An infrared-reflective cross-linked polyethylene sheath material and a medium- and low-voltage cable

By using SnO2/Sb2O3 co-doping to coat TiO2 composite particles and then modifying them, an infrared-reflective cross-linked polyethylene sheath material was prepared, achieving a combination of high near-infrared reflectivity and good mechanical properties in medium and low voltage cables. This solved the problem of temperature rise during outdoor use, extended cable life, and improved power transmission capacity.

CN123107218APending Publication Date: 2026-11-17GUANGZHOUZHUJIANG CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611557532.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When existing medium and low voltage cable sheath materials are used outdoors, it is difficult to balance infrared reflection performance and mechanical properties, which leads to increased surface temperature of the sheath and affects cable life and power transmission capacity.

Method used

Infrared reflective cross-linked polyethylene sheath material was prepared by using SnO2/Sb2O3 co-doped rutile TiO2 composite particles as infrared reflective fillers and modifying them with γ-aminopropyltriethoxysilane to improve the compatibility between the filler and the polyethylene matrix.

Benefits of technology

It improves the near-infrared reflectivity and mechanical properties of the sheath material, solves the problem of balancing reflectivity and mechanical properties, reduces the surface temperature of the sheath, extends the cable life, and improves the power transmission capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of cable sheathing technology, specifically relating to an infrared-reflective cross-linked polyethylene sheathing material and a medium- and low-voltage cable. This invention uses SnO2 / Sb2O3 co-doped rutile TiO2 composite particles as the infrared-reflective filler to prepare the required infrared-reflective cross-linked polyethylene sheathing material. Titanium dioxide provides basic visible-near-infrared reflectivity, while tin dioxide and antimony trioxide co-coating create a synergistic reflective effect in the near-infrared band. The overall carrier concentration and free electron absorption and reflection characteristics of the composite particles are optimized, making the filler's reflectivity in the near-infrared band significantly superior to that of a single oxide coating system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of cable sheathing technology, specifically relating to an infrared reflective cross-linked polyethylene sheathing material and a medium- and low-voltage cable. Background Technology

[0002] Medium and low voltage cables are among the most widely used critical line equipment in power transmission and distribution systems, commonly used in overhead laying, underground laying, and outdoor environments. The cable sheath, as a protective structure covering the insulation layer, serves to prevent moisture, mechanical damage, chemical corrosion, and atmospheric aging. Currently, cable sheath materials commonly fall into two main categories: polyvinyl chloride (PVC) and polyethylene (PE). PVC sheaths have good flame retardancy but poor heat and low-temperature resistance, and easily release halogen-containing fumes during combustion. Polyethylene sheaths, on the other hand, have good electrical properties, chemical corrosion resistance, and processing performance. Cross-linked polyethylene (XLPE) sheaths, in particular, have further improved heat resistance and mechanical properties, leading to their increasingly widespread application in medium and low voltage cables.

[0003] For outdoor cables, the cable sheath is exposed to solar radiation for a long time, which causes the sheath temperature to rise significantly. This accelerates the oxidative degradation and thermal aging of the polyethylene molecular chain, resulting in decreased mechanical properties, surface cracking, and deterioration of insulation performance. In severe cases, it can shorten the cable's service life. At the same time, overheating of the sheath can also reduce the cable's allowable current carrying capacity and restrict the power transmission capacity of the line.

[0004] To reduce the surface temperature rise of the sheath, existing technologies typically employ adding infrared reflective fillers to polyethylene, such as titanium dioxide, tin oxide, and antimony oxide. However, these methods have the following drawbacks: Rutile titanium dioxide has good reflectivity for visible light, but its reflectivity in the near-infrared band is limited, making it difficult to effectively reduce the sheath surface temperature when used alone; while tin dioxide or antimony trioxide possess certain near-infrared reflectivity, the improvement in near-infrared reflectivity from a single oxide coating is insufficient to meet the requirements for outdoor cables to withstand intense sunlight, and a single coating layer has limitations in terms of particle size distribution and conductivity uniformity. Furthermore, inorganic infrared reflective fillers are hydrophilic and have poor compatibility with the polyethylene matrix, easily agglomerating and dispersing unevenly when directly blended. On the one hand, filler agglomerates cause stress concentration, leading to a significant decrease in mechanical properties such as tensile strength and elongation at break; on the other hand, uneven dispersion can also create scattering defects in the matrix, further reducing reflectivity. Simply increasing the filler dosage to pursue higher reflectivity further deteriorates mechanical properties, making it difficult to achieve a balance between reflectivity and mechanical properties.

[0005] Therefore, how to prepare an infrared-reflective cross-linked polyethylene sheath material that combines high near-infrared reflectivity and good mechanical properties is a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention

[0006] To address the aforementioned technical problems, in a first aspect, the present invention provides an infrared-reflective cross-linked polyethylene sheath material.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] This invention discloses an infrared reflective cross-linked polyethylene sheath material, which, by weight, is composed of the following raw materials:

[0009] 100 parts of polyethylene

[0010] 3-6 parts of crosslinking agent

[0011] 10-25 parts of modified infrared reflective filler

[0012] 1-3 parts antioxidant

[0013] Lubricant 0.5 to 1 part

[0014] Light stabilizer 0.1 to 1 part

[0015] In some embodiments, the polyethylene is low-density polyethylene, and the low-density polyethylene has a melt index of 1 to 5 g / 10 min at 190°C and 2.16 kg.

[0016] In some embodiments, the crosslinking agent is selected from any one or a combination of two of dicumyl peroxide and bis-tert-butyl peroxide;

[0017] In some embodiments, the antioxidant is selected from any one or a combination of two or more of antioxidant 1010, antioxidant 1076, antioxidant 168, and antioxidant 626;

[0018] In some embodiments, the lubricant is selected from any one or a combination of two of calcium stearate or polyethylene wax;

[0019] In some embodiments, the light stabilizer is selected from any one or a combination of two of hindered amine light stabilizer 770 and hindered amine light stabilizer 944;

[0020] In some embodiments, the modified infrared reflective filler is a composite particle of rutile TiO2 co-doped with SnO2 / Sb2O3.

[0021] In some embodiments, the method for preparing the modified infrared reflective filler includes the following steps:

[0022] Step 1: Add 10-20 parts of rutile TiO2 powder, 100-300 parts of deionized water and 0.2-0.5 parts of ammonium polyacrylate dispersant to the reaction vessel, stir for 20-30 minutes to form a mixture;

[0023] Step 2: Dissolve SnCl4·5H2O and SbCl3 in 1-3 mol / L hydrochloric acid to form composite solution A. Add composite solution A and 8-10 wt% sodium hydroxide solution dropwise to the mixture obtained in Step 1. Control the pH of the reaction system between 2 and 2.5 and the reaction temperature between 60 and 85℃. After the addition is complete, continue to keep the reaction at the temperature for 2-3 hours. Then cool down, filter, wash, and dry to obtain product A.

[0024] Step 3: Calcine product A in air at 500-700℃ for 1-2 hours to obtain SnO2 / Sb2O3 coated TiO2 composite particles;

[0025] Step 4: Add 20-30 parts of the SnO2 / Sb2O3-coated TiO2 composite particles obtained in Step 3 to 90-300 parts of a 50wt% ethanol aqueous solution, add 2-3 parts of γ-aminopropyltriethoxysilane, stir and activate for 2-3 hours, centrifuge and dry to obtain activated powder; disperse the activated powder in 100-300 mL of xylene, add 5-10 parts of MAH-g-PE and react at 80-90℃ for 2-4 hours, centrifuge, wash and dry to obtain the modified infrared reflective filler.

[0026] In some embodiments, the particle size of the rutile TiO2 powder is 0.2–0.5 μm;

[0027] In some embodiments, the molar ratio of SnCl4·5H2O to SbCl3 is 10:1 to 2;

[0028] Secondly, this invention discloses a method for preparing an infrared reflective cross-linked polyethylene sheath material, comprising the following steps:

[0029] Step 1: Mix polyethylene, modified infrared reflective filler, crosslinking agent, lubricant, antioxidant and light stabilizer for 10-15 minutes to obtain premix;

[0030] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 170-180℃ and 10-20MPa pressure for 10-30 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0031] In some implementations, in step two, the temperature of the twin-screw extruder is 120-135°C in zone one, 130-145°C in zone two, 140-150°C in zone three, 135-145°C in the die head, and 30-50 rpm in screw speed.

[0032] Thirdly, the present invention provides a medium- and low-voltage cable. The sheath layer of the medium- and low-voltage cable is a double-layer co-extruded structure, wherein the inner layer of the double-layer co-extruded structure is a conventional cross-linked polyethylene sheath material, and the outer layer of the double-layer co-extruded structure is an infrared-reflective cross-linked polyethylene sheath material prepared according to the present invention.

[0033] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0034] This invention utilizes SnO2 / Sb2O3 co-doped rutile TiO2 composite particles as an infrared reflective filler to prepare the required infrared reflective cross-linked polyethylene sheath material. Titanium dioxide provides basic visible-near-infrared reflectivity, while the co-coating of tin dioxide and antimony trioxide creates a synergistic reflective effect in the near-infrared band. The overall carrier concentration and free electron absorption and reflection characteristics of the composite particles are optimized, making the filler's reflectivity in the near-infrared band significantly superior to that of a single oxide coating system.

[0035] To address the issues of poor compatibility and easy agglomeration between inorganic fillers and the polyethylene matrix, this invention first activates the surface of composite particles with γ-aminopropyltriethoxysilane, then reacts them with MAH-g-PE (maleic anhydride-grafted polyethylene) to introduce a polymer layer with good compatibility with the polyethylene matrix onto the filler surface. This modified layer improves the dispersibility of the filler in polyethylene, reducing agglomeration and stress concentration; it also enhances the interfacial bonding between the filler and the matrix.

[0036] The dual modification treatment in this application simultaneously improves the mechanical properties and infrared reflectivity of the sheath material, solving the problem that it is difficult to balance reflectivity and mechanical properties in the prior art. Detailed Implementation

[0037] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0038] The endpoints and any values ​​of the ranges described in this invention are not limited to the precise ranges or values; these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. This invention does not limit the source of the raw materials used; unless otherwise specified, the raw materials used in this invention are all commercially available products commonly found in this technical field.

[0039] Polyethylene: Low-density polyethylene, melt index 1-5 g / 10min (190℃, 2.16 kg), Lanzhou Petrochemical;

[0040] Rutile TiO2 powder: particle size D50 is 0.2-0.5μm, Panzhihua Iron & Steel Titanium Industry;

[0041] SnCl4·5H2O: Sinopharm Group;

[0042] SbCl3: Sinopharm Group;

[0043] MAH-g-PE: Maleic anhydride-grafted polyethylene, grafting rate 1-2%, Ningbo Nengzhiguang.

[0044] Preparation Example 1

[0045] The preparation method of the modified infrared reflective filler includes the following steps:

[0046] Step 1: Add 15g of rutile TiO2 powder, 300g of deionized water and 0.3g of ammonium polyacrylate dispersant to the reaction vessel, stir for 20 minutes to form a mixture;

[0047] Step 2: Dissolve 0.05 mol SnCl4·5H2O and 0.01 mol SbCl3 in 2 mol / L hydrochloric acid to form composite solution A. Add composite solution A and 10 wt% sodium hydroxide solution dropwise to the mixture obtained in Step 1. Control the pH of the reaction system between 2 and 2.5 and the reaction temperature at 65℃. After the addition is complete, continue to keep the reaction at this temperature for 2.5 h. Then cool down, filter, wash, and dry to obtain product A.

[0048] Step 3: Calcine product A in air at 600℃ for 1.5h to obtain SnO2 / Sb2O3 coated TiO2 composite particles;

[0049] Step 4: Add 20g of the SnO2 / Sb2O3-coated TiO2 composite particles obtained in Step 3 to 200mL of 50wt% ethanol aqueous solution, add 2g of γ-aminopropyltriethoxysilane, stir and activate for 2h, centrifuge and dry to obtain activated powder; disperse the activated powder in 200mL of xylene, add 8g of MAH-g-PE and react at 80℃ for 3h, centrifuge, wash and dry to obtain the modified infrared reflective filler A.

[0050] Comparative Preparation Example 1

[0051] The preparation method of the modified infrared reflective filler includes the following steps:

[0052] Step 1: Add 15g of rutile TiO2 powder, 300g of deionized water and 0.3g of ammonium polyacrylate dispersant to the reaction vessel, stir for 20 minutes to form a mixture;

[0053] Step 2: Dissolve 0.06 mol SnCl4·5H2O in 2 mol / L hydrochloric acid to form composite solution A. Add composite solution A and 10 wt% sodium hydroxide solution dropwise to the mixture obtained in Step 1. Control the pH of the reaction system between 2 and 2.5 and the reaction temperature at 65℃. After the addition is complete, continue to keep the reaction at the temperature for 2.5 h. Then cool down, filter, wash, and dry to obtain product A.

[0054] Step 3: Calcine product A in air at 600℃ for 1.5h to obtain SnO2-coated TiO2 composite particles;

[0055] Step 4: Add 20g of SnO2-coated TiO2 composite particles obtained in Step 3 to 200mL of 50wt% ethanol aqueous solution, add 2g of γ-aminopropyltriethoxysilane, stir and activate for 2h, centrifuge and dry to obtain activated powder; disperse the activated powder in 200mL of xylene, add 8g of MAH-g-PE and react at 80℃ for 3h, centrifuge, wash and dry to obtain the modified infrared reflective filler B.

[0056] Comparative Preparation Example 2

[0057] The preparation method of the modified infrared reflective filler includes the following steps:

[0058] Step 1: Add 15g of rutile TiO2 powder, 300g of deionized water and 0.3g of ammonium polyacrylate dispersant to the reaction vessel, stir for 20 minutes to form a mixture;

[0059] Step 2: Dissolve 0.06 mol SbCl3 in 2 mol / L hydrochloric acid to form composite solution A. Add composite solution A and 10 wt% sodium hydroxide solution dropwise to the mixture obtained in step 1. Control the pH of the reaction system between 2 and 2.5, and the reaction temperature at 65℃. After the addition is complete, continue to keep the reaction at the temperature for 2.5 h. Then cool down, filter, wash, and dry to obtain product A.

[0060] Step 3: Calcine product A in air at 600℃ for 1.5h to obtain Sb2O3-coated TiO2 composite particles;

[0061] Step 4: Add 20g of the Sb2O3-coated TiO2 composite particles obtained in Step 3 to 200mL of 50wt% ethanol aqueous solution, add 2g of γ-aminopropyltriethoxysilane, stir and activate for 2h, centrifuge and dry to obtain activated powder; disperse the activated powder in 200mL of xylene, add 8g of MAH-g-PE and react at 80℃ for 3h, centrifuge, wash and dry to obtain the modified infrared reflective filler C.

[0062] Example 1

[0063] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0064] 100 parts of polyethylene

[0065] 4 parts of dicumyl peroxide

[0066] Modified infrared reflective filler A, 15 parts

[0067] Antioxidant 1010 2 parts

[0068] 1 part calcium stearate

[0069] Light stabilizer 770 0.8 parts

[0070] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0071] Step 1: Mix polyethylene, modified infrared reflective filler A, dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 12 minutes to obtain a premix.

[0072] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0073] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0074] Example 2

[0075] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0076] 100 parts of polyethylene

[0077] 4 parts of dicumyl peroxide

[0078] Modified infrared reflective filler A, 20 parts

[0079] Antioxidant 1010 2 parts

[0080] 1 part calcium stearate

[0081] Light stabilizer 770 0.8 parts

[0082] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0083] Step 1: Mix polyethylene, modified infrared reflective filler A, dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 15 minutes to obtain a premix.

[0084] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0085] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0086] Example 3

[0087] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0088] 100 parts of polyethylene

[0089] 4 parts of dicumyl peroxide

[0090] Modified infrared reflective filler A, 25 parts

[0091] Antioxidant 1010 2 parts

[0092] 1 part calcium stearate

[0093] Light stabilizer 770 0.8 parts

[0094] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0095] Step 1: Mix polyethylene, modified infrared reflective filler A, dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 12 minutes to obtain a premix.

[0096] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0097] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0098] Comparative Example 1

[0099] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0100] 100 parts of polyethylene

[0101] 4 parts of dicumyl peroxide

[0102] Modified infrared reflective filler A, 8 parts

[0103] Antioxidant 1010 2 parts

[0104] 1 part calcium stearate

[0105] Light stabilizer 770 0.8 parts

[0106] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0107] Step 1: Mix polyethylene, modified infrared reflective filler A, dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 12 minutes to obtain a premix.

[0108] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0109] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0110] Comparative Example 2

[0111] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0112] 100 parts of polyethylene

[0113] 4 parts of dicumyl peroxide

[0114] Modified infrared reflective filler A 30 parts

[0115] Antioxidant 1010 2 parts

[0116] 1 part calcium stearate

[0117] Light stabilizer 770 0.8 parts

[0118] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0119] Step 1: Mix polyethylene, modified infrared reflective filler A, dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 12 minutes to obtain a premix.

[0120] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0121] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0122] Comparative Example 3

[0123] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0124] 100 parts of polyethylene

[0125] 4 parts of dicumyl peroxide

[0126] Modified infrared reflective filler B, 15 parts

[0127] Antioxidant 1010 2 parts

[0128] 1 part calcium stearate

[0129] Light stabilizer 770 0.8 parts

[0130] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0131] Step 1: Mix polyethylene, modified infrared reflective filler B, dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 12 minutes to obtain a premix.

[0132] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0133] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0134] Comparative Example 4

[0135] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0136] 100 parts of polyethylene

[0137] 4 parts of dicumyl peroxide

[0138] Modified infrared reflective filler C, 15 parts

[0139] Antioxidant 1010 2 parts

[0140] 1 part calcium stearate

[0141] Light stabilizer 770 0.8 parts

[0142] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0143] Step 1: Mix polyethylene, modified infrared reflective filler C, dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 12 minutes to obtain a premix.

[0144] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0145] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0146] Comparative Example 5

[0147] An infrared-reflective cross-linked polyethylene sheath material, by weight, is composed of the following raw materials:

[0148] 100 parts of polyethylene

[0149] 4 parts of dicumyl peroxide

[0150] SnO2 / Sb2O3 coated TiO2 composite particles (Preparation Example 1, Step 3) 15 parts

[0151] Antioxidant 1010 2 parts

[0152] 1 part calcium stearate

[0153] Light stabilizer 770 0.8 parts

[0154] The preparation method of the above-mentioned infrared reflective cross-linked polyethylene sheath material includes the following steps:

[0155] Step 1: Mix polyethylene, SnO2 / Sb2O3-coated TiO2 composite particles (Step 3 of Preparation Example 1), dicumyl peroxide, calcium stearate, antioxidant 1010 and light stabilizer 770 for 12 min to obtain a premix.

[0156] Step 2: The premixed material is fed into a twin-screw extruder for melt extrusion, followed by water ring pelletizing and drying to obtain crosslinkable granules; the crosslinkable granules are placed in a flat vulcanizing machine and vulcanized and crosslinked at 175°C and 10MPa pressure for 15 minutes to obtain infrared reflective crosslinked polyethylene sheath material.

[0157] The twin-screw extruder has a zone temperature of 125℃, a zone temperature of 135℃, a zone temperature of 140℃, a die temperature of 135℃, and a screw speed of 35 rpm.

[0158] Performance testing

[0159] The relevant properties of the infrared reflective cross-linked polyethylene sheath materials obtained in Examples 1-3 and Comparative Examples 1-5 were tested respectively, and the test methods are as follows:

[0160] 1) Tensile strength and elongation at break: Tensile strength and elongation at break were tested according to GB / T 1040.1-2018: The tensile rate was set to 20 mm / min; 5 parallel samples were tested for each group of specimens, and the arithmetic mean was taken after removing the maximum and minimum values.

[0161] 2) Near-infrared reflectance test: Prepare a 100×100×2mm experimental sample. Refer to the relative spectral method in Appendix A of JG / T 235-2014. Use an ultraviolet-visible-near-infrared spectrophotometer with an integrating sphere to test the spectral reflectance in the 780~2500 nm band. Calculate the near-infrared reflectance by weighting according to the relative spectral distribution of solar radiation specified in the standard. Test 5 parallel samples for each group of samples. Take the arithmetic mean after removing the maximum and minimum values.

[0162] 3) Material surface temperature difference test: A 100×100×2mm experimental sample was prepared. The sample was irradiated with an infrared lamp with a rated power of 250W for 50 minutes at a room temperature of 23℃ and a relative humidity of 50% for 30cm. The temperature difference of the sample surface before and after irradiation was measured. The results are shown in Table 1.

[0163] Table 1 Test Results

[0164]

[0165] As can be seen from the experimental results in Table 1, the infrared reflective cross-linked polyethylene sheath material prepared by the present invention has high mechanical properties, near-infrared reflectance and low surface temperature difference, and has broad application prospects in medium and low voltage cables.

[0166] Furthermore, comparing Comparative Examples 1-2 with Example 1, it is evident that the amount of modified infrared reflective filler used has a significant impact on the performance of the resulting infrared reflective cross-linked polyethylene sheath material. Both excessively low and excessively high amounts of modified infrared reflective filler are detrimental to obtaining a cross-linked polyethylene sheath material with both excellent mechanical properties and infrared reflective properties.

[0167] As can be seen from the comparison between Comparative Examples 3-4 and Example 1, SnO2 / Sb2O3 doping has a significant impact on improving the near-infrared reflectance of the infrared-reflective cross-linked polyethylene sheath material. SnO2 / Sb2O3 doping of TiO2 particles is more beneficial to improving the near-infrared reflectance of the infrared-reflective cross-linked polyethylene sheath material than using SnO2 or Sb2O3 alone.

[0168] As can be seen from the comparison between Comparative Example 5 and Example 1, the modification of SnO2 / Sb2O3-coated TiO2 composite particles by MAH-g-PE can further improve the mechanical properties and near-infrared reflective properties of infrared reflective cross-linked polyethylene sheath material.

[0169] The above embodiments are merely illustrative examples and are not intended to limit the implementation. Those skilled in the art will recognize that various variations and modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations. Therefore, any obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. An infrared-reflective cross-linked polyethylene sheath material, characterized in that, The raw materials, by weight, consist of the following components: 100 parts of polyethylene 3-6 parts of crosslinking agent 10-25 parts of modified infrared reflective filler 1-3 parts antioxidant Lubricant 0.5 to 1 part Light stabilizer 0.1 to 1 part The modified infrared reflective filler is a composite particle of rutile TiO2 co-doped with SnO2 / Sb2O3.

2. The infrared-reflective cross-linked polyethylene sheath material according to claim 1, characterized in that, The polyethylene is low-density polyethylene, and the melt index of the low-density polyethylene at 190°C and 2.16 kg is 1 to 5 g / 10 min.

3. The infrared-reflective cross-linked polyethylene sheath material according to claim 1, characterized in that, The crosslinking agent is selected from any one or a combination of two of dicumyl peroxide and bis-tert-butyl peroxide.

4. The infrared-reflective cross-linked polyethylene sheath material according to claim 1, characterized in that, The antioxidant is selected from any one or a combination of two or more of antioxidants 1010, 1076, 168, and 626.

5. The infrared-reflective cross-linked polyethylene sheath material according to claim 1, characterized in that, The lubricant is selected from any one or a combination of two of calcium stearate or polyethylene wax.

6. The infrared-reflective cross-linked polyethylene sheath material according to claim 1, characterized in that, The light stabilizer is selected from any one or a combination of two of hindered amine light stabilizer 770 and hindered amine light stabilizer 944.

7. The infrared-reflective cross-linked polyethylene sheath material according to claim 1, characterized in that, The preparation method of the modified infrared reflective filler includes the following steps: Step 1: Add 10-20 parts of rutile TiO2 powder, 100-300 parts of deionized water and 0.2-0.5 parts of ammonium polyacrylate dispersant to the reaction vessel, stir for 20-30 minutes to form a mixture; Step 2: Dissolve SnCl4·5H2O and SbCl3 in 1-3 mol / L hydrochloric acid to form composite solution A. Add composite solution A and 8-10 wt% sodium hydroxide solution dropwise to the mixture obtained in Step 1. Control the pH of the reaction system between 2 and 2.5 and the reaction temperature between 60 and 85℃. After the addition is complete, continue to keep the reaction at the temperature for 2-3 hours. Then cool down, filter, wash, and dry to obtain product A. Step 3: Calcine product A in air at 500-700℃ for 1-2 hours to obtain SnO2 / Sb2O3 coated TiO2 composite particles; Step 4: Add 20-30 parts of the SnO2 / Sb2O3-coated TiO2 composite particles obtained in Step 3 to 90-300 parts of a 50wt% ethanol aqueous solution, add 2-3 parts of γ-aminopropyltriethoxysilane, stir and activate for 2-3 hours, centrifuge and dry to obtain activated powder; disperse the activated powder in 100-300 mL of xylene, add 5-10 parts of MAH-g-PE and react at 80-90℃ for 2-4 hours, centrifuge, wash and dry to obtain the modified infrared reflective filler.

8. The infrared-reflective cross-linked polyethylene sheath material according to claim 7, characterized in that, The rutile TiO2 powder has a particle size of 0.2–0.5 μm.

9. The infrared-reflective cross-linked polyethylene sheath material according to claim 7, characterized in that, The molar ratio of SnCl4·5H2O to SbCl3 is 10:1 to 2.

10. A medium- and low-voltage cable, characterized in that, The sheath of the medium and low voltage cable is a double-layer co-extruded structure, wherein the inner layer of the double-layer co-extruded structure is conventional cross-linked polyethylene sheath material, and the outer layer of the double-layer co-extruded structure is the infrared-reflective cross-linked polyethylene sheath material as described in any one of claims 1 to 9.