 32.5 parts of small molecule chain extender (4,4'-methylenebis(2-chloroaniline)), and 0.83 parts of catechol derivative (N-(3,4-dihydroxyphenyl)diethanolamine); A method for preparing a wear-resistant polyurethane elastomer material includes the following steps: Step 1: Add polyol and hydroxyl silicone oil to the reactor and dehydrate under high temperature and reduced pressure at 120℃ and 300Pa for 2 hours. Then cool down to 75℃, add polyisocyanate and mix evenly. React under nitrogen atmosphere for 2.5 hours to obtain prepolymer. Step 2: Add the small molecule chain extender and catechol derivative to the prepolymer, stir and mix at 400 rpm for 2 minutes, then pour into a preheated mold and cure at 130℃ for 1.5 hours. After curing, the material is aged at 100℃ for 24 hours to obtain wear-resistant polyurethane elastomer material.
[0023] Example 2 A wear-resistant polyurethane elastomer material, by molar proportion, comprises the following components: Polyol (polycaprolactone diol, molecular weight 2000 g / mol) 19.2 parts, hydroxyl silicone oil (dihydroxy polydimethylsiloxane, molecular weight 1200 g / mol) 0.8 parts, polyisocyanate (terephthalic diisocyanate) 50 parts, small molecule chain extender (1,4-butanediol) 28.4 parts, catechol derivative (N-(3,4-dihydroxyphenyl)diisopropanolamine) 1.6 parts; A method for preparing a wear-resistant polyurethane elastomer material includes the following steps: Step 1: Add polyol and hydroxyl silicone oil to the reactor and dehydrate under high temperature and reduced pressure at 120℃ and 300Pa for 2 hours. Then cool down to 70℃, add polyisocyanate and mix evenly. React under nitrogen atmosphere for 2.5 hours to obtain prepolymer. Step 2: Add the small molecule chain extender and catechol derivative to the prepolymer, stir and mix at 450 rpm for 2 minutes, then pour into a preheated mold and cure at 130℃ for 1.5 hours. After curing, the resulting material is aged at 100℃ for 24 hours to obtain a wear-resistant polyurethane elastomer material.
[0024] Example 3 A wear-resistant polyurethane elastomer material, by molar proportion, comprises the following components: Polyol (polytetrahydrofuran diol, molecular weight 3000 g / mol) 12.25 parts, hydroxyl silicone oil (dihydroxy polydimethylsiloxane, molecular weight 2000 g / mol) 0.25 parts, polyisocyanate (4,4'-diphenylmethane diisocyanate) 50 parts, small molecule chain extender (1,3-propanediol) 36.25 parts, catechol derivative (N-(3,4-dihydroxyphenyl)di-n-butanolamine) 1.25 parts; A method for preparing a wear-resistant polyurethane elastomer material includes the following steps: Step 1: Add polyol and hydroxyl silicone oil to the reactor and dehydrate under high temperature and reduced pressure at 120℃ and 300Pa for 2 hours. Then cool down to 75℃, add polyisocyanate and mix evenly. React under nitrogen atmosphere for 2.5 hours to obtain prepolymer. Step 2: Add the small molecule chain extender and catechol derivative to the prepolymer, stir and mix at 300 rpm for 3 minutes, then pour into a preheated mold and cure at 130℃ for 1.5 hours. After curing, the material is aged at 100℃ for 24 hours to obtain wear-resistant polyurethane elastomer material.
[0025] Comparative Example 1 A polyurethane elastomer material, by molar amounts, comprises the following components: 16.67 parts of polyol (polycaprolactone diol, molecular weight 1000 g / mol), 50 parts of polyisocyanate (toluene diisocyanate), and 33.33 parts of small molecule chain extender (4,4'-methylenebis(2-chloroaniline)). A method for preparing a polyurethane elastomer material includes the following steps: Step 1: Add the polyol to the reactor and dehydrate it under high temperature and reduced pressure at 120℃ and 300Pa for 2 hours. Then cool it down to 75℃, add the polyisocyanate and mix it evenly. React it under a nitrogen atmosphere for 2.5 hours to obtain the prepolymer. Step 2: Add the small molecule chain extender to the prepolymer, stir and mix at 400 rpm for 2 minutes, then pour it into a preheated mold and cure it at 130℃ for 1.5 hours. After curing, the material is aged at 100℃ for 24 hours to obtain the polyurethane elastomer material.
[0026] Comparative Example 2 A polyurethane elastomer material, by molar amounts, comprises the following components: Polyol (polycaprolactone diol, molecular weight 1000 g / mol) 16.67 parts, polyisocyanate (toluene diisocyanate) 50 parts, small molecule chain extender (4,4'-methylenebis(2-chloroaniline)) 32.5 parts, catechol derivative (N-(3,4-dihydroxyphenyl)diethanolamine) 0.83 parts; A method for preparing a polyurethane elastomer material includes the following steps: Step 1: Add the polyol to the reactor and dehydrate it under high temperature and reduced pressure at 120℃ and 300Pa for 2 hours. Then cool it down to 75℃, add the polyisocyanate and mix it evenly. React it under a nitrogen atmosphere for 2.5 hours to obtain the prepolymer. Step 2: Add the small molecule chain extender and catechol derivative to the prepolymer, stir and mix at 400 rpm for 2 minutes, then pour into a preheated mold and cure at 130°C for 1.5 hours. After curing, the resulting material is aged at 100°C for 24 hours to obtain the polyurethane elastomer material.
[0027] Comparative Example 3 A polyurethane elastomer material, by molar amounts, comprises the following components: 15.67 parts of polyol (polycaprolactone diol, molecular weight 1000 g / mol), 1 part of hydroxyl silicone oil (dihydroxy polydimethylsiloxane, molecular weight 800 g / mol), 50 parts of polyisocyanate (toluene diisocyanate), and 33.33 parts of small molecule chain extender (4,4'-methylenebis(2-chloroaniline)). A method for preparing a polyurethane elastomer material includes the following steps: Step 1: Add polyol and hydroxyl silicone oil to the reactor and dehydrate under high temperature and reduced pressure at 120℃ and 300Pa for 2 hours. Then cool down to 75℃, add polyisocyanate and mix evenly. React under nitrogen atmosphere for 2.5 hours to obtain prepolymer. Step 2: Add the small molecule chain extender to the prepolymer, stir and mix at 400 rpm for 2 minutes, then pour it into a preheated mold and cure it at 130℃ for 1.5 hours. After curing, the material is aged at 100℃ for 24 hours to obtain the polyurethane elastomer material.
[0028] The specific formulations of Examples 1-3 and Comparative Examples 1-3 are shown in Table 1.
[0029] Table 1. Composition of polyurethane elastomer materials (in molar parts)
[0030] The polyurethane elastomer materials prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to abrasion resistance tests according to GB / T 3960-2016 standard. The test results are shown in Table 2.
[0031] Table 2 Abrasion resistance test results
[0032] As can be seen from Table 2, the wear rate of the polyurethane elastomer materials in Examples 1-3 of this invention is 3.7 × 10⁻⁶. -7 ~5.8×10 -7 The g / N·m ratio was significantly lower than that of Comparative Examples 1-3. Comparative Example 2 only added catechol derivatives, and Comparative Example 3 only added hydroxyl silicone oil. Although the wear resistance was improved compared to Comparative Example 1, the improvement effect was not as good as that of the embodiments of the present invention. This is because hydroxyl silicone oil and catechol derivatives were added as modifiers in Examples 1-3. The dihydroxyl structure of hydroxyl silicone oil can participate in the construction of the polyurethane backbone, rather than simple physical blending, thus avoiding the problem of easy migration and precipitation of traditional silicone oil additives. The catechol derivative is a catechol with diol hydroxyl end caps, which can be used to construct a high-density hydrogen bond network, resist microcrack propagation, maintain material integrity, and significantly improve the wear resistance of the prepared wear-resistant polyurethane elastomer material. It can be applied in the field of oil and mineral mining to prepare downhole seals, mine wear-resistant bushings and other components, effectively solving the pain point of rapid wear of traditional polyurethane materials in industrial and mining scenarios and extending the service life of workpieces.
[0033] Although embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, other modifications can be easily made. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details and embodiments shown and described herein.
Claims
1. A wear resistant polyurethane elastomer material, characterized in that, Based on molar parts, it includes the following components with a total molar number of 100 parts: 5-20 parts of polyol, 0.1-2 parts of hydroxyl silicone oil, 10-60 parts of polyisocyanate, 5-40 parts of small molecule chain extender, and 0.1-2 parts of catechol derivative.
2. The wear-resistant polyurethane elastomer material as described in claim 1, characterized in that, The polyol is one or more of polyester polyol, polyether polyol, polycaprolactone polyol, and polycarbonate polyol, with a number average molecular weight of 500-5000 g / mol; the hydroxyl silicone oil is dihydroxy polydimethylsiloxane, with a number average molecular weight of 500-2000 g / mol.
3. The wear-resistant polyurethane elastomer material as described in claim 2, characterized in that, The polyether polyol is polytetrahydrofuran diol; the polycaprolactone polyol is polycaprolactone diol.
4. The wear-resistant polyurethane elastomer material as described in claim 1, characterized in that, The polyisocyanate is one or more selected from 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, terephthalic diisocyanate, dimethylbenzene diisocyanate, and 3,3-dimethyl-4,4-diphenylmethane diisocyanate; the small molecule chain extender is one or more selected from 4,4'-methylenebis(2-chloroaniline), ethanolamine, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, ethylenediamine, 2-methyl-1,5-pentanediamine, and diethyltoluenediamine.
5. The wear-resistant polyurethane elastomer material as described in claim 1, characterized in that, The catechol derivative is a catechol with a diol hydroxyl end cap, and its general structural formula is shown in Formula I: 。 6. The wear-resistant polyurethane elastomer material as described in claim 5, characterized in that, The catechol containing diol hydroxyl-terminated end-capped hydroxyl group is one or more of N-(3,4-dihydroxyphenyl)diethanolamine, N-(3,4-dihydroxyphenyl)diisopropanolamine, and N-(3,4-dihydroxyphenyl)di-n-butanolamine.
7. The wear-resistant polyurethane elastomer material as described in claim 1, characterized in that, The wear-resistant polyurethane elastomer material may also contain one or more of the following as catalysts for polymerization: stannous octoate, dibutyltin dilaurate, triethylenediamine, and diethylenediamine; and colorants, antioxidants, light stabilizers, and ultraviolet absorbers may also be added as additives.
8. A method for preparing a wear-resistant polyurethane elastomer material as described in any one of claims 1-7, characterized in that, Includes the following steps: Step 1: Add polyol and hydroxyl silicone oil to the reactor and dehydrate them under high temperature and reduced pressure. Then cool down to the reaction temperature, add polyisocyanate and mix evenly. React under nitrogen atmosphere to obtain prepolymer. Step 2: Add the small molecule chain extender and catechol derivative to the prepolymer, stir and mix, and then pour it into a preheated mold for curing reaction. After curing, the material is aged to obtain wear-resistant polyurethane elastomer material.
9. The wear-resistant polyurethane elastomer material as described in claim 8, characterized in that, In step one, the temperature of the high-temperature decompression dehydration treatment is 110~130℃, the pressure of the high-temperature decompression dehydration treatment is 200~400Pa, and the time of the high-temperature decompression dehydration treatment is 1~3h; the reaction temperature is 70~80℃, and the reaction time is 1~4h.
10. The wear-resistant polyurethane elastomer material as described in claim 8, characterized in that, In step two, the stirring speed is 300~500 rpm, the stirring time is 1~5 min, the curing temperature is 120~140℃, the curing time is 1~3 h, the ripening temperature is 90~110℃, and the ripening time is 10~30 h.